Mask for stitching exposure process

A two-directional stitching process with energy adjustments and optical proximity corrections addresses interference in line and space patterns, ensuring uniform line widths and stable photoresist thickness for wire grid polarizers.

JP7566379B2Active Publication Date: 2024-10-15KOREA ADVANCED INST OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023549831
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-08
Filing Date
2022-09-16
Publication Date
2024-10-15
Estimated Expiration
2042-09-16

AI Technical Summary

Technical Problem

Existing stitching exposure processes for line and space patterns with line widths of 50 nm or less face interference issues, leading to reduced photoresist thickness and non-uniform line widths, which complicates the formation of wire grid polarizers.

Method used

A new stitching process and mask design that involves exposing a substrate in two directions, with specific energy adjustments and optical proximity corrections to manage interference regions, ensuring uniform line widths and maintaining photoresist thickness.

Benefits of technology

The process effectively forms wire grid polarizers by minimizing interference-related reductions in photoresist thickness and achieving consistent line widths across the substrate, enhancing the stability and performance of the polarizer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566379000001
    Figure 0007566379000001
  • Figure 0007566379000002
    Figure 0007566379000002
  • Figure 0007566379000003
    Figure 0007566379000003
Patent Text Reader

Abstract

According to an embodiment of the present invention, a method for forming a line and space pattern includes exposing a mask to a substrate in a first direction and a second direction, and performing a stitching process, the method includes performing a first exposure process on the substrate such that first shots of the mask contact each other in the first direction, and performing a second exposure process on the substrate such that second shots of the mask contact each other while being spaced apart in the two directions and offset from the first shots in the first direction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to optical proximity correction for photomasks, and more particularly to line and space pattern masks for optical proximity correction to eliminate shot interference effects due to stitching exposure processes. [Background technology]

[0002] A wire grid polarizer is an array of parallel wires arranged on the surface of a substrate, such as glass. Wire grid polarizers are formed with a nanoscale pattern of lines and spaces. Typically, polarizers work when the period (or pitch) of the wire grid is smaller than the wavelength of light.

[0003] In the case of metal wire grid polarizers used in polarized imaging devices, the reflected S-waves are re-reflected and scattered by the peripheral optical and mechanical parts of the imaging device, which causes the polarized image to be obstructed. Therefore, a method is required to reduce the S-wave reflection of the metal wire grid substrate polarizer and also to improve the transmittance of the P-waves.

[0004] In wire grid polarizing filters, the contrast ratio (C / R) increases as the wire grid line width decreases and the wire grid height increases. Therefore, a process in which the wire grid line width is 50 nm or less is required.

[0005] Meanwhile, wire grid polarizing filters require a large area to be used as a large aperture polarizing filter for cameras or flexible displays. However, a stitching exposure process is used as a method for forming a large area die. The stitching exposure process is a technique for continuously combining multiple shots to form a die or chip that is larger than the shot field of a photomask.

[0006] Typically, the exposure equipment's shot fields are spaced apart by a certain distance. This distance is called the scribe line, and a marker is embedded in it to cut out or align the chip. Therefore, the masks are generally spaced apart. Stitching exposure process, which forms a pattern with the mask distance set to "0", is not used. In the stitching exposure process, four shots are placed adjacent to each other on the substrate, so the shots provide interference with each other.

[0007] In particular, in the case of a line and space pattern with a line width of 50 nm or less, four shots are arranged adjacent to each other, so that at a pitch of 100 nm, the shots cannot provide three-times interference with each other to form a line and space pattern.

[0008] Therefore, a new method is required that can perform the stitching process even in the case of a line and space pattern in which the photoresist line width is on the order of 50 nm. Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention provides a new stitching process and a mask for the stitching process that allows line and space patterns to be performed in the stitching process.

[0010] The present invention provides a new stitching process and a mask for the stitching process that can minimize a decrease in thickness of a photoresist due to interference caused by a stitching exposure process.

[0011] The present invention provides a new stitching process and a mask for the stitching process that provides optical proximity correction to provide uniform line width in the stitching exposure process. [Means for solving the problem]

[0012] According to an embodiment of the present invention, a method for forming a line and space pattern includes exposing a mask to a substrate in a first direction and a second direction, and performing a stitching process, the method includes performing a first exposure process on the substrate such that first shots of the mask contact each other in the first direction, and performing a second exposure process on the substrate such that second shots of the mask contact each other while being spaced apart in the two directions and offset from the first shots in the first direction.

[0013] In one embodiment of the present invention, the offset is greater than the width of the interference area of ​​the shot.

[0014] In one embodiment of the present invention, each of the first shots and the second shots includes a reference energy area exposed at a reference energy, a one-time interference area having an energy higher than the reference energy due to interference between the first shots and the second shots, and a two-time interference area having an energy higher than the reference energy due to interference between the first shots and the second shots.

[0015] In one embodiment of the present invention, the single-interference mask region of the mask corresponding to the single-interference region has a first mask linewidth larger than the basic mask linewidth of the reference energy mask region of the mask corresponding to the reference energy region, and the double-interference mask region of the mask corresponding to the double-interference region has a second mask linewidth larger than the mask linewidth of the reference energy mask region of the mask corresponding to the reference energy region.

[0016] In one embodiment of the present invention, the pitch of the line and space pattern is the same in the first shots and the second shots, and the pitch of the photoresist of the line and space pattern is 80 nm to 140 nm.

[0017] In one embodiment of the present invention, the reference energy region is rectangular and located within a rectangular shot, and is located at the center of the shot, the one-time interference region is located on the sides surrounding the reference energy region, and the two-time interference region is locally located between a vertex of the reference energy region and a pair of vertices in the first direction.

[0018] In one embodiment of the present invention, the mask includes a rectangular reference energy mask region, a left region and a right region respectively located on the left and right sides of the reference energy mask region, an upper left vertex region and an upper right vertex region respectively located on the upper left and upper right sides of the reference energy mask region, a lower left vertex region and a lower right vertex region respectively located on the lower left and lower right sides of the reference energy mask region, an upper region located at the top of the reference energy mask region, an upper left region located between the upper region and the upper left vertex region, an upper right region located between the upper region and the upper right vertex region, a lower region located at the bottom of the reference energy mask region, a lower left region located between the lower region and the lower left vertex region, and a lower right region located between the lower region and the lower right vertex region. The line width of the reference energy mask region is a basic mask line width, the line widths of the left region, right region, upper left region, upper right region, lower left region, and lower right region are a first mask line width, and the line widths of the upper region, the lower region, upper left vertex region, upper right vertex region, lower left vertex region, and lower right vertex region are a second mask line width, the second mask line width is greater than the first mask line width, and the first mask line width is greater than the basic mask line width.

[0019] In one embodiment of the present invention, the basic mask line width is 50 nm, the first mask line width is 56 nm, and the second mask line width is 60 nm.

[0020] A wire grid polarizer according to an embodiment of the present invention is manufactured by the line and space pattern forming method according to the first aspect.

