Coated pigment particles, method for producing coated pigment particles, and ink

Coating pigment particles with amorphous alumina hydrate at a controlled pH forms a stable, dispersible layer, addressing the issue of gel formation and enhancing their use in resin compositions and inks, particularly for inkjet recording.

JP7566469B2Active Publication Date: 2024-10-15CANON KK
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020014475
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-31
Publication Date
2024-10-15
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

Conventional methods for producing coated pigment particles result in highly viscous gels when a liquid medium is added, leading to poor dispersibility and difficulty in incorporating them into resin compositions and inks.

Method used

Coating pigment particles with amorphous alumina hydrate, forming a layer that reverses the surface charge and enhances dispersibility by ensuring a zeta potential between +30mV and +100mV, using a method that maintains a pH of 6.0 or lower during heating to prevent crystallization.

Benefits of technology

The coated pigment particles achieve excellent dispersibility, allowing for stable incorporation into resin compositions and inks, with improved adhesion and reduced viscosity fluctuations, enabling high-quality inkjet recording.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566469000007
    Figure 0007566469000007
  • Figure 0007566469000008
    Figure 0007566469000008
  • Figure 0007566469000009
    Figure 0007566469000009
Patent Text Reader

Abstract

To provide: a coated pigment particle blended in products, such as resin compositions and inks, in an excellent dispersion state; and a method for manufacturing the coated pigment particle.SOLUTION: A coated pigment particle includes: a pigment; and a coating layer which is formed by an amorphous alumina hydrate and is disposed on at least a part of a particle surface of the pigment. A method for manufacturing the coated pigment particle includes: obtaining an aqueous pigment dispersing solution containing a pigment and aluminum salt; and disposing a coating layer formed by the amorphous alumina hydrate on at least a part of the particle surface of the pigment by heating the aqueous pigment dispersing solution while maintaining a pH thereof at 6.0 or below.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to coated pigment particles, a method for producing coated pigment particles, a resin composition, a resin molded product, an ink, an ink cartridge, and an inkjet recording method. [Background technology]

[0002] Coated pigment particles are produced by coating the surface of pigment particles with a coating layer formed from a desired compound. For example, a method has been proposed in which alumina sol is sprayed onto carbon black and then dried to obtain coated pigment particles (Patent Document 1). Also, a method has been proposed in which a pigment is dispersed in an aqueous aluminum chloride solution, followed by precipitation and drying to obtain coated pigment particles (Patent Document 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2001-323191 A [Patent Document 2] Japanese Patent Application Publication No. 11-172170 Summary of the Invention [Problem to be solved by the invention]

[0004] However, coated pigment particles produced by conventional methods tend to form a highly viscous gel when a liquid medium such as water is added, making it difficult to disperse them. This is presumably because no coating layer is formed on the surface of the pigment, and a simple mixture of the pigment and the aluminum compound is formed, or the coating layer is easily removed. In other words, with the methods proposed in Patent Documents 1 and 2, it is difficult to produce coated pigment particles that are required to have excellent dispersibility and are to be incorporated into products such as resin compositions and inks.

[0005] Therefore, an object of the present invention is to provide coated pigment particles that can be incorporated in a highly dispersed state into products such as resin compositions, inks, etc. Another object of the present invention is to provide a method for producing the coated pigment particles, and a resin composition, a resin molded product, an ink, an ink cartridge, and an inkjet recording method that use the coated pigment particles. [Means for solving the problem]

[0006] That is, according to the present invention, there is provided a self-dispersing pigment comprising at least one pigment selected from the group consisting of carbon black and organic pigments, and a coating layer formed of amorphous alumina hydrate disposed on at least a part of the particle surface of the pigment, the pigment being a self-dispersing pigment having an anionic group bonded directly or via another atomic group to the particle surface. The zeta potential is between +30mV and +100mV. The coated pigment particles are characterized in that Effect of the Invention

[0007] According to the present invention, it is possible to provide coated pigment particles that are blended in an excellent dispersed state into products such as resin compositions and inks. Furthermore, according to the present invention, it is possible to provide a method for producing the coated pigment particles, a resin composition, a resin molded product, an ink, an ink cartridge, and an inkjet recording method that use the coated pigment particles. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram illustrating one embodiment of a coated pigment particle of the present invention. [Diagram 2] 1 is a transmission electron microscope photograph showing one embodiment of a coated pigment particle of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view illustrating an embodiment of an ink cartridge of the present invention. [Figure 4] 1A and 1B are diagrams illustrating an example of an inkjet recording apparatus used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording apparatus, and (b) is a perspective view of a head cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt." In addition, water-based ink for inkjet printing may be simply referred to as "ink." Physical property values ​​are values ​​at room temperature (25°C) unless otherwise specified.

[0010] <Coated pigment particles> (covering layer) When an aqueous dispersion of alumina hydrate is applied to a fibrous material such as paper, the alumina hydrate adheres to the vicinity of the surface of the fibrous material. The alumina hydrate then spreads to cover each fiber constituting the fibrous material and adheres firmly to the fibrous material, as described in International Publication No. 2005-118304. In this document, crystalline alumina hydrate is used. It is presumed that the water dispersibility and adhesion to the fibrous material of the alumina hydrate are exerted by the hydroxyl groups of the alumina hydrate. That is, it is considered that the hydroxyl groups improve the water affinity and increase the water dispersibility. Furthermore, it is considered that the adhesion is increased by the interaction such as hydrogen bonding between the hydroxyl groups of the alumina hydrate and the hydroxyl groups present on the surface of the fibrous material.

