Logic switching element and its manufacturing method
The logic switching element with a ferroelectric and antiferroelectric domain switching layer addresses the limitations of silicon substrate transistors by achieving reduced subthreshold swing and enhanced control efficiency, facilitating scalable and efficient operation.
Patent Information
- Application Number
- JP2019150490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-22
- Filing Date
- 2019-08-20
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2039-08-20
AI Technical Summary
Existing silicon substrate transistors face limitations in improving operating characteristics and scaling down due to high power density and a subthreshold swing (SS) value limit of approximately 60 mV/dec, making it difficult to reduce operating voltage below 0.8V.
A logic switching element utilizing a domain switching layer composed of ferroelectric and antiferroelectric materials, arranged in specific configurations to achieve a negative capacitance effect, eliminating hysteresis and enhancing voltage amplification for improved subthreshold swing and control efficiency.
The solution enables a logic switching element with reduced subthreshold swing, increased control efficiency, and scalability, suitable for advanced electronic devices and circuits.
Smart Images

Figure 0007566397000003 
Figure 0007566397000004 
Figure 0007566397000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a logic switching element and a method for manufacturing the same. [Background technology]
[0002] The existing silicon substrate transistor has limitations in improving the operating characteristics and scaling down. For example, when the operating voltage and current characteristics of the existing silicon substrate transistor are measured, the subthreshold swing (SS) value is given by the following Equation 1, and it is known that the SS value has a limit of about 60 mV / dec.
[0003]
number
[0004] where k B is the Boltzmann constant, T is the absolute temperature, q is the elementary charge, and C D is the capacitance of the depletion layer, and C ins is the capacitance of the gate insulator.
[0005] As the size of transistors becomes smaller, the power density increases due to the difficulty of lowering the operating voltage below about 0.8V. Therefore, there is a limit to the scale-down of devices. There is a demand for development of devices that can improve operating characteristics such as subthreshold swing (SS), are favorable for scale-down, and can increase control efficiency. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a logic switching element using a negative capacitance effect, to provide a logic switching element using a ferroelectric material and an anti-ferroelectric material, to provide a logic switching element which can improve operating characteristics such as sub-threshold swing (SS), can increase control efficiency, and is advantageous for scale-down, and to provide a method for manufacturing the logic switching element. [Means for solving the problem]
[0007] According to one aspect, there is provided a logic switching device including a channel element, a source and a drain connected to the channel element, a gate electrode disposed facing the channel element, and a domain switching layer disposed between the channel element and the gate electrode, the domain switching layer being a non-memory element, the logic switching device including a ferroelectric material region including a ferroelectric domain, and an anti-ferroelectric material region including an anti-ferroelectric domain.
[0008] The domain switching layer may have a non-hysteresis behavior characteristic in the change of polarization due to an external electric field.
[0009] The domain switching layer may have a structure in which at least one ferroelectric material region and at least one antiferroelectric material region are arranged in a direction parallel to the gate electrode.
[0010] The domain switching layer may have a structure in which at least one ferroelectric material region and at least one antiferroelectric material region are arranged in a direction perpendicular to the gate electrode.
[0011] The domain switching layer may include a combination of a structure in which at least one of the ferroelectric material regions and at least one of the antiferroelectric material regions are arranged in a direction parallel to the gate electrode and a structure in which they are arranged in a direction perpendicular thereto.
[0012] The ferroelectric material region and the antiferroelectric material region may include the same base material but have different crystal phases.
[0013] The ferroelectric material region may include an orthorhombic crystalline phase, and the antiferroelectric material region may include a tetragonal crystalline phase.
[0014] The ferroelectric material region and the antiferroelectric material region may have different doping concentrations.
[0015] The ferroelectric material region and the antiferroelectric material region may contain different doping materials.
[0016] At least one of the ferroelectric material region and the antiferroelectric material region may include at least one of an Hf-based oxide and a Zr-based oxide.
[0017] At least one of the ferroelectric material region and the antiferroelectric material region may include a dopant, and the dopant may include at least one of Si, Al, Zr, Y, La, Gd, Sr, and Hf.
[0018] In the domain switching layer, the volume ratio of the ferroelectric material region to the antiferroelectric material region ranges from about 10:90 to about 90:10.
[0019] The domain switching layer may be in direct contact with the channel element.
[0020] The semiconductor device may further include an insulating layer disposed between the channel element and the domain switching layer.
[0021] The semiconductor device may further include an insulating layer disposed between the channel element and the domain switching layer, and a conductive layer disposed between the insulating layer and the domain switching layer.
[0022] The channel element may include at least one of Si, Ge, SiGe, a III-V semiconductor, an oxide semiconductor, a nitride semiconductor, a nitride-oxide semiconductor, a 2D material, a quantum dot, and an organic semiconductor.
[0023] According to another aspect, there is provided a method for manufacturing a logic switching device, the method including: providing a substrate including a channel element; forming an amorphous thin film on the channel element; forming a conductive material layer on the amorphous thin film; and annealing the amorphous thin film to form a domain switching layer from the amorphous thin film, the domain switching layer being a non-memory element and comprising a ferroelectric material region including a ferroelectric domain and an antiferroelectric material region including an antiferroelectric domain.
[0024] The ferroelectric material region and the antiferroelectric material region may have different crystal phases.
[0025] The ferroelectric material region may comprise an orthorhombic crystalline phase and the antiferroelectric material region may comprise a tetragonal crystalline phase.
[0026] The ferroelectric material region and the antiferroelectric material region may have different doping concentrations.
[0027] The ferroelectric material region and the antiferroelectric material region may contain different doping materials.
[0028] At least one of the ferroelectric material region and the antiferroelectric material region may include at least one of an Hf-based oxide and a Zr-based oxide.
[0029] The annealing can be carried out at a temperature of about 400°C to about 1,200°C.
[0030] The method may further include forming a gate electrode from the conductive material layer.
