Pillar-shaped semiconductor device and its manufacturing method
The manufacturing method for columnar semiconductor devices stabilizes gate and channel lengths in SGTs, addressing variations and enhancing performance and reliability in semiconductor devices.
Patent Information
- Application Number
- JP2022569328
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-14
AI Technical Summary
Variations in gate length and effective channel length in Surrounding Gate Transistors (SGTs) lead to inconsistencies in device characteristics and malfunctions, hindering high integration and performance in semiconductor devices.
A method for manufacturing columnar semiconductor devices involving precise control of gate insulating and conductor layers through masking, oxidation, and ion implantation to stabilize the gate length and channel length, using semiconductor pillars with controlled impurity regions and insulating layers.
This method reduces variations in transistor characteristics, enabling higher integration, lower power consumption, and improved reliability of SGT-based circuits.
Smart Images

Figure 0007565627000001 
Figure 0007565627000002 
Figure 0007565627000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a pillar-shaped semiconductor device and a method for manufacturing the same. [Background technology]
[0002] In recent years, three-dimensional structure transistors have been used in LSI (Large Scale Integration). Among them, the pillar-shaped semiconductor device SGT (Surrounding Gate Transistor) has attracted attention as a semiconductor element that provides highly integrated semiconductor devices. Furthermore, there is a demand for semiconductor devices with SGTs to be further integrated and have higher performance.
[0003] In a normal planar MOS transistor, the channel extends horizontally along the upper surface of the semiconductor substrate. In contrast, the channel of an SGT extends vertically relative to the upper surface of the semiconductor substrate (see, for example, Patent Document 1 and Non-Patent Document 1). Therefore, compared to a planar MOS transistor, an SGT can achieve a higher density semiconductor device.
[0004] 13 shows a schematic structure of an N-channel SGT. When one serves as a source, the other serves as a drain at the upper and lower positions of a Si pillar 220 (hereinafter, a silicon semiconductor pillar is referred to as an "Si pillar") having a P-type or i-type (intrinsic) conductivity. + The layers 221a and 221b (hereinafter, the semiconductor regions containing a high concentration of donor impurities are referred to as “N + The source and drain regions are called "N + The portion of the Si pillar 220 between the layers 221a and 221b becomes a channel region 222. A gate insulating layer 223 is formed to surround the channel region 222. A gate conductor layer 224 is formed to surround the gate insulating layer 223. In the SGT, N +The layers 221a and 221b, the channel region 222, the gate insulating layer 223, and the gate conductor layer 224 are formed in a columnar shape as a whole. Therefore, in a plan view, the area occupied by the SGT is approximately equal to the area of a single source or drain N + This corresponds to the occupied area of the layer. Therefore, a circuit chip with an SGT can achieve a further reduction in chip size compared to a circuit chip with a planar MOS transistor. In addition, if the driving capability of the SGT can be improved, the number of SGTs used per chip can be reduced, which also contributes to a reduction in chip size.
[0005] However, as mentioned above, there are problems associated with the vertical structure of SGT, which is advantageous for high integration. In a conventional transistor with a planar structure, the gate length and effective channel length are determined mainly by the accuracy of photolithography, but in an SGT, they are determined mainly by the film formation variation and the processing accuracy of etching and CMP. With regard to the precision of photolithography, recent advances in exposure equipment and resist materials have made it possible to achieve nano-order precision, but on the other hand, when it comes to film formation, etching, and CMP, particularly when forming and processing thick material layers, the precision of the film thickness, etching amount, and CMP polishing amount has not yet reached the nano-order level. For this reason, in SGT, a major issue is how to reduce the variations in gate length and effective channel length.
[0006] FIG. 14 shows a circuit diagram of an SRAM cell (Static Random Access Memory). This SRAM cell circuit includes two inverter circuits. One inverter circuit is composed of a P-channel SGT_Pc1 as a load transistor and an N-channel SGT_Nc1 as a drive transistor. The other inverter circuit is composed of a P-channel SGT_Pc2 as a load transistor and an N-channel SGT_Nc2 as a drive transistor. The gate of the P-channel SGT_Pc1 is connected to the gate of the N-channel SGT_Nc1. The drain of the P-channel SGT_Pc2 is connected to the drain of the N-channel SGT_Nc2. The gate of the P-channel SGT_Pc2 is connected to the gate of the N-channel SGT_Nc2. The drain of the P-channel SGT_Pc1 is connected to the drain of the N-channel SGT_Nc1.
[0007] As shown in FIG. 14, the sources of the P-channel SGT_Pc1 and Pc2 are connected to the power supply terminal Vdd. The sources of the N-channel SGT_Nc1 and Nc2 are connected to the ground terminal Vss. The selection N-channel SGT_SN1 and SN2 are arranged on both sides of the two inverter circuits. The gates of the selection N-channel SGT_SN1 and SN2 are connected to the word line terminal WLt. The source and drain of the selection N-channel SGT_SN1 are connected to the drains of the N-channel SGT_Nc1 and P-channel SGT_Pc1 and the bit line terminal BLt. The source and drain of the selection N-channel SGT_SN2 are connected to the drains of the N-channel SGT_Nc2 and P-channel SGT_Pc2 and the inverted bit line terminal BLRt. In this way, the circuit having the SRAM cell is composed of a total of six SGTs consisting of two P-channel SGT_Pc1 and Pc2 and four N-channel SGT_Nc1, Nc2, SN1, and SN2 (see, for example, Patent Document 2). In addition, multiple drive transistors can be connected in parallel to increase the speed of the SRAM circuit. Normally, the SGTs that make up the memory cells of an SRAM are formed in different semiconductor pillars. An important factor for stable operation and high quality of SRAM cell circuits is to suppress operational variations and malfunctions of individual SGTs. This is also true for other circuit formations that use SGTs. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 2-188966 [Patent Document 2] US Patent Application Publication No. 2010 / 0219483 [Patent Document 3] US Registration No. US8530960B2 [Non-patent literature]
[0009] [Non-Patent Document 1] Hiroshi Takato, Kazumasa Sunouchi, Naoko Okabe, Akihiro Nitayama, Katsuhiko Hieda, Fumio Horiguchi, and Fujio Masuoka: IEEE Transaction on Electron Devices, Vol.38, No.3, pp.573-578 (1991) [Non-Patent Document 2] CYTing, VJVivalda, and HGSchaefer: “Study of planarized sputter-deposited SiO2”, J.Vac.Sci. Technol. 15(3), pp1105-1112, May / June (1978) [Non-Patent Document 3] A.Raley, S.Thibaut, N. Mohanty, K. Subhadeep, S. Nakamura, etal. : “Self-aligned quadruple patterning integration using spacer on spacer pitch splitting at the resist level for sub-32nm pitch applications” Proc. Of SPIE Vol.9782, 2016 Summary of the Invention [Problem to be solved by the invention]
[0010] In circuits using SGTs, variations in gate length and effective channel length cause characteristic variations and operational failures. [Means for solving the problem]
[0011] A method for manufacturing a pillar-shaped semiconductor device according to an aspect of the present invention includes: an SGT having, on an upper portion of a substrate, a semiconductor pillar, a gate insulating layer surrounding the semiconductor pillar, a gate conductor layer surrounding the gate insulating layer, a first impurity region connected to a lower portion of the semiconductor pillar, and a second impurity region connected to a top portion of the semiconductor pillar, the semiconductor pillar between the first impurity region and the second impurity region serving as a channel; In the manufacture of a pillar-shaped semiconductor device having forming the first impurity region containing a donor or acceptor impurity on a surface of the substrate; forming the semiconductor pillar on the first impurity region; applying a first mask material layer over the entire surface; anisotropically etching the first mask material layer to leave the first mask material layer on the sidewall of the semiconductor pillar and to expose a surface of the first impurity region; a step of thermally or chemically oxidizing the entire surface to form a first insulating layer on the exposed surface of the first impurity region; removing the first mask material layer remaining on the sidewalls of the semiconductor pillars by isotropic etching; forming the gate insulating layer surrounding the semiconductor pillar and the gate conductor layer surrounding the gate insulating layer; forming the second impurity region at a top of the semiconductor pillar; having It is characterized by:
[0012] In the above-mentioned manufacturing method, It is desirable that the thickness of the first insulating layer is set so that the thickness of the first insulating layer is thicker than the thickness of the gate insulating layer, and so that the position of the lower end of the gate conductor layer is located at the same position as or lower than the upper end position of the first impurity region in the semiconductor pillar.
