Protective sheet for semiconductor processing and method for manufacturing semiconductor device
The protective sheet for semiconductor processing addresses the challenges of uneven wafer grinding by using a high-modulus, energy-curable layer to embed and protect the wafer surface, reducing cracks and adhesive residue for improved chip yield.
Patent Information
- Application Number
- JP2020060552
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Conventional backgrind tapes fail to adequately follow the unevenness of semiconductor wafers during grinding, leading to issues such as water intrusion, chip shifting, and adhesive residue on convex electrodes, which compromises the integrity and yield of semiconductor chips.
A protective sheet for semiconductor processing comprising a base material with an energy ray-curable intermediate and adhesive layer, having a Young's modulus of 600 MPa or more before curing, and optionally including a buffer layer, which can embed and protect the uneven wafer surface during grinding and peeling.
The protective sheet effectively follows the unevenness of semiconductor wafers, reduces cracks and chip shifting, and minimizes adhesive residue, ensuring high yield and integrity of semiconductor chips.
Smart Images

Figure 0007566480000003 
Figure 0007566480000004 
Figure 0007566480000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a protective sheet for semiconductor processing and a method for manufacturing a semiconductor device. In particular, the present invention relates to a protective sheet for semiconductor processing suitable for use in a method for grinding the back surface of a semiconductor wafer having unevenness and dividing the semiconductor wafer into individual pieces by using the resulting stress, and a method for manufacturing a semiconductor device using the protective sheet for semiconductor processing. [Background technology]
[0002] As various electronic devices become smaller and more multifunctional, the semiconductor chips mounted on them are also required to be smaller and thinner. In order to thin the chips, it is common to grind the backside of the semiconductor wafer to adjust the thickness. In order to obtain thin chips, a method called dicing before grinding (DBG) is sometimes used, in which grooves of a specified depth are formed on the front side of the wafer with a dicing blade, and then the wafer is ground from the backside, and the wafer is divided into individual pieces by grinding to obtain chips. With DBG, the backside grinding and wafer division can be performed simultaneously, so thin chips can be manufactured efficiently.
[0003] Conventionally, when grinding the backside of a semiconductor wafer or manufacturing chips using DBG, it is common to apply an adhesive tape called a backgrind sheet to the wafer surface to protect the circuits on the wafer surface and to hold the semiconductor wafer and semiconductor chips in place.
[0004] The backgrind sheet used in DBG is an adhesive tape having a substrate and an adhesive layer provided on one side of the substrate. As an example of such an adhesive tape, Patent Documents 1 and 2 disclose an adhesive tape having a substrate with a high Young's modulus, a buffer layer provided on one side of the substrate, and an adhesive layer provided on the other side.
[0005] In recent years, a method has been proposed as a variation of the dicing-before method, in which a modified region is provided inside the wafer by a laser, and the wafer is divided into individual pieces by stress during grinding the back surface of the wafer. Hereinafter, this method may be referred to as LDBG (Laser Dicing Before Grinding). In LDBG, the wafer is cut in the crystal direction starting from the modified region, so that the occurrence of chipping can be reduced more than in the dicing-before method using a dicing blade. As a result, chips with excellent bending strength can be obtained, and the chips can be further thinned. In addition, compared to DBG, in which a groove of a predetermined depth is formed on the wafer surface by a dicing blade, there is no region where the wafer is scraped off by the dicing blade, that is, the kerf width is extremely small, so that the chip yield is excellent.
[0006] On the other hand, when mounting a multi-pin LSI package used in an MPU, gate array, etc., on a printed wiring board, a flip-chip mounting method has been adopted in which a semiconductor chip with convex electrodes (bumps) made of eutectic solder, high-temperature solder, gold, etc. formed on its connection pads is used, and these bumps are brought face-to-face and into contact with corresponding terminal parts on a chip-mounting substrate by the so-called face-down method, and melt / diffusion bonding is performed. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2015 / 156389 [Patent Document 2] JP 2015-183008 A Summary of the Invention [Problem to be solved by the invention]
[0008] The semiconductor chips used in this mounting method are obtained by dividing a semiconductor wafer having irregularities, such as a semiconductor wafer having a convex electrode formed thereon. Even when grinding such a semiconductor wafer having irregularities by DBG, as described above, a backgrind tape is attached to the circuit surface of the semiconductor wafer in order to protect the circuit surface during grinding and to prevent the chips from moving after the wafer is divided.
[0009] However, when the backgrind tapes described in Patent Documents 1 and 2 are applied to the circuit surface of a semiconductor wafer having irregularities and ground by DBG, the backgrind tapes described in Patent Documents 1 and 2 cannot adequately conform to the irregularities of the semiconductor wafer, and there are problems such as water infiltration into the circuit surface during grinding and chip movement (chip shift) after the wafer is diced. In addition, when a soft intermediate layer is provided in such a backgrind tape to accommodate the irregularities, although it can conform to the irregularities, there is a problem that glue remains on the convex electrodes when the backgrind tape is peeled off from the semiconductor wafer.
[0010] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a protective sheet for semiconductor processing that can adequately follow the unevenness of the wafer, even when a semiconductor wafer having unevenness due to DBG or the like is thinned, can suppress cracks in the chip after grinding, and suppresses adhesive residue when peeled off. [Means for solving the problem]
[0011] The aspects of the present invention are as follows. [1] A protective sheet for semiconductor processing having a substrate, an intermediate layer and a pressure-sensitive adhesive layer on one main surface of the substrate, in this order; the intermediate layer and the pressure-sensitive adhesive layer are energy ray curable, The protective sheet for semiconductor processing has a Young's modulus of 600 MPa or more before being cured with energy rays at 50°C.
[0012] [2] The protective sheet for semiconductor processing according to [1], further comprising a buffer layer on the other main surface of the substrate.
[0013] [3] The protective sheet for semiconductor processing according to [1] or [2], wherein the Young's modulus of the substrate is 1000 MPa or more.
[0014] [4] The protective sheet for semiconductor processing according to any one of [1] to [3], wherein the thickness of the intermediate layer is 60 μm or more and 250 μm or less.
[0015] [5] A protective sheet for semiconductor processing according to any one of [1] to [4], which is attached to the surface of a semiconductor wafer in a process of grinding the back surface of a semiconductor wafer having grooves formed on the surface of the semiconductor wafer to separate the semiconductor wafer into semiconductor chips by grinding.
[0016] [6] A step of attaching the semiconductor processing protective sheet according to any one of [1] to [5] to a surface of a semiconductor wafer having projections and recesses; A step of forming a groove from a front surface side of a semiconductor wafer, or a step of forming a modified region inside the semiconductor wafer from the front surface or rear surface of the semiconductor wafer; A step of grinding a semiconductor wafer having a semiconductor processing protection sheet attached to a surface thereof and having grooves or modified regions formed thereon from a back surface thereof into a plurality of chips starting from the grooves or modified regions; and peeling the protective sheet for semiconductor processing from the individual semiconductor chips. Effect of the Invention
[0017] According to the present invention, it is possible to provide a protective sheet for semiconductor processing which can adequately conform to the unevenness of the wafer, suppress cracks in the chip after grinding, and suppress glue residue when peeled off, even when a semiconductor wafer having unevenness due to DBG or the like is processed to be thin. [Brief description of the drawings]
[0018] [Figure 1A]FIG. 1A is a schematic cross-sectional view showing an example of a protective sheet for semiconductor processing according to this embodiment. [Figure 1B] FIG. 1B is a schematic cross-sectional view showing another example of the protective sheet for semiconductor processing according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a state in which the protective sheet for semiconductor processing according to this embodiment is attached to the circuit surface of a semiconductor wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.
[0020] Singulating a semiconductor wafer refers to dividing a semiconductor wafer into individual circuits to obtain semiconductor chips.
[0021] The "front surface" of a semiconductor wafer refers to the surface on which circuits, electrodes, etc. are formed, and the "back surface" refers to the surface on which circuits, etc. are not formed.
[0022] DBG is a method in which a groove of a specified depth is formed on the front side of a wafer, and then the wafer is ground from the back side to separate the wafer. The grooves formed on the front side of the wafer are formed by methods such as blade dicing, laser dicing, and plasma dicing.
[0023] LDBG is a modified version of DBG, in which a modified region is created inside the wafer using a laser, and the wafer is divided into individual pieces by the stress generated during back grinding of the wafer.
[0024] The term "chip group" refers to a plurality of semiconductor chips held on the protective sheet for semiconductor processing according to the present embodiment after the semiconductor wafer is diced. These semiconductor chips as a whole have the same shape as the semiconductor wafer.
[0025] In this specification, for example, "(meth)acrylate" is used as a term indicating both "acrylate" and "methacrylate," and the same applies to other similar terms.
[0026] The term "energy rays" refers to ultraviolet rays, electron beams, etc., and is preferably ultraviolet rays.
[0027] (1. Protective sheet for semiconductor processing) The protective sheet for semiconductor processing 1 according to this embodiment has a configuration in which an intermediate layer 20 and a pressure-sensitive adhesive layer 30 are laminated in this order on a substrate 10, as shown in FIG. 1A.
[0028] The protective sheet for semiconductor processing according to this embodiment is used by being attached to a semiconductor wafer having projections and recesses. An example of the semiconductor wafer having projections and recesses is a semiconductor wafer having a protruding electrode formed thereon.
[0029] 2, the protective sheet for semiconductor processing 1 according to this embodiment is used by attaching the main surface 30a of the adhesive layer 30 to a bump-formed surface 101a of a bumped semiconductor wafer having bumps 102 formed as convex electrodes on a semiconductor wafer 101. The bumps are formed so as to be electrically connected to circuits formed on the semiconductor wafer, so the bump-formed surface 101a is a circuit surface.
[0030] In this embodiment, the semiconductor wafer with bumps is divided into individual semiconductor chips by DBG or LDBG. That is, before or after the attachment of the protective sheet for semiconductor processing, after a groove is formed on the front surface (circuit surface) or after a modified region is formed inside the semiconductor wafer, the back surface of the semiconductor wafer with the protective sheet for semiconductor processing attached to the circuit surface is ground.
[0031] When unevenness such as convex electrodes is formed on a semiconductor wafer, the size of the unevenness relative to the thickness of the semiconductor wafer becomes larger when the thickness of the semiconductor wafer is reduced by grinding. Therefore, if the unevenness is not properly embedded in the protective sheet for semiconductor processing, the following problems become more apparent when DBG or LDBG is performed. That is, problems such as water infiltrating into the circuit surface of the semiconductor wafer during back grinding, and chips that are divided after grinding move and collide with each other, causing cracks in the chips, become apparent. Furthermore, when the protective sheet for semiconductor processing is peeled off after grinding, the problem that the protective sheet for semiconductor processing is peeled off while partly adhering to the multiple semiconductor chips that are the adherends (residual adhesive is generated) also becomes apparent.
[0032] In this embodiment, the physical properties of the protective sheet for semiconductor processing are controlled as follows.
[0033] (1.1 Young's modulus of the semiconductor processing protection sheet before energy ray curing at 50°C) In this embodiment, the Young's modulus of the semiconductor processing protective sheet at 50° C. is 600 MPa or more. Since the Young's modulus is within the above range, the individual chips can be sufficiently held even after the wafer is divided into individual chips. As a result, the individual chips are prevented from moving and colliding with each other, causing cracks in the chips.