[0031] The method may further include forming a source and a drain coupled to the channel element. Effect of the Invention
[0032] According to the present invention, it is possible to realize a logic switching element using a negative capacitance effect, a logic switching element using both a ferroelectric material and an antiferroelectric material, a logic switching element having improved operating characteristics such as sub-threshold swing (SS), increased control efficiency, and advantageous for scale-down, and various electronic elements / devices / circuits / systems can be realized by using the logic switching element. [Brief description of the drawings]
[0033] [Figure 1] 1 is a cross-sectional view illustrating a logic switching element according to an embodiment. [Diagram 2] 13 is a cross-sectional view showing a stacked structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment. [Diagram 3] 13 is a cross-sectional view showing a stacked structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment. [Figure 4] 11 is a cross-sectional view illustrating a substructure that can be applied under a domain switching layer of a logic switching device according to another embodiment; [Diagram 5] 11 is a cross-sectional view illustrating a substructure that can be applied under a domain switching layer of a logic switching device according to another embodiment; [Figure 6] 13 is a cross-sectional view showing a stacked structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment. [Figure 7] 13 is a cross-sectional view showing a stacked structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment. [Figure 8] 1 is a graph showing an example of capacitance matching using a ferroelectric and an antiferroelectric in a domain switching layer configuration, according to an embodiment. [Figure 9] FIG. 11 is a cross-sectional view showing the configuration of an element according to a comparative example. [Figure 10] 11 is a graph showing capacitance matching using a ferroelectric material and a dielectric material according to a comparative example. [Figure 11A] 1 is a graph showing characteristics of a ferroelectric material. [Figure 11B] 1 is a graph showing characteristics of a ferroelectric material. [Figure 12A] 1 is a graph showing characteristics of an antiferroelectric material. [Figure 12B] 1 is a graph showing characteristics of an antiferroelectric material. [Figure 13A] 1 is a graph showing characteristics of a combination of a ferroelectric material and an antiferroelectric material. [Figure 13B] 1 is a graph showing characteristics of a combination of a ferroelectric material and an antiferroelectric material. [Figure 14A] 1 is a graph showing characteristics of a dielectric material. [Figure 14B] 1 is a graph showing characteristics of a dielectric material. [Figure 15] 1 is a graph showing the results of measuring the dielectric constant vs. voltage characteristics according to the composition / physical properties of a HfZrO layer in a metal / HfZrO layer / metal structure according to one embodiment. [Figure 16]16 is a graph showing the results of measuring polarization-voltage characteristics in the metal / HfZrO layer / metal structure described in FIG. 15, according to one embodiment. [Figure 17A] FIG. 2 is a cross-sectional view illustrating an example of the configuration (domain arrangement) of a domain layer DL1 in the case where the domain layer DL1 is anti-ferroelectric dominant. [Figure 17B] FIG. 2 is a cross-sectional view illustrating an example of the configuration (domain arrangement) of a domain layer DL2 in the case where the domain layer is ferroelectric dominant. [Figure 18] 1 is a graph showing the results of measuring dielectric constant-voltage characteristics according to the composition / physical properties of an Al:HfO thin film manufactured according to an embodiment. [Figure 19] FIG. 19 is a cross-sectional view showing the structure of the element used to obtain the results of FIG. 18. [Figure 20] 1 is a graph illustrating an effect of improving subthreshold swing (SS) characteristics of a logic switching device according to an embodiment; [Figure 21] 11 is a cross-sectional view showing a logic switching element according to another embodiment. [Figure 22A] 5A to 5C are cross-sectional views illustrating a method for manufacturing a logic switching element according to an embodiment. [Figure 22B] 5A to 5C are cross-sectional views illustrating a method for manufacturing a logic switching element according to an embodiment. [Figure 22C] 5A to 5C are cross-sectional views illustrating a method for manufacturing a logic switching element according to an embodiment. [Figure 23] FIG. 1 is a conceptual diagram illustrating an architecture of an electronic device according to one embodiment. [Figure 24] FIG. 13 is a conceptual diagram illustrating the architecture of an electronic device according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] Hereinafter, a logic switching element and a method for manufacturing the same according to the present invention will be described in detail with reference to the accompanying drawings. The widths and thicknesses of layers and regions illustrated in the accompanying drawings are slightly exaggerated for clarity of the specification and convenience of explanation. The same reference numerals denote the same elements throughout the detailed description.
[0035] 1 is a cross-sectional view showing a logic switching element according to an embodiment. Here, the logic switching element is also a logic transistor. The term "logic switching element" is a concept contrasted with a memory element (memory transistor) and means a non-memory on / off switching element.
[0036] Referring to FIG. 1, a channel element 10 may be provided, and a source 20 and a drain 30 may be provided that are electrically connected to the channel element 10. The source 20 may also be electrically connected / contacted to a first region of the channel element 10, and the drain 30 may also be electrically connected / contacted to a second region of the channel element 10. The channel element 10, the source 20, and the drain 30 may also be provided in a given substrate 100. The source 20 and the drain 30 may be formed by injecting impurities into different regions of the substrate 100, and the region of the substrate 100 between the source 20 and the drain 30 is also defined as the channel element (channel region) 10. The substrate 100 may be, for example, a Si substrate, but may also be a substrate including other materials than Si, for example, Ge, SiGe, III-V semiconductors, etc. In this case, the channel element 10 may include Si, Ge, SiGe, or III-V semiconductors. The material of the substrate 100 is not limited to the above and may be changed in various ways. The channel element 10 may also be provided by a material layer (thin film) that is not a part of the substrate 100 and is separate from the substrate 100. In that case, the material configuration of the channel element 10 may be various. For example, the channel element 10 may include at least one of an oxide semiconductor, a nitride semiconductor, a nitride oxide semiconductor, a two-dimensional material (2D), a quantum dot (QD), and an organic semiconductor. The oxide semiconductor may include, for example, InGaZnO, the two-dimensional material may include, for example, a transition metal dichalcogenide (TMD) or graphene, and the quantum dot may include a colloidal quantum dot (colloidal QD), a nanocrystal structure, etc., but these are merely examples and the embodiment of the present application is not limited thereto.
