Composite substrate and method of manufacturing same
The composite substrate with tailored inorganic fillers and resin composition addresses the need for low CTE and high rigidity, ensuring effective dielectric performance and heat resistance for 5G electronic components.
Patent Information
- Application Number
- JP2023004188
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-20
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-01-16
AI Technical Summary
Existing electronic substrates face challenges in achieving low coefficient of thermal expansion (CTE) and high rigidity modulus to meet the demands of high frequency transmission and low latency in 5G communications.
A composite material substrate is developed, comprising inorganic fillers with specific particle sizes and shapes, combined with a resin composition including bismaleimide, naphthalene ring-containing epoxy, and benzoxazine resins, dispersed with a dispersant to form a slurry that is cured, enhancing packing density and mechanical properties.
The composite substrate achieves reduced CTE and increased rigidity, maintaining excellent dielectric properties and heat resistance, suitable for high-frequency electronic applications.
Smart Images

Figure 0007566059000009 
Figure 0007566059000010 
Figure 0007566059000011
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composite substrate, and in particular to a composite substrate comprising an inorganic filler and a resin composition, and a method for producing the same. [Background technology]
[0002] Thermosetting resin compositions are widely used in electronic devices and other fields due to their crosslinked structure and high heat resistance or dimensional stability. In recent years, with the development of 5G communication, the industry has been facing increasing demands for high frequency transmission, high speed signal transmission, and low latency. Therefore, at present, the relevant field is devoted to the research and development of substrate materials with high glass transition temperature (Tg), low dielectric constant (Dk), low dissipation factor (Df), and good heat resistance to meet the requirements of dielectric properties (low dielectric constant and low dissipation factor) and heat resistance in electronic substrates. Summary of the Invention [Problem to be solved by the invention]
[0003] The present disclosure provides a composite substrate that has the advantages of a low coefficient of thermal expansion (CTE) and a high rigidity modulus. [Means for solving the problem]
[0004] At least one embodiment of the present disclosure provides a composite substrate. The composite substrate includes an inorganic filler, a resin composition, and a dispersant. The inorganic filler includes first spherical inorganic particles, and a filler material. The first spherical inorganic particles have an average particle size of 300 nm to 600 nm. The filler material includes at least one of second spherical inorganic particles and flaky inorganic particles. The second spherical inorganic particles have an average particle size of 20 nm to 50 nm, and the flaky inorganic particles have an average thickness of 0.5 μm to 2 μm. The resin composition includes a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoxazine resin. The inorganic filler, the resin composition, and the dispersant are mixed together.
[0005] At least one embodiment of the present disclosure provides a method for producing a composite substrate, the method including: mixing an inorganic filler, a dispersant, and a solvent to form a dispersion; dissolving a resin composition in the dispersion to form a slurry, the resin composition including a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoxazine resin; and curing the slurry. Effect of the Invention
[0006] Based on the above, since the filling density of the inorganic filler in the composite substrate is 60%-80%, the CTE of the composite substrate can be reduced and the rigidity of the composite substrate can be increased. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view of a composite substrate according to an embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a composite substrate according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a flow diagram of a method for manufacturing a composite material substrate according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1 is a schematic cross-sectional view of a composite substrate 10 according to one embodiment of the present disclosure. Referring to FIG. 1, the composite substrate 10 includes a resin composition 110, an inorganic filler 200, and a dispersing agent (not shown). In some embodiments, the composite substrate 10 also includes a curing agent (not shown), a siloxane coupling agent (not shown), and a catalyst (not shown). The resin composition 110, the inorganic filler 200, the dispersing agent, the curing agent, the siloxane coupling agent, and the catalyst are mixed together.
[0009] Resin composition 110 contains a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoxazine resin. In resin composition 110, the bismaleimide resin is 10 wt% to 70 wt%, the naphthalene ring-containing epoxy resin is 10 wt% to 50 wt%, and the benzoxazine resin is 10 wt% to 50 wt%.
[0010] In some embodiments, the bismaleimide resin is, for example, 4,4'-diphenylmethane bismaleimide, oligomers of phenylmethane maleimide, m-phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and 1,6-bismaleimide-(2,2,4-trimethyl)hexane, although the present disclosure is not limited thereto.