[0021] According to an embodiment of the present invention, a mask for forming a line and space pattern is exposed to a substrate in a first direction and a second direction to perform a stitching process. The mask includes a rectangular reference energy mask region formed on a mask substrate in the first direction and the second direction, a one-time interference mask region arranged on sides surrounding the reference energy mask region, and a two-time interference mask region locally arranged between a vertex of the reference energy mask region and a pair of vertices in the first direction. The reference energy mask region has a basic mask linewidth, the one-time interference mask region has the first mask linewidth, and the two-time interference mask region has the second mask linewidth, the second mask linewidth is larger than the basic mask linewidth, and the first mask linewidth is larger than the basic mask linewidth.

[0022] In one embodiment of the present invention, the basic mask line width is 50 nm, the first mask line width is 56 nm, and the second mask line width is 60 nm.

[0023] According to an embodiment of the present invention, a mask for forming an in-and-space pattern is exposed to a substrate in a first direction and a second direction to perform a stitching process, the mask includes a rectangular reference energy mask region, a left region and a right region disposed on the left and right sides of the reference energy mask region, a left upper apex region and a right upper apex region disposed on the left upper side and the right upper side of the reference energy mask region, a left lower apex region and a right lower apex region disposed on the left lower side and the right lower side of the reference energy mask region, an upper region disposed on the upper side of the reference energy mask region, a left upper region disposed between the upper region and the left upper apex region, a right upper region disposed between the upper region and the right upper apex region, a lower region disposed on the lower side of the reference energy mask region, a left lower region disposed between the lower region and the left lower apex region, and a right lower region disposed between the lower region and the right lower apex region. The linewidth of the reference energy mask region is a basic mask linewidth, the linewidths of the left region, right region, upper left region, upper right region, lower left region, and lower right region are a first mask linewidth, and the linewidths of the upper region, the lower region, upper left vertex region, upper right vertex region, lower left vertex region, and lower right vertex region are a second mask linewidth, the second mask linewidth being greater than the basic mask linewidth, and the first mask linewidth being greater than the basic mask linewidth.

[0024] In one embodiment of the present invention, the basic mask line width is 50 nm, the first mask line width is 56 nm, and the second mask line width is 60 nm.

[0025] According to an embodiment of the present invention, a method for manufacturing a mask for forming a line and space pattern includes the steps of: exposing a first mask for forming a line and space pattern on a substrate in a first direction and a second direction, and performing a first stitching process; measuring an exposure energy or a linewidth of a one-time interference region having energy higher than a reference energy without interference due to one-time interference of shots by the first stitching process; measuring an exposure energy or a linewidth of a two-time interference region having energy higher than a reference energy due to two-time interference of shots by the first stitching process; performing a first optical proximity correction based on the exposure energy or the linewidth of the one-time interference region to increase a linewidth of a one-time interference mask region of the first mask corresponding to the one-time interference region, and performing a second optical proximity correction based on the exposure energy or the linewidth of the two-time interference region to increase a linewidth of a two-time interference mask region of the first mask corresponding to the two-time interference region, thereby forming a second mask.

[0026] In one embodiment of the present invention, the first stitching process includes a step of performing a first exposure process on the substrate such that first shots of the first mask contact each other in the first direction, and a step of performing a second exposure process on the substrate such that second shots of the first mask contact each other while being spaced apart in the two directions and offset from the first shots.

[0027] In one embodiment of the present invention, the first optical proximity correction has the same pitch and increases the line width by a first variation amount, and the second optical proximity correction has the same pitch and increases the line width by a second variation amount, the second variation amount being greater than the first variation amount, and the first variation amount being proportional to the difference between the exposure energy of the one-time interference area and the basic exposure energy of the non-interference area. Effect of the Invention

[0028] The mask according to the embodiment of the present invention can form a wire grid polarizer over the entire substrate by performing a stitching process of a line and space pattern.

[0029] A wire grid polarizer according to an embodiment of the present invention may be formed by cutting a line and space pattern formed by a stitching process to a predetermined standard. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Shot field interference causes flare interference up to 10 um outside the shot field area, which changes the spatial uniformity of the exposure energy and creates an interference area that exceeds the reference exposure energy.

[0031] Shot field interference or shot interference generates a triple interference region, and the triple interference region collapses due to energy overexposure. In addition, the triple interference region cannot be corrected through optical proximity correction (OPC) under the condition of a 50 nm line width. On the other hand, the triple interference region can be corrected through OPC under the condition of a 60 nm line width. However, when OPC is performed on the triple interference region, the thickness of the photoresist (PR) pattern is significantly reduced. As a result, when etching the lower conductive film using the photoresist pattern as an etching mask, there is a limit to the etching depth, and the etching selectivity or etching aspect ratio is significantly reduced. This reduces the performance of the metal wire grid polarizer.

[0032] The stitching method according to an embodiment of the present invention uses shot offset to remove the triple interference region and generate only the single interference region and the double interference region. The single interference region and the double interference region increase the range of patternable pitches, while the line width of the photoresist in the single interference region and the second interference region decreases.

[0033] According to one embodiment of the present invention, the reduction in the line width of the photoresist in the first interference region and / or the second interference region is corrected through mask optical proximity correction (OPC). The first interference region and the second interference region are corrected through mask optical proximity correction (OPC). As a result, the same line width is obtained in all regions. In addition, the triple interference region is removed to expand the conditions for performing optical proximity correction (OPC). In addition, the triple interference region is removed to suppress the reduction in the thickness of the remaining photoresist.

[0034] According to an embodiment of the present invention, even if a pattern collapses in the second interference region, the pattern collapse in the second interference region is suppressed through optical proximity correction (OPC).

[0035] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the embodiments described herein, and may be embodied in different forms. Rather, the embodiments described herein are provided so that the disclosure will be thorough and complete, and will fully convey the concept of the present invention to those skilled in the art. In the drawings, the dimensions of components are exaggerated for clarity. The same reference numerals are used throughout the specification to refer to the same components.

[0036] FIG. 1 is a conceptual diagram illustrating exposure of an entire substrate by a stitching process according to an embodiment of the present invention.

[0037] FIG. 2 is an enlarged view showing the shot interference pattern caused by the stitching process of FIG.

[0038] FIG. 3 is an electron microscope photograph showing the interference morphology of the shot of FIG.

[0039] FIG. 4 is a graph showing the line width of the photoresist as a function of the exposure energy under the conditions of mask pitch (P=100 nm) and mask line width (LW=50 nm).

[0040] As shown in Figures 1 to 4, the stitching process exposes a number of shots 12 in a first direction (x-axis direction). Then, after being spaced apart at a predetermined interval in a second direction (y-axis direction), the shots 12 are exposed again in the first direction. This causes the shots 12 to be aligned in a matrix. Each shot 12 is exposed in a square shape. Each shot is an area where a mask 14 is exposed by an exposure tool to form a pattern in the photoresist on a substrate.