[0034] As described later, since the adhesive layer and intermediate layer, which are components of the semiconductor processing protection sheet according to this embodiment, are energy ray curable, the above Young's modulus is the Young's modulus before energy ray curing. Chip cracks occur before the adhesive layer and intermediate layer are cured with energy rays.
[0035] The Young's modulus of the protective sheet for semiconductor processing at 50° C. before energy ray curing is preferably 610 MPa or more, and more preferably 620 MPa or more.
[0036] The upper limit of the Young's modulus is not particularly specified, but from the viewpoint of adhesiveness of the protective sheet for semiconductor processing, it is, for example, 3000 MPa.
[0037] In this embodiment, the Young's modulus of the protective sheet for semiconductor processing before energy ray curing at 50° C. is measured by a tensile test. Specifically, a tensile test is performed in accordance with JIS K 7127 (1999), and the Young's modulus is calculated from the tensile load, tensile strain, etc.
[0038] The semiconductor processing protective sheet is not limited to the configuration shown in FIG. 1A, and may have other layers as long as the effect of the present invention can be obtained. That is, as long as the substrate, intermediate layer and adhesive layer are laminated in this order, for example, other layers may be formed between the substrate and intermediate layer, or other layers may be formed between the intermediate layer and adhesive layer. When the semiconductor processing protective sheet has other layers, the Young's modulus of the semiconductor processing protective sheet as a whole including the other layers may be within the above range.
[0039] In particular, in this embodiment, as shown in Fig. 1B, it is preferable that the substrate has a buffer layer 40 on the main surface 30b opposite to the main surface on which the pressure-sensitive adhesive layer is formed. By having the buffer layer 40, the occurrence of the above problems can be further suppressed.
[0040] In addition, since the buffer layer is relatively soft, it tends to reduce the Young's modulus of the semiconductor processing protection sheet. Therefore, when the semiconductor processing protection sheet has a buffer layer, it is necessary to adjust the Young's modulus of the semiconductor processing protection sheet to be within the above range.
[0041] The components of the protective sheet for semiconductor processing 1 shown in FIG. 1B will be described in detail below.
[0042] (2. Base material) The substrate is not limited as long as it is made of a material capable of supporting a semiconductor wafer. For example, various resin films used as substrates for backgrinding tapes are exemplified. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film made of a plurality of resin films laminated together.
[0043] (2.1 Physical properties of the substrate) In this embodiment, the substrate preferably has high rigidity. The high rigidity of the substrate makes it easy to set the Young's modulus of the semiconductor processing protective sheet within the above range. Even if the thickness of the semiconductor wafer is reduced by grinding, the wafer can be held without being damaged. Specifically, the Young's modulus of the substrate is preferably 1000 MPa or more, more preferably 1500 MPa or more, and even more preferably 2000 MPa or more.
[0044] In this embodiment, the thickness of the substrate is preferably 15 μm or more and 200 μm or less, and more preferably 40 μm or more and 150 μm or less.
[0045] (2.2 Substrate material) The material of the substrate is preferably a material having a Young's modulus within the above range. In this embodiment, examples of the material include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyester such as fully aromatic polyester, polyamide, polycarbonate, polyacetal, modified polyphenylene oxide, polyphenylene sulfide, polysulfone, polyether ketone, biaxially oriented polypropylene, etc. Among these, polyester is preferable, and polyethylene terephthalate is more preferable.
[0046] (3. Middle Class) The intermediate layer is a layer disposed between the substrate and the adhesive layer. In this embodiment, the intermediate layer is energy ray curable. Therefore, since the viscoelasticity of the intermediate layer is low before energy ray curing, the intermediate layer, together with the adhesive layer, can sufficiently follow the unevenness formed on the surface of the semiconductor wafer, and the unevenness can be embedded in the adhesive layer and the intermediate layer. As a result, even if the semiconductor wafer is ground very thin and a force is applied to the convex electrode, the adhesive layer and the intermediate layer can sufficiently protect the convex electrode.
[0047] On the other hand, after the energy ray curing, not only the adhesive layer but also the intermediate layer undergoes curing and shrinkage. Therefore, even if the protective sheet for semiconductor processing is peeled off from the semiconductor wafer or the semiconductor chip after singulation, the elastic modulus of the intermediate layer increases, so that the elastic modulus of the entire protective sheet for semiconductor processing also improves, and the adhesive layer is less likely to remain attached to the semiconductor wafer or the semiconductor chip after singulation (residual adhesive residue is suppressed).
[0048] Moreover, if the convex electrode etc. penetrates through the adhesive layer, the intermediate layer buries and protects the convex electrode etc. The intermediate layer may be composed of one layer (single layer) or may be composed of two or more layers.
[0049] The thickness of the intermediate layer 20 may be set in consideration of the size of the unevenness of the semiconductor wafer, for example, the height of the convex electrodes. In this embodiment, the thickness of the intermediate layer 20 is preferably 60 μm or more and 250 μm or less, and more preferably 100 μm or more and 200 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of an intermediate layer composed of multiple layers means the total thickness of all layers that make up the intermediate layer.
[0050] (3.1 Composition for intermediate layer) Since the intermediate layer is energy ray curable as described above, it is preferable that the intermediate layer is formed from a composition having energy ray curability (composition for intermediate layer). In this embodiment, the composition for intermediate layer preferably contains an acrylic polymer (A) having a weight average molecular weight of 300,000 to 1,500,000 and an energy ray curable acrylic polymer (B) having a weight average molecular weight of 50,000 to 250,000. The acrylic polymer (A) is non-energy ray curable or energy ray curable, but in this embodiment, it is preferable that the acrylic polymer (A) is non-energy ray curable.
[0051] In this specification, unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method can be performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.
[0052] (3.1.1 Acrylic polymer (A)) As described above, the acrylic polymer (A) may be energy ray curable or non-energy ray curable. In this embodiment, the case where the acrylic polymer (A) is non-energy ray curable will be described. (The acrylic polymer (A) is preferably a non-energy ray curable polymer having a structural unit derived from a (meth)acrylate. Specifically, the acrylic polymer (A) is more preferably an acrylic copolymer having a structural unit derived from an alkyl (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer (a2).
[0053] As the alkyl(meth)acrylate (a1), an alkyl(meth)acrylate having an alkyl group with a carbon number of 1 to 18 is used. Specific examples include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isooctyl(meth)acrylate, n-decyl(meth)acrylate, n-dodecyl(meth)acrylate, n-tridecyl(meth)acrylate, myristyl(meth)acrylate, palmityl(meth)acrylate, and stearyl(meth)acrylate.
[0054] Among these, the alkyl (meth)acrylate (a1) is preferably an alkyl (meth)acrylate having an alkyl group with a carbon number of 4 to 8. Specifically, n-butyl (meth)acrylate is preferable. The alkyl (meth)acrylate (a1) may be used alone or in combination of two or more kinds.
[0055] The content of the structural units derived from the alkyl (meth)acrylate (a1) in the acrylic polymer (A) is preferably 50 to 99.5 mass%, more preferably 60 to 99 mass%, and even more preferably 80 to 95 mass%, relative to all structural units (100 mass%) of the acrylic polymer (A).
[0056] If the content is 50% by mass or more, the holding performance of the pressure-sensitive adhesive sheet is improved, and the ability to conform to an adherend having large projections and recesses is easily improved. If the content is 99.5% by mass or less, a certain amount or more of the structural unit derived from the (a2) component can be secured.
[0057] The functional group-containing monomer (a2) is a monomer having a functional group such as a hydroxy group, a carboxy group, an epoxy group, an amino group, a cyano group, a nitrogen atom-containing cyclic group, an alkoxysilyl group, etc. Among the above, the functional group-containing monomer (a2) is preferably at least one selected from the group consisting of a hydroxy group-containing monomer, a carboxy group-containing monomer, and an epoxy group-containing monomer.
[0058] Examples of hydroxy group-containing monomers include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.
[0059] Examples of the carboxy group-containing monomer include (meth)acrylic acid, maleic acid, fumaric acid, and itaconic acid.
[0060] The epoxy-containing monomer includes an epoxy group-containing (meth)acrylic acid ester and a non-acrylic epoxy group-containing monomer. The epoxy group-containing (meth)acrylic acid ester includes, for example, glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, (3,4-epoxycyclohexyl)methyl (meth)acrylate, 3-epoxycyclo-2-hydroxypropyl (meth)acrylate, etc. The non-acrylic epoxy group-containing monomer includes, for example, glycidyl crotonate, allyl glycidyl ether, etc.
[0061] The functional group-containing monomer (a2) may be used alone or in combination of two or more kinds.
[0062] Among the functional group-containing monomers (a2), carboxyl group-containing monomers are more preferred, among which (meth)acrylic acid is even more preferred, and acrylic acid is the most preferred. When a carboxyl group-containing monomer is used as the functional group-containing monomer (a2), the cohesive strength of the intermediate layer is increased, and the retention performance of the intermediate layer is further improved.
[0063] The content of the structural units derived from the functional group-containing monomer (a2) in the acrylic polymer (A) is preferably 0.5 to 40 mass%, more preferably 3 to 20 mass%, and even more preferably 5 to 15 mass%, based on the total structural units (100 mass%) of the acrylic polymer (A).
[0064] If the content of the structural units derived from the (a2) component is 0.5% by mass or more, the cohesive strength of the intermediate layer is high and compatibility with the (B) component is easily improved. On the other hand, if the content is 40% by mass or less, a certain amount or more of the structural units derived from the (a1) component can be secured.
[0065] The acrylic polymer (A) may be a copolymer of an alkyl (meth)acrylate (a1) and a functional group-containing monomer (a2), or may be a copolymer of the (a1) component, the (a2) component, and a monomer (a3) other than the (a1) and (a2) components.
[0066] Examples of the other monomers (a3) include (meth)acrylates having a cyclic structure such as cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxyethyl (meth)acrylate, as well as vinyl acetate and styrene. The other monomers (a3) may be used alone or in combination of two or more.
[0067] The content of the structural units derived from the other monomer (a3) in the acrylic polymer (A) is preferably 0 to 20 mass%, more preferably 0 to 10 mass%, and even more preferably 0 to 5 mass%, relative to all structural units (100 mass%) of the acrylic polymer (A).
[0068] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 300,000 to 1,500,000, more preferably 400,000 to 1,100,000, and even more preferably 450,000 to 900,000. By setting Mw to the upper limit or less, the acrylic polymer (A) has good compatibility with the acrylic polymer (B). In addition, by setting Mw within the above range, the retention performance of the pressure-sensitive adhesive sheet is easily improved.
[0069] The content of the acrylic polymer (A) in the intermediate layer composition is preferably 40 to 95 mass%, more preferably 45 to 92 mass%, and even more preferably 60 to 90 mass% or more, relative to the total amount (100 mass%) of the intermediate layer composition.
[0070] In addition, when the intermediate layer composition is diluted with a diluent such as an organic solvent as described below, the total amount of the intermediate layer composition means the total amount of solids excluding the diluent. The same applies to the pressure-sensitive adhesive layer composition described below.