[0011] In some embodiments, the naphthalene ring-containing epoxy resin includes a naphthalene ring structure. The naphthalene ring structure has a small bond rotation ability, so that the heat resistance of the naphthalene ring-containing epoxy resin can be improved. In addition, the epoxy group of the naphthalene ring-containing epoxy resin has a high crosslink density after curing. Therefore, the naphthalene ring-containing epoxy resin, which combines the naphthalene ring structure and the epoxy group, has the advantages of a high rigidity modulus and high heat resistance, and can also reduce the CTE of the resin composition. In some embodiments, the naphthalene ring-containing epoxy resin includes a monomeric multifunctional naphthalene ring epoxy resin (as shown in Structural Formula 1), a novolac-type naphthalene-based epoxy resin (as shown in Structural Formula 2), and / or other naphthalene ring-containing epoxy resins. In Structural Formula 2, n is, for example, 1 to 7. [ka] [ka]
[0012] In some embodiments, the benzoxazine resin is prepared by a condensation polymerization reaction using a phenolic compound, formaldehyde, and a primary amine compound as reactants. In some embodiments, the benzoxazine resin has the advantage of accelerating the rate of crosslinking reaction of the resin composition 110. In some embodiments, the benzoxazine resin can include, for example, bisphenol A benzoxazine (as shown in Structure 3), bisphenol F benzoxazine (as shown in Structure 4), phenolphthalein benzoxazine (as shown in Structure 5), thiodiphenol benzoxazine (as shown in Structure 6), or other suitable benzoxazine resins. [ka] [ka] [ka] [ka]
[0013] The inorganic filler 200 is the main component of the composite substrate 10. In this embodiment, the inorganic filler 200 is mainly composed of the first spherical inorganic particles 210, and a small amount of filler material is used to increase the packing density of the inorganic material. In this embodiment, the filler material is the second spherical inorganic particles 220a, and the first spherical inorganic particles 210 and the second spherical inorganic particles 220a include different particle sizes. In other embodiments, the filler material may include a flake-like or one-dimensional structure inorganic filler. In some embodiments, the weight of the inorganic filler 200 is, for example, 100 parts by weight to 300 parts by weight relative to a total of 100 parts by weight of the resin composition 110, for example, 100 parts by weight, 150 parts by weight, 200 parts by weight, 250 parts by weight, or 300 parts by weight.
[0014] In some embodiments, the material of the first spherical inorganic particles 210 includes silicon oxide or other suitable materials. In some embodiments, the average particle size S1 of the first spherical inorganic particles 210 is 300 nm to 600 nm. In some embodiments, the first spherical inorganic particles 210 have a narrower particle size range, i.e., a smaller maximum allowable particle size, so that the first spherical inorganic particles 210 can be packed more orderly. For example, the maximum allowable particle size of the first spherical inorganic particles 210 is 5 μm or less, and the difference between D10 and D90 of the first spherical inorganic particles 210 is less than 500 nm. In some embodiments, by mixing inorganic fillers with different particle sizes and shapes, the composite material substrate 10 has the advantages of a low CTE and a high rigidity.
[0015] In some embodiments, the material of the first spherical inorganic particles 210 and the second spherical inorganic particles 220a includes silicon oxide or other suitable materials. In some embodiments, the average particle size S2 of the second spherical inorganic particles 220a is 20 nm to 50 nm. In some embodiments, the first spherical inorganic particles 210 and the second spherical inorganic particles 220a have a narrower particle size range, respectively, so that the first spherical inorganic particles 210 and the second spherical inorganic particles 220a have a denser packing effect as a whole. For example, the difference between D10 and D90 of the second spherical inorganic particles 220a is less than 20 nm. In some embodiments, the ratio of the average particle size S1 of the first spherical inorganic particles 210 to the average particle size S2 of the second spherical inorganic particles 220a is 3 to 20. Therefore, the second spherical inorganic particles 220a can be preferably packed between the first spherical inorganic particles 210. In some embodiments, the weight of the resin composition is 100 parts by weight, the weight of the first spherical inorganic particles 210 is 100-300 parts by weight, and the weight of the second spherical inorganic particles 220a is 20-50 parts by weight. In some embodiments, the composite substrate 10 has the advantages of low CTE and high rigidity by increasing the dense packing degree of the inorganic filler 200.