[0041] Each shot 12 has a rectangular shape. Each shot 12 has a reference energy region 20 in the center where no interference is formed, a one-time interference region 22 having one-time interference on the sides of the rectangle, and a three-time interference region 24 having three-times interference on the vertices of the rectangle. The width W of the one-time interference region 22 is on the order of 10 um. The width W of the three-time interference region 24 is on the order of 10 um. The width W of the interference region is determined by the shot field flare interference.

[0042] The width W of the interference region depends on the local flare effect. DUV (deep ultra violet) lithography generates a lot of stray light by passing through dozens of projection lenses after passing through a reticle or mask. The stray light appears as a flare phenomenon. In the DUV lithography process, the stray light generates flare in almost 10um area. The exposure tool is an ArF immersion scanner or an ArF stepper. The photoresist is a positive photoresist.

[0043] When a stitching process is performed on a line and space pattern with a line width of 100 nm or more, the effect of shot interference is relatively small compared to the line width, i.e., the sensitivity of photoresist reaction is low in a line and space pattern process with a line width of 100 nm or more.

[0044] However, as the line width decreases below 100nm, the area where the line and space pattern remains standing without collapsing due to the energy change of the photoresist decreases. In order for the line width to remain standing without collapsing, i.e. to become an effective line width, an appropriate energy range must be exposed. The CD (Critical Dimension) value fluctuates according to the amount of change in exposure energy. The effective energy fluctuation range is the energy latitude. The greater the energy latitude, the more stable the stitching pattern process can be formed.

[0045] For example, in the case of DUV lithography, interference due to a local flare effect occurs up to 10 um beyond each shot area.

[0046] In the case of a 100 nm line pattern, the line pattern is formed with a line width reduced by 10 to 20 nm. However, in the case of a 50 nm line pattern, the photoresist disappears completely due to the effect of flare, and no pattern is formed.

[0047] According to the present invention, in the reference energy region 20, the energy latitude is about ±9%, and the reference energy region 20 has an exposure energy of the reference energy BE. The single interference region 22 is a region where shot interference occurs once, and has an energy exposure of BE+A with one interference. A is the exposure energy (about 6 mJ / cm^2) added by one interference. The triple interference region 124 is a region where shot interference occurs three times, and has an energy exposure of BE+3A with three interferences. That is, BE+A is 125% compared to the reference energy BE, and BE+3A is =175% compared to the reference energy BE.

[0048] As a result of checking the degree of interference between the one-time interference region 22 and the three-time interference region 24, the one-time interference amount A is about 20 to 30% of BE, which is about 6 mJ / cm^2. For example, the reference energy BE is about 24 mJ / cm^2, and BE+A is about 30 mJ / cm^2. BE+3A is about 48 mJ / cm^2. That is, the exposure energy increases in proportion to the reference energy BE according to the interference recovery.

[0049] The smallest mask line width that an ArF immersion lithography tool can provide is 38 nm. Smaller mask line patterns are unable to transmit light.

[0050] To perform the stitching process with a 50nm photoresist line pattern, if it is a positive photoresist, it is composed of a 50nm line (where the light is hidden by the reticle) and a 50nm space (where the light passes through) of the mask. The sum of the line width and space width of the mask is the pitch.

[0051] The photoresist pitch should be 100 nm and the photoresist line width should be 50 nm over the entire surface of the substrate including the interference region.

[0052] If the reference exposure energy BE for achieving a line width of 50 nm in a photoresist line and space pattern is 100%, the triple interference region, which is the section of excess energy due to interference, is BE+3A, and receives 175% energy compared to the reference energy.

[0053] As shown in FIG. 4, the energy of the triple interference region 24 is 175%, so the photoresist line width is significantly reduced from 50 nm, and the line pattern is destroyed according to the experimental results using an ArF exposure tool.

[0054] On the other hand, even when optical proximity correction (OPC) is performed so as not to destroy the pattern of the triple interference region 24, the mask minimum line width is configured with a space width of 38 nm and a line width of 62 nm (to minimize the light transmitting portion) at a mask pitch of 100 nm. The mask minimum line width of 38 nm, that is, the space width, is determined by the wavelength of the exposure tool and the optical characteristics of the lens.

[0055] Even if a mask space width of 38 nm is applied, the exposure energy required to realize a 50 nm line width of the photoresist is about 160% of the energy, but the triple interference region is exposed to 175% of the energy, making it impossible to form a pattern.

[0056] As a result, even if the mask is subjected to optical proximity correction (OPC), it is not possible to correct the pattern width to 38 nm or less. Therefore, if the mask has the triple interference region 24, it is not possible to form a stitching line and space pattern having a photoresist line width of 50 nm.

[0057] FIG. 5 shows an experimental result showing the line width of a photoresist depending on exposure energy for each line width of a mask according to an embodiment of the present invention.

[0058] As shown in Figure 5, the mask pitch is twice the mask line width. The mask line widths are 40 nm (white circle), 44 nm (black circle), 50 nm (gray circle), 60 nm (white square), 70 nm (black square), 80 nm (gray square), and 90 nm (triangle), respectively. Therefore, the mask pitches are 80, 84, 100, 120, 140, 160, and 180 nm, respectively.

[0059] For a mask line width of 50 nm, the standard energy of the ArF exposure tool is 24 mJ / cm^2. If the exposure energy is 36 mJ / cm^2 or more, the photoresist pattern is not formed. The triple interference area has an energy of 42 mJ / cm^2, so the photoresist pattern is not formed.

[0060] For a mask line width of 60 nm, the reference energy is 23 mJ / cm^2. If the exposure energy is 40 mJ / cm^2 or more, the photoresist pattern is not formed. The triple interference area has an energy of 41 mJ / cm^2 (=23+3x6), so the photoresist pattern is not formed.

[0061] For a mask line width of 70 nm, the reference energy is 20 mJ / cm^2. If the exposure energy is more than 46 mJ / cm^2, the photoresist pattern will not be formed. The triple interference region has an energy of 42 mJ / cm^2 (=20+3x6), so the photoresist pattern can be formed. However, in the triple interference region, the line width of the photoresist is significantly reduced, making it impossible to provide stable wire grid polarizer characteristics. In the triple interference region, the thickness of the photoresist is significantly reduced, making the subsequent etching process difficult.

[0062] For mask line widths of 40nm and 44nm, the reference energy is about 23mJ / cm^2. When the exposure energy is about 34mJ / cm^2 or more, the photoresist pattern is not formed. The double interference area has an energy of 35mJ / cm^2 (23+2x6), so the photoresist pattern is not formed.

[0063] Using the stitching process of the present invention, the interference region is removed three times, so the stitching process is performed with a mask line width of 50 nm (100 nm pitch) and a mask line width of 60 nm (120 nm pitch).

[0064] Using the stitching process of the present invention, the interference regions are removed three times with a mask line width of 40 nm (80 nm pitch) and a mask line width of 44 nm (880 nm pitch), and the stitching process is performed through the proximity optical correction described below, thereby forming a photoresist pattern.

[0065] In addition, the stitching process of the present invention can be performed at a mask line width of 70 nm (140 nm pitch) or greater. The stitching process of the present invention removes interference areas three times even at a mask line width of 70 nm or greater, forming a stable photoresist pattern.