[0037] A gate electrode 500 may be provided to face the channel element 10. The gate electrode 500 may be provided between the source 20 and the drain 30, spaced apart from the channel element 10. A domain switching layer 300A may be provided between the channel element 10 and the gate electrode 500. The domain switching layer 300A is also a non-memory element. The domain switching layer 300A may include a ferroelectric material region F including a ferroelectric domain, and an antiferroelectric material region AF including an anti-ferroelectric domain. Due to the combination of the ferroelectric material region F and the antiferroelectric material region AF, the domain switching layer 300A may have a substantially non-hysteresis behavior characteristic in a polarization change due to an external electric field. In other words, the domain switching layer 300A does not have, or does not substantially have, a hysteresis characteristic.
[0038] Ferroelectric materials have a non-centrosymmetric charge distribution in a unit cell in a crystallized material structure, and have spontaneous electric dipoles, i.e., spontaneous polarization. The ferroelectric materials have remnant polarization due to the dipole even in the absence of an external electric field. At the same time, the polarization direction can be switched in domain units by the application of an external electric field. Antiferroelectric materials may contain an array of electric dipoles, but with zero or near-zero remnant polarization. In the absence of an electric field, adjacent dipoles are opposite in direction and cancel out in polarization, so that the overall spontaneous and remnant polarization is zero or near-zero. However, under the application of an external electric field, they can exhibit polarization and switching properties.
[0039] In this embodiment, the domain switching layer 300A does not have a hysteresis characteristic by performing capacitance matching using a combination of at least one ferroelectric material region F and at least one antiferroelectric material region AF in contact with each other. Therefore, domain switching occurs in each of the ferroelectric material region F and the antiferroelectric material region AF, and the switching characteristic of the logic switching element (logic transistor) can be improved by voltage amplification caused during domain switching. In particular, the effect of further lowering the subthreshold swing (SS) value of the logic switching element (logic transistor) can be obtained. In addition, since the domain switching layer 300A has a non-hysteresis behavior characteristic, an excellent switching element having an on / off characteristic that is not a memory can be obtained.
[0040] 1, the domain switching layer 300A may be in direct contact with the channel element 10. In this case, a separate dielectric layer is not used between the channel element 10 and the domain switching layer 300A, and deterioration of characteristics due to a dielectric layer having a low dielectric constant can be prevented.
[0041] 1 shows a structure in which the ferroelectric material regions F and the antiferroelectric material regions AF of the domain switching layer 300A are arranged in a direction parallel to the gate electrode 500, i.e., laterally arranged, but according to another embodiment, the ferroelectric material regions F and the antiferroelectric material regions AF may be arranged in a direction perpendicular to the gate electrode 500, i.e., vertically arranged, as shown in FIGS. 2 and 3.
[0042] 2 and 3 are cross-sectional views showing a stacked structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment.
[0043] 2 and 3, the domain switching layers 300B and 300C may have a structure in which at least one ferroelectric material region F and at least one antiferroelectric material region AF are arranged in a vertical direction to the gate electrode 500. In FIG. 2, the ferroelectric material region F contacts the gate electrode 500, and the antiferroelectric material region AF is provided below the ferroelectric material region F. In FIG. 3, the antiferroelectric material region AF contacts the gate electrode 500, and the ferroelectric material region F is provided below the antiferroelectric material region AF. The domain switching layers 300B and 300C of FIG. 2 and 3 may be applied instead of the domain switching layer 300A of FIG. 1. In the structures of FIG. 2 and FIG. 3, the domain switching layers 300B and 300C do not have hysteresis characteristics due to capacitance matching achieved by a combination of the ferroelectric material region F and the antiferroelectric material region AF.
[0044] 1, the domain switching layer 300A is in direct contact with the channel element 10, but the substructure disposed under the domain switching layer 300A may be different, examples of which are shown in FIGS.
[0045] FIG. 4 is a cross-sectional view illustrating a substructure applied below a domain switching layer of a logic switching device according to another embodiment.
[0046] Referring to FIG. 4, an insulating layer 150 may be provided on the channel element 10. The domain switching layers 300A, 300B, and 300C and the gate electrode 500 of FIGS. 1 to 3 may be disposed on the insulating layer 150. The insulating layer 150 has a thin thickness of about 5 nm or less or about 3 nm or less. However, the thickness of the insulating layer 150 is not limited to the above and may be 5 nm or more. For the insulating layer 150, for example, Si oxide, Al oxide, Hf oxide, Zr oxide, etc. may be applied, or a two-dimensional insulator such as h-BN (hexagonal boron nitride) may be used. However, the material of the insulating layer 150 is not limited thereto and may be different. In order to perform capacitance matching using the ferroelectric material region F and the antiferroelectric material region AF, it is easy to apply a dielectric having a relatively high dielectric constant in the insulating layer 150. The higher the dielectric constant of the insulating layer 150, the more advantageous it is for improving the performance of the switching element. Furthermore, the use of the insulating layer 150 can have the effect of suppressing or preventing electrical leakage.
[0047] FIG. 5 is a cross-sectional view showing a substructure that can also be applied below a domain switching layer of a logic switching device according to another embodiment.
[0048] Referring to FIG. 5, an insulating layer 160 may be provided on the channel element 10, and a conductive layer 200 may be further provided on the insulating layer 160. The domain switching layers 300A, 300B, and 300C and the gate electrode 500 of FIGS. 1 to 3 may be disposed on the conductive layer 200. The material of the insulating layer 160 may be the same as or similar to the insulating layer 150 of FIG. 4. The conductive layer 200 may be formed of a metal or a metal compound. The conductive layer 200 may be a floating electrode and may be involved in the manufacturing process and characteristic control of the domain switching layers 300A, 300B, and 300C. The insulating layer 160 may serve to insulate the channel element 10 and the conductive layer 200, and may have a thickness of, for example, about 10 nm or more.