[0071] (3.1.2 Acrylic polymer (B)) The acrylic polymer (B) is an acrylic polymer having energy ray curability due to the introduction of an energy ray polymerizable group. The acrylic polymer (B) has a weight average molecular weight (Mw) of 50,000 to 250,000. In the present invention, by using the (B) component in the intermediate layer, the convex electrode is sufficiently embedded during grinding of the back surface of the semiconductor wafer before energy ray curing, and by curing with energy ray after grinding, cohesive failure of the intermediate layer is prevented and good peeling from the semiconductor chip is facilitated.
[0072] The weight average molecular weight (Mw) of the acrylic polymer (B) is preferably from 60,000 to 220,000, more preferably from 70,000 to 200,000, and further preferably from 85,000 to 150,000.
[0073] The acrylic polymer (B) is an acrylic polymer having an energy ray polymerizable group introduced therein and a structural unit derived from (meth)acrylate. The energy ray polymerizable group of the acrylic polymer (B) is preferably introduced into a side chain of the acrylic polymer. The energy ray polymerizable group may be any group containing an energy ray polymerizable carbon-carbon double bond, and examples of the energy ray polymerizable group include a (meth)acryloyl group and a vinyl group, among which a (meth)acryloyl group is preferred.
[0074] The acrylic polymer (B) is preferably a reaction product obtained by reacting an acrylic copolymer (B0) having a structural unit derived from an alkyl (meth)acrylate (b1) and a structural unit derived from a functional group-containing monomer (b2) with a polymerizable compound (Xb) having an energy ray-polymerizable group.
[0075] As the alkyl(meth)acrylate (b1), an alkyl(meth)acrylate having an alkyl group with 1 to 18 carbon atoms is used, and specific examples thereof include those exemplified as the component (a1). Among these, the alkyl(meth)acrylate (b1) is preferably an alkyl(meth)acrylate having an alkyl group with 4 to 8 carbon atoms. Specifically, n-butyl(meth)acrylate is preferred. These may be used alone or in combination of two or more.
[0076] The content of the structural unit derived from the alkyl (meth)acrylate (b1) in the acrylic copolymer (B0) is preferably 50 to 95% by mass, more preferably 60 to 85% by mass, and even more preferably 65 to 80% by mass, based on the total structural units (100% by mass) of the acrylic copolymer (B0). If this content is 50% by mass or more, the shape of the intermediate layer formed can be sufficiently maintained. Also, if it is 95% by mass or less, a certain amount of structural units derived from the (b2) component, which become reaction sites with the polymerizable compound (Xb), can be secured.
[0077] The functional group-containing monomer (b2) may be any of the monomers having functional groups exemplified in the functional group-containing monomer (a2) described above, and is preferably at least one selected from the group consisting of hydroxyl group-containing monomers, carboxyl group-containing monomers, and epoxy group-containing monomers. Specific examples of these compounds include the same compounds exemplified as the component (a2).
[0078] As the functional group-containing monomer (b2), a hydroxy group-containing monomer is preferred, and among them, various hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate are more preferred. By using the hydroxyalkyl (meth)acrylate, it becomes possible to react the acrylic copolymer (B0) with the polymerizable compound (Xb) relatively easily.
[0079] In addition, the functional groups in the functional group-containing monomer (a2) used in the acrylic polymer (A) and the functional group-containing monomer (b2) used in the acrylic polymer (B) may be the same or different, but are preferably different. That is, for example, if the functional group-containing monomer (a2) is a carboxyl group-containing monomer, the functional group-containing monomer (b2) is preferably a hydroxyl group-containing monomer. In this way, when the functional groups are different from each other, for example, the acrylic polymer (B) can be preferentially crosslinked by a crosslinking agent described later, and the above-mentioned retention performance of the pressure-sensitive adhesive sheet can be improved.
[0080] The content of the structural unit derived from the functional group-containing monomer (b2) in the acrylic copolymer (B0) is preferably 10 to 45% by mass, more preferably 15 to 40% by mass, and even more preferably 20 to 35% by mass, based on the total structural units (100% by mass) of the acrylic copolymer (B0). If it is 10% by mass or more, a relatively large number of reaction sites with the polymerizable compound (Xb) can be secured, and it is easy to introduce energetic polymerizability into the side chain. Also, if it is 45% by mass or less, the shape of the intermediate layer formed can be sufficiently maintained.
[0081] The acrylic copolymer (B0) may be a copolymer of an alkyl (meth)acrylate (b1) and a functional group-containing monomer (b2), or may be a copolymer of a (b1) component, a (b2) component, and a monomer (b3) other than the (b1) and (b2) components.
[0082] Examples of the other monomer (b3) include those exemplified above as the monomer (a3).
[0083] The content of the structural units derived from the other monomer (b3) in the acrylic copolymer (B0) is preferably 0 to 30 mass%, more preferably 0 to 10 mass%, and even more preferably 0 to 5 mass%, relative to all structural units (100 mass%) of the acrylic copolymer (B0).
[0084] The polymerizable compound (Xb) is a compound having an energy ray-polymerizable group and a substituent (hereinafter, also simply referred to as a "reactive substituent") capable of reacting with a functional group in a structural unit derived from the component (b2) of the acrylic copolymer (B0).
[0085] As described above, examples of the energy ray polymerizable group include a (meth)acryloyl group and a vinyl group, and a (meth)acryloyl group is preferred. The polymerizable compound (Xb) is preferably a compound having 1 to 5 energy ray polymerizable groups per molecule.
[0086] The reactive substituent in the polymerizable compound (Xb) may be appropriately changed depending on the functional group possessed by the functional group-containing monomer (b2), and may be, for example, an isocyanate group, a carboxyl group, an epoxy group, etc., with the isocyanate group being preferred from the viewpoint of reactivity, etc. When the polymerizable compound (Xb) has an isocyanate group, for example, when the functional group of the functional group-containing monomer (b2) is a hydroxyl group, it becomes possible for the polymerizable compound (Xb) to easily react with the acrylic copolymer (B0).
[0087] Specific examples of the polymerizable compound (Xb) include (meth)acryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, (meth)acryloyl isocyanate, allyl isocyanate, glycidyl (meth)acrylate, (meth)acrylic acid, etc. These polymerizable compounds (Xb) may be used alone or in combination of two or more kinds.
[0088] Among these, (meth)acryloyloxyethyl isocyanate is preferred from the viewpoint of having a suitable isocyanate group as the reactive substituent and being a compound in which the distance between the main chain and the energy ray-polymerizable group is appropriate.
[0089] The polymerizable compound (Xb) reacts with the functional groups in an amount of preferably 40 to 98 equivalents, more preferably 60 to 90 equivalents, and even more preferably 70 to 85 equivalents, of the total amount (100 equivalents) of functional groups derived from the functional group-containing monomer (b2) in the acrylic polymer (B).
[0090] In the intermediate layer composition, the content of the acrylic polymer (B) is preferably 5 to 60 parts by mass, and more preferably 10 to 35 parts by mass, per 100 parts by mass of the acrylic polymer (A). By making the content of the (B) component relatively small in this manner, the intermediate layer can easily conform to the irregularities of the semiconductor wafer.
[0091] 3.1.3 Crosslinking Agents The intermediate layer composition preferably further contains a crosslinking agent. Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, and metal chelate-based crosslinking agents, and among these, isocyanate-based crosslinking agents are preferred. When an isocyanate-based crosslinking agent is used, for example, when component (B) has a hydroxyl group, the crosslinking agent preferentially crosslinks the acrylic polymer (B).
[0092] The composition for the intermediate layer is crosslinked by the crosslinking agent, for example, by heating after application. The intermediate layer is formed by appropriately forming a coating film by crosslinking the acrylic polymer, particularly the low molecular weight acrylic polymer (B), etc., and the intermediate layer is easily able to function as an intermediate layer.
[0093] The content of the crosslinking agent is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and further preferably 1 to 5 parts by mass, based on 100 parts by mass of the acrylic polymer (A).
[0094] Examples of the isocyanate crosslinking agent include polyisocyanate compounds. Specific examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, and alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate. In addition, biuret and isocyanurate forms of these compounds, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil, are also included.
[0095] These may be used alone or in combination of two or more. Among the above, an adduct of an aromatic polyisocyanate such as tolylene diisocyanate with a polyhydric alcohol (for example, trimethylolpropane) is preferred.
[0096] Examples of epoxy crosslinking agents include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, etc. These may be used alone or in combination of two or more.
[0097] Examples of metal chelate crosslinking agents include compounds in which acetylacetone, ethyl acetoacetate, tris(2,4-pentanedionate), etc. are coordinated to polyvalent metals such as aluminum, iron, copper, zinc, tin, titanium, nickel, antimony, magnesium, vanadium, chromium, zirconium, etc. These may be used alone or in combination of two or more.
[0098] Examples of the aziridine crosslinking agent include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, trimethylolpropane tri-β-(2-methylaziridine)propionate, and hexa[1-(2-methyl)-aziridinyl]triphosphatriazine.
[0099] (3.1.4 Photoinitiators) The intermediate layer composition preferably further contains a photopolymerization initiator. By containing the photopolymerization initiator, the intermediate layer composition is easily cured by energy rays such as ultraviolet rays.
[0100] Examples of the photopolymerization initiator include acetophenone, 2,2-diethoxybenzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, Michler's ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzyl diphenylsulfide, tetramethylthiuram monosulfide, benzyl dimethyl ketal, dibenzyl, diacetyl, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-ethylanthraquinone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropanone-1,2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-hydroxy-2-methyl-1-phenyl-propan-1-one, diethylthioxanthone, isopropylthioxanthone, low molecular weight polymerization initiators such as 2,4,6-trimethylbenzoyldiphenyl-phosphine oxide, oligomerized polymerization initiators such as oligo{2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone}, etc. These may be used alone or in combination of two or more. Among these, 1-hydroxycyclohexyl phenyl ketone is preferred.
[0101] The content of the photopolymerization initiator is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, per 100 parts by mass of the acrylic polymer (A), so that curing can proceed sufficiently even with a small content of the acrylic polymer (B).
[0102] The intermediate layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, tackifiers, etc. When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.01 to 2 parts by mass, based on 100 parts by mass of the acrylic polymer (A).
[0103] In addition, the Young's modulus of the semiconductor processing protection sheet can be adjusted by, for example, the type and amount of the monomer constituting the acrylic polymer (B), the amount of the energy ray polymerizable group introduced into the acrylic polymer (B), etc., when an acrylic polymer (B) is used. For example, the Young's modulus tends to increase when the amount of the energy ray polymerizable group is increased. Furthermore, it can be appropriately adjusted by the amount of the crosslinking agent and the amount of the photopolymerization initiator blended in the intermediate layer, etc.
[0104] (4. Adhesive Layer) The adhesive layer is attached to the circuit surface of the semiconductor wafer, and protects the circuit surface and supports the semiconductor wafer until it is peeled off from the circuit surface. In this embodiment, the adhesive layer is energy ray curable. Therefore, before energy ray curing, the adhesive layer and the intermediate layer can sufficiently follow the unevenness formed on the surface of the semiconductor wafer, and the unevenness can be embedded in the protective sheet for semiconductor processing. As a result, even if the semiconductor wafer is ground very thin and a force is applied to the convex electrode, the protective sheet for semiconductor processing can sufficiently protect the convex electrode, etc.