[0066] FIG. 6 is a conceptual diagram illustrating a stitching process according to an embodiment of the present invention.

[0067] FIG. 7 is an enlarged view showing the stitching process of FIG.

[0068] FIG. 8 is an electron microscope photograph showing the shot of FIG.

[0069] 6 to 8, the line and space pattern forming method forms a line and space pattern by exposing a mask to a substrate in a first direction (x-axis direction) and a second direction (y-axis direction) and performing a stitching process. The line and space pattern forming method includes a step of performing a first exposure process on the substrate so that first shots 112a of the mask contact each other in the first direction, and a step of performing a second exposure process on the substrate so that second shots 112b of the mask contact each other while being spaced apart in the two directions and offset from the first shots.

[0070] The first shot 112a and the second shot 112b sequentially expose the substrate 10. The exposure tool is an ArF scanner or an ArF stepper.

[0071] The substrate 10 is a semiconductor substrate or a glass substrate. The photoresist (not shown) coated on the substrate 10 is a positive photoresist or a negative photoresist. After the stitching exposure process, a baking process and a development process are performed. After forming a line and space pattern of the photoresist, the conductive film is etched using the line and space pattern of the photoresist as an etching mask to form a wire grid. The substrate 10 is cut to a size larger than the shot to provide the metal wire grid polarizer 30.

[0072] The mask (not shown) has the same pitch and the same line width in all areas. The exposure tool exposes the mask (not shown) at a magnification of 1:1.

[0073] The offset between the first shot 112a and the second shot 112b is greater than the width W of the interference region. The offset is greater than the width W of the interference region. The width W of the interference region is about 10 um. Preferably, the offset of the second shot 112b is half (D / 2) the size of the first shot in the first direction.

[0074] Each of the first shots and the second shots includes a reference energy region 120 exposed with a reference energy, one-time interference regions 122, 123 exposed with an energy BE+A higher than the reference energy BE due to interference between the first shots and the second shots, and two-time interference regions 124, 126 exposed with an energy BE+2A higher than the reference energy due to interference between the first shots and the second shots. As a result of checking the degree of interference between the one-time interference regions 122, 123 and the two-time interference regions 124, 126, the first interference amount A is about 20 to 30% of BE.

[0075] In the line and space pattern, the line width is 50 nm in the reference energy region 120. The reference energy is the exposure energy set to pattern the line width of the mask to the desired line width of the photoresist. The reference energy is determined by the pitch of the mask.

[0076] As shown in Figure 8, a mask without optical proximity correction is used. The mask pitch is 100 nm, and the mask line width is 50 nm. The photoresist line width in the reference energy region 120 is about 50 nm. The photoresist line width in the one-time interference regions 122 and 123 is about 40 nm. The line width in the two-time interference regions 124 and 126 is about 38 nm.

[0077] The pitch of the line and space pattern is the same in the first shot 112a and the second shot 112b, and the line width of the line and space pattern is 38 nm to 50 nm depending on the interference area.

[0078] Therefore, the line width is changed depending on the interference area at the same pitch, which changes the polarizer characteristics, and therefore optical proximity correction (OPC) is required on the mask to provide substantially the same line width in all interference areas.

[0079] The first optical proximity correction for the single-interference regions 122, 123 has the same pitch, and increases the line width of the mask by a first variation amount. The second optical proximity correction for the double-interference regions 124, 126 has the same pitch, and increases the line width of the mask by a second variation amount. The second variation amount is greater than the first variation amount, and the first variation amount is proportional to a difference A between the exposure energy of the single-interference region and the basic exposure energy of the non-interference region. The difference between the exposure energy of the single-interference region and the basic exposure energy of the non-interference region is the single-interference amount A, which is about 20 to 30% of BE.

[0080] FIG. 9 is an experimental result showing photoresist line width as a function of exposure energy according to mask line width at the same pitch in accordance with one embodiment of the present invention.

[0081] As shown in Figure 9, the photoresist is a positive photoresist. The pitch of the mask is 100 nm, and the line width is 50 nm, 56 nm, or 60 nm, respectively. The exposure process was performed through an ArF immersion scanner process at a magnification of 1:1.

[0082] For a mask line width of 50 nm (squares), after exposure and development steps, the line width of the photoresist is plotted as a function of exposure energy.

[0083] For a mask line width of 56 nm (triangles), after exposure and development steps, the photoresist line width is plotted as a function of exposure energy.

[0084] When the mask line width is 60 nm (circle), after the exposure and development process, the photoresist line width is plotted as a function of the exposure energy.

[0085] For a mask line width of 50 nm (square), the reference exposure energy BE to obtain a photoresist line width of 50 nm is approximately 24 mJ / cm^2.

[0086] The single interference region is exposed with energy BE+A, which is higher than the reference energy BE. Therefore, the exposure energy BE+A of the single interference region is 30mJ / cm^2, and when the mask line width is 56nm (triangle), the photoresist line width is 50nm.

[0087] The double interference region is exposed with an energy BE+2A higher than the reference energy BE. Therefore, the exposure energy BE+2A of the double interference region is 36 mJ / cm^2, and when the mask line width is 60 nm (circle), the photoresist line width is 50 nm.

[0088] In conclusion, the optical proximity correction is set so that the mask line width is 56 nm so that the line width of the one-time interference region is kept at 50 nm, and the optical proximity correction is set so that the mask line width is 60 nm so that the line width of the two-time interference region is kept at 50 nm.

[0089] Returning to Figures 5 and 9, for the mask line widths of 40 nm and 44 nm in Figure 5, the reference energy is 23 mJ / cm^2. When the exposure energy is about 34 mJ / cm^2 or more, the photoresist pattern is not formed. The double interference area has an energy of 35 mJ / cm^2 (23+2x6), so the photoresist pattern is not formed.

[0090] However, when the line width of the mask is increased at the same pitch through the optical proximity correction of the mask, the line width of the photoresist due to the exposure energy is shifted to the upper right corner as shown in Figures 5 and 9. For example, for a mask line width of 44 nm (pitch 88 nm), a photoresist pattern can be created by optical proximity correction of the mask line width to 50 nm (pitch 88 nm) in the double interference region.

[0091] As shown in Figures 5 and 9, for example, if a mask line width of 40 nm (pitch 80 nm) is corrected to a mask line width of 42 nm (pitch 80 nm) through optical proximity correction of the mask for the double interference region, a photoresist pattern is formed.

[0092] According to a modified embodiment of the present invention, in the stitching process with offset, the proximity optical correction is performed only on one of the one-time interference region and the two-time interference region, and preferably, the proximity optical correction is performed only on the two-time interference region.

[0093] FIG. 10A is a conceptual diagram showing the regional characteristics of a mask and resist without OPC according to one embodiment of the present invention.

[0094] FIG. 10B is a conceptual diagram showing characteristics of a mask and resist by region having an OPC according to an embodiment of the present invention.

[0095] As shown in FIG. 10A, a mask without OPC has a pitch P of 100 nm, the mask line width is 50 nm, and the mask space width is 50 nm.