[0016] The dispersant helps to disperse the inorganic filler more uniformly, thereby increasing the packing density of the inorganic filler. In some embodiments, the dispersant is, for example, an ionic dispersant, a polymeric dispersant, or other suitable dispersant. In some embodiments, the weight of the dispersant is greater than 0 parts by weight and less than or equal to 3 parts by weight, based on a total of 100 parts by weight of the resin composition 110.
[0017] The hardener serves to harden the resin composition 110. In some embodiments, the weight of the hardener is greater than 0 parts by weight and less than or equal to 30 parts by weight, based on a total of 100 parts by weight of the resin composition 110.
[0018] Siloxane binders include, but are not limited to, siloxane. In addition, depending on the type of functional group, they can be divided into aminosilane compounds, epoxysilane compounds, vinylsilane compounds, estersilane compounds, hydroxysilane compounds, isocyanatesilane compounds, methylsilane acryloyloxysilane compounds, and acryloxysilane compounds. In some embodiments, the weight of the siloxane binder is 0.1 to 4 parts by weight based on the total of 100 parts by weight of the resin composition 110.
[0019] Examples of the catalyst include catalysts and peroxides. For example, the catalysts include 1-cyanoethyl-2-phenylimidazole (2PZCN; CAS: 23996-12-5), 1-benzyl-2-phenylimidazole (1B2PZ; CAS: 37734-89-7), thiabendazole (TBZ; CAS: 148-79-8 ), or a combination thereof, and the imidazole compound with the best lifting effect is, for example, 1-benzyl-2-phenylimidazole, but the present disclosure is not limited thereto, and other suitable catalysts can be selected for catalytic effect according to actual design requirements. In some embodiments, the weight of the catalyst is more than 0 parts by weight and not more than 10 parts by weight, relative to a total of 100 parts by weight of the resin composition 110.
[0020] Composite substrate 20 of FIG. 2 is similar to composite substrate 10 of FIG. 1, except that the filler material in inorganic filler 200 of composite substrate 20 further includes a plurality of flaky inorganic particles 220b.
[0021] In some embodiments, the material of the flaky inorganic particles 220b includes silicon oxide or other suitable materials. In some embodiments, the average thickness T of the flaky inorganic particles 220b is 0.5 μm to 2 μm. In some embodiments, the average diameter W of the flaky inorganic particles 210 is 5 μm to 10 μm. In some embodiments, the ratio of the average diameter W to the average thickness T of the flaky inorganic particles 220b is 10 or more. In this embodiment, by mixing inorganic fillers with different particle sizes and shapes, the packing density of the inorganic filler can be increased, and the composite material substrate 20 can have the advantages of a low CTE and a high rigidity.
[0022] In this embodiment, the composite substrate 20 further includes a resin composition 110, a dispersant (not shown), a curing agent (not shown), a siloxane binder (not shown), and a catalyst (not shown). For the description of the resin composition 110, the dispersant, the curing agent, the siloxane binder, and the catalyst, please refer to the embodiment of FIG. 1, and the details will not be repeated here.
[0023] FIG. 3 is a flow diagram of a method for manufacturing a composite substrate (eg, a composite substrate in any of the previous embodiments) according to one embodiment of the present disclosure.
[0024] Referring to Fig. 3, in step ST1, an inorganic filler, a dispersant, and a solvent are mixed to form a dispersion. In some embodiments, the solvent may include, for example, water, an organic solvent, or a combination thereof. The inorganic filler may be, for example, a flake-shaped inorganic particle or a spherical inorganic particle, and the inorganic filler is uniformly dispersed in the dispersion.
[0025] In step ST2, a resin composition including a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoxazine resin is dissolved in a dispersion to form a varnish. In some embodiments, the solid content of the slurry is 40% by weight to 70% by weight. In some embodiments, a curing agent, a siloxane coupling agent, and a catalyst are also added to the dispersion.
[0026] In step ST3, the varnish is impregnated into a glass fiber cloth (Cloth type 1078, manufactured by Nanya Plastics Co., Ltd.) at room temperature in an impregnation machine, and then the cloth is dried for several minutes at 110°C in the impregnation machine to obtain a film (prepreg) having a resin content of 76% by weight.