[0105] On the other hand, after the energy ray curing, the adhesive layer is cured and shrunk. Therefore, even when the protective sheet for semiconductor processing is peeled off from the semiconductor wafer or the semiconductor chip after division, the adhesive layer is unlikely to undergo cohesive failure, so that a part of the adhesive layer is unlikely to remain attached to the semiconductor wafer or the semiconductor chip after division (glue residue is suppressed).
[0106] The pressure-sensitive adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers.
[0107] The thickness of the adhesive layer is not particularly limited as long as it is thick enough to support a semiconductor wafer. In this embodiment, the thickness of the adhesive layer is preferably 5 μm or more and 500 μm or less, and more preferably 8 μm or more and 100 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.
[0108] (4.1 Composition for adhesive layer) Since the pressure-sensitive adhesive layer is energy ray curable as described above, it is preferable that the pressure-sensitive adhesive layer is formed from a composition having energy ray curability (composition for pressure-sensitive adhesive layer). In this embodiment, the composition for pressure-sensitive adhesive layer is preferably a composition having a resin.
[0109] The composition for the adhesive layer contains, as an adhesive component (adhesive resin) capable of imparting adhesiveness to the adhesive layer, for example, an acrylic polymer, a polyurethane, a rubber-based polymer, a polyolefin, a silicone, etc. Among these, an acrylic polymer is preferred.
[0110] The adhesive layer composition may have energy ray curability by blending an energy ray curable compound separately from the adhesive resin, but it is preferable that the above-mentioned adhesive resin itself has energy ray curability. When the adhesive resin itself has energy ray curability, an energy ray polymerizable group is introduced into the adhesive resin, and it is preferable that the energy ray polymerizable group is introduced into the main chain or side chain of the adhesive resin.
[0111] In addition, when an energy ray curable compound is blended separately from the adhesive resin, a monomer or oligomer having an energy ray polymerizable group is used as the energy ray curable compound. The oligomer is an oligomer having a weight average molecular weight (Mw) of less than 10,000, for example, urethane (meth)acrylate. In addition, even if the adhesive resin itself has energy ray curability, the composition for adhesive layer may be blended with an energy ray curable compound other than the adhesive resin.
[0112] Hereinafter, a more detailed description will be given of the case where the energy ray-curable adhesive resin contained in the composition for adhesive layer is an acrylic polymer (hereinafter, also referred to as "acrylic polymer (C)").
[0113] (4.1.1 Acrylic polymer (C)) The acrylic polymer (C) is an acrylic polymer having an energy ray polymerizable group introduced therein and a structural unit derived from a (meth)acrylate. The energy ray polymerizable group is preferably introduced into a side chain of the acrylic polymer.
[0114] The acrylic polymer (C) is preferably a reaction product obtained by reacting an acrylic copolymer (C0) having a structural unit derived from an alkyl (meth)acrylate (c1) and a structural unit derived from a functional group-containing monomer (c2) with a polymerizable compound (Xc) having an energy ray-polymerizable group.
[0115] As the alkyl(meth)acrylate (c1), an alkyl(meth)acrylate having an alkyl group with 1 to 18 carbon atoms is used, and specific examples thereof include those exemplified as the component (a1). Among these, the alkyl(meth)acrylate (c1) is preferably an alkyl(meth)acrylate having an alkyl group with 4 to 8 carbon atoms. Specifically, 2-ethylhexyl(meth)acrylate and n-butyl(meth)acrylate are preferred, and n-butyl(meth)acrylate is more preferred. These may be used alone or in combination of two or more.
[0116] From the viewpoint of improving the adhesive strength of the pressure-sensitive adhesive layer to be formed, the content of the structural units derived from the alkyl (meth)acrylate (c1) in the acrylic copolymer (C0) is preferably 50 to 99 mass%, more preferably 60 to 97 mass%, and even more preferably 70 to 96 mass%, relative to all structural units (100 mass%) of the acrylic copolymer (C0).
[0117] For example, the alkyl (meth)acrylate (c1) may contain ethyl (meth)acrylate methyl (meth)acrylate in addition to the above-mentioned 2-ethylhexyl (meth)acrylate and n-butyl (meth)acrylate. By containing these monomers, it becomes easier to adjust the adhesive performance of the adhesive layer to a desired one.
[0118] The functional group-containing monomer (c2) may be any of the monomers having functional groups exemplified as the functional group-containing monomer (a2) described above, and more specifically, it is preferably one or more selected from hydroxyl group-containing monomers, carboxyl group-containing monomers, and epoxy group-containing monomers. Specific examples of these compounds include the same compounds exemplified as the component (a2).
[0119] As the functional group-containing monomer (c2), among the above, a hydroxy group-containing monomer is more preferable, among which a hydroxyalkyl (meth)acrylate is more preferable, 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are further preferable, and 4-hydroxybutyl (meth)acrylate is particularly preferable.
[0120] By using hydroxyalkyl (meth)acrylate as component (c2), it becomes relatively easy to react the polymerizable compound (Xc) with the acrylic copolymer (C0). In addition, by using 4-hydroxybutyl (meth)acrylate, the tensile strength of the intermediate layer increases, making it easier to prevent adhesive residue.
[0121] The content of the structural units derived from the functional group-containing monomer (c2) in the acrylic copolymer (C0) is preferably 1 to 40 mass%, more preferably 2 to 35 mass%, even more preferably 3 to 30 mass%, and still more preferably 10 to 30 mass%, based on the total structural units (100 mass%) of the acrylic copolymer (C0).
[0122] If the content is 1% by mass or more, a certain amount of functional groups that become reaction sites with the polymerizable compound (Xc) can be secured. Therefore, the pressure-sensitive adhesive layer can be appropriately cured by irradiation with energy rays, so that the adhesive strength after irradiation with energy rays can be reduced. In addition, if the content is 40% by mass or less, a sufficient pot life can be secured when applying a solution of the pressure-sensitive adhesive layer composition to form a pressure-sensitive adhesive layer.
[0123] The acrylic copolymer (C0) may be a copolymer of an alkyl (meth)acrylate (c1) and a functional group-containing monomer (c2), or may be a copolymer of a (c1) component, a (c2) component, and a monomer (c3) other than the (c1) and (c2) components.
[0124] Examples of the other monomer (c3) include those exemplified above as the monomer (a3).
[0125] The content of the structural units derived from the other monomer (c3) in the acrylic copolymer (C0) is preferably 0 to 30 mass%, more preferably 0 to 10 mass%, and even more preferably 0 to 5 mass%, relative to all structural units (100 mass%) of the acrylic copolymer (C0).
[0126] The polymerizable compound (Xc), like the above-mentioned polymerizable compound (Xb), is a compound having an energy ray-polymerizable group and a substituent (reactive substituent) capable of reacting with a functional group in the structural unit derived from the component (c2) of the acrylic copolymer (C0), and is preferably a compound having 1 to 5 energy ray-polymerizable groups per molecule.
[0127] Specific examples of the reactive substituent and the energy ray polymerizable group are the same as those of the polymerizable compound (Xb), and therefore the reactive substituent is preferably an isocyanate group, and the energy ray polymerizable group is preferably a (meth)acryloyl group.
[0128] In addition, specific examples of the polymerizable compound (Xc) include the same as those exemplified as the above-mentioned polymerizable compound (Xb), and (meth)acryloyloxyethyl isocyanate is preferred. The polymerizable compound (Xc) may be used alone or in combination of two or more kinds.
[0129] The polymerizable compound (Xc) preferably reacts with the functional group in an amount of 30 to 98 equivalents, more preferably 40 to 95 equivalents, of the total amount (100 equivalents) of functional groups derived from the functional group-containing monomer (c2) in the acrylic copolymer (C0).
[0130] The weight average molecular weight (Mw) of the acrylic polymer (C) is preferably from 10,000 to 1,500,000, more preferably from 250,000 to 1,000,000, and even more preferably from 350,000 to 800,000. By having such an Mw, it is possible to impart appropriate adhesiveness to the pressure-sensitive adhesive layer.
[0131] Even if the adhesive resin has energy ray curability, the composition for adhesive layer preferably contains an energy ray curable compound other than the adhesive resin. As such an energy ray curable compound, a monomer or oligomer having an unsaturated group in the molecule and capable of being polymerized and cured by irradiation with energy rays is preferable.
[0132] Specific examples include polyvalent (meth)acrylate monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; and oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and epoxy (meth)acrylate.
[0133] Among these, urethane (meth)acrylate oligomers are preferred from the viewpoints of having a relatively high molecular weight and being less likely to reduce the elastic modulus of the pressure-sensitive adhesive layer.
[0134] 4.1.2 Crosslinking Agents The adhesive layer composition preferably further contains a crosslinking agent. The adhesive layer composition is crosslinked by the crosslinking agent, for example, by heating after application. The adhesive layer is formed by appropriately forming a coating film by crosslinking the acrylic polymer (C) with the crosslinking agent, and is easily able to function as an adhesive layer.
[0135] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, and chelate-based crosslinking agents, and among these, isocyanate-based crosslinking agents are preferred. The crosslinking agents may be used alone or in combination of two or more. Specific examples of the isocyanate-based crosslinking agent include those exemplified as crosslinking agents that can be used in the intermediate layer composition, and the preferred compounds thereof are also the same.
[0136] The content of the crosslinking agent is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 7 parts by mass, and further preferably 0.3 to 4 parts by mass, based on 100 parts by mass of the acrylic polymer (C).
[0137] (4.1.3 Photoinitiators) The adhesive layer composition preferably further contains a photopolymerization initiator. Examples of the photopolymerization initiator include those exemplified as the photopolymerization initiator used in the intermediate layer composition described above. The photopolymerization initiator may be used alone or in combination of two or more. Among the above, 2,2-dimethoxy-1,2-diphenylethan-1-one and 1-hydroxycyclohexyl phenyl ketone are preferred.
[0138] The content of the photopolymerization initiator is preferably 0.5 to 15 parts by mass, more preferably 1 to 12 parts by mass, and further preferably 4.5 to 10 parts by mass, based on 100 parts by mass of the acrylic polymer (C).
[0139] The pressure-sensitive adhesive layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include tackifiers, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are contained, the content of each additive is preferably 0.01 to 6 parts by mass, more preferably 0.02 to 2 parts by mass, based on 100 parts by mass of the acrylic polymer (C).
[0140] In addition, the Young's modulus of the semiconductor processing protection sheet can be adjusted by, for example, the type and amount of the monomer constituting the acrylic polymer (C), the amount of the energy ray polymerizable group introduced into the acrylic polymer (C), etc., when an acrylic polymer (C) is used. For example, the Young's modulus tends to increase when the amount of the energy ray polymerizable group is increased. Furthermore, it can be appropriately adjusted by the amount of the crosslinking agent and the amount of the photopolymerization initiator blended in the pressure-sensitive adhesive layer, etc.
[0141] (5.Buffer layer) As shown in FIG. 1B, the buffer layer is formed on the main surface of the substrate opposite to the main surface on which the adhesive layer is formed. The buffer layer 40 is a layer softer than the substrate, and relieves stress during back grinding of the semiconductor wafer, preventing cracks and chips from occurring in the semiconductor wafer. In addition, the semiconductor wafer to which the protective sheet for semiconductor processing is attached is placed on a vacuum table via the protective sheet for semiconductor processing during back grinding, and the presence of the buffer layer as a constituent layer of the protective sheet for semiconductor processing makes it easier to properly hold the semiconductor wafer on the vacuum table.