[0049] 1 shows an example in which domain switching layer 300A is composed of one ferroelectric material region F and one antiferroelectric material region AF, but in other embodiments, a plurality of ferroelectric material regions F and a plurality of antiferroelectric material regions AF can form one domain switching layer, an example of which is shown in FIG.
[0050] FIG. 6 is a cross-sectional view showing a laminated structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment.
[0051] 6, the domain switching layer 300D may have a structure in which a plurality of ferroelectric material regions F and a plurality of antiferroelectric material regions AF are horizontally (transversely) arranged one on top of the other. The ratio and size of the ferroelectric material regions F and the antiferroelectric material regions AF are merely examples and may be different.
[0052] According to another embodiment, the domain switching layer may include a combination of a structure in which at least one of the ferroelectric material regions and at least one of the antiferroelectric material regions are arranged in a direction parallel to the gate electrode and a structure in which they are arranged in a direction perpendicular to the gate electrode, an example of which is shown in FIG.
[0053] FIG. 7 is a cross-sectional view showing a laminated structure of a domain switching layer and a gate electrode that can be applied to a logic switching element according to another embodiment.
[0054] 7, the domain switching layer 300E may include a combination of a structure in which a plurality of ferroelectric material regions F and a plurality of antiferroelectric material regions AF are arranged horizontally (sideways) and vertically (up and down). Such a combination arrangement may be formed depending on the conditions of the manufacturing process. However, the structure of FIG. 7 is merely an example, and may be variously changed.
[0055] In the above embodiment, the ferroelectric material region F and the antiferroelectric material region AF may have different crystalline phases although they contain the same base material. The ferroelectric material region F and the antiferroelectric material region AF are composed of the same material series but have different crystalline phases, so that one (F) exhibits ferroelectric properties and the other (AF) exhibits antiferroelectric properties. For example, the ferroelectric material region F may have an orthorhombic crystalline phase, and the antiferroelectric material region AF may have a tetragonal crystalline phase. For example, the ferroelectric material region F and the antiferroelectric material region AF may include Hf-based oxide or Zr-based oxide. For example, after forming an HfO-based amorphous thin film, a part of the ferroelectric material region F may have an orthorhombic crystalline phase, and the other part of the antiferroelectric material region AF may have a tetragonal crystalline phase through annealing (heat treatment) control.
[0056] The ferroelectric material region F and the antiferroelectric material region AF can be formed by controlling the doping concentration and the doping material in a different manner, as well as controlling the annealing (heat treatment). For example, a part of the HfO-based amorphous thin film can have a first doping concentration, and another part can have a second doping concentration. By annealing (heat treating) them under a predetermined condition, the region having the first doping concentration can be the ferroelectric material region F, and the region having the second doping concentration can be the antiferroelectric material region AF. Such an effect can also be obtained by making the doping material different instead of the doping concentration. Thus, in some cases, the ferroelectric material region F and the antiferroelectric material region AF can have different doping concentrations and / or contain different doping materials. When at least one of the ferroelectric material region F and the antiferroelectric material region AF contains a dopant, the dopant can include at least one of Si, Al, Zr, Y, La, Gd, Sr, and Hf.
[0057] In other embodiments, the base material of the ferroelectric material regions F and the base material of the antiferroelectric material regions AF may be different from each other.
[0058] In the above embodiment, the volume ratio (vol%) of the ferroelectric material regions F and the antiferroelectric material regions AF of the domain switching layers 300A-300E may be determined within a range of about 0.1:99.9 to 99.9:0.1. For example, the volume ratio (vol%) of the ferroelectric material regions F and the antiferroelectric material regions AF of the domain switching layers 300A-300E may be determined within a range of about 10:90 to 90:10. The volume ratio may be determined so as to satisfy the condition that the domain switching layers 300A-300E do not have or substantially do not have a hysteresis characteristic.
[0059] 8 is a graph showing an example of capacitance matching using a ferroelectric and an antiferroelectric in a domain switching layer configuration according to an embodiment, in which the X-axis represents the charge (Q) of the material and the Y-axis represents the energy (U) of the material.
[0060] Referring to FIG. 8, the graph of the ferroelectric (ferro) has well shapes on both the left and right sides. The two well shapes correspond to two stable polarization states, and such a graph shape indicates hysteresis behavior. At the transition region between the two wells, there is a point with negative capacitance. The device according to the present embodiment includes a ferroelectric and utilizes the negative capacitance effect of the ferroelectric, so in this aspect, it is said to be a logic switching device utilizing the negative capacitance effect.
[0061] The graph of the anti-ferroelectric (anti-ferro) has a different bend from the graph of the ferroelectric (ferro). When the ferroelectric and anti-ferroelectric are appropriately mixed and designed, the combination of the ferroelectric and anti-ferroelectric (ferro+anti-ferro) has a U-shaped graph that is not in the form of two wells and shows virtually no hysteresis behavior. In other words, hysteresis-free results can be obtained through capacitance matching using ferroelectric and anti-ferroelectric.
[0062] At this time, when the domain switching layer contacts the channel region, the capacitance of the channel region can be taken into consideration to perform the above-mentioned capacitance matching. The above-mentioned capacitance matching can also be performed taking into consideration the parasitic capacitance between the channel region and the source and drain. When the domain switching layer contacts the insulating layer (dielectric layer) therebelow, the capacitance of the insulating layer (dielectric layer) can also be taken into consideration to perform the above-mentioned capacitance matching. As a result, the domain switching layer does not have hysteresis due to the capacitance matching.
[0063] When the domain switching layer contacts the channel region and the capacitance matching is performed while taking into account the capacitance of the channel region, the combination of the domain switching layer and the channel region is deemed to have no hysteresis. Or, when the domain switching layer contacts the channel region, the domain switching layer is deemed to have no hysteresis. Similarly, when the domain switching layer contacts the insulating layer (dielectric layer) and the capacitance matching is performed while taking into account the capacitance of the insulating layer (dielectric layer), the combination of the domain switching layer and the insulating layer (dielectric layer) is deemed to have no hysteresis. Or, when the domain switching layer contacts the insulating layer (dielectric layer), the domain switching layer is deemed to have no hysteresis.