[0013] In the above-mentioned manufacturing method, It is desirable that the thickness of the first mask material layer is less than twice the thickness of the gate insulating layer.
[0014] In the above-mentioned manufacturing method, It is preferable that the method further includes a step of, after anisotropically etching the first mask material layer, injecting at least one of oxygen ions and an impurity having the same conductivity type as the first impurity region into the exposed surface of the first impurity region by ion implantation.
[0015] In the above-mentioned manufacturing method, After forming the first insulating layer, it is desirable to inject an impurity having the same conductivity type as the first impurity region into the entire region by ion implantation with energy sufficient to inject the impurity into the region below the first insulating layer.
[0016] In the above-mentioned manufacturing method, The method further includes the step of forming a semiconductor layer by selective epitaxial growth on the exposed surface of the substrate after anisotropically etching the first mask material layer, The step of forming the first insulating layer desirably includes thermally or chemically oxidizing the semiconductor layer as a whole to form the first insulating layer on the exposed surface of the substrate.
[0017] In the above-mentioned manufacturing method, It is desirable that the oxide film growth rate of the semiconductor layer by thermal or chemical oxidation is higher than the oxide film growth rate of the first impurity region by thermal or chemical oxidation.
[0018] In the above-mentioned manufacturing method, It is preferable that the semiconductor layer is doped with an impurity of the same conductivity type as that of the first impurity region during epitaxial growth.
[0019] In the above-mentioned manufacturing method, After the semiconductor layer is formed, it is preferable to implant at least one of oxygen ions and an impurity having the same conductivity type as the first impurity region into the entire semiconductor layer by ion implantation.
[0020] In the above-mentioned manufacturing method, After the semiconductor layer is formed, the semiconductor layer is thermally or chemically oxidized to convert the entire semiconductor layer into an oxide film, thereby forming the first insulating film having a desired film thickness. layer It is preferable that the thickness of the semiconductor layer is set so that the above-mentioned can be formed.
[0021] A method for manufacturing a pillar-shaped semiconductor device according to another aspect of the present invention includes the steps of: an SGT having, on an upper portion of a substrate, a semiconductor pillar, a gate insulating layer surrounding the semiconductor pillar, a gate conductor layer surrounding the gate insulating layer, a first impurity region connected to a lower portion of the semiconductor pillar, and a second impurity region connected to a top portion of the semiconductor pillar, the semiconductor pillar between the first impurity region and the second impurity region serving as a channel; In the manufacture of a pillar-shaped semiconductor device having forming a second mask material layer on the semiconductor pillar and on the top of the semiconductor pillar over the first impurity region; forming the gate insulating layer surrounding the semiconductor pillar; forming the gate conductor layer surrounding the gate insulating layer; covering the entire surface with a second insulating layer to a thickness greater than the height of the surface of the second mask material layer; polishing and planarizing the second insulating layer so that a surface of the second mask material layer is exposed; removing the exposed second mask material layer to expose tops of the semiconductor pillars; forming the second impurity region on the exposed top of the semiconductor pillar; having It is characterized by:
[0022] In the above-mentioned manufacturing method, It is preferable that the thickness of the second mask material layer is set so that the upper end of the gate conductor layer is located at the same position as or higher than the lower end of the second mask material layer.
[0023] In the above-mentioned manufacturing method, It is desirable to form a third masking material layer on top of the semiconductor pillar and the second masking material layer on top of that.
[0024] In the above-mentioned manufacturing method, It is preferable that the thicknesses of the first and third mask material layers are set so that the lower end of the third mask material layer is located at the same position as or lower than the upper end position of the gate conductor layer.