[0142] The thickness of the buffer layer is preferably 1 to 100 μm, more preferably 5 to 80 μm, and further preferably 10 to 60 μm. By setting the thickness of the buffer layer within the above range, the buffer layer can appropriately relieve stress during back grinding.
[0143] The buffer layer may be a layer formed from a buffer layer composition containing an energy ray-polymerizable compound, or may be a film such as a polypropylene film, an ethylene-vinyl acetate copolymer film, an ionomer resin film, an ethylene-(meth)acrylic acid copolymer film, an ethylene-(meth)acrylic acid ester copolymer film, an LDPE film, or an LLDPE film.
[0144] The substrate having a buffer layer can be obtained by laminating a buffer layer on one or both sides of the substrate.
[0145] (5.1 Composition for buffer layer) The buffer layer composition containing the energy ray-polymerizable compound can be cured by being irradiated with energy rays.
[0146] More specifically, the buffer layer composition containing the energy ray polymerizable compound preferably contains a urethane (meth)acrylate (d1) and a polymerizable compound (d3) having an alicyclic group or a heterocyclic group with 6 to 20 ring atoms. The buffer layer composition may contain a multifunctional polymerizable compound (d2) and / or a polymerizable compound (d4) having a functional group in addition to the above components (d1) and (d3). The buffer layer composition may contain a photopolymerization initiator in addition to the above components. Furthermore, the buffer layer composition may contain other additives and resin components within the range that does not impair the effects of the present invention.
[0147] Hereinafter, each component contained in the buffer layer composition containing the energy ray-polymerizable compound will be described in detail.
[0148] (5.1.1 Urethane (meth)acrylates (d1)) The urethane (meth)acrylate (d1) is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized and cured by irradiation with energy rays. The urethane (meth)acrylate (d1) is an oligomer or a polymer.
[0149] The weight average molecular weight (Mw) of component (d1) is preferably 1,000 to 100,000, more preferably 2,000 to 60,000, and even more preferably 3,000 to 20,000. The number of (meth)acryloyl groups in component (d1) (hereinafter also referred to as "functionality") may be monofunctional, bifunctional, or trifunctional or higher, but is preferably monofunctional or bifunctional.
[0150] Component (d1) can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting a (meth)acrylate having a hydroxyl group. Component (d1) may be used alone or in combination of two or more kinds.
[0151] The polyol compound used as the raw material of component (d1) is not particularly limited as long as it has two or more hydroxyl groups. It may be any of a difunctional diol, a trifunctional triol, and a polyol having four or more functional groups, but a difunctional diol is preferred, and a polyester type diol or a polycarbonate type diol is more preferred.
[0152] Examples of the polyisocyanate compound include aliphatic polyisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic diisocyanates such as isophorone diisocyanate, norbornane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and ω,ω'-diisocyanate dimethylcyclohexane; and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, tolidine diisocyanate, tetramethylene xylylene diisocyanate, and naphthalene-1,5-diisocyanate.
[0153] Among these, isophorone diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are preferred.
[0154] The above-mentioned polyol compound is reacted with a polyisocyanate compound to give a terminal isocyanate urethane prepolymer, and then a hydroxyl group-containing (meth)acrylate is reacted with the urethane (meth)acrylate (d1). The hydroxyl group-containing (meth)acrylate is not particularly limited as long as it is a compound having a hydroxyl group and a (meth)acryloyl group in at least one molecule.
[0155] Specific examples of (meth)acrylates having a hydroxy group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 5-hydroxycyclooctyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, pentaerythritol tri(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glycol mono(meth)acrylate; hydroxy group-containing (meth)acrylamides such as N-methylol (meth)acrylamide; and reaction products obtained by reacting a diglycidyl ester of vinyl alcohol, vinylphenol, or bisphenol A with (meth)acrylic acid; and the like.
[0156] Among these, hydroxyalkyl (meth)acrylate is preferred, and 2-hydroxyethyl (meth)acrylate is more preferred.
[0157] The conditions for reacting the isocyanate-terminated urethane prepolymer and the (meth)acrylate having a hydroxyl group are preferably such that the reaction is carried out at 60 to 100° C. for 1 to 4 hours in the presence of a solvent and a catalyst, which are added as necessary.
[0158] The content of component (d1) in the buffer layer composition is preferably 10 to 70 mass%, more preferably 20 to 60 mass%, and even more preferably 25 to 55 mass%, relative to the total amount (100 mass%) of the buffer layer composition.
[0159] (5.1.2 Polyfunctional polymerizable compound (d2)) The polyfunctional polymerizable compound refers to a compound having two or more photopolymerizable unsaturated groups. The photopolymerizable unsaturated group is a functional group containing a carbon-carbon double bond, such as a (meth)acryloyl group, a vinyl group, an allyl group, a vinylbenzyl group, etc. Two or more types of photopolymerizable unsaturated groups may be combined. A three-dimensional network structure (crosslinked structure) is formed by reacting a photopolymerizable unsaturated group in the polyfunctional polymerizable compound with a (meth)acryloyl group in component (d1) or by reacting photopolymerizable unsaturated groups in component (d2) with each other. When a polyfunctional polymerizable compound is used, the number of crosslinked structures formed by energy beam irradiation increases compared to when a compound containing only one photopolymerizable unsaturated group is used, so that the buffer layer exhibits unique viscoelasticity, making it easier to relieve stress during back grinding.
[0160] The definition of component (d2) overlaps with the definitions of components (d3) and (d4) described below, but the overlapping parts are included in component (d2). For example, a compound having an alicyclic group or heterocyclic group with 6 to 20 ring atoms and having two or more (meth)acryloyl groups is included in the definitions of both components (d2) and (d3), but in the present invention, the compound is included in component (d2). In addition, a compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group and having two or more (meth)acryloyl groups is included in the definitions of both components (d2) and (d4), but in the present invention, the compound is included in component (d2).
[0161] From the above viewpoints, the number of photopolymerizable unsaturated groups (number of functional groups) in the polyfunctional polymerizable compound is preferably 2 to 10, and more preferably 3 to 6.
[0162] The weight average molecular weight of the component (d2) is preferably 30-40,000, more preferably 100-10,000, and even more preferably 200-1,000.
[0163] Specific examples of component (d2) include diethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, divinylbenzene, vinyl (meth)acrylate, divinyl adipate, and N,N'-methylenebis(meth)acrylamide. Among these, dipentaerythritol hexa(meth)acrylate is preferred. Note that component (d2) may be used alone or in combination of two or more.
[0164] The content of component (d2) in the buffer layer composition is preferably 2 to 40 mass %, more preferably 3 to 20 mass %, and even more preferably 5 to 15 mass %, relative to the total amount (100 mass %) of the buffer layer composition.
[0165] (5.1.3 Polymerizable compound (d3) having an alicyclic group or heterocyclic group having 6 to 20 ring atoms) Component (d3) is a polymerizable compound having an alicyclic group or a heterocyclic group with 6 to 20 ring atoms, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group. By using component (d3), the film-forming property of the obtained buffer layer composition can be improved.
[0166] The definition of component (d3) overlaps with the definition of component (d4) described below, but the overlapping portion is included in component (d4). For example, a compound having at least one (meth)acryloyl group, an alicyclic group or heterocyclic group having 6 to 20 ring atoms, and a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group is included in the definitions of both component (d3) and component (d4), but in the present invention, the compound is included in component (d4).
[0167] Specific examples of the component (d3) include alicyclic group-containing (meth)acrylates such as isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, and adamantane (meth)acrylate; heterocyclic group-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate; etc. The component (d3) may be used alone or in combination of two or more kinds.
[0168] Of the alicyclic group-containing (meth)acrylates, isobornyl (meth)acrylate is preferred, and of the heterocyclic group-containing (meth)acrylates, tetrahydrofurfuryl (meth)acrylate is preferred.
[0169] The content of component (d3) in the buffer layer composition is preferably 10 to 70 mass %, more preferably 20 to 60 mass %, and even more preferably 25 to 55 mass %, relative to the total amount (100 mass %) of the buffer layer composition.
[0170] The content ratio of the component (d2) to the component (d3) in the buffer layer composition [(d2) / (d3)] is preferably 0.1 to 3.0, more preferably 0.15 to 2.0, and even more preferably 0.18 to 1.0.
[0171] (5.1.4 Polymerizable compound having a functional group (d4)) Component (d4) is a polymerizable compound containing a functional group such as a hydroxyl group, an epoxy group, an amide group, or an amino group, and is preferably a compound having at least one (meth)acryloyl group, more preferably a compound having one (meth)acryloyl group.
[0172] The component (d4) has good compatibility with the component (d1), and the viscosity of the buffer layer composition can be easily adjusted to an appropriate range. In addition, the buffer layer has good buffer performance even if it is relatively thin.
[0173] Examples of the component (d4) include hydroxyl group-containing (meth)acrylates, epoxy group-containing compounds, amide group-containing compounds, amino group-containing (meth)acrylates, etc. Among these, hydroxyl group-containing (meth)acrylates are preferred.
[0174] Examples of hydroxyl group-containing (meth)acrylates include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, phenylhydroxypropyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl acrylate. Among these, hydroxyl group-containing (meth)acrylates having an aromatic ring, such as phenylhydroxypropyl (meth)acrylate, are more preferred. The component (d4) may be used alone or in combination of two or more.
[0175] In order to improve the film-forming properties of the buffer layer composition, the content of component (d4) in the buffer layer composition is preferably 5 to 40 mass %, more preferably 7 to 35 mass %, and even more preferably 10 to 30 mass %, relative to the total amount (100 mass %) of the buffer layer composition.
[0176] The content ratio of the component (d3) to the component (d4) in the buffer layer composition [(d3) / (d4)] is preferably 0.5 to 3.0, more preferably 1.0 to 3.0, and even more preferably 1.3 to 3.0.
[0177] (5.1.5 Polymerizable compound (d5) other than components (d1) to (d4)) The composition for forming a buffer layer may contain a polymerizable compound (d5) other than the above components (d1) to (d4) within the range that does not impair the effects of the present invention.
[0178] Examples of the component (d5) include alkyl (meth)acrylates having an alkyl group having 1 to 20 carbon atoms, and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam. The component (d5) may be used alone or in combination of two or more kinds.
[0179] The content of component (d5) in the buffer layer composition is preferably 0 to 20 mass %, more preferably 0 to 10 mass %, further preferably 0 to 5 mass %, and particularly preferably 0 to 2 mass %.
[0180] 5.1.6 Photoinitiators It is preferable that the buffer layer composition further contains a photopolymerization initiator from the viewpoint of shortening the polymerization time by light irradiation and reducing the amount of light irradiation when forming the buffer layer.
[0181] Examples of the photopolymerization initiator include benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, peroxide compounds, and further photosensitizers such as amines and quinones. More specifically, examples of the photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl phenyl sulfide, tetramethylthiuram monosulfide, azobisisobutyrolnitrile, dibenzyl, diacetyl, 8-chloroanthraquinone, and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide. These photopolymerization initiators can be used alone or in combination of two or more.
[0182] The content of the photopolymerization initiator in the composition for the buffer layer is preferably 0.05 to 15 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.3 to 5 parts by mass, relative to 100 parts by mass of the total amount of the energy ray-polymerizable compounds.