[0096] The reference energy region 120 of the photoresist has an exposure energy of BE (approximately 24 mJ / cm^2). The single interference regions 122, 123 of the photoresist have an exposure energy of BE+A (approximately 30 mJ / cm^2). The double interference regions 124, 126 of the photoresist have an exposure energy of BE+2A (approximately 36 mJ / cm^2). The single interference regions 122, 123 have a reduced photoresist height due to flare interference of 6 mJ. The double interference regions 124, 126 of the photoresist have a reduced photoresist height due to flare interference of 12 mJ.

[0097] If it is assumed that there is a triple interference region, the height of the photoresist is further reduced by the 18 mJ flare interference, so that the stitching process with the triple interference region does not proceed with a limited under-etching process due to the low photoresist thickness.

[0098] However, the present invention removes the triple interference region. The present invention has only the single interference region and the double interference region. The stitching process of the present invention suppresses the reduction in the thickness of the photoresist, and the subsequent etching process proceeds stably.

[0099] As shown in FIG. 10B, when the mask with OPC has a pitch P of 100 nm, the line widths of the mask are 50 nm, 56 nm, and 60 nm for each interference region, and the space widths of the mask are 50 nm, 44 nm, and 40 nm for each interference region.

[0100] The reference energy mask region 311 has a basic mask linewidth LW. The one-time interference mask regions 312a, 312b, 316a, 316b, 317a, 317b have the first mask linewidth LW1. The two-time interference mask regions 313a, 313b, 314a, 314b, 315a, 315b have the second mask linewidth LW2. The second mask linewidth LW2 is larger than the first mask linewidth LW1, and the first mask linewidth LW1 is larger than the basic mask linewidth LW. The one-time interference mask regions 312a, 312b, 316a, 316b, 317a, 317b increase the linewidth of the chrome pattern and reduce the exposure energy profile. This increases the linewidth of the photoresist.

[0101] That is, the basic mask space width SW=P-LW of the reference energy mask region 311 is 50 nm. The first mask space width SW1=P-LW1 of the one-time interference mask regions 312a, 312b, 316a, 316b, 317a, and 317b is 44 nm. The second mask space width SW2=P-LW2 of the two-time interference mask regions 313a, 313b, 314a, 314b, 315a, and 315b is 40 nm. Due to the reduced space width, the space width of the photoresist is reduced to maintain 50 nm. That is, due to the reduced space width, the line width of the photoresist is increased to maintain 50 nm.

[0102] The reference energy region 220 of the photoresist has an exposure energy of BE (approximately 24 mJ / cm^2). The single interference regions 222, 223 of the photoresist have an exposure energy of BE+A (approximately 30 mJ / cm^2) but have a narrower energy profile. The double interference regions 224, 226 of the photoresist have an exposure energy of BE+2A (approximately 36 mJ / cm^2) but have a narrower energy profile. The reduced energy profile reduces the space width of the photoresist.

[0103] Therefore, the single-interference regions 222 and 223 of the photoresist and the double-interference regions 224 and 226 of the photoresist all have the same line width of 50 nm, which allows the metal wire grid polarizer to provide stable characteristics. FIG. 11A shows the variation in mask optical proximity correction due to differences in exposure energy at a mask pitch of 100 nm in one embodiment of the present invention.

[0104] As shown in Figure 11A, to obtain the same photoresist line width of 50 nm in all interference regions, the variation in mask optical proximity correction due to the exposure energy difference can be seen. The amount of interference due to one-time interference is A, the amount of interference due to two-time interference is 2A, and the amount of interference due to three-time interference is 3A. To perform optical proximity correction for the amount of interference A due to one-time interference, the mask line width is corrected from 50 nm to 56 nm. To perform optical proximity correction for the amount of interference 2A due to two-time interference, the mask line width is corrected from 50 nm to 60 nm.

[0105] Meanwhile, in order to optically correct the interference amount 3A due to triple interference, the line width of the mask is corrected from 50nm to approximately 65nm. However, when the mask line width is 65nm, the space line width is 35nm (100-65nm). In this case, the ArF exposure tool does not form a pattern due to the limitations of the tool. Therefore, such conditions cannot be achieved. After correcting the mask line width to 62nm (the limit of the ArF immersion equipment), an exposure experiment was conducted on the triple interference area, but the height of the photoresist was significantly reduced and the line width also collapsed, failing to approach by 40nm.

[0106] FIG. 11B shows the variation in mask optical proximity correction due to differences in exposure energy at a mask pitch of 120 nm in one embodiment of the present invention.

[0107] As shown in Figure 11B, in all interference regions, the variation in mask optical proximity correction due to the exposure energy difference can be seen to obtain the same photoresist line width of 60 nm. The amount of interference due to one-time interference is A, the amount of interference due to two-time interference is 2A, and the amount of interference due to three-time interference is 3A. To perform optical proximity correction for the amount of interference A due to one-time interference, the mask line width is corrected from 60 nm to 66 nm. To perform optical proximity correction for the amount of interference 2A due to two-time interference, the mask line width is corrected from 60 nm to 70 nm.

[0108] To optically correct the interference amount 3A caused by triple interference, the mask line width is corrected from 60nm to 75nm. However, when the mask line width is 75nm, the space width is 45nm (120-75nm). Although an ArF exposure tool can form a photoresist pattern with a mask line width of 75nm, the height of the photoresist pattern is significantly reduced. This makes it difficult to proceed with the subsequent etching process. The difference in photoresist height will cause a decrease in the transmittance performance of wire grid polarizers in the future.

[0109] FIG. 12 is an electron micrograph showing a shot of photoresist using a mask with optical proximity correction according to one embodiment of the present invention.

[0110] 12, when a stitching process with offset is performed using a mask with optical proximity correction, the first shot 212a and the second shot 212b each have an exposure energy of BE (about 24 mJ / cm^2) in the reference energy region 220. The first interference regions 222 and 223 have an exposure energy of BE+A (about 30 mJ / cm^2). The second interference regions 224 and 226 have an exposure energy of BE+2A (about 36 mJ / cm^2).

[0111] The reference energy region 220 is a rectangle located within a rectangular shot and is located at the center of the shot, the one-time interference regions 222, 223 are located on the sides surrounding the reference energy region, and the two-time interference regions 224, 226 are locally located between a vertex of the reference energy region and a pair of vertices in the first direction.

[0112] The following description will be given for a case where the magnification of the mask and the photoresist pattern is 1. A single-interference mask region of the mask corresponding to the single-interference region has a first mask linewidth larger than a basic mask linewidth of a reference energy mask region of the mask corresponding to the reference energy region.

[0113] A double-interference mask region of the mask corresponding to the double-interference region has a second mask linewidth that is greater than a mask linewidth of a reference energy mask region of the mask corresponding to the reference energy region.

[0114] Therefore, in order to obtain a photoresist line width of 50 nm in the one-time interference region, the corresponding mask line width is increased to 56 nm, while in order to obtain a photoresist line width of 50 nm in the two-time interference region, the corresponding mask line width is increased to 60 nm.