[0025] A method for manufacturing a pillar-shaped semiconductor device according to yet another aspect of the present invention includes the steps of: an SGT having, on an upper portion of a substrate, a semiconductor pillar, a gate insulating layer surrounding the semiconductor pillar, a gate conductor layer surrounding the gate insulating layer, a first impurity region connected to a lower portion of the semiconductor pillar, and a second impurity region connected to a top portion of the semiconductor pillar, the semiconductor pillar between the first impurity region and the second impurity region serving as a channel; In the manufacture of a pillar-shaped semiconductor device having forming the first impurity region containing a donor or acceptor impurity on a surface of the substrate; forming a second mask material layer on the semiconductor pillar and on the top of the semiconductor pillar on the first impurity region; applying a first mask material layer over the entire surface; anisotropically etching the first mask material layer to leave the first mask material layer on the sidewalls of the semiconductor pillars and to leave the second mask material layer on the tops of the semiconductor pillars in a plan view, while exposing a surface of the first impurity region in an area other than the semiconductor pillars; a step of thermally or chemically oxidizing the entire surface of the first impurity region to form a first insulating layer on the exposed surface of the first impurity region; removing the first mask material layer remaining on the sidewalls of the semiconductor pillars by isotropic etching; forming the gate insulating layer surrounding the semiconductor pillar and the gate conductor layer surrounding the gate insulating layer; A second insulating film is formed on the entire surface with a thickness greater than the height of the semiconductor pillar. layer and coating the The second insulating layer is formed so that the second mask material layer on the top of the semiconductor pillar is exposed. layer and polishing and planarizing the surface. removing the exposed second mask material layer to expose tops of the semiconductor pillars; forming the second impurity region on the exposed top of the semiconductor pillar; having It is characterized by: [Brief description of the drawings]
[0026] [Figure 1A] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1B] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1C] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1D] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1E] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1F] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1G] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1H] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1I] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1J]1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1K] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1L] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Figure 1M] 1A and 1B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a first embodiment. [Diagram 2] 10A and 10B are a cross-sectional structural view and an enlarged view of a main portion for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a second embodiment of the present invention. [Diagram 3] 13A and 13B are a cross-sectional structural view and an enlarged view of a main portion for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a third embodiment of the present invention. [Figure 4] 13A to 13C are cross-sectional structural views illustrating a method for manufacturing a pillar-shaped semiconductor device having an SGT according to a fourth embodiment of the present invention. [Diagram 5] 13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a fifth embodiment of the present invention. [Figure 6A] 13A and 13B are plan views and cross-sectional structural views for explaining a method for manufacturing a pillar-shaped semiconductor device having an SGT according to the sixth, seventh and eighth embodiments of the present invention. [Figure 6B] 13A and 13B are plan views and cross-sectional structural views for explaining a method for manufacturing a pillar-shaped semiconductor device having an SGT according to the sixth, seventh and eighth embodiments of the present invention. [Figure 7] 13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a ninth embodiment of the present invention. [Figure 8] 13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a tenth embodiment of the present invention. [Figure 9A]13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to an eleventh embodiment of the present invention. [Figure 9B] 13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to an eleventh embodiment of the present invention. [Figure 9C] 13A and 13B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to an eleventh embodiment of the present invention. [Figure 10] 23A and 23B are a cross-sectional structural view and an enlarged view of a main portion for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a twelfth embodiment of the present invention. [Figure 11A] 23A and 23B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a thirteenth embodiment of the present invention. [Figure 11B] 23A and 23B are a plan view and a cross-sectional structural view for explaining a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a thirteenth embodiment of the present invention. [Figure 12] 23A and 23B are a cross-sectional structural view and an enlarged view of a main portion, illustrating a manufacturing method of a pillar-shaped semiconductor device having an SGT according to a fourteenth embodiment of the present invention. [Figure 13] FIG. 1 is a schematic structural diagram showing a conventional SGT. [Figure 14] FIG. 1 is a circuit diagram of an SRAM cell using a conventional SGT. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, a method for manufacturing a pillar-shaped semiconductor device according to an embodiment of the present invention will be described with reference to the drawings.
[0028] (First embodiment) 1A to 1M, a method for manufacturing an SGT according to a first embodiment of the present invention, for example, an N-type transistor, will be described below, in which (a) is a plan view, (b) is a cross-sectional view taken along line XX' in (a), and (c) is a cross-sectional view taken along line YY' in (a).
[0029] On the P layer 1 (which is an example of the "substrate" in the claims), + The layer 2 (an example of a "first impurity region" in the claims) and the i-layer 6 (an example of a "semiconductor pillar" in the claims) are formed by epitaxial crystal growth, and then, as shown in FIG. 1A, a mask material layer 7 (an example of a "second mask material layer" in the claims) of SiN, a mask semiconductor layer 8 of silicon germanium (SiGe), a SiO 2 Then, a mask semiconductor layer 9 is deposited in this order. The i-layer 6 may be made of N-type or P-type Si containing a small amount of donor or acceptor impurity atoms.
[0030] Next, the mask semiconductor layer 9 is etched using a resist layer (not shown) that is circular or rectangular in plan view and is formed by lithography as a mask. 2 Using the mask semiconductor layer 9 as an etching mask, etching is performed, for example, by RIE (Reactive Ion Etching) to form a circular or rectangular mask semiconductor layer 9. Next, using the circular or rectangular mask semiconductor layer 9 as a mask, the SiGe mask semiconductor layer 8 is etched, for example, by the RIE method to form a circular or rectangular SiGe mask semiconductor layer 8 as shown in FIG. 1B. 2 The mask semiconductor layer 9 may be removed before etching the SiGe mask semiconductor layer 8, or may be left remaining.
[0031] Next, the aforementioned SiO 2 Using the mask semiconductor layer 9 and the SiGe mask semiconductor layer 8 as an etching mask, etching is performed successively by, for example, RIE to form a circular or rectangular mask material layer 7 and an i-layer 6 as shown in FIG. 1C, and the mask semiconductor layer 9 and the SiGe layer 8 remaining on the mask material layer 7 are removed. 2 The mask semiconductor layer 9 and the SiGe mask semiconductor layer 8 may be left as they are without being removed.
[0032] Next, as shown in FIG. 1D, an oxidation-resistant mask material layer 21 (one example of the "first mask material layer" in the claims), for example a SiN layer, is formed by ALD to cover the entire surface.
[0033] Next, a resist layer (not shown) formed by lithography is used as a mask to pattern the transistor operating region and insulating region, and the mask material layer 21 and the substrate present in the insulating region that is the resist opening are etched by RIE. Next, after removing the photoresist, the whole is covered with SiO 2 Next, the entire surface is etched by a CMP method using a SiO 2 The layer 23 is polished so that the upper surface of the layer 23 is at the upper surface of the mask material layer 7 present on the semiconductor pillars. Then, as shown in FIG. 1E, a SiO 2 The layer 23 is etched back so that the upper surface of the layer 23 is at the same level as the upper surface of the mask material layer 21, thereby forming an inter-element insulating region.
[0034] Next, as shown in FIG. 1F, mask material layer 21 is etched by RIE to leave mask material layer 21 on the sidewalls of the semiconductor pillars and to expose mask material layer 7 on the tops of the semiconductor pillars and the substrate surface in plan view.
[0035] Next, as shown in FIG. 1G, an oxide film 100 (an example of the "first insulating layer" in the claims) is thermally or chemically formed on the surface of the substrate.
[0036] Next, as shown in FIG. 1H, the mask material layer 21 is isotropically etched to remove the mask material layer 21 remaining on the side walls of the semiconductor pillars.
[0037] Next, the whole is covered with a HfO2 layer 24 (an example of a "gate insulating layer" in the claims), a TiN layer 26 (an example of a "gate conductor layer" in the claims), and a W layer 25 (an example of a "gate conductor layer" in the claims), and the whole is polished by a CMP method so that the upper surface of the W layer 25 is positioned at the upper surface of the mask material layer 7 present on the semiconductor pillar. Then, as shown in FIG. 1I, the W layer 25 planarized by the RIE method is etched back so as to be separated from the top of the semiconductor pillar 6, and the HfO 2 The layer 24 and the TiN layer 26 are removed by isotropic etching.