[0064] FIG. 9 is a cross-sectional view showing the configuration of an element according to a comparative example. 9, a channel element 2, a source 3, and a drain 4 may be provided on a substrate 1. A dielectric layer 5 may be disposed on the channel element 2, a ferroelectric layer 6 may be disposed on the dielectric layer 5, and a gate electrode 7 may be disposed on the ferroelectric layer 6. The ferroelectric layer 6 is provided between the channel element 2 and the gate electrode 7, and the dielectric layer 5 is provided between the ferroelectric layer 6 and the channel element 2. This comparative example is a case where capacitance matching is performed using the ferroelectric layer 6 and the dielectric layer 5.
[0065] FIG. 10 is a graph showing capacitance matching using a ferroelectric material and a dielectric material according to a comparative example. Referring to Figure 10, a ferroelectric (ferro) has a graph shape as described with reference to Figure 8. A dielectric (dielectric) has a relatively narrow U-shaped graph shape. When a ferroelectric and a dielectric are combined (ferro+dielectric), the hysteresis disappears due to capacitance matching, and a relatively wide U-shaped graph shape is shown.
[0066] However, when capacitance matching is performed using a ferroelectric and a dielectric as in the comparative example of Fig. 10, a problem occurs in that gate efficiency decreases because a dielectric with a low dielectric constant is used. In this embodiment, the use of a dielectric with a low dielectric constant can be eliminated, and the problem associated therewith can be solved. For example, in this embodiment, the dielectric constant of HfZrO applied to the domain switching layer and the SiO used as the dielectric in the comparative example are 2The dielectric constants of the antiferroelectric and ferroelectric materials are significantly different, about 50:4. In addition, the dielectric does not have a ferroelectric domain and does not have domain switching when a gate voltage is applied, but the antiferroelectric material used in the embodiment of the present application has domain switching characteristics, so that the sub-threshold swing (SS) value of the switching element can be further reduced by the voltage amplification that occurs during switching. Therefore, a logic switching element that eliminates hysteresis through capacitance matching while maximizing the domain switching effect by combining the antiferroelectric and ferroelectric materials can be realized.
[0067] 11A to 14B are graphs showing the characteristics of a ferroelectric (ferro), an antiferroelectric (anti-ferro), a combination of a ferroelectric and an antiferroelectric (ferro+anti-ferro), and a dielectric, respectively. The graphs of FIG. 11A, FIG. 12A, FIG. 13A, and FIG. 14A show the relationship between the electric field (E) applied to the material layer and the polarization (P), and the graphs of FIG. 11B, FIG. 12B, FIG. 13B, and FIG. 14B show the relationship between the charge (Q) and the energy (U) of the material layer. In particular, FIG. 13A and FIG. 13B correspond to the characteristics of a combination (mixture) of a ferroelectric and an antiferroelectric, which is also applied to the domain switching layer according to the present embodiment.
[0068] Fig. 15 is a graph showing the results of measuring the dielectric constant vs. voltage characteristics depending on the composition / physical properties of the HfZrO layer in a metal / HfZrO layer / metal structure according to this embodiment. Fig. 15 includes results for the cases where the HfZrO layer is a dielectric, the HfZrO layer is anti-ferroelectric dominant, and the HfZrO layer is ferroelectric dominant.
[0069] 15, an amorphous HfZrO layer that has not been annealed (heat treated) exhibits dielectric properties, and when the amorphous HfZrO layer is annealed under a first condition, it can exhibit antiferroelectric dominant properties, and when the amorphous HfZrO layer is annealed under a second condition, it can exhibit ferroelectric dominant properties. The ratio of ferroelectric to antiferroelectric can be controlled by the annealing conditions for the HfO thin film or HfO-based thin film.
[0070] FIG. 16 is according to this embodiment, and is a graph showing the results of measuring the polarization-voltage characteristics in the metal / HfZrO layer / metal structure described in FIG.
[0071] Referring to FIG. 16, when the antiferroelectricity is dominant, the remanent polarization is close to 0 and the hysteresis is reduced, whereas when the ferroelectricity is dominant, the remanent polarization increases to about 10 and the hysteresis increases.
[0072] FIG. 17A is a cross-sectional view exemplarily showing the configuration (domain arrangement) of the domain layer DL1 in the case where it is antiferroelectric dominant.
[0073] FIG. 17B is a cross-sectional view showing an example of the configuration (domain arrangement) of the domain layer DL2 in the case where the domain layer DL2 is ferroelectrically dominant.
[0074] 17A and 17B, in the domain layer DL1 when antiferroelectric dominant, the total volume of antiferroelectric AF is much larger than the total volume of ferroelectric F, and in the domain layer DL2 when ferroelectric dominant, the total volume of ferroelectric F is much larger than the total volume of antiferroelectric AF. Depending on the annealing (heat treatment) conditions, orthorhombic crystal regions having ferroelectric properties and tetragonal crystal regions having antiferroelectric properties are mixed in the thin film. In Fig. 17A and Fig. 17B, M1 and M2 denote metal layers (metal).
[0075] Fig. 18 is a graph showing the results of measuring the dielectric constant vs. voltage characteristics depending on the composition / physical properties of the Al:HfO thin film manufactured according to the present embodiment. Fig. 18 includes the results when the Al:HfO thin film is a dielectric, when the Al:HfO thin film is antiferroelectric dominant, and when the Al:HfO thin film is ferroelectric dominant. Here, the Al:HfO thin film means an HfO thin film doped with Al.