[0183] 5.1.7 Other Additives The buffer layer composition may contain other additives within the range that does not impair the effects of the present invention. Examples of other additives include antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, pigments, dyes, etc. When these additives are blended, the content of each additive in the buffer layer composition is preferably 0.01 to 6 parts by mass, more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total amount of the energy ray polymerizable compounds.
[0184] The buffer layer formed from the composition for buffer layer containing the energy ray-polymerizable compound is obtained by polymerizing and curing the composition for buffer layer having the above-mentioned composition by irradiation with energy rays. In other words, the buffer layer is a product obtained by curing the composition for buffer layer.
[0185] Therefore, the buffer layer preferably contains polymerization units derived from component (d1) and polymerization units derived from component (d3). The buffer layer may also contain polymerization units derived from component (d2) and / or polymerization units derived from component (d4), or may contain polymerization units derived from component (d5). The content ratio of each polymerization unit in the buffer layer usually corresponds to the ratio (feed ratio) of each component constituting the buffer layer composition.
[0186] (6. Release Sheet) A release sheet may be attached to the surface of the semiconductor processing protective sheet. Specifically, the release sheet is attached to the surface of the adhesive layer of the semiconductor processing protective sheet. The release sheet is attached to the surface of the adhesive layer to protect the adhesive layer during transportation and storage. The release sheet is releasably attached to the semiconductor processing protective sheet, and is peeled off and removed from the semiconductor processing protective sheet before the semiconductor processing protective sheet is used (i.e., before the wafer is attached).
[0187] The release sheet used is a release sheet having at least one surface that has been subjected to a release treatment, and specifically includes a release sheet having a release agent applied onto the surface of a release sheet substrate.
[0188] The substrate for the release sheet is preferably a resin film, and examples of the resin constituting the resin film include polyester resin films such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin, polyolefin resins such as polypropylene resin and polyethylene resin, etc. Examples of the release agent include rubber-based elastomers such as silicone-based resins, olefin-based resins, isoprene-based resins, and butadiene-based resins, long-chain alkyl-based resins, alkyd-based resins, and fluorine-based resins.
[0189] The thickness of the release sheet is not particularly limited, but is preferably 10 to 200 μm, and more preferably 20 to 150 μm.
[0190] (7. Manufacturing method of protective sheet for semiconductor processing) The method for manufacturing the semiconductor processing protective sheet of this embodiment is not particularly limited as long as it is a method that can form an intermediate layer and an adhesive layer on one main surface of the substrate and a buffer layer on the other main surface of the substrate, and any known method may be used.
[0191] First, as a composition for forming an intermediate layer, for example, a composition for intermediate layer containing the above-mentioned components, or a composition obtained by diluting the composition for intermediate layer with a solvent or the like is prepared. Similarly, as a composition for adhesive layer for forming an adhesive layer, for example, a composition for adhesive layer containing the above-mentioned components, or a composition obtained by diluting the composition for adhesive layer with a solvent or the like is prepared. Similarly, as a composition for buffer layer for forming a buffer layer, for example, a composition for buffer layer containing the above-mentioned components, or a composition obtained by diluting the composition for adhesive layer with a solvent or the like is prepared.
[0192] Examples of the solvent include organic solvents such as methyl ethyl ketone, acetone, ethyl acetate, tetrahydrofuran, dioxane, cyclohexane, n-hexane, toluene, xylene, n-propanol, and isopropanol.
[0193] Then, the buffer layer composition is applied to the release-treated surface of the first release sheet by a known method such as spin coating, spray coating, bar coating, knife coating, roll coating, blade coating, die coating, or gravure coating to form a coating film, and the coating film is semi-cured to form a buffer layer film on the release sheet. The buffer layer film formed on the release sheet is attached to a substrate, and the buffer layer film is completely cured to form a buffer layer.
[0194] In the present embodiment, the coating film is preferably cured by irradiation with energy rays. The coating film may be cured in a single curing treatment or in multiple steps.
[0195] Next, the intermediate layer composition is applied to the release-treated surface of the second release sheet by a known method and dried by heating to form an intermediate layer on the second release sheet. After that, the intermediate layer on the second release sheet and the surface of the substrate on which the buffer layer is not formed are bonded together, and the second release sheet is removed.
[0196] Next, the adhesive layer composition is applied to the release-treated surface of the third release sheet by a known method, and then heated and dried to form an adhesive layer on the third release sheet.Then, the adhesive layer on the third release sheet and the intermediate layer are laminated together to obtain a semiconductor processing protection sheet in which the intermediate layer and the adhesive layer are formed in this order on one main surface of the substrate, and a buffer layer is formed on the other main surface of the substrate.The third release sheet can be removed when using the semiconductor processing protection sheet.
[0197] (8. Manufacturing method of semiconductor device) The protective sheet for semiconductor processing according to the present invention is preferably used in DBG when it is attached to the surface of a semiconductor wafer and the back grinding of the wafer is performed. In particular, the protective sheet for semiconductor processing according to the present invention is preferably used in LDBG, which obtains a group of chips with a small kerf width when the semiconductor wafer is divided into individual pieces.
[0198] As a non-limiting example of the use of the protective sheet for semiconductor processing, a method for manufacturing a semiconductor device will be described in more detail below.
[0199] Specifically, the method for manufacturing a semiconductor device includes at least the following steps 1 to 4. Step 1: A step of attaching the above-mentioned protective sheet for semiconductor processing to the surface of a semiconductor wafer having irregularities Step 2: A step of forming a groove from the front surface side of the semiconductor wafer, or forming a modified region inside the semiconductor wafer from the front surface or rear surface of the semiconductor wafer. Step 3: A step of grinding the semiconductor wafer having the semiconductor processing protective sheet attached to the front surface and the grooves or modified regions formed therein from the rear surface side to separate the semiconductor wafer into a plurality of chips starting from the grooves or modified regions. Step 4: A step of peeling off the protective sheet for semiconductor processing from the individual semiconductor wafers (i.e., a plurality of semiconductor chips)
[0200] Each step of the method for manufacturing the semiconductor device will now be described in detail.
[0201] (Process 1) In step 1, the semiconductor processing protective sheet according to the present embodiment is attached to the uneven semiconductor wafer surface via an adhesive layer. Since the semiconductor processing protective sheet according to the present embodiment has the above-mentioned characteristics, it can sufficiently conform to the unevenness and bury it to protect it.
[0202] This step may be performed before step 2 described below, or after step 2. For example, when forming a modified region in a semiconductor wafer, it is preferable to perform step 1 before step 2. On the other hand, when forming grooves on the semiconductor wafer surface by dicing or the like, step 1 is performed after step 2. That is, in this step 1, a protective sheet for semiconductor processing is attached to the surface of the wafer having the grooves formed in step 2 described below.
[0203] The semiconductor wafer used in the present manufacturing method may be a silicon wafer, or may be a wafer of gallium arsenide, silicon carbide, lithium tantalate, lithium niobate, gallium nitride, indium phosphide, or the like, or a glass wafer. The thickness of the semiconductor wafer before grinding is not particularly limited, but is usually about 500 to 1000 μm. In addition, the semiconductor wafer usually has a circuit formed on its surface. The formation of the circuit on the wafer surface can be performed by various methods including conventionally widely used methods such as an etching method and a lift-off method. In particular, in this embodiment, a convex electrode (bump) is formed on the circuit surface of the semiconductor wafer. As a result, the circuit surface of the semiconductor wafer has unevenness compared to a semiconductor wafer without the convex electrode. The height of the convex electrode is not particularly limited, but is usually 5 to 200 μm.
[0204] (Process 2) In step 2, a groove is formed from the front surface side of the semiconductor wafer, or a modified region is formed inside the semiconductor wafer from the front surface or rear surface of the semiconductor wafer.
[0205] The grooves formed in this step are shallower than the thickness of the semiconductor wafer. The grooves can be formed by dicing using a conventionally known wafer dicing device or the like. In step 3 described below, the semiconductor wafer is divided into a plurality of semiconductor chips along the grooves.
[0206] The modified region is an embrittled portion of the semiconductor wafer, and is a region that becomes the starting point for breaking the semiconductor wafer and dicing it into semiconductor chips due to the thinning of the semiconductor wafer caused by grinding in the grinding process or the application of grinding force. That is, the grooves and modified region in step 2 are formed so as to follow the dividing lines that will be formed when the semiconductor wafer is divided and diced into semiconductor chips in step 3 described below.
[0207] The modified region is formed by irradiating a laser focused on the inside of the semiconductor wafer, and the modified region is formed inside the semiconductor wafer. The laser may be irradiated from the front side or the back side of the semiconductor wafer. In the embodiment in which the modified region is formed, when the step 2 is performed after the step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated to the semiconductor wafer through the semiconductor processing protective sheet.
[0208] The semiconductor wafer to which the protective sheet for semiconductor processing is attached and on which the grooves or modified regions are formed is placed on the chuck table and adsorbed and held on the chuck table. At this time, the semiconductor wafer is adsorbed with the front side placed on the table side.
[0209] (Step 3) After steps 1 and 2, the back surface of the semiconductor wafer on the chuck table is ground to separate the semiconductor wafer into a plurality of semiconductor chips.
[0210] Here, when grooves are formed in the semiconductor wafer, the back grinding is performed so as to thin the semiconductor wafer at least to a position that reaches the bottom of the groove. By this back grinding, the grooves become cuts that penetrate the wafer, and the semiconductor wafer is divided by the cuts and singulated into individual semiconductor chips.
[0211] On the other hand, when a modified region is formed, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. That is, it is sufficient to grind to a position close to the modified region so that the semiconductor wafer is broken and divided into semiconductor chips starting from the modified region. For example, the actual division into semiconductor chips may be performed by attaching a pick-up tape described later and then stretching the pick-up tape.
[0212] After the back surface grinding is completed, dry polishing may be performed prior to picking up the chips.
[0213] The shape of the individual semiconductor chips may be square or elongated, such as rectangular. The thickness of the individual semiconductor chips is not particularly limited, but is preferably about 5 to 100 μm, and more preferably 10 to 45 μm. According to LDBG, which provides a modified region inside the wafer with a laser and divides the wafer into individual chips by stress during wafer back grinding, it is easy to make the thickness of the individual semiconductor chips 50 μm or less, and more preferably 10 to 45 μm. The size of the individual semiconductor chips is not particularly limited, but the chip size is preferably 600 mm or less. 2 Less than 400mm, more preferably 2 Less than 120mm, more preferably 2 is less than.
[0214] By using the semiconductor processing protective sheet of this embodiment, even in the case of a thin and / or small semiconductor chip like this, cracks are prevented from occurring in the semiconductor chip when the backside is ground (step 3) and when the semiconductor processing protective sheet is peeled off (step 4).
[0215] (Step 4) Next, the protective sheet for semiconductor processing is peeled off from the individual semiconductor wafer (i.e., a plurality of semiconductor chips). This step is carried out, for example, by the following method.