[0011] The present inventors have found that by covering the surface of a pigment particle with a coating layer formed of amorphous alumina hydrate, water dispersibility and adhesive strength equivalent to those of crystalline alumina hydrate can be obtained, and have arrived at the present invention. FIG. 1 is a schematic diagram showing one embodiment of the coated pigment particle of the present invention. As shown in FIG. 1, the coated pigment particle 10 of this embodiment includes a pigment 2 and a coating layer 4 formed of amorphous alumina hydrate arranged on at least a part of the particle surface of the pigment 2. A polar group such as a hydroxyl group is present on the particle surface of a general pigment. It is presumed that a reaction occurs between the hydroxyl group present on the particle surface of the pigment 2 and the amorphous alumina hydrate, and thus the particle surface and the aluminum atom are bonded by an ether bond. It is presumed that this reaction is dehydration condensation. In addition, since the amorphous alumina hydrate has a hydroxyl group (-OH group), a hydroxyl group is present on the surface of the coating layer 4. Pigments coated with amorphous alumina hydrate have the advantage that they are less thixotropic than crystalline alumina hydrate, and therefore do not require consideration of the effects of viscosity fluctuations. Thixotropy is the property of viscosity decreasing when shear force is applied.

[0012] Amorphous alumina hydrate is an alumina hydrate in which no crystal structure is observed, and is represented by the composition AlOOH, and is called boehmite. The fact that the coating layer is formed of amorphous alumina hydrate can be confirmed using a transmission electron microscope and elemental analysis. FIG. 2 is a transmission electron microscope photograph showing one embodiment of the coated pigment particle of the present invention. In FIG. 2, a pigment-coated particle is observed in which a coating layer formed of amorphous alumina hydrate is arranged on the particle surface of the pigment (a large number of carbon black particles connected in a tuft shape). A striped pattern indicating a crystal structure is observed in the carbon black. In contrast, no striped pattern indicating a crystal structure is observed in the coating layer. In this way, when no striped pattern is observed in the coating layer in a transmission electron microscope photograph, it can be determined that the coating layer is formed of an amorphous substance.

[0013] In addition, a transmission electron microscope equipped with an elemental analyzer is used to perform elemental analysis of the coating layer and the pigment particles, and it is confirmed that aluminum, oxygen atoms, and hydrogen atoms are detected in the coating layer, while aluminum is not detected in the pigment particles. This allows it to be determined that the coating layer is formed of alumina hydrate. Note that, although X-ray diffraction is commonly used as a method for analyzing the crystal structure of a substance, the coating layer formed of amorphous alumina hydrate is thin, making it difficult to observe its crystal structure by X-ray diffraction.

[0014] The thickness of the coating layer is preferably 1 nm or more and 10 nm or less. The thickness of the coating layer can be measured by observing the coated pigment particles using a transmission electron microscope.

[0015] The presence of a coating layer on the pigment particle surface can be confirmed by the following method, in addition to the method of observation using a transmission electron microscope. The zeta (ζ) potential of a pigment that does not have a coating layer usually shows a negative (-) value. Furthermore, since general-purpose self-dispersing pigments have anionic groups, the zeta potential shows a negative value. In contrast, the zeta potential of coated pigment particles that have a coating layer shows a positive (+) value because the surface charge of the particles is inverted. The surface charge is inverted when the pigment particle surface is covered to some extent with amorphous alumina hydrate. Therefore, if the pigment is not covered with amorphous alumina hydrate, the surface charge will not be inverted and the zeta potential will not be a positive value.

[0016] From the viewpoint of dispersibility, the zeta potential of the coated pigment particles is sufficient if it is +25 mV or more, and preferably +30 mV or more. On the other hand, if the zeta potential is less than +25 mV, the coating layer may not be sufficiently coated, and sufficient dispersibility may not be obtained. The zeta potential of the coated pigment particles is preferably +100 mV or less, and more preferably +70 mV It is preferable that the zeta potential of the coated pigment particles is as follows: The zeta potential of the coated pigment particles can be measured by a zeta potential measuring device.

[0017] The zeta potential of the coated pigment particles has only one peak top, and does not have multiple peak tops. In addition, the zeta potential peak shape of the coated pigment particles is sharp, not broad. Therefore, the uniformity of the coating layer can be estimated from the zeta potential peak shape.

[0018] (Pigments) As the pigment (pigment type), for example, inorganic pigments such as carbon black, graphite, calcium carbonate, and titanium oxide; organic pigments such as azo, phthalocyanine, and quinacridone can be used. Among them, inorganic pigments such as carbon black and graphite, and organic pigments are preferably used, and at least one of carbon black and graphite is more preferably used. As the graphite, graphene can be used. In particular, carbon black is preferably used as a pigment because it has more reactive active sites on the particle surface compared to other pigments and can efficiently form a coating layer. As the carbon black, any carbon black such as furnace black, lamp black, acetylene black, and channel black can be used.