[0076] 18, when the Al doping level is 19 at% and the annealing temperature is 500° C., an Al:HfO thin film having dielectric properties can be obtained. When the Al doping level is 7 at% and the annealing temperature is 700° C., an Al:HfO thin film having antiferroelectric dominant properties can be obtained. When the Al doping level is 12 at% and the annealing temperature is 800° C., an Al:HfO thin film having ferroelectric dominant properties can be obtained. The physical properties of the Al:HfO thin film can be changed by adjusting the Al doping level and / or the annealing conditions for the amorphous Al:HfO thin film.
[0077] FIG. 19 is a cross-sectional view showing the structure of the element used to obtain the results of FIG. 19, a silicon oxide layer 52 may be formed on a silicon substrate 51, a first metal layer 53 may be formed thereon, and an Al:HfO thin film 54 may be formed on the first metal layer 53. Next, a second metal layer 55 may be formed on the Al:HfO thin film 54. At this time, the first metal layer 53 and the second metal layer 55 are both Mo layers, and the thickness of the Al:HfO thin film 54 is about 10 nm. The width of the Al:HfO thin film 54 is about 5 μm to 400 μm.
[0078] The doping level and / or annealing temperature of the Al:HfO thin film 54 can control the ferroelectric and antiferroelectric properties of the Al:HfO thin film 54. That is, the Al:HfO thin film 54 can have dielectric properties, antiferroelectric dominant properties, or ferroelectric dominant properties, depending on the doping level and / or annealing temperature of the Al:HfO thin film 54. Thus, the ratio of ferroelectric and antiferroelectric materials formed in the Al:HfO thin film 54 can be controlled.
[0079] For example, the change in characteristics depending on the doping level and annealing temperature is shown in Table 1 below.
[0080] [Table 1]
[0081] In Table 1, D indicates dielectric properties, F dominant indicates ferroelectric dominant properties, and AF dominant indicates antiferroelectric dominant properties. The appropriate annealing temperature may vary depending on the material and doping level used. In this regard, the annealing temperature used in manufacturing the logic switching device according to the present embodiment is about 400° C. to 1,200° C.
[0082] FIG. 20 is a graph illustrating an effect of improving the sub-threshold swing (SS) characteristics of a logic switching element according to an embodiment.
[0083] 20, in the case of a conventional silicon substrate transistor (dashed line graph), the sub-threshold swing (SS) value is known to be limited to about 60 mV / dec. However, in the case of the logic switching device according to the present embodiment (solid line graph), the sub-threshold swing (SS) value falls to about 60 mV / dec or less due to the negative capacitance effect and the domain switching effect of the antiferroelectric.
[0084] FIG. 21 is a cross-sectional view showing a logic switching element according to another embodiment. 21, a channel layer 11 may be provided on a substrate 101. In other words, the channel layer 11 may be provided as a material layer (thin film) separate from the substrate 101, which is not a part of the substrate 101. The channel layer 11 may include at least one of an oxide semiconductor, a nitride semiconductor, a nitride oxide semiconductor, a two-dimensional (2D) material, a quantum dot, and an organic semiconductor. The oxide semiconductor may include, for example, InGaZnO, the two-dimensional material may include, for example, TMD or graphene, and the quantum dot may include a colloidal quantum dot, a nanocrystal structure, etc., but these are merely exemplary and the embodiment of the present application is not limited thereto.
[0085] A source electrode 21 and a drain electrode 31 may be provided in electrical contact with different regions of the channel layer 11. The source electrode 21 may be provided on a first end of the channel layer 11, and the drain electrode 31 may be provided on a second end of the channel layer 11. The source electrode 21 and the drain electrode 31 may be formed of a conductive material such as a metal, a metal compound, or a conductive polymer.
[0086] A domain switching layer 301 may be provided on a region of the channel layer 11 between the source electrode 21 and the drain electrode 31. The domain switching layer 301 may be the same as or similar to the domain switching layer 300A described with reference to FIG. 1. The domain switching layer 301 may include at least one ferroelectric material region F and at least one antiferroelectric material region AF. A gate electrode 501 may be provided on the domain switching layer 301. The device of FIG. 21 may be modified as described with reference to FIGS. 2 to 7.
[0087] 22A through 22C are cross-sectional views illustrating a method for fabricating a logic switching device according to an embodiment.
[0088] 22A, a substrate 105 including a channel element 15 may be provided, and a stacked structure of an amorphous thin film 305a and a gate electrode 505 may be formed on the channel element 15. An amorphous material layer and a conductive material layer may be sequentially deposited on the substrate 105, and then patterned to form an amorphous thin film 305a from the amorphous material layer and a gate electrode 505 from the conductive material layer. The stacked structure of the amorphous thin film 305a and the gate electrode 505 may be referred to as a "gate stack." The amorphous material layer may be deposited by a process such as atomic layer deposition (ALD) or chemical vapor deposition (CVD), and the conductive material layer may be deposited by a process such as ALD, CVD, or physical vapor deposition (PVD).
[0089] The amorphous thin film 305a is a thin film having a relatively high dielectric constant. For example, the dielectric constant of the amorphous thin film 305a is about 10 or more. In relation to this, the amorphous thin film 305a can be called a high-k dielectric layer. The amorphous thin film 305a may include at least one of an Hf-based oxide and a Zr-based oxide. The Hf-based oxide may be HfO or HfZrO. The Zr-based oxide may be ZrO. Here, HfO, HfZrO, and ZrO are expressed ignoring the composition ratio of the constituent elements. If necessary, the amorphous thin film 305a may further include a dopant. The dopant may include at least one of Si, Al, Zr, Y, La, Gd, Sr, and Hf. When the amorphous thin film 305a contains a dopant, it may be doped to the same concentration (substantially the same concentration) throughout, or different regions may be doped to different concentrations (levels). Different regions of the amorphous thin film 305a may be doped with different dopants. The doping of the amorphous thin film 305a may be performed during the formation of the amorphous material layer, or may be performed in a separate process after the formation of the amorphous material layer.