[0038] Next, using a resist layer (not shown) formed by lithography as a mask, the W layer 25 and the TiN layer 26 are etched by RIE to pattern the gate conductor layer, and then the entire structure is covered with an interlayer insulating film 27 (an example of a "second insulating layer" in the claims), and the entire structure is polished by CMP so that the upper surface of the interlayer insulating film 27 becomes the upper surface of the semiconductor pillar, as shown in Figure 1J.
[0039] Next, the top of the semiconductor pillar 6 exposed on the surface in plan view is recess-etched so that the top surface is recessed relative to the surface of the interlayer insulating layer 27, and as shown in FIG. 1K, N doped with donor impurities is formed on the exposed top of the semiconductor pillar 6 by selective epitaxial crystal growth. + A layer 29 (which is an example of the "second impurity region" in the claims) is formed.
[0040] Next, the whole is covered with an interlayer insulating film layer 30, and polished and flattened by the CMP method. Next, using a resist layer (not shown) formed by the lithography method as a mask, N + The interlayer insulating film layer 30 on the layer 29 is etched and removed. Next, a TiN layer (not shown) and a W layer 33 are coated so as to cover the entire structure, and the entire structure is polished by the CMP method so that the upper part of the interlayer insulating film 30 is exposed, as shown in FIG. 1L. In addition, this process is SiO 2Prior to the layer 30, a TiN layer (not shown) and a W layer 33 are coated, and then the N + After leaving the TiN layer and W layer so as to contact at least a part of the layer 29, the entire surface is covered with SiO 2 Alternatively, the layer 30 may be coated and the entire surface polished by CMP until the surface of the W layer is exposed.
[0041] Next, the whole is covered with SiO 2 Layer 35 is formed. + A source or drain wiring metal layer X1 is formed through a contact hole C1 formed on the layer 2. Next, a SiO 2 Then, a word wiring metal layer X2 is formed through a contact hole C2 formed on the W layer 25. Next, a SiO 2 1M, a source or drain wiring metal layer X3 is formed through a contact hole C3 formed on the W layer 33. This completes the creation of the N-type transistor of the SGT.
[0042] In addition, N shown in Figure 1E + Layer 2, N shown in Figure 1K + In the layer 29, the donor impurities are diffused by a heat treatment after the formation, and a donor impurity region is formed inside the semiconductor pillar 6. + Similarly, when formed as a layer, the acceptor impurities diffuse, and an acceptor impurity region is formed inside the semiconductor pillar 6 as well.
[0043] When trying to increase speed and reduce power consumption in circuits that use SGT, efforts are made to reduce the channel length of the transistor and the parasitic capacitance, such as the capacitance between the gate and the substrate. Assignment 1. When the channel length of a transistor is reduced, the short channel effect becomes prominent, causing variations in the transistor characteristics due to the variations in the channel length and a decrease in the transistor breakdown voltage. Task 2. In the SGT structure, the parasitic capacitance between the gate and the substrate can be reduced by forming a thick insulating film between the gate electrode and the substrate directly below the gate electrode. However, depending on the method of formation, variations in the gate length can occur, causing malfunctions.
[0044] The manufacturing method according to the first embodiment has the following features to address the above problems. 1. The mask material layers 7 and 21 having oxidation resistance are left on the top and side walls of the semiconductor pillar 6 before the gate insulating layer and the gate electrode are formed, and the other N + In the region where the surface of layer 2 is exposed, an insulating film 100 can be selectively and controllably formed by a thermal or chemical oxidation method, and the lower end of the gate electrode formed thereon can be formed at the desired position without variation. 2. In this embodiment, an example in which the present invention is applied to an N-type transistor has been described. + Layer 2, N shown in Fig. 1K onwards + Layer 29 P + By forming a layer, a P-type transistor can be formed. 3. In addition, since both N-type and P-type transistors can be easily created using the present invention, it can be used not only for logic but also for memories such as SRAM and Flash. Furthermore, in this embodiment, a semiconductor pillar 6 is formed that is circular in plan view. The shape of part or all of this semiconductor pillar in plan view can be easily formed into a shape such as a circle, an ellipse, or a shape elongated in one direction. Also, in a logic circuit region formed away from the SRAM region, semiconductor pillars of different shapes in plan view can be formed in the logic circuit region according to the logic circuit design. This makes it possible to realize a high-performance, low-power consumption microprocessor circuit.
[0045] Second embodiment Hereinafter, a method for manufacturing an SGT according to a second embodiment of the present invention, for example, an N-type transistor, will be described with reference to Fig. 2. (a) is a cross-sectional view taken along line X-X' in Fig. 1G in the first embodiment, (c) is an enlarged view of the main part of this embodiment in (a), (b) is a cross-sectional view taken along line X-X' in Fig. 1M in the first embodiment, and (d) is an enlarged view of the main part of this embodiment in (b).
[0046] As shown in Figure 2(d), N + Top end position g of layer 2, HfO 2 The upper end of the layer 24, i.e., the lower end position of the gate electrode 25, is h. The position of g is not lower than h. membrane 1 When forming 00, as shown in (c), the insulating membrane 1 Set the film thickness f to 00.
[0047] This embodiment has the following features. 1. As shown in Figure 2, the insulation film By appropriately setting the thickness of 100, the gate electrode W layer 25, the TiN layer 26 and the N + The layers 2 overlap sufficiently in the vertical direction, making it possible to suppress characteristic defects and variations. 2. In addition, the insulating layer is sufficiently thicker than the thickness of the gate insulating layer HfO2 layer 24. film Since it is possible to form a gate electrode having a gate insulating film 100, the parasitic capacitance between the substrate and the gate electrode is reduced, which contributes to the increase in speed and the reduction in power consumption of products using this structure.
[0048] Third embodiment Hereinafter, a method for manufacturing an SGT according to a third embodiment of the present invention, for example, an N-type transistor, will be described with reference to Fig. 3. (a) is a cross-sectional structural diagram taken along line XX' in Fig. 1G in the first embodiment, (c) is an enlarged view of the main part of this embodiment in (a), and (b) is a cross-sectional diagram of a gate insulator HfO 2 FIG. 1(d) shows an enlarged view of the main part of the present embodiment shown in FIG. 1(b).
[0049] A mask material layer 21 is left on the sidewall of the semiconductor pillar 6 in FIG. 3(a) by anisotropic etching, and then an insulating film In the step of forming 100, as shown in (c), the film thickness p of the mask material layer 21 remaining on the sidewall of the lower part of the semiconductor pillar 6 is approximately equal to the film thickness immediately after the formation of the mask material layer 21 in FIG. 1D of the first embodiment. Next, the remaining mask material layer 21 is removed by isotropic etching, and at that time, the lower part of the semiconductor pillar 6 and the insulating layer 21 are removed. film 100, a recess is generated between the gate insulating layer HfO 2 As shown in FIG. 3(d), the gate insulating layer HfO 2 In order to fill this recess with the thickness q of the layer 24, the thickness p of the mask material layer 21 is set to the thickness of the gate oxide film HfO 2 It is desirable to set the thickness to less than twice the thickness q of the layer 24 .
