Improved Film Stack Overlay for 3D NAND Applications
By employing a substrate support and showerhead with tailored curvature and controlled plasma density, the method addresses film stress non-uniformity, reducing overlay errors and enhancing the uniformity of film layers in semiconductor manufacturing.
Patent Information
- Application Number
- JP2021529279
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-30
- Filing Date
- 2019-11-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-11-08
AI Technical Summary
The challenge in manufacturing vertically integrated devices is reducing substrate and layer stack distortion due to film stress non-uniformity during plasma etching or deposition processes, leading to local deformation and undesirable overlay errors.
A method involving the use of a substrate support and showerhead with specific curvature profiles, combined with controlled plasma density and RF power application, to minimize film stress variation and in-plane distortion during deposition processes.
This approach results in consistent film stress across the substrate, minimizing overlay errors and ensuring uniformity of film layers, thereby improving the manufacturing precision of semiconductor devices.
Smart Images

Figure 0007565918000001 
Figure 0007565918000002 
Figure 0007565918000003
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE
[0001] Embodiments of the present disclosure generally relate to processing chambers and methods for reducing film stack overlay problems caused by film stress non-uniformity during substrate processing. [Background technology]
[0002]
[0002] A long-recognized challenge in manufacturing vertically integrated devices is to reduce distortion of the substrate and layer stack introduced during the manufacturing process. Due to thermal expansion, plasma non-uniformity distribution, and / or plasma density difference during plasma etching or plasma deposition process, various film stresses may be created between one layer and the next, resulting in local deformation of the substrate surface and undesirable overlay errors. When overlay errors occur, the size, dimensions, or structure of the device die formed on the substrate may be irregularly deformed or distorted, thus increasing the possibility of mismatch between the film layers stacked thereon, which may disadvantageously increase the possibility of mismatch in the subsequent manufacturing process. Summary of the Invention
[0003] In one embodiment, a method for forming a film layer on a substrate is provided, the method includes: positioning the substrate on a substrate support in a processing chamber; flowing a deposition gas mixture including a silicon-containing gas and a reactive gas into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to a stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically arranged around a center point of the showerhead; and performing a deposition process while rotating the substrate to deposit a thin film on the substrate.
[0004]
[0004] In another embodiment, the method includes positioning a substrate on a substrate support in a processing chamber, the substrate support having a substrate-supporting concave surface or a substrate-supporting convex surface according to a stress profile of the substrate; flowing a deposition gas mixture including a silicon-containing gas and a reactive gas into the processing chamber through a showerhead; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead arranged symmetrically around a center point of the showerhead; and performing a deposition process while rotating the substrate to deposit a film layer on the substrate.
[0005]
[0005] In another embodiment, the method includes positioning a substrate on a substrate support in a processing chamber, the substrate support having a substrate-supporting concave surface or a substrate-supporting convex surface according to a stress profile of the substrate; flowing a deposition gas mixture including a silicon-containing gas and a reactive gas into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to the stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead arranged symmetrically around a center point of the showerhead; and performing the deposition process while rotating the substrate to deposit a film layer on the substrate and adjusting the height of the substrate support to adjust the plasma density in the transverse or longitudinal direction above the substrate.
[0006]
[0006] So that the above-mentioned features of the present disclosure can be understood in detail, a more particular description of the present disclosure briefly summarized above can be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings show only exemplary embodiments and therefore should not be considered as limiting the scope thereof, and that the present disclosure may admit of other equally effective embodiments. [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a processing chamber according to one or more embodiments. [Figure 2A-B]
[0008] FIG. 1 is a schematic cross-sectional view of a showerhead in accordance with one or more embodiments. [Figure 3A-B]
[0009] 1 is a schematic cross-sectional view of a substrate support according to one or more embodiments. [Figure 4]
[0010] FIG. 1 is a schematic top view of a showerhead according to one embodiment. [Diagram 5]
[0011] 1 illustrates a method for forming a membrane layer according to one or more embodiments. [Figure 6A-B]
[0012] 6 is a cross-sectional view of a film layer on a substrate according to the method of FIG. 5. [Figure 7]
[0013] FIG. 1 is a cross-sectional view of a stepped structure according to one or more embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008]
[0014] For ease of understanding, wherever possible, like reference numerals have been used to designate identical elements common to the figures. It is believed that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.
[0009]
[0015] The embodiments of the present disclosure describe an apparatus and method for depositing a film layer that can have minimal contribution to overlay error after a series of deposition and lithography exposure processes. In one embodiment, the deposition method can form a film layer with minimal stress variation or in-plane distortion (IPD) across the film layer surface to provide consistent film stress for each film layer formed on a substrate. Thus, when all the film layers from the series of deposition and lithography exposure processes are integrated to form a semiconductor device, overlay error can be minimized or eliminated.
[0010]
[0016] FIG. 1 is a schematic cross-sectional view of a processing chamber 100 according to one or more embodiments. The processing chamber 100 may be a plasma enhanced chemical vapor deposition (PECVD) chamber utilized to deposit a dielectric film stack, such as an oxide and nitride alternating layer stack or an oxide and polysilicon alternating layer stack. As shown in FIG. 1, the processing chamber 100 includes a chamber wall 102, a substrate support 104 disposed within the chamber wall 102, and a showerhead (e.g., gas distribution plate) 106 disposed within the chamber wall 102. The substrate support 104 is disposed below the showerhead 106 and configured to support a substrate 108. The substrate 108 may be a dummy wafer or a production wafer. A slit valve opening 152 may be formed in the chamber wall for loading or unloading one or more substrates, such as the substrate 108. A vacuum pump 111 is coupled to the bottom of the processing chamber 100 to evacuate the processing chamber 100. A valve 113 may be selectively opened and closed to control the degree of vacuum within the vacuum pump 111.