[0090] The source 25 and the drain 35 may be formed in the substrate 105 before the amorphous thin film 305a and the gate electrode 505 are formed. A predetermined dopant may be ion-implanted into different regions of the substrate 105 to form the source 25 and the drain 35, and then the amorphous thin film 305a and the gate electrode 505 may be formed. However, the time points at which the source 25 and the drain 35 are formed may be different. The source 25 and the drain 35 may also be formed in the substrate 105 after the amorphous thin film 305a and the gate electrode 505 are formed.
[0091] Referring to FIG. 22B, an annealing process may be performed on the amorphous thin film 305a. The annealing process may be performed at a temperature ranging from about 400° C. to about 1,200° C. The amorphous thin film 305a may be crystallized through the annealing process, and a ferroelectric material region and an antiferroelectric material region may be formed from the amorphous thin film 305a. If the annealing process is performed while the gate electrode 505 is in contact with the amorphous thin film 305a, the amorphous thin film 305a may be crystallized more easily. The result of the annealing process is shown in FIG. 22C.
[0092] Referring to FIG. 22C, a domain switching layer 305b may be formed from the amorphous thin film 305a (FIG. 22B). The domain switching layer 305b may include at least one ferroelectric material region F and at least one antiferroelectric material region AF. The ferroelectric material region F and the antiferroelectric material region AF may have different crystal phases. For example, the ferroelectric material region F may include an orthorhombic crystal phase, and the antiferroelectric material region AF may include a tetragonal crystal phase. In this case, the ferroelectric material region F may be provided to contact the gate electrode 505, and the antiferroelectric material region AF may be disposed between the ferroelectric material region F and the channel element 15. The arrangement and positional relationship between the ferroelectric material region F and the antiferroelectric material region AF may vary depending on the annealing conditions and the configuration of the amorphous thin film 305a (FIG. 22B). Here, for example, a case is illustrated in which a ferroelectric material region F is provided on an antiferroelectric material region AF, but their arrangement and positional relationship may be different as described with reference to Figures 1 to 7.
[0093] The annealing conditions control the ratio of the ferroelectric material regions F and the antiferroelectric material regions AF formed in the domain switching layer 305b, thereby achieving capacitance matching. Therefore, the domain switching layer 305b is also a non-memory element. Due to the combination of the ferroelectric material regions F and the antiferroelectric material regions AF, the domain switching layer 305b can have a substantially non-hysteretic behavior characteristic in the polarization change caused by the external electric field. In other words, the domain switching layer 305b does not have, or substantially does not have, a hysteresis characteristic. In some cases, the ferroelectric material regions F and the antiferroelectric material regions AF are regions having different doping concentrations from each other, or are regions doped with different dopants from each other.
[0094] If necessary, the domain switching layer 305b may be formed through two or more deposition steps or two or more doping steps. Also, the domain switching layer 305b may be formed through two or more annealing steps instead of one annealing step. Also, the process of this embodiment may be modified to form various modified structures as described with reference to FIGS. 1 to 7.
[0095] The logic switching element (logic transistor) according to the present embodiment can be applied to various electronic devices, logic devices, etc. The logic switching element (logic transistor) can also be a basic component of various electronic devices / logic devices. According to the present embodiment, it is possible to improve operating characteristics such as sub-threshold swing (SS), increase control efficiency, and realize a logic switching element that is advantageous for scale-down, and thus it is possible to manufacture electronic devices / logic devices with excellent performance by applying the same.
[0096] FIG. 23 is a schematic diagram illustrating the architecture of an electronic device according to one embodiment. Referring to FIG. 23, a memory unit 1010, an arithmetic logic unit (ALU) 1020, and a control unit 1030 may be formed in one chip 1000. The memory unit 1010, the ALU 1020, and the control unit 1030 may be monolithically integrated on the same substrate to form the chip 1000. Each of the ALU 1020 and the control unit 1030 may include a "logic switching element" according to the above-mentioned embodiment. For example, the logic switching element may include a domain switching layer having a substantially non-hysteretic behavior characteristic while including a ferroelectric domain. The memory unit 1010 may include a memory element. For example, the memory element may include a domain layer having a hysteretic behavior characteristic while including a ferroelectric domain. The memory unit 1010, the ALU 1020, and the control unit 1030 may be interconnected by metal lines on-chip and directly communicate with each other. The memory unit 1010 may include both a main memory and a cache memory. Such a chip 1000 is referred to as an on-chip memory processing unit. An input / output element 2000 coupled to the chip 1000 may further be included.
[0097] Such an electronic device is advantageous in terms of cost since the memory unit and the logic device unit can be integrated and manufactured on one chip. In addition, if the electronic device of the present embodiment is applied to an application field where a large amount of data is transmitted between the memory unit and the logic device unit and the data transmission is continuous, for example, the field of neuromorphic devices, various effects such as improved efficiency, improved speed, and reduced power consumption can be obtained. The basic configuration and operation method of a neuromorphic device are well known, so a detailed description thereof will be omitted.
[0098] In some cases, the electronic device according to the present embodiment may be embodied as an architecture in which computing unit devices and memory unit devices are formed adjacent to each other on one chip without division into sub-units.
[0099] FIG. 24 is a schematic diagram illustrating the architecture of an electronic device according to another embodiment.
[0100] 24, a central processing unit (CPU) chip 1500 may include a cache memory 1510, an ALU 1520, and a control unit 1530. The ALU 1520 and the control unit 1530 may each include a "logic switching element" according to the above-described embodiments. For example, the logic switching element may include a domain switching layer having a substantially non-hysteretic behavior characteristic while including a ferroelectric domain.
[0101] A main memory 1600 and auxiliary storage 1700 may be provided separately from the CPU chip 1500, and an input / output element 2500 may be provided. For example, the cache memory 1510 may be configured with a static random access memory (SRAM), and the main memory 1600 may be configured with a dynamic random access memory (DRAM).
[0102] According to the present disclosure, it is possible to realize a logic switching element using a negative capacitance effect. According to the present disclosure, it is possible to realize a logic switching element using both a ferroelectric material and an antiferroelectric material. According to the present disclosure, it is possible to realize a logic switching element that can improve operating characteristics such as sub-threshold swing (SS), increase control efficiency, and is advantageous for scale-down. According to the present disclosure, it is possible to realize various electronic elements / devices / circuits / systems by using the logic switching element.