[0216] In this embodiment, the intermediate layer and the adhesive layer of the semiconductor processing protective sheet are formed from an energy ray curable adhesive, so that the intermediate layer and the adhesive layer are cured and shrunk by irradiating them with energy rays, thereby reducing the adhesive force to the adherend (diced semiconductor wafer). Next, a pick-up tape is attached to the back side of the diced semiconductor wafer, and the position and direction are adjusted so that the wafer can be picked up. At this time, a ring frame arranged on the outer periphery of the wafer is also attached to the pick-up tape, and the outer periphery of the pick-up tape is fixed to the ring frame. The wafer and the ring frame may be attached to the pick-up tape at the same time, or may be attached at different times. Next, the semiconductor processing protective sheet is peeled off from the multiple semiconductor chips held on the pick-up tape.
[0217] Since the protective sheet for semiconductor processing according to this embodiment has the above-mentioned characteristics, it can be peeled off smoothly without remaining attached to uneven surfaces, particularly to convex electrodes.
[0218] Thereafter, a plurality of semiconductor chips on the pickup tape are picked up and fixed onto a substrate or the like to manufacture a semiconductor device.
[0219] The pickup tape is not particularly limited, but may be composed of, for example, a substrate and an adhesive sheet having an adhesive layer provided on one surface of the substrate.
[0220] The above describes examples of the use of the protective sheet for semiconductor processing according to the present invention in a method for singulating semiconductor wafers by DBG or LDBG. However, the protective sheet for semiconductor processing according to the present invention can be preferably used for LDBG, which produces a group of chips with a smaller kerf width and thinner thickness when the semiconductor wafer is singulated.
[0221] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES
[0222] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.
[0223] The measurement and evaluation methods in the present examples are as follows.
[0224] (Young's modulus of protective sheet for semiconductor processing before energy ray curing at 50℃) The protective sheets for semiconductor processing produced in the Examples and Comparative Examples before energy ray curing were subjected to a tensile test at 50° C. at a test speed of 200 mm / min in accordance with JIS K 7127 (1999) to measure the Young's modulus.
[0225] (DBG chip crack evaluation) After forming grooves on the surface of a 12-inch diameter silicon wafer, the protective sheets for semiconductor processing made in the examples and comparative examples were attached to the surface of the wafer, and the wafer was divided by back grinding, and then divided into chips with a thickness of 50 μm and a chip size of 5 mm square by a first dicing method. After that, without peeling off the protective sheet for semiconductor processing, the corners of the chips divided from the ground surface of the wafer were observed with a digital microscope (product name "VHX-1000", manufactured by KEYENCE Corporation) to observe the presence or absence of cracks in each chip, and the crack occurrence rate in 700 chips was measured and evaluated according to the following evaluation criteria. A: Less than 1.0%, B: 1.0-2.0%, C: More than 2.0%
[0226] (LDBG chip crack evaluation) The semiconductor processing protection sheets prepared in the Examples and Comparative Examples were attached to a silicon wafer having a diameter of 12 inches and a thickness of 775 μm using a backgrind tape laminator (manufactured by Lintec Corporation, device name "RAD-3510F / 12"). A lattice-shaped modified region was formed on the wafer using a laser saw (manufactured by Disco Corporation, device name "DFL7361"). The lattice size was 5 mm x 5 mm.
[0227] Next, a back grinding machine (manufactured by Disco Corporation, machine name "DGP8761") was used to perform grinding (including dry polishing) until the thickness reached 50 μm, and the wafer was divided into a plurality of chips.
[0228] After the grinding process, the chips were irradiated with energy rays (ultraviolet rays), a dicing tape (Adwill D-176, manufactured by Lintec Corporation) was applied to the surface opposite to the surface to which the protective sheet for semiconductor processing was applied, and the protective sheet for semiconductor processing was then peeled off. The individual chips were then observed with a digital microscope (product name "VHX-1000", manufactured by KEYENCE Corporation), the number of chips with cracks was counted, and the crack occurrence rate for 700 chips was measured and evaluated according to the following criteria. A: Less than 1.0%, B: 1.0-2.0%, C: More than 2.0%
[0229] (Bump absorption evaluation) The protective sheets for semiconductor processing prepared in the following Examples and Comparative Examples were attached to a wafer (8-inch wafer, manufactured by Waltz Corporation) with spherical bumps made of Sn-3Ag-0.5Cu alloy with bump height of 80 μm, pitch of 200 μm, and diameter of 100 μm, using a laminator (product name "RAD-3510F / 12", manufactured by Lintec Corporation). During attachment, the temperature of the laminating table and laminating roll of the device was set to 50°C.
[0230] After lamination, the diameter of the circular voids generated around the bumps was measured from the substrate side using a digital optical microscope (product name "VHX-1000", manufactured by KEYENCE Corporation).
[0231] The smaller the diameter of the voids, the higher the bump absorption of the semiconductor processing protection sheet. The superiority or inferiority of the bump absorption was judged according to the following criteria. ◯: The void diameter is less than 150 μm. ×: The diameter of the void is 150 μm or more.
[0232] (Evaluation of adhesive residue on bumps) The protective sheets for semiconductor processing prepared in the following Examples and Comparative Examples were attached to a wafer (8-inch wafer, manufactured by Waltz Corporation) with spherical bumps made of Sn-3Ag-0.5Cu alloy with bump height of 80 μm, pitch of 200 μm, and diameter of 100 μm, using a laminator (product name "RAD-3510F / 12", manufactured by Lintec Corporation). During attachment, the temperature of the laminating table and laminating roll of the device was set to 50°C.
[0233] After lamination, UV was irradiated from the semiconductor processing protective sheet side at an irradiation speed of 15 mm / sec using a UV irradiation device (product name "RAD-2000m / 12", manufactured by Lintec Corporation). Next, the semiconductor processing protective sheet was peeled off from the evaluation wafer at a peeling speed of 4 mm / sec and a temperature of 40°C using a wafer mounter (product name "RAD-2700F / 12", manufactured by Lintec Corporation). Using an electron microscope (product name "VE-9800", manufactured by KEYENCE Corporation), the part where the bumps were embedded on the adhesive layer surface of the semiconductor processing protective sheet after peeling was observed from an observation angle of 45° to confirm whether the adhesive layer was broken or not.
[0234] The quality of adhesive residue was judged based on the following criteria. A: No broken areas (no glue residue). B: There are broken areas (glue residue).
[0235] Example 1 (1) Base material As a substrate, a PET film with adhesive layers on both sides (Cosmoshine A4300 manufactured by Toyobo Co., Ltd., thickness: 50 μm, Young's modulus at 23° C.: 2550 MPa) was prepared.
[0236] (2)Buffer layer (Synthesis of urethane acrylate oligomers) A urethane acrylate oligomer (UA-1) having a weight average molecular weight (Mw) of approximately 5,000 was obtained by reacting a terminal isocyanate urethane prepolymer obtained by reacting a polyester diol with isophorone diisocyanate with 2-hydroxyethyl acrylate.
[0237] (Preparation of Buffer Layer Composition) A buffer layer composition was prepared by blending 50 parts by weight of the urethane acrylate oligomer (UA-1) synthesized above, 40 parts by weight of isobornyl acrylate (IBXA), and 20 parts by weight of 2-hydroxy-3-phenoxypropyl acrylate (HPPA), and further blending 1.0 part by weight of 2-hydroxy-2-methyl-1-phenyl-propan-1-one (manufactured by BASF Japan, product name "Irgacure 1173") as a photopolymerization initiator.
[0238] (Creating a substrate with a buffer layer) The buffer layer composition was applied to the release-treated surface of another release sheet (manufactured by Lintec Corporation, product name "SP-PET381031") to form a coating film. Next, the coating film was irradiated with ultraviolet light to semi-cure the coating film and form a buffer layer-forming film with a thickness of 53 μm.
[0239] The above ultraviolet irradiation was performed using a belt conveyor type ultraviolet irradiation device (manufactured by I-Graphics, device name "US2-0801") and a high-pressure mercury lamp (manufactured by I-Graphics, device name "H08-L41") with a lamp height of 230 mm, output of 80 mW / cm, and illuminance of 90 mW / cm at a light wavelength of 365 nm. 2 , irradiation amount 50mJ / cm 2 The irradiation conditions were as follows:
[0240] The surface of the buffer layer-forming film thus formed was then bonded to a substrate, and the buffer layer-forming film was again irradiated with ultraviolet light from the release sheet side to completely harden the buffer layer-forming film, forming a buffer layer having a thickness of 53 μm. The ultraviolet light irradiation was performed using the above-mentioned ultraviolet light irradiation device and high-pressure mercury lamp, with a lamp height of 220 mm, a converted output of 120 mW / cm, and an illuminance of 160 mW / cm at a light wavelength of 365 nm. 2 , irradiation amount 650mJ / cm 2 The irradiation conditions were as follows:
[0241] (3) Base material with intermediate layer A non-energy ray curable acrylic copolymer (a) (Mw: 600,000) was obtained by copolymerizing 91 parts by mass of n-butyl acrylate (BA) and 9 parts by mass of acrylic acid (AA).
[0242] Separately from the acrylic copolymer (a), 62 parts by mass of n-butyl acrylate (BA), 10 parts by mass of methyl methacrylate (MMA), and 28 parts by mass of 2-hydroxyethyl acrylate (2HEA) were copolymerized to obtain an acrylic polymer, which was then reacted with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 80 equivalents of the hydroxyl groups out of the total hydroxyl groups (100 equivalents) of the acrylic polymer, to obtain an energy ray-curable acrylic copolymer (b) (Mw: 100,000).
[0243] To 100 parts by weight of this non-energy ray curable acrylic copolymer (a), 13 parts by weight of energy ray curable acrylic copolymer (b) was added, 2.79 parts by weight of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") was added as a crosslinking agent, and 3.71 parts by weight of 1-hydroxycyclohexyl phenyl ketone (manufactured by BASF, Irgacure 184) was added as a photoinitiator. The solids concentration was adjusted to 37% using toluene, and the mixture was stirred for 30 minutes to prepare a composition for the intermediate layer.
[0244] Next, the prepared solution of the intermediate layer composition was applied to a PET-based release film (SP-PET381031, thickness 38 μm, manufactured by Lintec Corporation) and dried to form an intermediate layer with a thickness of 55 μm. This was attached to the opposite side of the substrate with the buffer layer on which the buffer layer was formed, and the solution of the intermediate layer composition was further applied to the PET-based release film (SP-PET381031, thickness 38 μm, manufactured by Lintec Corporation) in a layered manner, and this was repeated three times in total to form a substrate with an intermediate layer with a thickness of 165 μm.
[0245] (4) Adhesive layer (Preparation of Composition for Pressure-Sensitive Adhesive Layer) An energy ray-curable acrylic copolymer (c) (Mw: 500,000) was obtained by reacting an acrylic polymer obtained by copolymerizing 52 parts by mass of n-butyl acrylate (BA), 20 parts by mass of methyl methacrylate (MMA), and 28 parts by mass of 2-hydroxyethyl acrylate (2HEA) with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 90 equivalents of the hydroxyl groups of the total hydroxyl groups (100 equivalents) of the acrylic polymer.
[0246] 100 parts by mass of this energy ray curable acrylic copolymer (c) was mixed with 12 parts by mass of a multifunctional urethane acrylate (manufactured by Mitsubishi Chemical Corporation, Shikoh UT-4332), which is an energy ray curable compound, 1.1 parts by mass of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and 1 part by mass of bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (manufactured by BASF, Irgacure TPO) as a photopolymerization initiator, and diluted with methyl ethyl ketone to prepare a coating liquid of a composition for adhesive layer with a solids concentration of 34% by mass.