[0019] The DBP oil absorption of carbon black is preferably 50 mL / 100 g or more and 200 mL / 100 g or less. In particular, it is more preferably 120 mL / 100 g or more and 170 mL / 100 g or less, and particularly preferably 120 mL / 100 g or more and 150 mL / 100 g or less. The DBP oil absorption can be measured by a method conforming to JIS K6221 or ASTM D 2414. These methods involve dropping dibutyl phthalate onto 100 g of carbon black under stirring, and measuring the amount of dibutyl phthalate added at the point where the torque reaches a maximum.

[0020] The specific surface area of ​​carbon black by the BET method is 100 m 2 / g or more 600m 2The specific surface area by the BET method can be measured by a method conforming to JIS K 6217, ASTM D 6556, etc. These methods involve immersing degassed carbon black in liquid nitrogen and measuring the amount of nitrogen adsorbed on the particle surfaces of the carbon black when equilibrium is reached.

[0021] The primary particle diameter of carbon black is preferably 10 nm or more and 40 nm or less. Carbon black usually exists in a state where multiple primary particles are connected three-dimensionally like a bunch of grapes. The primary particle diameter means the particle diameter of the smallest unit of carbon black (primary particle) that forms one pigment particle. The primary particle diameter of carbon black can be determined by observing and measuring the particle diameters of about 100 smallest units of carbon black that form pigment particles using a transmission or scanning electron microscope, and taking the arithmetic average value.

[0022] The average particle size of carbon black is preferably 50 nm or more and 200 nm or less. The average particle size means the particle size of carbon black in the form in which it is usually present. In the present invention, the average particle size is measured as the 50% cumulative value [D50 (nm)] of the volume-based particle size distribution using a dynamic light scattering particle size distribution measuring device or the like.

[0023] The organic pigment preferably has a primary particle size of 50 nm or more and 150 nm or less. The organic pigment preferably has an average particle size of 50 nm or more and 250 nm or less. The definitions of the primary particle size and average particle size of the organic pigment are the same as those of the carbon black.

[0024] As the pigment, a resin-dispersed pigment using a resin as a dispersant, a self-dispersed pigment in which an ionic group such as an anionic group is bonded to the pigment particle surface, etc. can be used. In addition, a resin-bonded pigment in which an organic group containing a resin is chemically bonded to the pigment particle surface, and a microcapsule pigment in which the surface of the pigment particle is coated with a resin or the like can be used. Among them, it is preferable to use a self-dispersed pigment. In the present invention, for the sake of convenience, the term "pigment" is used not only when the target on whose particle surface the amorphous alumina hydrate is disposed is a pigment that has not been treated with a resin dispersant or an ionic group, but also when it is a resin-dispersed pigment or a self-dispersed pigment.

[0025] As the self-dispersing pigment, an anionic group such as a carboxylic acid group, a sulfonic acid group, or a phosphonic acid group can be used, which is bonded to the particle surface of the pigment directly or via another atomic group (-R-). The anionic group may be either an acid type or a salt type, and when it is a salt type, it may be either a partially dissociated state or a completely dissociated state. When the anionic group is a salt type, examples of the cation that serves as the counter ion include an alkali metal cation, ammonium, and organic ammonium. Specific examples of the other atomic group (-R-) include a linear or branched alkylene group having 1 to 12 carbon atoms; an arylene group such as a phenylene group or a naphthylene group; a carbonyl group; an imino group; an amide group; a sulfonyl group; an ester group; and an ether group. In addition, it may be a group that is a combination of these groups.

[0026] In the case of self-dispersing pigments, the coating layer can be efficiently formed because ionic groups are present on the surface of the pigment particles, either directly or via other atomic groups. The ionic group density (mmol / g) of the self-dispersing pigment is preferably 0.05 mmol / g or more and 1.00 mmol / g or less, and more preferably 0.10 mmol / g or more and 0.50 mmol / g or less. The ionic group density is a physical property value expressed as the number of moles (mmol) of ionic groups per 1 g of pigment, and is determined by colloid titration. Methyl glycol chitosan can be used for the analysis of anionic groups by colloid titration, and hydrochloric acid can be used for the analysis of cationic groups.

[0027] As the resin dispersant for dispersing the pigment in the aqueous medium, it is preferable to use one that can disperse the pigment in the aqueous medium by the action of anionic groups. As the resin dispersant, a resin described below, especially a water-soluble resin, can be used. The content (mass%) of the pigment in the ink is preferably 0.3 times or more and 10.0 times or less in mass ratio to the content of the resin dispersant.

[0028] As the pigment to be coated, it is preferable to use a self-dispersed pigment or a resin-dispersed pigment rather than an untreated pigment, and it is more preferable to use a self-dispersed pigment. This is because a stable coating layer is easily formed. In addition, when a self-dispersed pigment or a resin-dispersed pigment is used, it is also advantageous in that the aluminum salt reacts easily and the unreacted aluminum salt is less likely to remain in the reaction system compared to a pigment that has not been treated with these. When a self-dispersed pigment is used, purification after the reaction is also easier than with a resin-dispersed pigment.