[0011]
[0017] In operation, the substrate support 104 may rotate to rotate the substrate 108 disposed thereon. The rotation of the substrate support 104 may be a continuous rotation in one direction (either clockwise or counterclockwise) or may oscillate in the opposite direction, such as rotating 180 degrees and then changing the direction of rotation. Rotation of the substrate support 104 may improve the thickness uniformity of the deposited film stack. In some implementations, the substrate support 104 may be heated to high temperatures, such as up to 700° C., for high temperature processing.
[0012]
[0018] The RF power source 107 is coupled to the blocking plate 140, which is disposed above the showerhead 106. The blocking plate 140 and the showerhead 106 together define a gas mixing space 142 (between the blocking plate 140 and the showerhead 106) and a reaction space 144 (between the blocking plate 140 and the substrate support 104) of the processing chamber 100. A plurality of apertures 146 are formed through the blocking plate 140.
[0013]
[0019] The showerhead 106 includes a first surface 114 facing the substrate support 104 and a second surface 116 opposite the first surface 114. A plurality of gas passages 115 are formed in the showerhead 106 extending from the first surface 114 to the second surface 116. The showerhead 106 is sized to cover the substrate support 104. The showerhead 106 is typically fabricated from stainless steel, aluminum (Al), anodized aluminum, nickel (Ni), or other RF conductive materials. The showerhead 106 may be cast, brazed, forged, hot isostatically pressed, or sintered. The showerhead 106 may be circular or polygonal, such as rectangular or square.
[0014]
[0020] A gas source 110 may be coupled to the blocking plate 140 to deliver one or more process gases into the processing chamber 100. A remote plasma source 112 may also be coupled to the showerhead 106 to deliver a cleaning agent, such as dissociated fluorine, into the processing chamber 300 to remove deposition by-products and films from the processing chamber hardware, such as the showerhead 106.
[0015]
[0021] Various approaches may be used in the processing chamber 100 to minimize or eliminate in-plane distortion (IPD) resulting from processing of a film stack on a substrate. IPD includes radial distortion and / or in-plane distortion. Radial distortion as used herein refers to the distortion between points along a desired radius of the substrate, which may be determined by calculating the difference between the radial components of the distortion of a distortion vector originating at two points of interest. In-plane distortion as used herein refers to dilational, rotational, and translational distortions that may occur in small regions or across the entire surface of the substrate. Various approaches described below may be used to reduce radial and / or in-plane distortion of a film stack, such as a stack of alternating oxide and nitride layers.
[0016]
[0022] It has been observed that profiled electrodes can be used to reduce or eliminate radial distortion of the film stack on the substrate 108. In some embodiments, the showerhead 106 and the substrate support 104 have a curvature to tailor the plasma density across the substrate 108. In some embodiments, the showerhead 106 and the substrate support 104 have different curvatures from one another. Figures 2A and 2B are schematic cross-sectional side views of a showerhead 206.
[0017]
[0023] When the center of the substrate 108 is observed to have more tensile stress than the edges of the substrate 108, a convex showerhead and / or a concave substrate support may be used to change the spacing D1 between the showerhead 106 and the substrate support 104 during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. In various implementations, the spacing D1 may range between about 10 mils and about 30 mils, for example about 15 mils. The spacing D1 between the showerhead 106 and the substrate support 104 may change the plasma density across the substrate 108, such that the center of the substrate 108 becomes more compressed. For example, the showerhead 206 shown in FIG. 2A may be used in place of the showerhead 106 of FIG. 1. In this implementation, the showerhead 206 has a first surface 204 facing a substrate support (not shown, such as the substrate support 104 of FIG. 1) and a second surface 208 opposite the first surface 204. The showerhead 206 further includes a plurality of gas passages 207 formed in the showerhead 206 that extend from the first surface 204 to the second surface 208. Unlike the planar first surface 114 shown in FIG. 1, the first surface 204 may have a curvature, such as a convex surface, as shown in FIG. 2A. In the convex first surface 204, the central region of the first surface 204 is closer to the substrate support 104 or the substrate 108 than the edge region of the first surface 204. The convex surface of the showerhead 206 can reduce the spacing D1 of the central region, which in turn increases the plasma density at the central region of the substrate 108. As a result, the center of the substrate 108 can be more compressed to balance the tensile stress initially caused by the substrate 108. Thus, the IPD / overlay error of the film stack on the substrate 108 is reduced.
[0018]
[0024] Additionally or alternatively, a substrate support such as the substrate support 304 shown in FIG. 3A may have a curvature such as a concave surface 306 as shown in FIG. 3A. The substrate support 304 may be used in place of the substrate support 104 in FIG. 1. With the concave surface 306, a central region of the concave surface 306 is farther away from the showerhead (not shown, such as the showerhead 106 in FIG. 1) than an edge region of the concave surface 306. Thus, to reduce the plasma density in the central region of the substrate 108, the distance D1 in the central region is increased. The center of the substrate 108 may be more compressed to balance the tensile stress initially caused by the substrate 108. It is envisioned that the concave surface 306 of the substrate support 304 may be used in conjunction with either the showerhead 206, 210 in FIGS. 2A and 2B to control the plasma density in order to reduce or minimize the IPD / overlay error of the film stack on the substrate 108.