[0247] (Production of protective sheets for semiconductor processing) The coating liquid of the adhesive layer composition obtained above was applied to the release-treated surface of a release sheet (manufactured by Lintec Corporation, product name "SP-PET381031") and dried by heating to form an adhesive layer with a thickness of 10 μm on the release sheet.
[0248] Thereafter, an adhesive layer was attached to the surface of the intermediate layer-attached substrate to prepare a protective sheet for semiconductor processing. The type of substrate, and the composition and thickness of the intermediate layer and adhesive layer are shown in Table 1.
[0249] Example 2 A protective sheet for semiconductor processing was obtained in the same manner as in Example 1, except that the buffer layer was formed using the following buffer layer composition and the thickness of the intermediate layer was 120 μm. The type of substrate, and the composition and thickness of the intermediate layer and pressure-sensitive adhesive layer are shown in Table 1.
[0250] A composition for forming a buffer layer was prepared by blending 50 parts by weight of urethane acrylate oligomer (UA-1), 40 parts by weight of isobornyl acrylate (IBXA), 20 parts by weight of 2-hydroxy-3-phenoxypropyl acrylate (HPPA), and 10 parts by weight of pentaerythritol triacrylate (PETA), and further blending 1.0 part by weight of 2-hydroxy-2-methyl-1-phenyl-propan-1-one (manufactured by BASF Japan, product name "Irgacure 1173") as a photopolymerization initiator.
[0251] Example 3 Except for the fact that the thickness of the intermediate layer was 240 μm, a protective sheet for semiconductor processing was obtained in the same manner as in Example 1. The type of substrate, and the compositions and thicknesses of the intermediate layer and pressure-sensitive adhesive layer are shown in Table 1.
[0252] Example 4 A protective sheet for semiconductor processing was obtained in the same manner as in Example 1, except that the substrate with a buffer layer in Example 1 was changed to the substrate with a buffer layer below. The type of substrate, and the composition and thickness of the intermediate layer and pressure-sensitive adhesive layer are shown in Table 1.
[0253] A low-density polyethylene film (thickness: 27.5 μm) was prepared as a buffer layer. The buffer layers were laminated by dry lamination on both sides of the substrate used in Example 1 to obtain a substrate with a buffer layer in the order LDPE / PET / LDPE.
[0254] Example 5 A semiconductor processing protection sheet was obtained in the same manner as in Example 1, except that the substrate with the buffer layer in Example 1 was changed to the PET substrate in Example 1. In other words, no buffer layer was formed on the substrate. The type of substrate, and the composition and thickness of the intermediate layer and adhesive layer are shown in Table 1.
[0255] Comparative Example 1 A semiconductor processing protection sheet was obtained in the same manner as in Example 1, except that the substrate with the buffer layer in Example 1 was changed to an EVA film substrate (Fanclear LEAG120 manufactured by Gunze Co., Ltd.), the amount of acrylic copolymer (b) added in the intermediate layer composition was changed to 67 parts by mass, the thickness of the intermediate layer was set to 100 μm, and the following adhesive layer composition was used as the adhesive layer composition. That is, no buffer layer was formed on the substrate. The type of substrate, and the composition and thickness of the intermediate layer and adhesive layer are shown in Table 1.
[0256] An energy ray-curable acrylic copolymer (d) (Mw: 500,000) was obtained by reacting an acrylic polymer obtained by copolymerizing 70 parts by mass of n-butyl acrylate (BA), 15 parts by mass of i-butyl acrylate (iBA), 5 parts by mass of methyl methacrylate (MMA), and 10 parts by mass of 4-hydroxybutyl acrylate (4HBA) with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 90 equivalents of the hydroxyl groups of the total hydroxyl groups (100 equivalents) of the acrylic polymer.
[0257] 100 parts by mass of this energy ray-curable acrylic copolymer (d) was mixed with 1.8 parts by mass of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") and 7.29 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (manufactured by BASF, Irgacure 651) as a photopolymerization initiator, and the mixture was diluted with toluene to prepare a coating liquid of an adhesive composition with a solid content concentration of 25% by mass.
[0258] Comparative Example 2 A protective sheet for semiconductor processing was obtained in the same manner as in Example 1, except that the substrate with intermediate layer prepared as described below was used and the composition for adhesive layer described below was used as the composition for adhesive layer. The type of substrate, and the composition and thickness of the intermediate layer and adhesive layer are shown in Table 1.
[0259] Base material with intermediate layer A UV-curable resin composition was prepared by mixing 40 parts by mass (solid content ratio) of monofunctional urethane acrylate, 45 parts by mass (solid content ratio) of isobornyl acrylate (IBXA), 15 parts by mass (solid content ratio) of hydroxypropyl acrylate (HPA), 3.5 parts by mass (solid content ratio) of pentaerythritol tetrakis(3-mercaptobutyrate) (product name "Karrenz MT PE1", manufactured by Showa Denko K.K., secondary tetrafunctional thiol-containing compound, solid content concentration 100% by mass), 1.8 parts by mass of a UV-reactive thermal crosslinking agent, and 1.0 part by mass of 2-hydroxy-2-methyl-1-phenyl-propan-1-one (product name "Darocur 1173", manufactured by BASF, solid content concentration 100% by mass) as a photopolymerization initiator, and the mixture was applied to a polyethylene terephthalate (PET) film-based release film (SP-PET381031 manufactured by Lintec Corporation). The coating was applied onto a 38-μm thick substrate using a fountain die method so that the thickness after curing would be 400 μm. Then, ultraviolet light was irradiated from the coating side to form a semi-cured layer.
[0260] The ultraviolet irradiation was performed using a belt conveyor type ultraviolet irradiation device (product name "ECS-401GX", manufactured by iGraphics Co., Ltd.) as the ultraviolet irradiation device, a high-pressure mercury lamp (H04-L41, manufactured by iGraphics Co., Ltd.) as the ultraviolet light source, and irradiation conditions were a light wavelength of 365 nm and an illuminance of 112 mW / cm. 2 , light intensity 177mJ / cm 2 (Measured using UVPF-A1 manufactured by iGraphics)
[0261] A polyethylene terephthalate (PET) film (Toray Lumirror 75U403, thickness 75 μm) was laminated on the formed semi-cured layer, and ultraviolet light was further irradiated from the PET film side (using the above-mentioned ultraviolet light irradiation device and ultraviolet light source, irradiation conditions were illuminance 271 mW / cm 2 , light intensity 1200mJ / cm 2 ) and completely cured to form an intermediate layer having a thickness of 400 μm on the PET film substrate.
[0262] An energy ray-curable acrylic copolymer (e) (Mw: 500,000) was obtained by reacting an acrylic polymer obtained by copolymerizing 60 parts by mass of 2-ethylhexyl acrylate (2EHA), 15 parts by mass of ethyl acrylate (EA), 5 parts by mass of methyl methacrylate (MMA), and 20 parts by mass of 2-hydroxyethyl acrylate (2HEA) with 2-methacryloyloxyethyl isocyanate (MOI) so as to add to 60 equivalents of the hydroxyl groups of the total hydroxyl groups (100 equivalents) of the acrylic polymer.
[0263] 100 parts by mass of this energy ray-curable acrylic copolymer (e) was mixed with 1.2 parts by mass of an isocyanate-based crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") and 7.29 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (manufactured by BASF, Irgacure 651) as a photopolymerization initiator, and the mixture was diluted with toluene to prepare a coating liquid of an adhesive composition with a solids concentration of 25% by mass.
[0264] Comparative Example 3 Except for not including the acrylic copolymer (b) in the intermediate layer composition, a protective sheet for semiconductor processing was obtained in the same manner as in Example 1. The type of substrate, and the composition and thickness of the intermediate layer and pressure-sensitive adhesive layer are shown in Table 1.
[0265] Comparative Example 4 Except for the thickness of the intermediate layer being 300 μm, a protective sheet for semiconductor processing was obtained in the same manner as in Example 1. The type of substrate, and the compositions and thicknesses of the intermediate layer and pressure-sensitive adhesive layer are shown in Table 1.
[0266] [Table 1]
[0267] The above measurements and evaluations were carried out on the obtained samples (Examples 1 to 5 and Comparative Examples 1 to 4). The results are shown in Table 2.
[0268] [Table 2]
[0269] From Table 2, it was confirmed that when the Young's modulus of the semiconductor processing protective sheet is within the above-mentioned range and the intermediate layer contains a UV-curable compound, even when a wafer having unevenness is diced by DBG and LDBG, the unevenness is sufficiently embedded, the incidence of cracks caused by chip shift is low, and it is possible to achieve both the embedding of bumps and the peeling ability from the bumps. [Explanation of symbols]
[0270] 1...Semiconductor processing protection sheet 10...Base material 20. Middle class 30...Adhesive layer 40...Buffer layer
Claims
1. A semiconductor processing protection sheet having a substrate, and an intermediate layer and a pressure-sensitive adhesive layer in this order on one main surface of the substrate, the intermediate layer and the pressure-sensitive adhesive layer are energy ray-curable, the intermediate layer does not contain a filler; A protective sheet for semiconductor processing, the protective sheet having a Young's modulus of 600 MPa or more and 1800 MPa or less before being cured with energy rays at 50°C.
2. 2. The protective sheet for semiconductor processing according to claim 1, further comprising a buffer layer on the other main surface of the substrate.
3. 3. The protective sheet for semiconductor processing according to claim 1, wherein the substrate has a Young's modulus of 1000 MPa or more.
4. 4. The protective sheet for semiconductor processing according to claim 1, wherein the thickness of the intermediate layer is 60 μm or more and 250 μm or less.
5. 5. A semiconductor processing protective sheet according to claim 1, which is attached to the surface of a semiconductor wafer in a process of grinding the back surface of a semiconductor wafer having grooves formed on the surface of the semiconductor wafer to separate the semiconductor wafer into semiconductor chips by grinding.
6. A protective sheet for semiconductor processing described in any of claims 1 to 5, wherein the intermediate layer composition for forming the intermediate layer contains an acrylic polymer (A) having a weight-average molecular weight of 300,000 to 1,500,000, and an energy ray-curable acrylic polymer (B) having a weight-average molecular weight of 50,000 to 250,000.
7. A step of attaching the semiconductor processing protective sheet according to any one of claims 1 to 6 to a surface of a semiconductor wafer having projections and recesses; forming a groove from the front surface side of the semiconductor wafer, or forming a modified region inside the semiconductor wafer from the front surface or rear surface of the semiconductor wafer; A step of grinding the semiconductor wafer having the semiconductor processing protective sheet attached to the front surface and the groove or the modified region formed thereon from the rear surface side to separate the semiconductor wafer into a plurality of chips starting from the groove or the modified region; and peeling the protective sheet for semiconductor processing from each of the individual semiconductor chips.
Citation Information
Patent Citations
Method for producing adhesive sheet for processing semiconductor and method for producing semiconductor chip
JP2005343997A
Semiconductor processing adhesive sheet
JP2006012998A
Adhesive tape for surface protection
JP2011216513A
Adhesive sheet
JP2015183008A
Base for back grind tapes, and back grind tape
WO2015156389A1