[0029] <Method of manufacturing coated pigment particles> The method for producing the coated pigment particles of the present invention is a method for producing the above-mentioned coated pigment particles. The method for producing coated pigment particles of the present invention includes a pigment aqueous dispersion preparation step and a coating step. The pigment aqueous dispersion preparation step is a step of obtaining a pigment aqueous dispersion containing a pigment and an aluminum salt. The coating step is a step of heating the pigment aqueous dispersion while maintaining the pH at or below 6.0 to provide a coating layer formed of amorphous alumina hydrate on at least a portion of the pigment particle surface.

[0030] In the pigment aqueous dispersion preparation step, a pigment aqueous dispersion containing a pigment and an aluminum salt is obtained. In the subsequent coating step, the pigment aqueous dispersion is heated while being maintained at a pH of 6.0 or less, so it is preferable to use an acidic aluminum salt as the aluminum salt. Examples of the acidic aluminum salt include aluminum sulfate, aluminum nitrate, aluminum hydrochloride, and (poly)aluminum chloride. Of these, it is preferable to use polyaluminum chloride as the acidic aluminum salt. Compared with other aluminum salts, polyaluminum chloride does not lower the pH too much in the coating step, and the pigment aqueous dispersion obtained by mixing it with the pigment is less likely to gel.

[0031] The amount of aluminum salt relative to the pigment can be appropriately set depending on the thickness of the coating layer to be formed. Specifically, it is preferable to use 30 parts by mass or more and 200 parts by mass or less of aluminum salt relative to 100 parts by mass of pigment. In addition, the content (mass%) of solids (pigment and aluminum compound) in the pigment aqueous dispersion is preferably 1.0% by mass or more and 20.0% by mass or less based on the total mass of the pigment aqueous dispersion.

[0032] A water-based liquid medium is used as the liquid medium constituting the pigment aqueous dispersion. This liquid medium may be one that constitutes a pigment dispersion or an aqueous solution of an aluminum compound. Specifically, an aqueous medium consisting of only water or a mixture of water and an organic solvent can be used. As the organic solvent, it is preferable to use one that is miscible or soluble with water at any ratio. In particular, it is preferable to use a uniform mixed solvent containing 50% by mass or more of water as the aqueous medium. As the water, it is preferable to use ion-exchanged water or pure water.

[0033] For example, the pigment aqueous dispersion can be obtained by (i) mixing an aqueous pigment dispersion with an aluminum salt; (ii) mixing a pigment with an aqueous aluminum solution; or (iii) mixing an aqueous pigment dispersion with an aqueous aluminum solution. The method is not limited to these, and any method may be used as long as it can maintain the pH of the resulting pigment aqueous dispersion at 6.0 or less. In addition, an acid or alkali may be added to the pigment aqueous dispersion as necessary to adjust the pH of the pigment aqueous dispersion to 6.0 or less.

[0034] In the coating step, the obtained pigment aqueous dispersion is heated while maintaining the pH at 6.0 or less. This allows a coating layer formed of amorphous alumina hydrate to be arranged on at least a part of the pigment particle surface, and the desired coated pigment particles are produced. For example, the pigment aqueous dispersion can be heated using an apparatus such as an autoclave. By maintaining the pH at 6.0 or less during heating, amorphous alumina hydrate that becomes the amorphous coating layer is produced. If the pH during heating is greater than 6.0 and less than 11.0, boehmite that becomes the crystalline coating layer is produced. Furthermore, if the pH during heating is greater than 11.0, bayerite that becomes the crystalline coating layer is produced. In other words, if the pH during heating is greater than 6.0, crystalline alumina hydrate is produced, and therefore an amorphous coating layer cannot be obtained.

[0035] The pigment aqueous dispersion is heated, preferably with stirring. Aluminum is hydrated in water to form hydroxyl groups. The formed hydroxyl groups react with polar groups such as hydroxyl groups present on the pigment particle surface to form amorphous alumina hydrate on the pigment particle surface. The temperature at which the pigment aqueous dispersion is heated is preferably 80°C or higher and 150°C or lower. If the heating temperature is lower than 80°C, it may be somewhat difficult to coat the pigment particle surface with amorphous alumina hydrate to form a coating layer. On the other hand, if the heating temperature is higher than 150°C, the formed alumina hydrate may be more likely to crystallize.

[0036] The coating step forms the desired coated pigment particles. More specifically, an aqueous dispersion of the coated pigment particles can be obtained. If necessary, the aqueous dispersion may be purified to remove raw materials and reaction by-products remaining therein. The coated pigment particles can be purified by a filtration method such as ultrafiltration or an ion exchange method using an ion exchange resin. When purifying by ultrafiltration, it is preferable to purify the aqueous dispersion until the electrical conductivity is 50 mS / m or less.