[0019]
[0025] When the center of the substrate 108 is observed to have more compressive stress than the edges of the substrate 108, a concave showerhead and / or a convex substrate support may be used to change the spacing D1 between the showerhead 106 and the substrate support 104 during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. The spacing D1 between the showerhead 106 and the substrate support 104 may change the plasma density across the substrate 108, so that the center of the substrate 108 is less compressible. For example, the showerhead 210 shown in FIG. 2B may be used in place of the showerhead 106 of FIG. 1. In this embodiment, the showerhead 210 includes a first surface 212 facing a substrate support (not shown, such as the substrate support 104 of FIG. 1) and a second surface 214 opposite the first surface 212. The first surface 212 may have a curvature, such as a concave surface, as shown in FIG. 2B. With a concave first surface 212, a central region of the first surface 212 is farther away from the substrate support 104 or substrate 108 than an edge region of the first surface 212. The concave surface of the showerhead 210 can reduce the distance D1 in the central region, which in turn can reduce the plasma density in the central region of the substrate 108. As a result, the center of the substrate 108 can become less compressive to balance the higher compressive stress initially caused by the substrate 108. Thus, the IPD / overlay error of the film stack on the substrate 108 is reduced.
[0020]
[0026] Additionally or alternatively, a substrate support such as the substrate support 308 shown in FIG. 3B may have a curvature such as a convex surface 310 as shown in FIG. 3B. The substrate support 308 may be used in place of the substrate support 104 in FIG. 1. With the convex surface 310, the central region of the concave surface 306 is closer to the showerhead (not shown, such as the showerhead 106 in FIG. 1) than the edge region of the convex surface 310. Thus, to reduce the plasma density in the central region of the substrate 108, the distance D1 in the central region is reduced. The center of the substrate 108 may be less compressible to balance the higher compressive stress initially caused by the substrate 108. It is envisioned that the convex surface 310 of the substrate support 308 may control the plasma density in conjunction with either of the showerheads 206, 210 in FIGS. 2A and 2B to reduce or minimize the IPD / overlay error of the film stack on the substrate 108.
[0021]
[0027] In some embodiments, which may include or be combined with any of the other embodiments described in this disclosure, during substrate processing, such as a deposition process of a film stack of alternating oxide and nitride layers, the substrate support 104 may include two or more electrodes to adjust plasma density radially across the substrate 108. For example, in the embodiment shown in FIG. 1, the first electrode 120 may be integrated into the substrate support 104 or coupled to a surface of the substrate support 104. The first electrode 120 may be a plate, a perforated plate, a mesh, a wire screen, or any other distributed configuration of conductive elements. The second electrode 122 may be integrated into the substrate support 104 or coupled to a surface of the substrate support 104. Similarly, the second electrode 122 may be a plate, a perforated plate, a mesh, a wire screen, or any other distributed configuration of conductive elements. In one embodiment, the first electrode and the second electrode 120, 122 are both meshes. The first electrode 120 may extend across the substrate support 104 at a first height. The first electrode 120 may have a length equal to the diameter of the substrate 108. The second electrode 122 may be disposed at an edge region of the substrate support 104 at a second height different from the first height. In one embodiment, which may be combined with other embodiments, the second height is greater than the first height. In one embodiment, which may be combined with other embodiments, the second height is less than the first height. The second electrode 122 is disposed radially outward of the first electrode 120 and may or may not overlap a portion of the first electrode 120.
[0022]
[0028] The first electrode 120 is coupled to a power source 124 by a conductor 126, e.g., a cable disposed in the shaft 128 of the substrate support 104. A first controller 130, e.g., an impedance matching circuit, may be disposed between the power source 124 and the first electrode 120 to independently control the impedance of the first electrode 120 at the inner zone of the substrate support 104. The power source 124 may be DC power, pulsed DC power, RF bias power, pulsed RF source or bias power, or a combination thereof. The second electrode 122 is coupled to a power source 132 by a conductor 134, e.g., a cable disposed in the shaft 128 of the substrate support 104. A second controller 136, e.g., an impedance matching circuit, may be disposed between the power source 132 and the second electrode 122 to independently control the impedance of the second electrode 122 at the outer zone of the substrate support 104. The outer zone may surround the inner zone and have a radial distance covering the area from the edge of the substrate to the edge of the substrate support 104. The inner zone may have a radial distance at least equal to the diameter of the substrate. The power source 132 may be DC power, pulsed DC power, RF bias power, pulsed RF source or bias power, or a combination thereof. The first electrode 120 and the second electrode 122 may thus have independently controlled impedance.
[0023]
[0029] When the center of the substrate 108 is observed to have more compressive stress than the edge of the substrate 108, the second controller 136 may be configured to make the impedance of the second electrode 122 in the outer zone lower than the impedance of the inner zone during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. Alternatively, the first controller 130 may be configured to make the impedance of the inner zone higher than the impedance of the outer zone. In either case, the lower impedance in the outer zone of the substrate support 104 may couple more plasma to the outer zone, resulting in a substrate 108 with higher compressive stress at the edge region. Thus, uniformity of stress across the substrate 108 is achieved, thereby reducing or eliminating radial distortion of the film stack on the substrate 108.