[0050] This embodiment has the following features. The lower part of the semiconductor pillar 6 and the insulating film The depressions that exist locally between 100 and the gate oxide film HfO 2 By filling the recess with layer 24, the gate electrode W layer 25 and TiN layer 26 can penetrate into the recess, suppressing a local increase in parasitic capacitance between the gate electrode and the semiconductor pillar, thereby contributing to higher speeds and lower power consumption of products using this structure.
[0051] (Fourth embodiment) Hereinafter, a method for manufacturing an SGT, for example, an N-type transistor, according to a fourth embodiment of the present invention will be described with reference to FIG. 4. FIG. 4 shows the manufacturing method of the SGT after the step of FIG. 1F in the first embodiment is completed. 4 1 shows the state in which the embodiment is implemented, where (a) is a plan view, (b) is a cross-sectional structural view taken along line XX' in (a), and (c) is a cross-sectional structural view taken along line YY' in (a).
[0052] As shown in FIG. 4, the mask material layer 21 is etched by the RIE method, so that the mask material layer 21 remains on the side walls of the semiconductor pillars, and the mask material layer 7 on the tops of the semiconductor pillars and the substrate surface are exposed in a plan view. The entire surface is then ionized with oxygen ions or N + An impurity having the same conductivity type as the impurity region of layer 2, or both, are implanted into the exposed surface layer of the substrate by ion implantation to form an impurity region layer 3.
[0053] The subsequent steps are the same as those in the first embodiment from FIG. 1G onwards.
[0054] This embodiment has the following features. Before forming the oxide film 100 thermally or chemically, oxygen or impurities of the same conductivity type are injected into the substrate surface on which the oxide film is to be formed, which significantly increases the oxide film growth rate and allows the oxide film to be formed at a low temperature and in a short time. Furthermore, if the oxidation is performed using an ozone thermal oxidation method, an even greater effect can be obtained. This suppresses the diffusion of impurities due to heat, and can suppress characteristic variations and voltage resistance defects.
[0055] Fifth embodiment Hereinafter, a method for manufacturing an SGT according to a fifth embodiment of the present invention, for example, an N-type transistor, will be described with reference to Fig. 5. Fig. 5 shows a state in which the fifth embodiment is carried out after the process shown in Fig. 1G in the first embodiment is completed, where (a) is a plan view, (b) is a cross-sectional structure view taken along line X-X' in (a), and (c) is a cross-sectional structure view taken along line Y-Y' in (a).
[0056] As shown in FIG. 5, an oxide film 100 is thermally or chemically formed on the surface of the substrate. + An impurity having the same conductivity type as the impurity region of layer 2 is implanted into the entire surface by ion implantation with energy sufficient to implant the impurity into the region under the first insulating layer, thereby forming an impurity region 200 .
[0057] The subsequent steps are the same as those in the first embodiment from FIG. 1H onwards.
[0058] This embodiment has the following features. When an oxide film 100 is thermally or chemically formed on the substrate surface, N + The impurity concentration of layer 2 becomes low, and the electrical resistance becomes high. film After forming 100, N + By injecting an impurity of the same conductivity type as the impurity region 2, the decrease in the impurity concentration is compensated for and an increase in electrical resistance is suppressed. At this time, the impurity may be injected into the top of the semiconductor pillar 6 through the mask material layer 7. However, if the N + When forming layer 29, the tops of semiconductor pillars 6 are not affected since they are removed by a recess etch.
[0059] (Sixth, Seventh and Eighth Embodiments) Hereinafter, a method for manufacturing an SGT according to the sixth, seventh and eighth embodiments of the present invention, for example, an N-type transistor, will be described with reference to Figures 6A and 6B. Figures 6A and 6B (a) are plan views, (b) are cross-sectional views taken along line X-X' in (a), and (c) are cross-sectional views taken along line Y-Y' in (a).
[0060] As shown in FIG. 6A, after the step of FIG. 1F in the first embodiment, a semiconductor layer 400 (which is an example of the "semiconductor layer" in the claims) is selectively formed by epitaxial growth on the exposed substrate surface.
[0061] Next, as shown in FIG. 6B, the semiconductor layer 400 is thermally and chemically oxidized and insulated. film At this time, the oxide film growth rate is N + By using a material larger than the impurity region 2, the oxide film can be formed at a low temperature and in a short time.
[0062] Furthermore, the semiconductor layer 400 is N + If the semiconductor layer is doped with impurities of the same conductivity type as the impurity region 2, the oxide film growth rate is further increased, and the oxide film can be formed at a low temperature in a short time.
[0063] The subsequent steps are the same as those in the first embodiment from FIG. 1I onwards.
[0064] This embodiment has the following features. 1. As shown in FIG. 6B, in order to selectively oxidize the epitaxially grown semiconductor layer, the upper end of the insulating film 100, which corresponds to the lower end position of the gate electrode, is made of N + This allows the semiconductor device to be set at a position sufficiently higher than the upper end of the impurity region 2, and the risk of an offset structure occurring, which is one of the causes of a significant deterioration in the characteristics of a transistor, is extremely reduced. 2. When forming the insulating film 100, the oxidation rate of the semiconductor layer 400 is increased to reduce the amount of N + Since the impurity region 2 is hardly oxidized, N + The impurity concentration of the impurity region 2 is not affected, and there is no variation in the transistor characteristics or deterioration in the driving capability, which can contribute to the increase in speed and the reduction in power consumption of products using this structure.
[0065] Ninth embodiment Hereinafter, a method for manufacturing an SGT, for example an N-type transistor, according to a ninth embodiment of the present invention will be described with reference to FIG. 7 1A is a plan view, FIG. 1B is a cross-sectional view taken along line X-X' in FIG. 1A, and FIG. 1C is a cross-sectional view taken along line Y-Y' in FIG.
[0066] In the step of FIG. 6A of the seventh embodiment, after the semiconductor layer 400 is selectively epitaxially grown, oxygen ions or N ions are implanted in the entire surface as shown in FIG. + The impurity of the same conductivity type as the impurity region of layer 2, or both, are implanted by ion implantation. ,half The ions are implanted with such energy that they remain in the conductor layer 400 film.
[0067] The subsequent steps are the same as those in the first embodiment from FIG. 1H onwards, via FIG. 6B.