[0115] According to the experimental results of the present invention, the line width of the reference energy region 220 is 50 nm, the line width of the single-interference regions 222 and 223 is 50 nm, and the line width of the double-interference regions 224 and 226 is 48 nm. Therefore, the double-interference regions 224 and 226 are 2 nm off the target value of 50 nm, but are within the error range. Therefore, the optical proximity correction forms a uniform line and space pattern that is not dependent on shot interference.

[0116] According to a modified embodiment of the present invention, the pitch of the line and space pattern is the same in the first shot 212as and the second shot 212b, and the line width of the line and space pattern is 38 nm to 50 nm.

[0117] The experiments of the present invention were carried out using an ArF immersion exposure tool, but the present invention is similarly applicable to an EUV exposure tool.

[0118] FIG. 13 is a conceptual diagram showing a mask with optical proximity correction according to one embodiment of the present invention.

[0119] 13, a mask 314 that has undergone optical proximity correction includes a rectangular reference energy mask region 311 formed in the first and second directions on a mask substrate 310, one-time interference mask regions 312a, 312b, 316a, 316b, 317a, and 317b arranged on the sides so as to surround the reference energy mask region 311, and two-time interference mask regions 313a, 313b, 314a, 314b, 315a, and 315b that are locally arranged between the vertices of the reference energy mask region and a pair of vertices in the first direction. The width W' of the one-time interference mask regions 312a, 312b, 316a, 316b, 317a, and 317b corresponds to the width W of the interference region of the shot.

[0120] The reference energy mask region 311 has a basic mask linewidth. The one-time interference mask regions 312a, 312b, 316a, 316b, 317a, 317b have the first mask linewidth. The two-time interference mask regions 313a, 313b, 314a, 314b, 315a, 315b have the second mask linewidth. The second mask linewidth is larger than the first mask linewidth, and the first mask linewidth is larger than the basic mask linewidth. The one-time interference mask regions 312a, 312b, 316a, 316b, 317a, 317b increase the linewidth of the chrome pattern and reduce the exposure energy profile. This increases the linewidth of the photoresist.

[0121] The mask 314 that has undergone optical proximity correction includes a rectangular reference energy mask region 311, a left region 312a and a right region 312b that are respectively disposed on the left and right sides of the reference energy mask region 311, and a left upper vertex region 313a and a right upper vertex region 313b that are respectively disposed on the upper left and upper right sides of the reference energy mask region 311. The energy mask region 311 includes a right upper vertex region 313b, a left lower vertex region 314a and a right lower vertex region 314b respectively arranged at the left lower and right lower portions of the reference energy mask region 311, an upper region 315a arranged at the upper portion of the reference energy mask region 311, a left upper region arranged between the upper region 315a and the left upper vertex region 313a, a right upper region 316b arranged between the upper region 315a and the right upper vertex region 313b, a lower region 315b arranged at the lower portion of the reference energy mask region 311, a left lower region 317a arranged between the lower region 315b and the left lower vertex region 314a, and a right lower vertex region 314b arranged between the lower region 315b and the right lower vertex region 315b.

[0122] The line width of the reference energy mask region 311 is a basic mask line width. The line width of the left region 312a, the right region 312b, the left upper region 316a, the right upper region 316b, the left lower region 317a, and the right lower region 317b is a first mask line width. The line width of the upper region 315a, the lower region 315b, the left upper vertex region 313a, the right upper vertex region 313b, the left lower vertex region 314a, and the right lower vertex region 314b is a second mask line width. The second mask line width is larger than the first mask line width, and the first mask line width is larger than the basic mask line width.

[0123] When the magnification ratio between the mask pattern and the photoresist pattern is 1:1, the basic mask line width is 50 nm, the first mask line width is 56 nm, and the second mask line width is 60 nm.

[0124] When the magnification ratio between the mask pattern and the photoresist pattern is 4:1, the basic mask line width is 50x4 nm, the first mask line width is 56x4 nm, and the second mask line width is 60x4 nm.

[0125] FIG. 14 is an enlarged view showing a stitching process according to another embodiment of the present invention.

[0126] FIG. 15 is a diagram showing a mask for performing a stitching process in another embodiment of the present invention.

[0127] 14 and 15 show the result of a stitching process using a mask that has been subjected to optical proximity correction. The method of forming a line and space pattern includes exposing a mask 500 to a substrate in a first direction and a second direction and performing a stitching process. The method of forming a line and space pattern includes performing a first exposure process on the substrate such that first shots 412a of the mask contact each other in the first direction, and performing a second exposure process on the substrate such that second shots 412b of the mask contact each other while being spaced apart in the two directions and offset from the first shots 412a in the first direction. The offset is greater than a width W of an interference region of the shots.

[0128] Each of the first shot 412a and the second shot 412b includes a reference energy region 420 exposed at a reference energy, one-time interference regions 422, 423 having energy higher than the reference energy due to interference between the first shot and the second shot, and two-time interference regions 424, 426 having energy higher than the reference energy due to interference between the first shot and the second shot.

[0129] The one-time interference mask regions 512 a , 512 b , 516 a , 516 b , 517 a , and 517 b of the mask 500 corresponding to the one-time interference regions 422 , 423 have a first mask linewidth that is greater than the basic mask linewidth of the reference energy mask region 511 of the mask corresponding to the reference energy region 420 .

[0130] The two-time interference mask regions 513a, 513b, 514a, 514b, 515a, 515b of the mask 500 corresponding to the two-time interference regions 424, 426 have a second mask linewidth greater than the mask linewidth of the reference energy mask region of the mask corresponding to the reference energy region.

[0131] The pitch of the line and space pattern is the same in the first shot 412a and the second shot 412b, and the line width of the line and space pattern is 38 nm to 50 nm.

[0132] The reference energy region 420 is a square located in the center of a shot having a square shape. The one-time interference regions 422 and 423 are located on the sides surrounding the reference energy region.

[0133] The two-time interference regions 424, 426 are locally disposed between a vertex of the reference energy region 420 and a pair of vertices in the first direction.

[0134] The mask 500 includes a rectangular reference energy mask region 511, a left region 512a and a right region 512b disposed on the left and right sides of the reference energy mask region, an upper left vertex region 513a and an upper right vertex region 513b disposed on the upper left and upper right sides of the reference energy mask region 511, a lower left vertex region 514a and a lower right vertex region 514b disposed on the lower left and lower right sides of the reference energy mask region 511, and a lower right vertex region 514b disposed on the upper part of the reference energy mask region 511. the left upper region 516a disposed between the upper region 515a and the left upper vertex region 513a; the right upper region 516b disposed between the upper region 515a and the right upper vertex region 513b; the lower region 515b disposed at the bottom of the reference energy mask region 511; the left lower region 517a disposed between the lower region 515b and the left lower vertex region 514a; and the right lower region 517a disposed between the lower region 515b and the right lower vertex region 514b.