[0037] <Resin composition and resin molded product> The resin composition of the present invention contains the coated resin particles and resin described above. The coated pigment particles described above can exhibit various physical or chemical properties by selecting the type of pigment that is a constituent component. For example, in the case of coated pigment particles in which a coating layer is disposed on the surface of carbon black or graphite particles, the coated pigment particles of such a configuration exhibit thermal conductivity or electrical conductivity. Therefore, by molding a resin composition in which such coated pigment particles are blended with a resin, it is possible to obtain various types of resin molded products that exhibit thermal conductivity or electrical conductivity. Examples of resin molded products that exhibit thermal conductivity or electrical conductivity and are obtained by molding a resin composition containing coated pigment particles and a resin include coloring materials such as masterbatches; resin products such as resin sheets and trays; sealing materials such as gaskets; and electrode members. By molding a resin composition containing coated pigment particles in which a coating layer is disposed on the surface of graphene particles and a resin, resin molded products such as conductive sheets and thermally conductive sheets, as well as strength members and sliding members can be obtained.

[0038] (resin) In general, when dispersing pigments such as organic pigments in resins, problems such as pigment aggregation are likely to occur, and the affinity between the pigment and the resin is often an issue. For this reason, advanced aggregation suppression technology is required to disperse pigments in resins, and it is necessary to add components that assist dispersion, such as surfactants and dispersants. In contrast, the above-mentioned coated pigment particles have a coating layer formed of amorphous alumina hydrate, and the surface thereof exhibits properties unique to inorganic substances. Therefore, the coated pigment particles have excellent compatibility with various resins compared to normal pigments that do not have a coating layer, and can be dispersed in resins in a good state without adding components that assist dispersion, such as surfactants and dispersants.

[0039] The content of the coated pigment particles in the resin composition can be appropriately set according to the type and use of the intended resin molded product, and is not particularly limited. The content (mass%) of the coated pigment particles in the resin composition is usually 0.1 mass% or more and 70.0 mass% or less, preferably 0.5 mass% or more and 50.0 mass% or less, based on the entire resin composition. If it is within the above range, the desired performance such as thermal conductivity or electrical conductivity can be easily obtained by using the coated pigment particles, and the properties of the resin such as mechanical strength or hardness are not impaired.

[0040] Examples of the resin include polyethylene, polystyrene, vinyl acetate resin, vinyl chloride resin, acrylic resin, polyacrylonitrile, polyamide, cellulose acetate resin, cellulose nitrate resin, phenol resin, epoxy resin, silicone resin, and natural rubber.

[0041] Among the above, silicone resin is preferred. As the silicone resin, general silicone resins such as methyl silicone resin, methylphenyl silicone resin, and phenyl silicone resin can be used. In addition to the above general silicone resins, modified silicone resins such as alkyd-modified silicone resin, polyester-modified silicone resin, epoxy-modified silicone resin, urethane-modified silicone resin, and acrylic-modified silicone resin can also be used.

[0042] As the silicone resin, a two-liquid type silicone resin (reactive silicone resin) can also be used. Examples of reactive silicone resins include addition curing silicone resins, condensation curing silicone resins, peroxide curing silicone resins, and cationic UV silicone resins. Among them, addition curing silicone resins are preferred because they are easy to obtain and can be cured at room temperature. Addition curing silicone resins are formed from vinyl polysiloxane and hydropolysiloxane.

[0043] By molding a resin composition containing coated pigment particles and a resin, various resin molded products such as those listed above can be obtained. When a two-liquid type silicone resin is used as the resin, a resin molded product such as a resin sheet can be obtained by applying the resin composition to a substrate or the like and curing it. In addition, after blending the coated pigment particles with a resin, it can be molded using a molding machine such as a twin-screw extruder to form pellets. Furthermore, the obtained pellets can be extrusion molded to form a resin molded product having a desired shape.

[0044] <Ink> The ink of the present invention is an ink suitable for inkjet printing, containing the above-mentioned coated pigment particles and a liquid medium. That is, the ink of the present invention contains the coated pigment particles as a coloring material. The content (mass%) of the coated pigment particles in the ink is preferably 0.1 mass% or more and 15.0 mass% or less, based on the total mass of the ink, and more preferably 1.0 mass% or more and 10.0 mass% or less. The ink may further contain a coloring material such as a dye for color matching or the like.

[0045] (liquid medium) The ink contains a liquid medium such as water or an aqueous medium which is a mixed solvent of water and a water-soluble organic solvent. In particular, it is preferable to use an aqueous ink containing at least water as the aqueous medium. As the water, it is preferable to use deionized water or ion-exchanged water. The content (mass %) of water in the ink is preferably 50.0 mass % or more and 95.0 mass % or less based on the total mass of the ink.

[0046] Examples of the water-soluble organic solvent that can be used include alcohols, polyhydric alcohols, polyglycols, glycol ethers, nitrogen-containing polar solvents, sulfur-containing polar solvents, etc. The content (mass %) of the water-soluble organic solvent in the ink is preferably 5.0 mass % or more and 90.0 mass % or less, and more preferably 10.0 mass % or more and 50.0 mass % or less, based on the total mass of the ink.

[0047] (resin) The ink may contain a resin. The content (mass %) of the resin in the ink is preferably from 0.1 to 20.0% by mass, and more preferably from 0.5 to 15.0% by mass, based on the total mass of the ink.

[0048] The resin can be added to the ink (i) to stabilize the dispersion state of the coated pigment particles, that is, as a resin dispersant or its auxiliary. Also, the resin can be added to the ink (ii) to improve various properties of the recorded image. Examples of the form of the resin include block copolymers, random copolymers, graft copolymers, and combinations thereof. The resin may be a water-soluble resin that can be dissolved in an aqueous medium, or may be resin particles that are dispersed in an aqueous medium. The resin particles do not need to encapsulate a colorant.