[0027] Finally, in step ST4, multiple (e.g., four) films are stacked between two copper foils with a thickness of 35 μm and subjected to a pressure of 25 kg / cm 2 The temperature was then kept constant at 85°C for 20 minutes, raised to 185°C at a rate of 3°C / min, and then held constant again for 120 minutes. Then, the temperature was slowly cooled to 130°C to obtain a copper foil substrate (COPPER CLAD LAMINATES, CCL) having a thickness of 0.8 mm.
[0028] Table 1 provides the formulations of several examples and comparative examples of composite substrates, in which the content of each component is expressed in weight percent. [Table 1]
[0029] In Table 1, the spherical inorganic particles dispersed in the dispersion correspond to the first spherical inorganic particles 210 in the embodiment of FIG. 1 or FIG. 2, and the maximum allowable particle size of the spherical inorganic particles dispersed in the dispersion is smaller (5 μm), with the difference between D10 and D90 being less than 500 nm. In Table 1, the maximum allowable particle size of the spherical inorganic particles in the state of a dry powder is larger (45 μm), with the difference between D10 and D90 being greater than 800 nm. In Table 1, the flaky inorganic particles and the nano-spherical inorganic particles correspond to the flaky inorganic particles 220b and the second spherical inorganic particles 220a, respectively, in the embodiment of FIG. 2.
[0030] In Example 1 and Example 3 in Table 1, the spherical inorganic particles, the flake-shaped inorganic particles, and the nano-spherical inorganic particles were dispersed in a dispersion liquid, and then the resin composition was added to form a varnish. In Example 2 in Table 1, the spherical inorganic particles and the nano-spherical inorganic particles were dispersed in a dispersion liquid, and then the resin composition was added to form a varnish. In Comparative Example 1 in Table 1, the spherical inorganic particles and the nano-spherical inorganic particles were mixed in a dry powder state, and then the resin composition was added to form a varnish. In Comparative Example 2 in Table 1, the spherical inorganic particles and the flake-shaped inorganic particles were mixed in a dry powder state, and then the resin composition was added to form a varnish. In Comparative Example 3 in Table 1, the spherical inorganic particles, the flake-shaped inorganic particles, and the nano-spherical inorganic particles were mixed in a dry powder state, and then the resin composition was added to form a varnish. In Comparative Example 4 in Table 1, the spherical inorganic particles dispersed in the dispersion liquid were directly added to the resin composition to form a varnish, and the nano-spherical inorganic particles and the flake-shaped inorganic particles were not added to the dispersion liquid.
[0031] When comparing the packing densities of the inorganic fillers obtained in the various examples and comparative examples in Table 1, it is known that the dense packing effect may not be obtained when using spherical inorganic particles alone in a dry powder state, when using spherical inorganic particles alone in a dry powder state plus nano-inorganic particles, or when using spherical inorganic particles alone in a dry powder state plus flake-shaped inorganic particles, due to their large maximum allowable particle size.
[0032] Also, Table 1 shows that using only a single size of spherical inorganic particles dispersed in the dispersion may not provide the advantage of high packing density, despite the smaller maximum allowable particle size. Only the combination of larger size spherical inorganic particles dispersed in the dispersion with flake inorganic particles and / or nano inorganic particles dispersed in the dispersion can provide a significant reduction in CTE.