[0135] The line width of the reference energy mask region 511 is a basic mask line width. The line widths of the left region 512a, the right region 512b, the left upper region 516a, the right upper region 516b, the left lower region 517a, and the right lower region 517b are a first mask line width. The line widths of the upper region 515a, the lower region 515b, the left upper vertex region 513a, the right upper vertex region 513b, the left lower vertex region 514a, and the right lower vertex region 514b are a second mask line width. The second mask line width is larger than the first mask line width, and the first mask line width is larger than the basic mask line width.

[0136] When the magnification between the mask and the photoresist pattern is 1:1, the basic mask line width is 50 nm, the first mask line width is 56 nm, and the second mask line width is 60 nm.

[0137] FIG. 16 shows linewidth of a negative photoresist according to another embodiment of the present invention.

[0138] The photoresist is a negative photoresist, as shown in Figure 16. The pitch of the mask is 100 nm, and the line width is 50 nm, 56 nm, or 60 nm. The exposure process is performed through an ArF immersion scanner process at a magnification of 1:1.

[0139] For a mask line width of 50 nm (squares), after exposure and development steps, the line width of the photoresist is plotted as a function of exposure energy.

[0140] For a mask line width of 56 nm (triangles), after exposure and development steps, the photoresist line width is plotted as a function of exposure energy.

[0141] When the mask line width is 60 nm (circle), after the exposure and development process, the photoresist line width is plotted as a function of the exposure energy.

[0142] For a mask line width of 50 nm (square), the reference exposure energy BE to obtain a photoresist line width of 50 nm is approximately 20 mJ / cm^2.

[0143] The single interference region is exposed with energy BE+A, which is higher than the reference energy BE. Therefore, the exposure energy BE+A of the single interference region is 24 mJ / cm^2, and when the mask line width is 56 nm (triangle), the photoresist line width is 50 nm.

[0144] The double interference region is exposed with an energy BE+2A higher than the reference energy BE. Therefore, the exposure energy BE+2A of the double interference region is 28mJ / cm^2, and when the mask line width is 60nm (circle), the photoresist line width is 50nm.

[0145] In conclusion, the optical proximity correction is set so that the mask line width is 56 nm so that the line width of the one-time interference region is kept at 50 nm, and the optical proximity correction is set so that the mask line width is 60 nm so that the line width of the two-time interference region is kept at 50 nm.

[0146] FIG. 17 is a flow chart for explaining a method for manufacturing a mask for forming a line and space pattern.

[0147] As shown in FIG. 17, a method for manufacturing a mask for forming a line and space pattern includes a step S110 of exposing a first mask for forming a line and space pattern in a first direction and a second direction on a substrate and performing a first stitching process, a step S120 of measuring an exposure energy or a line width of a one-time interference region having energy higher than a reference energy without interference due to one-time interference of shots by the first stitching process, a step S130 of measuring an exposure energy or a line width of a two-time interference region having energy higher than a reference energy due to two-time interference of shots by the first stitching process, and a step S140 of forming a second mask by performing a first optical proximity correction based on the exposure energy or line width of the one-time interference region to increase a line width in a one-time interference mask region of the first mask corresponding to the one-time interference region and performing a second optical proximity correction based on the exposure energy or line width of the two-time interference region to increase a line width in a two-time interference mask region of the first mask corresponding to the two-time interference region.

[0148] The first stitching process S110 includes a step of performing a first exposure process on the substrate so that first shots of the first mask contact each other in the first direction, and a step of performing a second exposure process on the substrate so that second shots of the first mask contact each other while being spaced apart in the two directions and offset from the first shots.

[0149] The first optical proximity correction has the same pitch and increases the line width by a first variation amount, and the second optical proximity correction has the same pitch and increases the line width by a second variation amount, the second variation amount being greater than the first variation amount, and the first variation amount being proportional to a difference between an exposure energy of the one-time interference area and a base exposure energy of an interference-free area.

[0150] Then, a stitching process is performed using the second mask on which the first and second optical proximity corrections have been performed.

[0151] Although the present invention has been illustrated and described with respect to specific preferred embodiments, the present invention is not limited to such embodiments and includes all various forms of embodiments that can be implemented by a person having ordinary skill in the art to which the invention pertains without departing from the technical spirit of the present invention as claimed in the claims. [Brief description of the drawings]

[0152] [Figure 1] 1 is a conceptual diagram illustrating exposure of an entire substrate by a stitching process according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an enlarged view showing the interference pattern of shots due to the stitching process of FIG. 1. [Diagram 3] 3 is an electron microscope photograph showing the interference morphology of the shot in FIG. 2. [Figure 4] 1 is a graph showing photoresist line width as a function of exposure energy under the condition of mask pitch (P=100 nm) and mask line width (LW=50 nm). [Diagram 5] 11 is an experimental result showing a line width of a photoresist depending on exposure energy for each line width of a mask according to an embodiment of the present invention. [Figure 6] 1 is a conceptual diagram illustrating a stitching process according to an embodiment of the present invention. [Figure 7] FIG. 7 is an enlarged view showing the stitching step of FIG. 6. [Figure 8] 7 is an electron microscope photograph showing the shot of FIG. 6. [Figure 9] 4 is an experimental result showing photoresist line width as a function of exposure energy according to a mask line width at the same pitch in accordance with one embodiment of the present invention. [Figure 10A] 1 is a conceptual diagram showing characteristics of a mask and resist by region without OPC according to an embodiment of the present invention; [Figure 10B]1 is a conceptual diagram showing characteristics of a mask and resist by region having an OPC according to an embodiment of the present invention; [Figure 11A] In one embodiment of the present invention, the variation of mask optical proximity correction in response to differences in exposure energy at a mask pitch of 100 nm is shown. [Figure 11B] In one embodiment of the present invention, the variation of mask optical proximity correction in response to differences in exposure energy at a mask pitch of 120 nm is shown. [Figure 12] 1 is an electron micrograph showing a shot of photoresist using a mask with optical proximity correction according to one embodiment of the present invention. [Figure 13] FIG. 2 is a conceptual diagram showing a mask with optical proximity correction according to one embodiment of the present invention. [Figure 14] 11A-11C are enlarged views showing a stitching process according to another embodiment of the present invention. [Figure 15] 13 is a view showing a mask for performing a stitching process in another embodiment of the present invention. [Figure 16] 4 illustrates linewidth of a negative photoresist according to another embodiment of the present invention. [Figure 17] 4 is a flow chart illustrating a method for manufacturing a mask for forming a line and space pattern.

Claims

1. A method for forming a line and space pattern by exposing a mask to a substrate in a first direction and a second direction and performing a stitching process, the method comprising: performing a first exposure process on the substrate such that first shots of the mask contact each other in the first direction; performing a second exposure process on the substrate such that second shots of the mask contact each other to have an offset with respect to the first shots in the first direction, the second shots contacting the first shots in the second direction; Including, Each of the first shots and the second shots is a reference energy area exposed at a reference energy; a one-time interference region having energy higher than the reference energy due to interference between the first shots and the second shots; a double interference region having energy higher than the reference energy due to interference between the first shots and the second shots; Including, a single-interference mask region of the mask corresponding to the single-interference region has a first mask linewidth greater than a basic mask linewidth of a reference energy mask region of the mask corresponding to the reference energy region; a second interference mask region of the mask corresponding to the second interference region having a second mask linewidth greater than a mask linewidth of a reference energy mask region of the mask corresponding to the reference energy region;

2. 2. The method of claim 1, wherein the offset is greater than a width of an interference region between the first shots and the second shots.