[0049] Examples of the resin include acrylic resins, urethane resins, olefin resins, etc. Among them, acrylic resins and urethane resins are preferred, and acrylic resins composed of units derived from (meth)acrylic acid or (meth)acrylate are more preferred.

[0050] The acrylic resin preferably has a hydrophilic unit and a hydrophobic unit as constituent units. Among them, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one of a monomer having an aromatic ring and a (meth)acrylic acid ester monomer is preferred. In particular, a resin having a hydrophilic unit derived from (meth)acrylic acid and a hydrophobic unit derived from at least one of styrene and α-methylstyrene is preferred. These resins are easily interacted with pigments, and therefore can be suitably used as a resin dispersant for dispersing pigments.

[0051] The hydrophilic unit is a unit having a hydrophilic group such as an anionic group. The hydrophilic unit can be formed, for example, by polymerizing a hydrophilic monomer having a hydrophilic group. Specific examples of the hydrophilic monomer having a hydrophilic group include acidic monomers having a carboxylic acid group such as (meth)acrylic acid, itaconic acid, maleic acid, and fumaric acid, and anionic monomers such as anhydrides and salts of these acidic monomers. Examples of cations constituting the salts of acidic monomers include ions of lithium, sodium, potassium, ammonium, and organic ammonium. The hydrophobic unit is a unit not having a hydrophilic group such as an anionic group. The hydrophobic unit can be formed, for example, by polymerizing a hydrophobic monomer not having a hydrophilic group such as an anionic group. Specific examples of the hydrophobic monomer include monomers having an aromatic ring such as styrene, α-methylstyrene, and benzyl (meth)acrylate; and (meth)acrylic acid ester monomers such as methyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0052] The urethane resin can be obtained by reacting, for example, polyisocyanate with a polyol. In addition, a chain extender may be further reacted with the urethane resin. Examples of the olefin resin include polyethylene and polypropylene.

[0053] (Other additives) The ink may contain various additives such as surfactants, pH adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters, and chelating agents, as necessary. Examples of surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants. The content (mass %) of the surfactant in the ink is preferably 0.1% by mass or more and 5.0% by mass or less, and more preferably 0.1% by mass or more and 2.0% by mass or less, based on the total mass of the ink.

[0054] <Ink cartridges> The ink cartridge of the present invention includes ink and an ink storage section that stores the ink. The ink stored in the ink storage section is the ink of the present invention described above. FIG. 3 is a cross-sectional view that shows a schematic diagram of an embodiment of the ink cartridge of the present invention. As shown in FIG. 3, an ink supply port 12 for supplying ink to a recording head is provided on the bottom surface of the ink cartridge. The inside of the ink cartridge is an ink storage section for storing ink. The ink storage section is composed of an ink storage chamber 14 and an absorber storage chamber 16, which are communicated with each other via a communication port 18. The absorber storage chamber 16 is also communicated with the ink supply port 12. The ink storage chamber 14 stores liquid ink 20, and the absorber storage chamber 16 stores absorbers 22 and 24 that hold the ink in an impregnated state. The ink storage section may not have an ink storage chamber that stores liquid ink, and may be in a form in which the entire amount of ink stored is held by the absorber. The ink storage section may also be in a form in which the entire amount of ink stored is stored in a liquid state, without having an absorber. Furthermore, the ink cartridge may be configured to have an ink container and a recording head.

[0055] <Inkjet recording method> The inkjet recording method of the present invention is a method of ejecting the ink of the present invention described above from an inkjet recording head to record an image on a recording medium. Methods for ejecting the ink include a method of applying mechanical energy to the ink and a method of applying thermal energy to the ink. In the present invention, it is particularly preferable to adopt a method of ejecting the ink by applying thermal energy to the ink. Other than using the ink of the present invention, the steps of the inkjet recording method may be known.

[0056] FIG. 4 is a diagram showing an example of an inkjet recording device used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording device, and (b) is a perspective view of a head cartridge. The inkjet recording device is provided with a conveying means (not shown) for conveying a recording medium 32, and a carriage shaft 34. A head cartridge 36 can be mounted on the carriage shaft 34. The head cartridge 36 includes recording heads 38 and 40, and is configured so that an ink cartridge 42 is set thereon. While the head cartridge 36 is conveyed in the main scanning direction along the carriage shaft 34, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, an image is recorded on the recording medium 32 by conveying the recording medium 32 in the sub-scanning direction by a conveying means (not shown). EXAMPLES

[0057] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples without departing from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified.

[0058] <Method for measuring anionic group density> The anionic group density (mmol / g) of the self-dispersing pigment was measured by colloid titration using methyl glycol chitosan as the titration reagent.

[0059] <Pigments> The types of pigments shown in Table 1 were prepared.