[0024]
[0030] Similarly, when the center of the substrate 108 is observed to have less compressive stress than the edge of the substrate 108, the second controller 136 may be configured to have a higher impedance of the second electrode 122 in the outer zone than the inner zone during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. Alternatively, the first controller 130 may be configured to have a lower impedance in the inner zone than the outer zone. In either case, the higher impedance in the outer zone of the substrate support 104 may couple less plasma to the outer zone, resulting in a substrate 108 with lower compressive stress at the edge region. Thus, uniformity of stress across the substrate 108 is achieved, thereby reducing or eliminating radial distortion of the film stack on the substrate 108.
[0025]
[0031] In some embodiments, which may include or be combined with any of the other embodiments described in this disclosure, the apertures 146 of the blocking plate 140 may be configured to adjust the deposition rate during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. When the center of the substrate 108 is observed to have more compressive stress than the edge of the substrate 108, the blocking plate 140 may have more apertures 146 in the center region than the apertures in the edge region of the blocking plate 140, as shown in FIG. 1. For example, the apertures 146 in the center region may have a first density and the apertures 146 in the edge region may have a second density, and the ratio of the first density to the second density may be about 1.2:1 to about 5:1, such as about 1.5:1 to about 3:1.
[0026]
[0032] The density of the apertures 146 can be calculated by dividing the total area defined by the openings of the apertures 146 on the first surface 148 (facing the substrate support 104) by the total area of the first surface 148 of the blocking plate 140 in the measurement area. The density of the apertures 146 in the center region of the blocking plate 140 can range from about 10% to about 100%, for example, from about 60% to about 100%. To increase the gas flow in the center region, the density of the apertures 146 is higher in the center region than in the edge region. The change in density from the center region to the edge region needs to be gradual and smooth to ensure a uniform and smooth deposition and film property profile. The higher density of the apertures 146 in the center of the blocking plate 140 can increase the gas flow in the center region of the gas mixing space 142, thus increasing the gas flow and plasma density in the center region of the reaction space 144. Therefore, the film stack will have a higher deposition rate in the center region of the substrate 108. By having a high deposition rate in the central region of the substrate 108, the center of the substrate 108 may be less compressible than the edges of the substrate 108. As a result, IPD (e.g., radial distortion) and overlay errors of the film stack on the substrate 108 are reduced or minimized.
[0027]
[0033] When the center of the substrate 108 is observed to have less compressive stress than the edges of the substrate 108, the blocking plate 140 can have fewer apertures 146 in the center region than the apertures in the edge regions of the blocking plate 140. For example, the apertures 146 in the center region can have a first density and the apertures 146 in the edge regions can have a second density, where the ratio of the first density to the second density can be from about 1:1.2 to about 1:5, such as from about 1:1.5 to about 1:3.
[0028]
[0034] In this embodiment, the density of the apertures 146 in the center region of the blocking plate 140 may range from about 10% to about 100%, for example, from about 10% to about 40%. The density of the apertures 146 is lower in the center region than in the edge region, which reduces the gas flow in the center region. The change in density from the center region to the edge region needs to be gradual and smooth to ensure a uniform and smooth deposition and film property profile. The lower density of the apertures 146 in the center of the blocking plate 140 can reduce the gas flow in the center region of the gas mixing space 142, thus reducing the gas flow and plasma density in the center region of the reaction space 144. Therefore, the film stack will have a lower deposition rate in the center region of the substrate 108. By having a lower deposition rate in the center region of the substrate 108, the center of the substrate 108 can be more compressive than the edge of the substrate 108. As a result, the IPD (e.g., radial distortion) / overlay error of the film stack on the substrate 108 is reduced or minimized.
[0029]
[0035] The design concept of aperture 146 density can also be applied to the design of gas passages 115 to improve center-to-edge uniformity.
[0030]
[0036] In various embodiments, the matching network 154 may be disposed above the top of the processing chamber 100. The matching network 154 may be electrically coupled to a radio frequency (RF) power source 158 by a transmission line 156. RF power is generated by the RF power source 158 and applied to the showerhead 106 by an RF supply 160. The RF supply 160 may have a first end 162 electrically coupled to the matching network 154 and a second end 164 electrically coupled to the showerhead 106. The RF supply 160 may be made of a flexible conductive material, such as a copper strip. As described in more detail below, the second end 164 of the RF supply 160 may be coupled to a different location on the showerhead 106 to reduce plasma non-uniformity.
[0031]
[0037] FIG. 4 is a schematic top view of a showerhead 406 according to one embodiment. The showerhead 406 may be used in place of the showerhead 106 of FIG. 1. As shown in FIG. 4, the showerhead 406 may be circular and have a top surface 408 facing away from the substrate support 104 (FIG. 1). A number of coupling points 410a, 410b, 410c, 410d may be located on the top surface 408 of the showerhead 406. Each coupling point 410a-410d may be used to secure a second end (e.g., second end 164) of the RF supply 160 shown in FIG. 1. The coupling points 410a-410d are located at positions on the showerhead 406 that are symmetrical about a center point 412 of the showerhead 406. An RF power source 402 is electrically coupled to the coupling points at multiple positions via transmission lines (collectively labeled 414) during substrate processing, such as a deposition process of a film stack of alternating oxide and nitride layers. A matching network 403 (e.g., matching network 154) may be disposed between the RF power source 402 and the nodes 410a-410d. The nodes 410a-410d are symmetrically disposed to improve plasma uniformity across the substrate 108 (FIG. 1). As a result, residual non-uniformity of the IPD is reduced.