[0033] Table 2 provides a comparison of the properties of the composite substrates of several examples and comparative examples of Table 1. [Table 2]
[0034] From the contents of Tables 1 and 2, it can be seen that the CTE in the planar direction of the composite material substrate can be reduced by dispersing an inorganic filler in the dispersion liquid. In addition, from Table 2, it can be seen that, even though the CTE is reduced, Examples 1 to 3 of the present disclosure still have excellent dielectric loss, dielectric constant, and peel strength, and also exhibit excellent performance in the solder heat resistance test at 288°C. [Industrial Applicability]
[0035] With the development of 5G communications, the composite substrates of the present disclosure may be applied in electronic devices and other fields. [Explanation of symbols]
[0036] 10, 20: Composite material substrate 110: Resin composition 200: Inorganic filler 210: First spherical inorganic particle 220a: second spherical inorganic particle 220b: flake-shaped inorganic particles S1,S2: Average particle size ST1, ST2, ST3: Step T: average thickness W: Average diameter
Claims
1. 1. A composite material substrate, comprising: an inorganic filler comprising first spherical inorganic particles and a filler material, wherein the first spherical inorganic particles have an average particle size of 300 nm to 600 nm, the filler material comprises at least one of second spherical inorganic particles and flaky inorganic particles, the second spherical inorganic particles have an average particle size of 20 nm to 50 nm, and the flaky inorganic particles have an average thickness of 0.5 μm to 2 μm; A resin composition comprising a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoxazine resin, wherein the bismaleimide resin is present in an amount of 10% by weight to 70% by weight, the naphthalene ring-containing epoxy resin is present in an amount of 10% by weight to 50% by weight, and the benzoxazine resin is present in an amount of 19.9% by weight to 50% by weight in the resin composition; a dispersant, wherein the inorganic filler, the resin composition and the dispersant are mixed together; A composite substrate comprising:
2. The composite material substrate of claim 1 further comprising: a curing agent, the weight of which is greater than 0 parts by weight and less than or equal to 30 parts by weight per 100 parts by weight of the total of the resin composition; a siloxane binder, the weight of the siloxane binder being 0.1 parts by weight to 4 parts by weight based on 100 parts by weight of the total of the resin composition; and a catalyst, the weight of which is greater than 0 parts by weight and less than or equal to 10 parts by weight per 100 parts by weight of the total of the resin composition; and wherein the inorganic filler, the resin composition, the dispersant, the curing agent, the siloxane coupling agent, and the catalyst are mixed together. Composite material substrate.
3. 10. The composite substrate of claim 1, wherein the filler material comprises the flaky inorganic particles, the flaky inorganic particles having a ratio of average diameter to average thickness of 10 or greater.
4. 2. The composite substrate according to claim 1, wherein the filler material comprises the second spherical inorganic particles, and the ratio of the average particle size of the first spherical inorganic particles to the average particle size of the second spherical inorganic particles is 3 to 20.
5. 2. The composite material substrate according to claim 1, wherein the weight of the inorganic filler is 100 parts by weight to 300 parts by weight per 100 parts by weight of the total of the resin composition.
6. 2. The composite substrate according to claim 1, wherein the maximum allowable particle size of the first spherical inorganic particles is 5 μm or less, the difference between D10 and D90 of the first spherical inorganic particles is less than 500 nm, and the difference between D10 and D90 of the second spherical inorganic particles is less than 20 nm.
7. 1. A method for manufacturing a composite substrate, comprising: a step of mixing an inorganic filler, a dispersant, and a solvent to form a dispersion, the inorganic filler including first spherical inorganic particles and a filler material, the first spherical inorganic particles having an average particle size of 300 nm to 600 nm, the filler material including at least one of second spherical inorganic particles and flaky inorganic particles, the second spherical inorganic particles having an average particle size of 20 nm to 50 nm, and the flaky inorganic particles having an average thickness of 0.5 μm to 2 μm; After forming the dispersion, a step of dissolving a resin composition in the dispersion to form a varnish, the resin composition being a bismaleimide resin, a naphthalene ring-containing epoxy resin, and a benzoic acid resin, forming a varnish comprising a benzoxazine resin, the resin composition comprising 10% by weight to 70% by weight of the bismaleimide resin, 10% by weight to 50% by weight of the naphthalene ring-containing epoxy resin, and 19.9% by weight to 50% by weight of the benzoxazine resin; A manufacturing method comprising:
8. The method of claim 7, further comprising: impregnating a glass fiber cloth with the varnish; drying the varnish and the fiberglass cloth to form a film; A manufacturing method comprising:
9. The method according to claim 8, further comprising: sandwiching the film between two copper foils to obtain a copper foil substrate; A manufacturing method comprising:
Citation Information
Patent Citations
Resin composition for printed wiring board, prepreg, resin substrate, metal clad laminated board, printed wiring board, and semiconductor device
JP2016196548A
Thermosetting resin composition for semiconductor package and prepreg and metal foil laminate using the same
JP2016529371A
Molding material for sealing and electronic part device
JP2017165922A
Thermosetting resin composition for semiconductor packages and prepreg using the same
JP2018518563A
Resin composition, cured product of resin composition, resin sheet, printed wiring board and semiconductor device
JP2020158705A