[0060] TIFF0007566469000001.tif66170

[0061] The pigments shown in Table 2 were each subjected to self-dispersion or resin dispersion treatment according to a standard method to prepare the pigments shown in Table 2. Pigment 21 is a resin-dispersed pigment prepared by encapsulating carbon black with a resin dispersant in accordance with the description in JP2009-518524. As the resin dispersant, a styrene / acrylic acid / methacrylic acid copolymer (copolymerization [mass] ratio 77 / 10 / 13, acid value 152 mgKOH / g, weight average molecular weight 8,600) was used.

[0062] TIFF0007566469000002.tif115170

[0063] <Treatment agent> As treatment agents for coating the pigment, aluminum salt 1 and alumina sol 1 shown below were prepared. Aluminum salt 1: Polyaluminum chloride (product name "Takibain #1500", manufactured by Taki Chemical Industry, solids concentration (equivalent to aluminum oxide) 23.6%) Alumina sol 1: Alumina sol (product name "Alumina sol 520-A", manufactured by Nissan Chemical Industries, Ltd.)

[0064] <Production of Coated Pigment Particles> Example 1 Pigment 1 was mixed with water to obtain a 5% aqueous dispersion of pigment 1. 10 parts of aluminum salt 1 was added to 100 parts of pigment to the obtained aqueous dispersion of pigment 1, and then the mixture was stirred at 1,500 rpm for 30 minutes using a stirrer (product name "TK Robomix", manufactured by Primix) to obtain an aqueous pigment dispersion with a pH of 5.8. The obtained aqueous pigment dispersion was placed in a flask, heated to 80°C and stirred for 3 hours, and then cooled to 25°C. The pH after stirring was 5.8. Next, the mixture was purified using an ultrafiltration device until the electrical conductivity was 50 mS / m or less to obtain coated pigment particles. Observation using a transmission electron microscope confirmed that the coating layer was formed of amorphous alumina hydrate.

[0065] (Examples 2 to 32) Coated pigment particles were obtained in the same manner as in Example 1 above, except that the type of pigment, the amount of treating agent per 100 parts of pigment, pH, and heating temperature were as shown in Table 3-1.

[0066] (Comparative Examples 1 to 6) The same operation as in Example 1 was carried out, except that the type of pigment, the amount of treatment agent per 100 parts of pigment, the pH of the pigment aqueous dispersion before heating, and the heating temperature were as shown in Table 3-2. The pH of the pigment aqueous dispersion was adjusted with a 0.1 mol / L aqueous potassium hydroxide solution. However, the pigment aqueous dispersion gelled, and coated resin particles could not be obtained.

[0067] (Comparative Examples 7 to 10) Pigments 1, 2, 6, and 9 were not surface-coated, and were used as Comparative Examples 7-10.

[0068] (Comparative Examples 11 and 12) According to the description in "Example 2" of Patent Document 1 (JP Patent Publication 2001-323191 A), alumina sol 1 was sprayed onto pigments 2 and 6. As a result, the entire mixture gelled, making further operations impossible, and the pigments could not be coated.

[0069] (Comparative Examples 13 to 16) According to the description in Patent Document 2 (JP Patent Publication 11-172170), pigment particles 2, 4, 6, and 18 were each subjected to a surface modification treatment using aluminum salt 1. Specifically, each pigment was mixed with aluminum salt 1, and then treated at 10,000 rpm for 10 minutes using a centrifuge. As a result, the entire mixture gelled, and it was not possible to coat the pigment.

[0070] TIFF0007566469000003.tif227170

[0071] TIFF0007566469000004.tif121170

[0072] <Evaluation> The produced coated pigment particles were subjected to the following evaluations. In the evaluation criteria for each item below, "A" and "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown in Tables 4-1 and 4-2.

[0073] (Production of coated pigment particles) The pigment aqueous dispersion was dropped onto a TEM grid (product name "Hi-Res Carbon HRC-C10 STEM", manufactured by Oken Shoji) and then dried to prepare a sample. Using a transmission electron microscope (product name "TecnaiF20", manufactured by FEI), the sample was observed at a magnification of 1 million times and images were taken to observe the state of the coating layer. In addition, the fluidity of the prepared pigment aqueous dispersion was visually observed. From these results, the generation of coated pigment particles was evaluated according to the following evaluation criteria. A: No striped pattern indicating a crystal structure was observed, an amorphous coating layer was disposed on the surface of the pigment particles, and the pigment aqueous dispersion had fluidity. C: A striped pattern indicating a crystal structure was observed, and the coating layer was crystalline, or the pigment aqueous dispersion gelled and did not exhibit fluidity.

[0074] (Ease of purification) The number of ultrafiltration cycles required until the electrical conductivity of the pigment aqueous dispersion reached 10 mS / m or less was measured, and the ease of purification was evaluated according to the following evaluation criteria. A: Less than five times. B: More than 5 times but less than 10 times. C: Even after more than 10 times, it did not drop below 10mS / m.

[0075] (Zeta potential) The zeta potential (mV) of the coated pigment particles was measured using a zeta potential meter (product name "ZETASISER NANO", manufactured by MALVERN).

[0076] (dispersibility) A 5% aqueous dispersion of the coated pigment particles was prepared, placed in a sealed container, and stored for 3 months in an environment of 25° C. After storage, the aqueous dispersion was visually observed, and the dispersibility was evaluated according to the following evaluation criteria. A: No sediment was observed even after storage for 3 months. B: No sediment was observed at one month, but sediment was observed after three months. C: Sediment was observed at one month.