[0068] This embodiment has the following features. 1. The semiconductor layer 400 is doped with oxygen ions and N + By ion-implanting at least one of the impurities having the same conductivity type as the impurity region of the layer 2, the semiconductor layer 400 can be oxidized at a low temperature and in a short time. Furthermore, if the oxidation is performed by an ozone thermal oxidation method, an even greater effect can be obtained. This makes it possible to suppress the diffusion of impurities due to heat, and to suppress characteristic variations, voltage resistance failure, and the like. 2. The semiconductor layer 400 is doped with oxygen ions and N + By ion-implanting at least one of the impurities having the same conductivity type as the impurity region of the layer 2, the oxide film growth rate of the semiconductor layer 400 is increased by N + It can be made even larger than impurity region 2, and N + Since the oxidation of the impurity region 2 can be suppressed, N + The impurity concentration of the impurity region 2 is not affected, and there is no variation in the transistor characteristics or deterioration in the driving capability, which can contribute to the increase in speed and the reduction in power consumption of products using this structure.
[0069] Tenth embodiment Hereinafter, a method for manufacturing an SGT according to a tenth embodiment of the present invention, for example, an N-type transistor, will be described with reference to Fig. 8. Fig. 8(a) is a plan view, (b) is a cross-sectional view taken along line X-X' in (a), and (c) is a cross-sectional view taken along line Y-Y' in (a).
[0070] In the process of FIG. 6B in the seventh embodiment, when the selectively epitaxially grown semiconductor layer 400 is thermally oxidized, as shown in FIG. 8, the semiconductor layer 400 is oxidized under conditions that change the entire semiconductor layer 400 into an insulating film 100, and the thickness of the semiconductor layer 400 is set so that the insulating film 100 has a desired thickness.
[0071] The subsequent steps are the same as those in the first embodiment from FIG. 1H onwards.
[0072] This embodiment has the following features. Semiconductor layer 400 and N +By utilizing the difference in the oxide film growth rate of the impurity region 2, it is possible to form the insulating film 100 by oxidizing only the semiconductor layer 400, and as a result, it is possible to form the thickness of the insulating film 100 with good controllability. This makes it possible to further suppress the variation in transistor characteristics.
[0073] Eleventh embodiment Hereinafter, the present invention will be described with reference to FIGS. 9A, 9B, and 9C. 11 An N-type transistor will be described as an example of a method for manufacturing an SGT according to an embodiment. In Figures 9A, 9B, and 9C, (a) is a plan view, (b) is a cross-sectional view taken along line X-X' in (a), and (c) is a cross-sectional view taken along line Y-Y' in (a).
[0074] 9A corresponds to Fig. 1J in the first embodiment, and after patterning the gate conductor layer, the entire structure is covered with an interlayer insulating film 27, and the entire structure is polished by CMP so that the upper surface of the interlayer insulating film 27 coincides with the upper surface of the SiN mask material layer 7. In this process, the SiN mask material layer 7 is used as a polishing stopper by CMP, so the thickness of the SiN mask material layer 7 is set in Fig. 1A. Next, as shown in FIG. 9B, the remaining SiN mask material layer 7 is removed by isotropic etching. Next, as shown in FIG. 9C, N doped with donor impurities is grown on the exposed top of the semiconductor pillar 6 by selective epitaxial crystal growth. + Layer 29 is formed. In this way, the SiN mask material layer 7 serves not only as a mask material layer for forming the semiconductor pillars 6 but also as a layer for removing impurities N from the top of the semiconductor pillars 6. + This film is also used to determine the position for forming layer 29. For this reason, when forming SiN mask material layer 7 in Fig. 1A, the film thickness is set to be thick enough to function as a stopper for polishing by the CMP method in Fig. 9A.
[0075] The subsequent steps are the same as those in the first embodiment from FIG. 1L onwards.
[0076] This embodiment has the following features. The SiN mask material layer 7 is used not only as a mask material layer for forming the semiconductor pillars 6 but also as a stopper when the interlayer insulating film 27 is polished by the CMP method, so that the impurity N on the top of the semiconductor pillars 6 is removed. + This reduces the variation in the position where layer 29 is formed, and as a result, reduces the variation in the length of semiconductor pillar 6, which corresponds to the channel length of the SGT, thereby making it possible to reduce the variation in transistor characteristics.
[0077] 1I to 1K in the first embodiment, the eleventh embodiment is carried out as described above, thereby making it possible to suppress variations in both the gate length and the channel length of the SGT. That is, in the first embodiment, as described above, the variation in the position of the bottom end of the gate electrode is suppressed, thereby suppressing variations in the gate length, while in the eleventh embodiment, the variation in the position of the top of the semiconductor pillar 6, which corresponds to the channel length, is suppressed, thereby suppressing variations in the channel length.
[0078] Twelfth embodiment Hereinafter, a method for manufacturing an SGT according to a twelfth embodiment of the present invention, for example, an N-type transistor, will be described with reference to FIG. 11 9A in an embodiment, (c) is an enlarged view of a main part of this embodiment in (a), (b) is a cross-sectional view of the first embodiment in (a) in an embodiment, (d) is an enlarged view of a main part of this embodiment in (b).
[0079] As shown in FIG. 10(d), the lower end position m of the impurity region 29, between layers The lower end of the insulating film 27, i.e., the upper end position of the gate electrode 25, is n, and so that the position of n is not lower than m, in the process of etching back the gate electrode 25 in FIG. 10(a) by the RIE method, the film thickness j of the mask material layer 7 present on the semiconductor pillar 6 is set to be larger than the film thickness k of the etching of the gate electrode W layer 25 and the TiN layer 26, as shown in (c).
[0080] This embodiment has the following features. 1. As shown in FIG. 10, by appropriately setting the film thickness of the mask material layer 7, the gate electrode W layer 25, the TiN layer (not shown), and the impurity N + The layer 29 overlaps the gate electrode sufficiently in the vertical direction and has a high conductivity. + This makes it possible to prevent electrical short circuits with the layer 29, and thus makes it possible to prevent characteristic defects and variations. 2. In addition, the thickness of the interlayer insulating film 27 on the gate electrode, which is determined by the thickness j of the mask material layer 7 and the thickness k of the gate electrode to be etched, can be formed to be sufficiently thicker than the thickness of the insulating layer HfO2 layer 24. + The parasitic capacitance between the layer 29 and the gate electrode 25 is reduced, which contributes to higher speed and lower power consumption of products using this structure.
[0081] Thirteenth embodiment Hereinafter, a method for manufacturing an SGT, for example an N-type transistor, according to a thirteenth embodiment of the present invention will be described with reference to FIGS. 11A and 11B. 11 A,Fig. 11 1B, (a) is a plan view, (b) is a cross-sectional view taken along line X-X' in (a), and (c) is a cross-sectional view taken along line Y-Y' in (a).