[0032]
[0038] Although four connection points 410a-410d are shown in FIG. 4, more or less connection points are contemplated. In one embodiment, six connection points are used. In another embodiment, eight connection points are used. In yet another embodiment, a single connection point may be used and located at the center of the showerhead 406. When multiple connection points are used, the connection points may be symmetrically located at the showerhead 106 to reduce or eliminate the planarity and / or residual distortion of the film stack on the substrate 108. It is contemplated that the concepts described herein may also be applied to the substrate support, in the case where RF power is coupled to the substrate support. In such a case, one or more RF supplies may be coupled to electrodes (e.g., the first and / or second electrodes 120, 122 shown in FIG. 1) at multiple locations on the substrate support 104.
[0033]
[0039] Other techniques may also be used to help reduce or eliminate the plane and / or residual distortion of the film stack on the substrate 108 during substrate processing. For example, as shown in FIG. 1, the adjustment devices 170, 172 may be attached to the bottom of the substrate support 104. The adjustment devices 170, 172 may be arranged symmetrically about a central axis (not shown) passing through the longitudinal direction of the shaft 128. The adjustment devices 170, 172 may extend through the bottom of the processing chamber 100 and rotate to adjust the leveling of the substrate support 104 during, before, or after substrate processing. The adjustment devices 170, 172 may be any device or mechanism suitable for adjusting the height of the substrate support 104. The leveling of the substrate support 104 may be altered to adjust the plasma density across or back-to-front across the substrate 108. As a result, a uniform side-to-side stress profile of the film stack is obtained.
[0034]
[0040] In some implementations, which may include or be combined with any other implementations of the present disclosure, during substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers, the in-plane distortion of the film stack may be reduced or eliminated by rotating the substrate support 104. The rotation of the substrate support 104 may be a continuous rotation in one direction or may oscillate in the opposite direction, such as rotating 180 degrees and then changing the direction of rotation. In one implementation, the deposition of the film stack is split into two deposition processes, and the substrate 108 is rotated 180 degrees to eliminate the IPD in-plane distortion. For example, the film stack may include a total of about 2 to 90 pairs of oxide and nitride layers. The first half of the film stack (e.g., 1 to 45 pairs of oxide and nitride layers) may be deposited and the substrate support 104 may be fixed, and the second half of the film stack (e.g., 46 to 90 pairs of oxide and nitride layers) may be deposited and the substrate support 104 may be rotated 180 degrees, thereby offsetting the difference in the film deposition profile caused by the IPD distortion. As a result, the thickness uniformity of the deposited film stack is improved.
[0035]
[0041] It is contemplated that the concepts described herein may be equally applied to multiple deposition processes. For example, the deposition of a film stack may be split into three deposition processes and the substrate 108 may be rotated 120 degrees. Alternatively, the deposition of a film stack may be split into four deposition processes and the substrate 108 may be rotated 90 degrees, etc.
[0036]
[0042] Due to the large area of the showerhead 106 or electrodes, the RF voltage applied to them may have interference fringes that distort the plasma. An example of interference fringes is a standing wave. Standing waves may occur at or near the center of an electrode such as the showerhead 106. Because the plasma is not uniformly distributed due to the standing wave effect or interference fringes, the film stack deposited on the substrate 108 may not have a uniform thickness across the substrate 108. As a result, the uniformity of the film stress is compromised.
[0037]
[0043] To improve plasma uniformity, RF power can be applied to an electrode such as the showerhead 106 at low frequency RF during substrate processing such as a deposition process of a film stack with alternating oxide and nitride layers. The low RF frequency can range from about 0.3 MHz to about 60 MHz, for example, from about 13.56 MHz to about 40 MHz. In one embodiment, the low RF frequency is from about 14 MHz to about 27 MHz. Using a low RF frequency can result in RF power delivery at a shorter wavelength. For example, 13.56 MHz RF corresponds to a wavelength of 22 meters, and 27 MHz RF corresponds to a wavelength of 11 meters. It can be seen that the RF power delivered at the shorter wavelength is comparable or comparable to the showerhead 106. As a result, standing wave effects or interference fringes occurring at or near the center of the showerhead 106 can be reduced.
[0038]
[0044] RF power at low RF frequencies can be applied to electrodes through multiple connection points, such as connection points 410a-410d, disposed on the showerhead 106 as described above. Additionally or alternatively, RF power at low RF frequencies can be applied to electrodes of the substrate support 104, such as the first and / or second electrodes 120, 122 shown in FIG.