[0103] Although many details have been specifically described in the above description, they should be construed as examples of specific embodiments rather than as limiting the scope of the invention. For example, a person skilled in the art to which the present invention pertains would know that the configurations of the logic switching elements of FIGS. 1 to 7 and 21 can be modified in various ways. Also, a person skilled in the art would know that the manufacturing method of the logic switching element described with reference to FIGS. 22A to 22C can be modified in various ways. Therefore, the scope of the present invention should be determined not by the described embodiments but by the technical ideas described in the claims. [Industrial Applicability]
[0104] The logic switching element and the manufacturing method thereof according to the present invention can be effectively applied to, for example, technical fields related to electronic elements. [Explanation of symbols]
[0105] 10 Channel Elements 20 Source 30 Drain 100 Substrates 150,160 Insulation layer 200 Conductive layer 300A, 300B, 300C, 300D, 300E Domain Switching Layer 500 Gate electrode AF Antiferroelectric material region F Ferroelectric materials region
Claims
1. A channel element; a source and a drain coupled to the channel element; a gate electrode disposed opposite the channel element; a domain switching layer disposed between the channel element and the gate electrode; The domain switching layer has no hysteresis characteristic and includes a ferroelectric material region including a ferroelectric domain and an antiferroelectric material region including an antiferroelectric domain.
2. The logic switching element according to claim 1 , wherein the domain switching layer has a non-hysteresis characteristic in a change in polarization caused by an external electric field.
3. 3. The logic switching element according to claim 1, wherein the domain switching layer has a structure in which at least one of the ferroelectric material regions and at least one of the antiferroelectric material regions are arranged in a direction parallel to the gate electrode.
4. 3. The logic switching element of claim 1, wherein the domain switching layer has a structure in which at least one of the ferroelectric material regions and at least one of the antiferroelectric material regions are arranged in a direction perpendicular to the gate electrode.
5. 3. The logic switching element of claim 1, wherein the domain switching layer includes a combination of a structure in which at least one of the ferroelectric material regions and at least one of the antiferroelectric material regions are arranged in a direction parallel to the gate electrode and a structure in which they are arranged in a direction perpendicular thereto.
6. 6. The logic switching element of claim 1, wherein the ferroelectric material region and the antiferroelectric material region contain the same base material but have different crystal phases.
7. 7. A logic switching element according to claim 1, wherein the ferroelectric material region includes an orthorhombic crystal phase, and the antiferroelectric material region includes a tetragonal crystal phase.
8. The logic switching element of claim 1 , wherein the ferroelectric material region and the antiferroelectric material region have different doping concentrations.
9. The logic switching element of claim 1 , wherein the ferroelectric material region and the antiferroelectric material region contain different doping materials.
10. 10. The logic switching element of claim 1, wherein at least one of the ferroelectric material region and the antiferroelectric material region includes at least one of an Hf-based oxide and a Zr-based oxide.
11. 11. The logic switching element of claim 1, wherein at least one of the ferroelectric material region and the antiferroelectric material region includes a dopant, the dopant including at least one of Si, Al, Zr, Y, La, Gd, Sr, and Hf.
12. 12. The logic switching element of claim 1, wherein a volume ratio of the ferroelectric material region to the antiferroelectric material region in the domain switching layer ranges from 10:90 to 90:
10.
13. 13. A logic switching element as claimed in any preceding claim, wherein the domain switching layer is in direct contact with the channel element.
14. 13. The logic switching element of claim 1, further comprising an insulating layer disposed between the channel element and the domain switching layer.
15. an insulating layer disposed between the channel element and the domain switching layer; The logic switching element according to claim 1 , further comprising: a conductive layer disposed between the insulating layer and the domain switching layer.
16. 16. The logic switching element of claim 1, wherein the channel element comprises at least one of Si, Ge, SiGe, a III-V semiconductor, an oxide semiconductor, a nitride semiconductor, a nitride-oxide semiconductor, a two-dimensional material, a quantum dot, and an organic semiconductor.
17. Providing a substrate including a channel element; forming an amorphous thin film on the channel element; forming a conductive material layer on the amorphous thin film; annealing the amorphous thin film to form a domain switching layer from the amorphous thin film; The domain switching layer does not have a hysteresis characteristic and is formed to include a ferroelectric material region including a ferroelectric domain and an antiferroelectric material region including an antiferroelectric domain.
18. 20. The method of claim 17, wherein the ferroelectric material region and the antiferroelectric material region have different crystal phases.
19. 19. The method of claim 17, wherein the ferroelectric material region includes an orthorhombic crystal phase, and the antiferroelectric material region includes a tetragonal crystal phase.
20. 20. The method of claim 17, wherein the ferroelectric material region and the antiferroelectric material region have different doping concentrations.
21. 20. The method of claim 17, wherein the ferroelectric material region and the antiferroelectric material region contain different doping materials.
22. 22. The method of claim 17, wherein at least one of the ferroelectric material region and the antiferroelectric material region includes at least one of an Hf-based oxide and a Zr-based oxide.
23. 23. The method of claim 17, wherein the annealing is performed at a temperature of 400[deg.] C. to 1,200[deg.] C.
24. 24. The method of claim 17, further comprising forming a gate electrode from the conductive material layer.
25. 25. The method of claim 17, further comprising forming a source and a drain connected to the channel element.
Citation Information
Patent Citations
Ferroelectric capacitor and ferroelectric field effect tube and manufacturing method thereof
CN101047189A
Ferroelectric device
JP1993090599A
Ferroelectric memory, manufacturing method of the same, ferroelectric film, and manufacturing method of the same
JP2017059751A
Integrated circuit including a dielectric layer
US20100006953A1
Multilevel Ferroelectric Memory Cell for an Integrated Circuit
US20170162250A1