[0082] FIG. 11A corresponds to FIG. 1A in the first embodiment. In FIG. 11A, an i-layer 6 is formed on a substrate, and the i-layer 6 is made of, for example, SiO 2 a mask material layer 300 (an example of the "third mask material layer" in the claims), a mask material layer 7 of SiN, a mask semiconductor layer 8 of silicon germanium (SiGe), and a SiO 2 The mask semiconductor layer 9 is then deposited in sequence.
[0083] Next, as shown in FIG. 11B, which corresponds to FIG. 1C in the first embodiment, a silicon germanium (SiGe) layer 8, a SiO 2 Using the mask semiconductor layer 9 as a mask, the SiN layer 7, the mask material layer of the SiO2 layer 300, and the i-layer 6 are formed by RIE, and the SiGe layer 8 and the SiO 2 Layer 9 is removed.
[0084] The subsequent steps are the same as those in the first embodiment from FIG. 1D onwards.
[0085] This embodiment has the following features. In addition to the features of the third embodiment, a mask material layer 300 (e.g., a SiN layer) is provided between the semiconductor pillar 6 and the mask material layer 7 (e.g., a SiN layer). 2 By forming a layer, it is possible to reduce process damage to the top of the semiconductor pillar 6. Then, N containing donor impurities is formed on the top of the semiconductor pillar 6 by epitaxial crystal growth. + When forming the layer 29, it is possible to prevent damage to the top of the semiconductor pillar 6 from impeding crystal growth.
[0086] Fourteenth embodiment Hereinafter, a method for manufacturing an SGT according to the fourteenth embodiment of the present invention, for example, an N-type transistor, will be described with reference to Fig. 12. Fig. 12(a) corresponds to Fig. 1I in the first embodiment when the fourteenth embodiment is applied, and shows a cross-sectional structure diagram along line X-X', (c) shows an enlarged view of the main part of this embodiment of (a), (b) corresponds to Fig. 1M in the first embodiment, and shows a cross-sectional structure diagram along line X-X', and (d) shows an enlarged view of the main part of this embodiment of (b).
[0087] In the cross-sectional structure diagram after the process is completed in FIG. 12(b), as shown in (d), the lower end position t of the impurity region 29, between layers The lower end of the insulating film 27, i.e., the upper end position of the gate electrode 25, is u, and in the process of etching back the gate electrode 25 in FIG. 12(a) by the RIE method, the total film thickness r of the mask material layer 300 and the mask material layer 7 present on the semiconductor pillar 6 is set to be larger than the film thickness s of the etching of the gate electrode W layer 25 and the TiN layer (not shown), as shown in (c).
[0088] This embodiment has the following features. In addition to the features of the thirteenth embodiment, as shown in FIG. 12, by appropriately setting the film thicknesses of the mask material layers 300 and 7, the gate electrode W layer 25, the TiN layer (not shown), and the impurity N + The layer 29 overlaps the gate electrode sufficiently in the vertical direction and has a high conductivity. + This makes it possible to prevent electrical short circuits with the layer 29, and thus makes it possible to prevent characteristic defects and variations.
[0089] In the embodiment of the present invention, one SGT is formed in one semiconductor pillar, but the present invention can also be applied to a circuit formation in which two or more SGTs are formed. In the circuit formation in which two or more SGTs are formed, the SGT described in the present invention is the SGT located at the bottom of the semiconductor pillar.
[0090] In the first embodiment, the semiconductor pillars are made of Si, but may be made of other semiconductor materials, and this also applies to the other embodiments of the present invention.
[0091] In the first embodiment, the N + Layer 2 and N at the top of the semiconductor pillar + The layer 29 is a P + The layer may be made of silicon or other semiconductor material, as in other embodiments of the present invention.
[0092] In the first embodiment, N + The layer 29 was formed by selective epitaxial crystal growth, and N was grown on the top of the semiconductor pillar 6 by CDE (Chemical Dry Etching) and normal epitaxial crystal growth. + The method of forming the layer 29 may be modified in other ways. + layer 29 This also applies to the other embodiments of the present invention.
[0093] In the first embodiment, the mask material layer 7 on the top of the semiconductor pillar 6 and the mask material layer 21 on the periphery may be made of other material layers including organic or inorganic materials, which are made of a single layer or multiple layers, as long as the material is suitable for the purpose of the present invention. This also applies to the other embodiments of the present invention.
[0094] In the first embodiment, the mask material layer and the mask semiconductor layer are formed of a SiN layer 7, a silicon germanium (SiGe) layer 8, and a SiO 2 Although layer 9 is used, other material layers, including organic or inorganic materials, may be used in single or multiple layers as long as the materials are suitable for the purpose of the present invention, and this also applies to other embodiments of the present invention.
[0095] In the first embodiment, the materials of the various wiring metal layers X1, X2, and X3 may be not only metals but also conductive material layers such as alloys, semiconductor layers containing a large amount of acceptor or donor impurities, and may be configured as a single layer or a combination of multiple layers, which is the same in the other embodiments of the present invention.
[0096] In the first embodiment, as shown in FIG. 1I, a TiN layer 26 is used as the gate metal layer. The TiN layer 26 can be a single or multiple layer material layer as long as the material is suitable for the purpose of the present invention. The TiN layer 26 can be formed of a conductor layer such as a single or multiple metal layer having at least a desired work function. In this embodiment, a W layer is used on the outside and serves as a metal wiring layer, but a single or multiple metal layer other than the W layer may be used. In addition, the HfO2 layer 24 is used as the gate insulating layer, but other material layers each consisting of a single or multiple layers may be used. This is the same in other embodiments of the present invention.
[0097] In the first embodiment, the shape of the semiconductor pillar 6 in plan view is circular. However, the shape of part or all of the semiconductor pillar 6 in plan view can easily be circular, elliptical, elongated in one direction, or the like. This also applies to the other embodiments of the present invention.
[0098] In the first embodiment, the N + Layer 2 was formed. + An alloy layer such as a metal or silicide may be formed on the top surface of layer 2. + Instead of layers, P + The same applies when a layer is formed.
[0099] In the first embodiment, the SGT is formed on the P-layer substrate 1, but an SOI (Silicon On Insulator) substrate may be used instead of the P-layer substrate 1. Alternatively, a substrate made of another material may be used as long as it functions as a substrate. This also applies to the other embodiments of the present invention.
[0100] In the first embodiment, N + Tier 2 and N + Although the SGT in which the layer 29 constitutes the source and drain has been described, the present invention can also be applied to a tunnel-type SGT having a source and drain with different polarities, and the same is true for other embodiments of the present invention.
[0101] In the first embodiment, after the gate HfO2 layer 24 and the gate TiN layer 26 are formed, + Layer 29 was formed. + The gate HfO2 layer 24 and the gate TiN layer 26 may be formed after the layer 29 is formed. This also applies to the other embodiments of the present invention.