[0039]
[0045] It is envisioned that the approach of applying a low RF frequency to the electrodes may be combined with any of the embodiments discussed in this disclosure. For example, in some embodiments, a low RF frequency may be used in conjunction with a convex or concave showerhead 106 and / or a convex or concave substrate support 104 to maintain the spacing D1 (FIG. 1) at 15 mils. In one embodiment, a low RF frequency may be used in conjunction with multiple RF feed locations and a convex or concave showerhead 106 and / or a convex or concave substrate support 104 to maintain the spacing D1 at 15 mils. In some embodiments, a low RF frequency may be used in conjunction with multiple RF feed locations, various densities of apertures in the central region of the blocking plate, and a convex or concave showerhead 106 and / or a convex or concave substrate support 104 to maintain the spacing D1 within a predetermined range or at a predetermined value, such as 15 mils.
[0040]
[0046] The various embodiments may be combined in any order to perform substrate processing, such as a deposition process of a film stack with alternating oxide and nitride layers. FIG. 5 illustrates a method 500 for forming a film layer, such as a dielectric layer, which may later be used to form a gate structure for a semiconductor device. In one embodiment, the film layer may be used to form a gate structure for a three-dimensional (3D) NAND semiconductor application. In the manufacture of three-dimensional (3D) NAND semiconductor applications, stepped oxide and nitride pair structures are often used in high aspect ratio gate stack NAND cells to increase circuit density.
[0041] The sequence depicted in FIG. 5 corresponds to the manufacturing stages depicted in FIGS. 6A-6B (described below). The method 500 begins in operation 502 by providing a substrate 602 in a deposition processing chamber, such as the processing chamber 100 depicted in FIG. 1. The substrate 602 has a first film layer 606 formed thereon. The first film layer 606 can be a silicon-containing layer, such as a silicon oxide-containing layer, a silicon nitride-containing layer, amorphous silicon, polycrystalline silicon, or any suitable crystalline silicon layer. In the example depicted in FIG. 6A, the first film layer 606 is a silicon oxide-containing layer, such as a silicon oxide layer. The substrate 602 is a crystalline silicon (e.g., Si <100> Or Si <111> ), silicon oxide, strained silicon, silicon germanium, doped or undoped polysilicon, silicon on insulator (SOI) of doped or undoped silicon wafers and patterned or unpatterned wafers, carbon doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, or sapphire.
[0042]
[0048] In operation 504, a deposition gas mixture is provided into the process chamber to form a second film layer 608, such as a silicon nitride-containing layer, on the first film layer 606, as shown in FIG. 6B. The deposition gas mixture may include a silicon-containing gas and a reactive gas. Suitable silicon-containing gases include, but are not limited to, silane (SiH4), disilane (S i2 H6), silicon tetrafluoride (SiF4), silicon tetrachloride (SiC l4 ), dichlorosilane (SiH2Cl2), tetraethyl orthosilicate (TEOS), and the like. The reactive gas may be an oxygen-containing gas for forming a silicon oxide-containing layer, a nitrogen-containing gas for forming a silicon nitride-containing layer, or a carbon-containing gas for forming a silicon carbide-containing layer. Suitable examples of oxygen-containing gases include O2, N2O, NO2, O3, H2O, and the like. Suitable examples of nitrogen-containing gases include N2, N2O, NO2, NH3, N2H2, and the like. Suitable examples of carbon-containing gases include CO2, CO, CH4, CF4, other suitable carbon-based polymer gases, and the like. One or more inert gases may be included in the deposition gas mixture. The inert gases may include, but are not limited to, Ar, He, and Xe, or a noble gas such as N2. The chamber pressure may be maintained in a range between about 10 mTorr and about 15 Torr, and the substrate temperature may be maintained in a range between about 200 degrees Celsius and about 700 degrees Celsius. Depending on the stress profile of the substrate, the showerhead and / or the substrate support of the processing chamber can have a curvature to obtain a predetermined spacing between the showerhead and the substrate support, such as about 10 mils to about 30 mils, as discussed above with respect to FIGS. 1, 2A, 2B, 3A, and 3B.
[0043]
[0049] In operation 506, radio frequency (RF) power is generated by a power source, such as RF power source 158 (FIG. 1), and coupled to the deposition gas mixture to aid in dissociation of the deposition gas mixture into reactive species in a plasma. The RF power may be operated at a low RF frequency in the range of about 13.56 MHz to about 40 MHz, for example about 27 MHz, as discussed above. The RF power may be operated at about 10 Watts to about 5000 Watts, for example about 500 Watts. RF bias power may be provided by one or more power sources, such as power sources 124, 132, in a manner as discussed above to improve plasma density during the deposition process. The RF bias power may be supplied between about 10 Watts and about 100 Watts at a frequency of 300 kHz. In one embodiment, the RF bias power may be pulsed at a frequency between about 500 Hz and about 10 kHz with a duty cycle of between about 10% and about 95%. Unless otherwise stated, the processing parameters discussed in this disclosure are based on substrates having a 200 mm diameter, a 300 mm diameter, and a 450 mm diameter.
[0044]
[0050] In operation 508, while forming a plasma from the deposition gas mixture, a substrate support, such as substrate support 104 (FIG. 1), may be continuously rotated or oscillated in the opposite direction, such as rotating 180 degrees and then changing rotation direction, to help expose the substrate more uniformly to the plasma. The substrate support 104 may be rotated between about 1° and about 360°, e.g., between about 30° and about 270°, e.g., between about 90° and about 180°, depending on the division number discussed above. The substrate support may continuously rotate the substrate throughout the deposition process.