3. the pitch of the line and space pattern is the same in the first shots and the second shots; 2. The method of claim 1, wherein the pitch of the photoresist of the line and space pattern is 80 nm to 140 nm.

4. the reference energy region is a rectangle located within a rectangular shot and is located at the center of the shot; the one-time interference region is arranged on a side so as to surround the reference energy region, 2. The method of claim 1, wherein the double interference region is locally disposed between a vertex of a reference energy region and a pair of vertices in the first direction.

5. A method for forming a line and space pattern comprising exposing a mask to a substrate in a first direction and a second direction to proceed with a stitching process, the method comprising: performing a first exposure process on the substrate such that first shots of the mask contact each other in the first direction; performing a second exposure process on the substrate such that second shots of the mask contact each other to have an offset with respect to the first shots in the first direction, the second shots contacting the first shots in the second direction; Including, The mask comprises: A rectangular reference energy mask region; a left region and a right region disposed respectively on the left and right sides of the reference energy mask region; a left upper vertex region and a right upper vertex region respectively disposed at the left upper portion and the right upper portion of the reference energy mask region; a left lower vertex region and a right lower vertex region respectively disposed at the left lower portion and the right lower portion of the reference energy mask region; an upper region disposed above the reference energy mask region; a left upper region disposed between the upper region and the left upper vertex region; a right upper region disposed between the upper region and the right upper vertex region; a lower region disposed below the reference energy mask region; a left lower region disposed between the lower region and the left lower vertex region; a right lower region disposed between the lower region and the right lower apex region; Including, the linewidth of the reference energy mask region is a base mask linewidth; the line widths of the left region, the right region, the upper left region, the upper right region, the lower left region, and the lower right region are first mask line widths; line widths of the upper region, the lower region, the left upper vertex region, the right upper vertex region, the left lower vertex region, and the right lower vertex region are second mask line widths; the second mask line width is greater than the first mask line width; 2. A method for forming a line and space pattern, wherein the first mask line width is greater than the base mask line width.

6. The basic mask line width is 50 nm; the first mask line width is 56 nm; 6. The method of claim 5, wherein the second mask line width is 60 nm.

7. A mask for forming a line and space pattern, which is used to perform a stitching process by exposing a mask to a substrate in a first direction and a second direction, the mask for forming the line and space pattern comprising: a rectangular reference energy mask region formed on a mask substrate in the first direction and the second direction; A single interference mask region arranged on the sides so as to surround the reference energy mask region; a double interference mask region locally disposed between a vertex of the reference energy mask region and a pair of vertices in the first direction; Including, the reference energy mask region has a base mask linewidth; the one-time interference mask region has a first mask linewidth; the second interference mask region has a second mask linewidth; the second mask line width is greater than the base mask line width; A mask for forming a line and space pattern, wherein the first mask line width is greater than the base mask line width.

8. The basic mask line width is 50 nm; the first mask line width is 56 nm; 8. The mask for forming a line and space pattern according to claim 7, wherein the second mask line width is 60 nm.

9. A mask for forming a line and space pattern, which is used to perform a stitching process by exposing a mask to a substrate in a first direction and a second direction, the mask for forming the line and space pattern comprising: A rectangular reference energy mask region; a left region and a right region disposed respectively on the left and right sides of the reference energy mask region; a left upper vertex region and a right upper vertex region respectively disposed at the left upper portion and the right upper portion of the reference energy mask region; a left lower vertex region and a right lower vertex region respectively disposed at the left lower portion and the right lower portion of the reference energy mask region; an upper region disposed above the reference energy mask region; a left upper region disposed between the upper region and the left upper vertex region; a right upper region disposed between the upper region and the right upper vertex region; a lower region disposed below the reference energy mask region; a left lower region disposed between the lower region and the left lower vertex region; a right lower region disposed between the lower region and the right lower apex region; Including, the linewidth of the reference energy mask region is a base mask linewidth; the line widths of the left region, the right region, the upper left region, the upper right region, the lower left region, and the lower right region are first mask line widths; line widths of the upper region, the lower region, the left upper vertex region, the right upper vertex region, the left lower vertex region, and the right lower vertex region are second mask line widths; the second mask line width is greater than the base mask line width; A mask for forming a line and space pattern, wherein the first mask line width is greater than the base mask line width.

10. The basic mask line width is 50 nm; the first mask line width is 56 nm; 10. The mask of claim 9, wherein the second mask line width is 60 nm.

11. A method for manufacturing a mask for forming a line and space pattern, comprising the steps of: performing a first stitching process by exposing a first mask to the substrate to form a line and space pattern in a first direction and a second direction; measuring an exposure energy or a line width of a one-time interference region having an energy higher than a reference energy without interference due to one-time interference of shots by the first stitching process; measuring an exposure energy or a line width of a double interference region having an energy higher than a reference energy due to double interference of shots by the first stitching process; forming a second mask by performing a first optical proximity correction based on the exposure energy or line width of the first interference region to increase a line width in a first interference mask region of the first mask corresponding to the first interference region, and performing a second optical proximity correction based on the exposure energy or line width of the second interference region to increase a line width in a second interference mask region of the first mask corresponding to the second interference region; A method for producing a mask for forming a line and space pattern comprising the steps of:

12. The first stitching step includes: performing a first exposure process on the substrate such that first shots of the first mask contact each other in the first direction; performing a second exposure process on the substrate such that second shots of the first mask contact each other to have an offset with respect to the first shots in the first direction, the second shots contacting the first shots in the second direction; The method for producing a mask for forming a line and space pattern according to claim 11, comprising:

13. the first optical proximity correction having the same pitch and increasing the linewidth of the lines by a first variation; the second optical proximity correction having the same pitch and increasing the linewidth of the lines by a second variation; the second fluctuation amount is greater than the first fluctuation amount, 12. The method of claim 11, wherein the first variation is proportional to a difference between an exposure energy of the first interference area and a basic exposure energy of a non-interference area.

Citation Information

Patent Citations

  • Resist pattern line width calculating method, mask pattern line width correction method, optical proximity effect correction method, exposure mask fabricating method, electron drawing method for fabricating the exposure mask, exposure method, and semiconductor device manufacturing method

    JP2006156864A

  • Exposure mask, exposure method, method for manufacturing exposure mask, three-dimensional device, and method for manufacturing three-dimensional device

    JP2007193243A

  • Uniform background radiation of maskless lithography

    JP2008235909A

  • Polarizer, method for manufacturing the same, and electron beam irradiation device

    JP2016133667A

  • Process dose and process bias determination for beam lithography

    JP2018101127A