[0077] (Adhesion) A 0.1% aqueous dispersion of coated pigment particles was prepared, and a drop was dropped onto a filter paper using a dropper and spread in a circular shape on the filter paper. The diameters of the colored part (colored part) and the uncolored part (colorless part) formed outside of the circularly spread aqueous dispersion were measured. The "bleed rate" was calculated according to the following formula (1), and the adhesion of the coated pigment particles to the paper substrate was evaluated according to the following evaluation criteria. This evaluation can be used as an index of image quality when recording with an ink containing coated pigment particles. If it is ranked B, a clear image without bleeding of fine lines can be recorded even when recording characters of about 2 points on ordinary plain paper. Bleeding rate = diameter of colored part / diameter of colorless part (1) A: The bleeding rate was 0.5 or less. B: The bleeding rate was more than 0.5 and 0.8 or less. C: The bleeding rate was more than 0.8.

[0078] (Viscosity of Resin Composition) The coated pigment particles and silicone oil (product name "Silicone Oil-V41", manufactured by Shin-Etsu Silicone) were mixed to prepare a resin composition containing 20 volume % of the coated pigment particles. The viscosity of the prepared resin composition was measured at 25°C using a cone-plate type E-type viscometer, and the viscosity of the resin composition was evaluated according to the following evaluation criteria. A: The viscosity was less than 5,000 Pa·s. B: Viscosity was 5,000 Pa·s or more and less than 10,000 Pa·s. C: Viscosity was 10,000 Pa·s or more.

[0079] TIFF0007566469000005.tif219170

[0080] TIFF0007566469000006.tif116170

[0081] (Evaluation of images obtained by the inkjet recording method) Inks having the following compositions were prepared using the coated pigment particles of Example 3 and the pigment of Comparative Example 7. As the surfactant, a product named "Acetylenol E100" (manufactured by Kawaken Fine Chemicals) was used. Coated pigment particles (pigment): 3.0% Glycerin: 10.0% Triethylene glycol: 10.0% Surfactant: 0.3% Ion-exchanged water: Remainder

[0082] The prepared ink was filled into a black ink cartridge of an inkjet recording device (trade name "PIXUS TS-5130", manufactured by Canon), and a solid image with a recording duty of 100% was recorded on plain paper (trade name "PB paper", manufactured by Canon). In this inkjet recording device, an image recorded under the condition that two drops of 11.2ng±10% ink are applied to a unit area of ​​1 / 600 inch×1 / 600 inch is defined as having a recording duty of 100%. The optical density of the recorded image was measured using a densitometer (trade name "FD-7", manufactured by Konica Minolta). As a result, the optical density of the image recorded with the ink prepared using the coated pigment particles of Example 3 was 1.2. On the other hand, the optical density of the image recorded with the ink prepared using the pigment of Comparative Example 7 was 1.0.

Claims

1. At least one pigment selected from the group consisting of carbon black and organic pigments; and a coating layer formed of amorphous alumina hydrate disposed on at least a portion of a particle surface of the pigment, the pigment is a self-dispersing pigment having an anionic group bonded to the particle surface directly or via another atomic group, A coated pigment particle having a zeta potential of +30 mV or more and +100 mV or less.

2. 2. The coated pigment particle of claim 1, wherein the pigment is carbon black.

3. A method for producing the coated pigment particles according to claim 1 or 2, comprising the steps of: obtaining an aqueous pigment dispersion having a pH of 6.0 or less, the aqueous pigment dispersion containing at least one pigment selected from the group consisting of carbon black and organic pigments, and an aluminum salt; a step of heating the pigment aqueous dispersion while maintaining the pH at or below 6.0 to form a coating layer formed of amorphous alumina hydrate on at least a portion of the surface of the pigment particles; having The method for producing coated pigment particles is characterized in that the pigment is a self-dispersing pigment having an anionic group bonded to the particle surface directly or via another atomic group.

4. 4. The method for producing coated pigment particles according to claim 3, wherein the aluminum salt is polyaluminum chloride.

5. 5. The method for producing coated pigment particles according to claim 3, wherein the amount of the aluminum salt used is 30 parts by mass or more and 200 parts by mass or less based on 100 parts by mass of the pigment used.

6. A resin composition comprising the coated pigment particles according to claim 1 or 2 and a resin.

7. A resin molded product formed from the resin composition according to claim 6.

8. 3. An ink comprising the coated pigment particles according to claim 1 or 2 and a liquid medium.

9. The ink according to claim 8, which is for ink-jet use.

10. An ink cartridge including an ink and an ink storage section for storing the ink, 10. An ink cartridge, wherein the ink is the ink according to claim 9.

11. An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, comprising:

10. An ink jet recording method, comprising the ink according to claim 9.

Citation Information

Patent Citations

  • Organic pigment coated with metal oxide fixed by ethyl cellulose

    JP1989020267A

  • Surface treatment of azo lake pigment

    JP1991043462A

  • Nonelectroconductive carbonaceous powder and its production

    JP1996259838A

  • Surface modified carbon black

    JP1997272816A

  • Ink for ink-jet printing

    JP1999172170A