[0045]
[0051] In operation 510, the second membrane layer 608 is deposited to a desired thickness. After deposition to the desired thickness, the deposition process is terminated. In one example, the second membrane layer 608 may have a thickness between about 10 nm and about 60 nm, for example about 30 nm. In an embodiment in which the second membrane layer 608 is a silicon nitride layer, the silicon nitride layer may have a stress in the range between about -200 MPa and about +1200 MPa with a stress uniformity of less than 50%. The second membrane layer 608 may have a local bow range in the range of less than 50 μm. Stress uniformity (U%) as discussed herein refers to the variation (Δ) of absolute stress values measured across a substrate surface (e.g., the variation between the maximum and minimum stress values obtained from either a 9-point, 49-point, or 69-point stress measurement) divided by the average (σ) of stress measured from a film layer (e.g., the average of stress values obtained from a 9-point, 49-point, or 69-point stress measurement) (e.g., σ / Δ=U%).
[0046]
[0052] The deposition process for forming the first and second film layers 606, 608 may be repeated to form a film stack 702, which may later be patterned to form a staircase structure for a 3D NAND semiconductor device. FIG. 7 illustrates a cross-sectional view of a staircase structure 704 according to one or more embodiments. In the example illustrated in FIG. 7, the film stack 702 may include alternating layers of the first and second film layers 606, 608 (illustrated as 606a, 608a, 606b, 608b, . . . , 606n, 608n) discussed above. The film stack 702 may have a total thickness between about 600 nm and about 4000 nm. The film stack 702 may include a total of about 5 to 90 pairs of the first and second film layers 606, 608. In a subsequent patterning or etching process, the photoresist layer can be used to sequentially trim to different dimensions while acting as an etching mask for the stair-like structure 704 to complete the gate structure for a 3D NAND semiconductor device.
[0047]
[0053] While the above is directed to embodiments of the disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, the scope of which is determined by the following claims.
Claims
1. 1. A method for forming a film layer on a substrate, comprising: Positioning a substrate on a substrate support in a processing chamber; flowing a deposition gas mixture, including a silicon-containing gas and a reactive gas, into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to a compressive or tensile stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process while rotating the substrate to deposit a film layer on the substrate; delivering the deposition gas mixture through a blocking plate disposed above the showerhead; flowing the deposition gas mixture through apertures in a central region of the blocking plate having a first density and through apertures in an edge region of the blocking plate having a second density lower than the first density, when a central region of the substrate has a compressive stress higher than a compressive stress in an edge region of the substrate; or flowing the deposition gas mixture through apertures in the central region of the blocking plate having a third density and through apertures in the edge region of the blocking plate having a fourth density greater than the third density, when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. delivering the deposition gas mixture by A method comprising:
2. 2. The method of claim 1 , wherein the silicon-containing gas comprises at least one of silane, disilane, silicon tetrafluoride, silicon tetrachloride, dichlorosilane, and tetraethylorthosilicate, and the reactive gas comprises at least one of an oxygen-containing gas, a nitrogen-containing gas, and a carbon-containing gas.
3. The method of claim 1 , further comprising adjusting a transverse or longitudinal plasma density across the substrate by adjusting a height of the substrate support during the deposition process.
4. 2. The method of claim 1, wherein the membrane layer is a membrane stack including a first membrane layer and a second membrane layer disposed on the first membrane layer, the first membrane layer and the second membrane layer being alternately and repeatedly formed in the membrane stack, and the membrane stack has a range of local deformation of less than 200 μm. maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate support at a second impedance higher than the first impedance when the central region of the substrate has a compressive stress higher than a compressive stress in the edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. adjusting a plasma density across the substrate by The method of claim 1 further comprising:
6. 1. A method for forming a film layer on a substrate, comprising: Positioning the substrate in a processing chamber on a substrate support having a concave or convex substrate supporting surface according to a compressive or tensile stress profile of the substrate; flowing a deposition gas mixture comprising a silicon-containing gas and a reactive gas into the processing chamber through a showerhead; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process while rotating the substrate to deposit a film layer on the substrate; delivering the deposition gas mixture through a blocking plate disposed above the showerhead; flowing the deposition gas mixture through apertures in a central region of the blocking plate having a first density and through apertures in an edge region of the blocking plate having a second density lower than the first density, when a central region of the substrate has a compressive stress higher than a compressive stress in an edge region of the substrate; or flowing the deposition gas mixture through apertures in the central region of the blocking plate having a third density and through apertures in the edge region of the blocking plate having a fourth density greater than the third density, when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. delivering the deposition gas mixture by A method comprising:
7. The method of claim 6 , further comprising adjusting a transverse or longitudinal plasma density across the substrate by adjusting a height of the substrate support during the deposition process.
8. 7. The method of claim 6, wherein the membrane layer is a membrane stack including a first membrane layer and a second membrane layer disposed on the first membrane layer, the first membrane layer and the second membrane layer being alternately and repeatedly formed in the membrane stack, and the membrane stack has a range of local deformation of less than 200 μm. maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate support at a second impedance higher than the first impedance when the central region of the substrate has a compressive stress higher than a compressive stress in the edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. adjusting a plasma density across the substrate by The method according to claim 6.