[0102] In addition, in a vertical NAND flash memory circuit, a semiconductor pillar is used as a channel, and memory cells each composed of a tunnel oxide layer, a charge storage layer, an interlayer insulating layer, and a control conductor layer surrounding the semiconductor pillar are formed in multiple stages in the vertical direction. The semiconductor pillars at both ends of these memory cells have a source line impurity layer corresponding to the source and a bit line impurity layer corresponding to the drain. In addition, if one of the memory cells on both sides of a memory cell serves as the source, the other serves as the drain. In this way, a vertical NAND flash memory circuit is one type of SGT circuit. Therefore, the present invention can also be applied to a mixed circuit with a NAND flash memory circuit.
[0103] Similarly, the present invention can be applied to inverters and logic circuits used inside and outside the memory cell region in magnetic memory circuits and ferroelectric memory circuits.
[0104] The present invention allows various embodiments and modifications without departing from the broad spirit and scope of the present invention. The above-described embodiment is for explaining one example of the present invention and does not limit the scope of the present invention. The above-described embodiments and modifications can be combined in any combination. Furthermore, even if some of the constituent elements of the above-described embodiment are omitted as necessary, the technical idea of the present invention will still be within the scope of the present invention. [Industrial Applicability]
[0105] According to the method for manufacturing a pillar-shaped semiconductor device of the present invention, variations in characteristics and operational failures are suppressed, contributing to improved quality of circuits and products using SGTs. [Explanation of symbols]
[0106] 1:P layer board 2:N + The N layer substrate and the lower part of the semiconductor pillar 6 + layer 6: i-layer 7, 21: SiN mask material layer 23, 27, 30, 35.37.39, 100:SiO 2 layer 24:HfO 2 layer 25, 33: W layer 26:TiN layer 29: N at the top of semiconductor pillar 6 + layer 200:N ++ layer 300:SiO 2 Mask material layer 400: Epitaxial semiconductor layer C1, C2, C3: Contact holes X1, X2, X3: Connection wiring metal layers f:SiO 2 Thickness of layer 100 g: N at the bottom of the semiconductor pillar 6 + Top position of layer 2 (height) h:HfO 2 The position (height) of the top end of the layer 24 or the bottom end of the gate electrode 25 j: thickness of the SiN mask material layer 7 k, s: Etching thicknesses of the gate electrode W layer 25 and the TiN layer 26 m, t: N at the top of the semiconductor pillar 6 + Bottom end position (height) of layer 29 n, u: SiO 2 The lower end of the layer 27 or the upper end position (height) of the gate electrode 25 and the TiN layer 26 p: thickness of the SiN mask material layer 21 q:HfO 2 Thickness of layer 24 r: SiN mask material layer 7 and SiO 2 Total thickness of the mask material layer 300
Claims
1. an SGT having, on an upper portion of a substrate, a semiconductor pillar, a gate insulating layer surrounding the semiconductor pillar, a gate conductor layer surrounding the gate insulating layer, a first impurity region connected to a lower portion of the semiconductor pillar, and a second impurity region connected to a top portion of the semiconductor pillar, the semiconductor pillar between the first impurity region and the second impurity region serving as a channel; In the manufacture of a pillar-shaped semiconductor device having forming the first impurity region containing a donor or acceptor impurity on a surface of the substrate; forming the semiconductor pillar on the first impurity region; covering the entire surface with a first mask material layer; anisotropically etching the first mask material layer to leave the first mask material layer on the sidewall of the semiconductor pillar and to expose a surface of the first impurity region; a step of thermally or chemically oxidizing the entire surface of the first impurity region to form a first insulating layer on the exposed surface of the first impurity region, the first insulating layer defining a lower end position of the gate conductor layer, separately from an inter-element insulating region; removing the first mask material layer remaining on the sidewalls of the semiconductor pillars by isotropic etching; forming the gate insulating layer surrounding the semiconductor pillar and the gate conductor layer surrounding the gate insulating layer; forming the second impurity region at the top of the semiconductor pillar; having 4. A method for manufacturing a pillar-shaped semiconductor device comprising the steps of:
2. the thickness of the first insulating layer is set so that the thickness of the first insulating layer is thicker than the thickness of the gate insulating layer, and the position of the lower end of the gate conductor layer is located at the same position as or lower than the upper end position of the first impurity region in the semiconductor pillar; 2. The method for manufacturing a pillar-shaped semiconductor device according to claim 1,
3. the first mask material layer has a thickness smaller than twice the thickness of the gate insulating layer; 2. The method for manufacturing a pillar-shaped semiconductor device according to claim 1,
4. the method further includes a step of, after anisotropically etching the first mask material layer, implanting at least one of oxygen ions and an impurity having the same conductivity type as the first impurity region into the exposed surface of the first impurity region by an ion implantation method.
2. The method for manufacturing a pillar-shaped semiconductor device according to claim 1,
5. After forming the first insulating layer, an impurity having the same conductivity type as the first impurity region is implanted into the entire region by an ion implantation method with energy sufficient to implant the impurity into the region under the first insulating layer.
2. The method for manufacturing a pillar-shaped semiconductor device according to claim 1,
6. The method further includes the step of forming a semiconductor layer by selective epitaxial growth on the exposed surface of the substrate after anisotropically etching the first mask material layer, The step of forming the first insulating layer includes forming the first insulating layer on the exposed surface of the substrate by thermally or chemically oxidizing the semiconductor layer as a whole.
2. The method for manufacturing a pillar-shaped semiconductor device according to claim 1,
7. an oxide film growth rate of the thermal or chemical oxidation of the semiconductor layer is greater than an oxide film growth rate of the thermal or chemical oxidation of the first impurity region; 7. The method for manufacturing a pillar-shaped semiconductor device according to claim 6.
8. The semiconductor layer is doped with an impurity of the same conductivity type as the first impurity region during epitaxial growth.
7. The method for manufacturing a pillar-shaped semiconductor device according to claim 6.
9. After forming the semiconductor layer, at least one of oxygen ions and an impurity having the same conductivity type as that of the first impurity region is implanted into the entire semiconductor layer by an ion implantation method.
7. The method for manufacturing a pillar-shaped semiconductor device according to claim 6.
10. the thickness of the semiconductor layer is set so that the first insulating layer having a desired thickness can be formed by thermally or chemically oxidizing the semiconductor layer after the semiconductor layer is formed so that the entire semiconductor layer is converted into an oxide film; 7. The method for manufacturing a pillar-shaped semiconductor device according to claim 6.
Citation Information
Patent Citations
Semiconductor device and manufacture thereof
JP1990148852A
MOS semiconductor device
JP1990188966A
Manufacture of semiconductor device
JP1995045715A
Manufacturing method of semiconductor device
JP2013026382A
Method for forming a semiconductor device with reduced VFET bottom contact resistance and semiconductor device
JP2020520110A