10. 1. A method for forming a film layer on a substrate, comprising: Positioning a substrate in a processing chamber on a substrate support having a concave or convex substrate supporting surface according to a compressive or tensile stress profile of said substrate; flowing a deposition gas mixture, including a silicon-containing gas and a reactive gas, into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to a compressive or tensile stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process by depositing a film layer on a substrate while rotating the substrate and adjusting a plasma density in a transverse or longitudinal direction above the substrate by adjusting a height of the substrate support; delivering the deposition gas mixture through a blocking plate disposed above the showerhead; flowing the deposition gas mixture through apertures in a central region of the blocking plate having a first density and through apertures in an edge region of the blocking plate having a second density lower than the first density, when a central region of the substrate has a compressive stress higher than a compressive stress in an edge region of the substrate; or flowing the deposition gas mixture through apertures in the central region of the blocking plate having a third density and through apertures in the edge region of the blocking plate having a fourth density greater than the third density, when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. delivering the deposition gas mixture by A method comprising:
11. 11. The method of claim 10, wherein the membrane layer is a membrane stack including a first membrane layer and a second membrane layer disposed on the first membrane layer, the first membrane layer and the second membrane layer being alternately and repeatedly formed in the membrane stack, and the membrane stack has a range of local deformation of less than 200 μm.
12. said adjusting a plasma density across the substrate comprising: maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate at a second impedance higher than the first impedance when the central region of the substrate has a higher compressive stress than the compressive stress in the edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate; The method of claim 10, comprising:
13. The method of claim 4 , wherein the first membrane layer is a silicon oxide layer and the second membrane layer is a silicon nitride layer.
14. 7. The method of claim 6, wherein the silicon-containing gas comprises at least one of silane, disilane, silicon tetrafluoride, silicon tetrachloride, dichlorosilane, and tetraethylorthosilicate, and the reactive gas comprises at least one of an oxygen-containing gas, a nitrogen-containing gas, and a carbon-containing gas.
15. The method of claim 8 , wherein the first membrane layer is a silicon oxide layer and the second membrane layer is a silicon nitride layer.
16. 11. The method of claim 10, wherein the silicon-containing gas comprises at least one of silane, disilane, silicon tetrafluoride, silicon tetrachloride, dichlorosilane, and tetraethylorthosilicate, and the reactive gas comprises at least one of an oxygen-containing gas, a nitrogen-containing gas, and a carbon-containing gas.
17. The method of claim 11 , wherein the first membrane layer is a silicon oxide layer and the second membrane layer is a silicon nitride layer.
18. A method for forming a film layer on a substrate, comprising the steps of: Positioning a substrate on a substrate support in a processing chamber; flowing a deposition gas mixture, including a silicon-containing gas and a reactive gas, into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to a compressive or tensile stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process while rotating the substrate to deposit a film layer on the substrate; adjusting a plasma density across the substrate, maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate at a second impedance higher than the first impedance when a central region of the substrate has a higher compressive stress than an edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. and adjusting the plasma density by A method comprising:
19. The method of claim 18, wherein the first electrode overlaps a portion of the second electrode.
20. A method for forming a film layer on a substrate, comprising the steps of: Positioning a substrate in a processing chamber on a substrate support having a concave or convex substrate supporting surface according to a compressive or tensile stress profile of said substrate; flowing a deposition gas mixture comprising a silicon-containing gas and a reactive gas into the processing chamber through a showerhead; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process while rotating the substrate to deposit a film layer on the substrate; adjusting a plasma density across the substrate, maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate at a second impedance higher than the first impedance when a central region of the substrate has a higher compressive stress than an edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. and adjusting the plasma density by A method comprising:
21. The method of claim 20, wherein the first electrode overlaps a portion of the second electrode.
22. A method for forming a film layer on a substrate, comprising the steps of: Positioning the substrate in a processing chamber on a substrate support having a concave or convex substrate supporting surface according to a compressive or tensile stress profile of the substrate; flowing a deposition gas mixture, including a silicon-containing gas and a reactive gas, into the processing chamber through a showerhead having a convex surface facing the substrate support or a concave surface facing the substrate support according to a compressive or tensile stress profile of the substrate; forming a plasma in the presence of the deposition gas mixture in the processing chamber by applying RF power to a plurality of nodes of the showerhead symmetrically disposed about a center point of the showerhead; performing a deposition process while rotating the substrate to deposit a film layer on the substrate and adjusting a plasma density across or to the front and rear of the substrate by adjusting a height of the substrate support; Including, adjusting the plasma density in the transverse or longitudinal direction across the substrate; maintaining a first electrode in an outer zone of the substrate support at a first impedance and a second electrode in an inner zone of the substrate at a second impedance higher than the first impedance when a central region of the substrate has a higher compressive stress than an edge region of the substrate; or maintaining the first electrode in the outer zone of the substrate support at a third impedance and the second electrode in the inner zone of the substrate at a fourth impedance lower than the third impedance when the central region of the substrate has a compressive stress lower than a compressive stress in the edge region of the substrate. method.
23. The method of claim 22, wherein the first electrode overlaps a portion of the second electrode.
Citation Information
Patent Citations
Plasma cvd film forming device
JP2000269146A
Plasma processing apparatus
JP2004311646A
PECVD oxide-nitride stacks and oxide-silicon stacks for 3D memory
JP2013546169A
Substrate support device, and substrate processing apparatus having the same
JP2015004131A
Gate stack material for semiconductor applications to improve lithography overlays
JP2018508980A