Fuel pipe and fuel transport method using same

A double-pipe structure with an EVOH and elastomer inner pipe and polyethylene outer pipe addresses fuel leakage and deformation issues, providing enhanced fuel barrier properties and efficient underground transport.

JP7566633B2Active Publication Date: 2024-10-15KURARAY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020559335
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-14
Filing Date
2019-12-13
Publication Date
2024-10-15
Estimated Expiration
2039-12-13

AI Technical Summary

Technical Problem

Conventional fuel pipes made of steel and resin with nylon barrier layers suffer from corrosion, fuel leakage, and poor fuel barrier properties when deformed, especially when buried underground.

Method used

A double-pipe structure comprising an inner pipe made of a resin composition containing EVOH and an elastomer, with specific thickness ratios and a polyethylene outer pipe, enhances fuel barrier properties and flat strength, preventing deterioration even when deformed.

Benefits of technology

The fuel pipe maintains high fuel barrier properties and lightweight construction, ensuring safe and efficient fuel transport, reducing installation costs and minimizing fuel leakage risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566633000001
    Figure 0007566633000001
  • Figure 0007566633000002
    Figure 0007566633000002
  • Figure 0007566633000003
    Figure 0007566633000003
Patent Text Reader

Abstract

A fuel pipe consisting of a double pipe having an inner pipe and an outer pipe placed outside the inner pipe, wherein the inner pipe has a layer made of a resin composition containing an ethylene-vinyl alcohol copolymer (A) and an elastomer (B) and a layer made of polyethylene, and the outer pipe has a layer made of polyethylene, the thickness of the inner pipe is 5 mm or more, the ratio of the thickness of the layer made of the resin composition to the thickness of the inner pipe (resin composition layer / inner pipe) is 0.02 to 0.2, and the ratio of the thickness of the outer pipe to the thickness of the inner pipe (outer pipe / inner pipe) is 0.1 to 5. This fuel pipe has high flattening strength, and its fuel barrier properties are prevented from decreasing even when it is deformed in a direction perpendicular to the longitudinal direction (the direction of fuel flow).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fuel pipe made of a double tube and a fuel transport method using the same. [Background technology]

[0002] Conventionally, steel pipes have been used as fuel pipes buried underground at gas stations and the like. However, steel pipes buried underground have sometimes corroded, resulting in fuel leakage. Furthermore, steel pipes are heavy, making installation and other workability difficult. Fuel pipes made of resin with a nylon barrier layer are also known. However, nylon has poor fuel barrier properties, and fuels such as gasoline have sometimes evaporated from the pipes, contaminating the soil.

[0003] Meanwhile, ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as "EVOH") has excellent gas barrier properties, aroma retention, solvent resistance, oil resistance, transparency, etc., and taking advantage of these properties, it is widely used as a packaging material for food and medicine, and as a barrier layer in containers and pipes for fuel and water, etc.

[0004] Patent Document 1 describes a fuel oil pipe buried underground at a gas station, in which a shielding layer made of an ethylene-vinyl alcohol copolymer is bonded to the inner surface of an outer layer made of a polyethylene resin via an adhesive layer made of modified polyethylene. However, the fuel barrier property of the pipe was still insufficient. In particular, when the pipe was buried underground, the fuel barrier property was significantly reduced when a load was applied from the ground side and the pipe was deformed in a direction perpendicular to the axis.

[0005] Patent Document 2 describes a fuel pipe made of a multilayer structure having a resin composition layer containing EVOH and resin fine particles having a core-shell structure as a barrier layer. It also describes that the fuel pipe had excellent gasoline barrier properties and impact resistance. However, when the fuel pipe was deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows), the fuel barrier properties were significantly reduced. Patent Document 2 does not describe burying the fuel pipe underground. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-62734 A [Patent Document 2] Japanese Patent Application Publication No. 10-24505 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above problems, and aims to provide a fuel pipe that has high flattening strength and can prevent a decrease in fuel barrier properties even when deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows). It also aims to provide a method for transporting fuel safely without causing fuel leakage. [Means for solving the problem]

[0008] The above-mentioned problem is solved by providing a fuel pipe consisting of a double pipe having an inner pipe and an outer pipe placed outside the inner pipe, in which the inner pipe has a layer made of a resin composition containing EVOH (A) and an elastomer (B) and a layer made of polyethylene, and the outer pipe has a layer made of polyethylene, the thickness of the inner pipe is 5 mm or more, the ratio of the thickness of the layer made of the resin composition to the thickness of the inner pipe (resin composition layer / inner pipe) is 0.02 to 0.2, and the ratio of the thickness of the outer pipe to the thickness of the inner pipe (outer pipe / inner pipe) is 0.1 to 5.

[0009] In this case, the elastomer (B) is preferably at least one selected from the group consisting of acrylic elastomers, olefin elastomers, urethane elastomers, styrene elastomers and conjugated diene elastomers.

[0010] It is also preferred that the resin composition contains multilayered polymer particles as the elastomer (B). In this case, the average primary particle size of the multilayered polymer particles is preferably 0.2 to 1 μm. It is also preferred that the average secondary particle size of the multilayered polymer particles is 1.1 to 10 μm.

[0011] It is preferable that the multilayered polymer particles have at least an outermost layer and an innermost layer, and more preferably, the glass transition temperature of the polymer component constituting the outermost layer is 30° C. or higher, and the glass transition temperature of the polymer component constituting the innermost layer is −10° C. or lower.

[0012] The ethylene content of the EVOH (A) is preferably 20 to 50 mol %. It is also preferable that the mass ratio (B / A) of the elastomer (B) to the EVOH (A) is 1 / 99 to 40 / 60.

[0013] The above problem can also be solved by providing a fuel transport method, in which fuel is transported using the fuel pipe.

[0014] A fuel pipe for underground burial comprising the above-mentioned fuel pipe is a preferred embodiment of the present invention.

[0015] The above problem can also be solved by providing a fuel transportation method, in which the fuel pipe is buried in the ground and then the fuel is transported using the fuel pipe. Effect of the Invention

[0016] The fuel pipe of the present invention has high flattening strength, and the fuel barrier property is prevented from being deteriorated even when it is deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows). Moreover, since the fuel pipe of the present invention does not use steel material and is light, the work efficiency during installation is high. Therefore, by transporting fuel using the fuel pipe of the present invention, particularly by transporting fuel using the pipe after burying the pipe underground, the fuel can be transported safely and the installation cost can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The fuel pipe of the present invention is a double-walled fuel pipe having an inner pipe and an outer pipe placed outside the inner pipe, wherein the inner pipe has a layer made of a resin composition containing EVOH (A) and an elastomer (B) and a layer made of polyethylene, and the outer pipe has a layer made of polyethylene, the thickness of the inner pipe is 5 mm or more, the ratio of the thickness of the layer made of the resin composition to the thickness of the inner pipe (resin composition layer / inner pipe) is 0.02 to 0.2, and the ratio of the thickness of the outer pipe to the thickness of the inner pipe (outer pipe / inner pipe) is 0.1 to 5.

[0018] (inner tube) The inner pipe used in the fuel pipe of the present invention is made of a multilayer structure having a layer made of a resin composition containing EVOH (A) and an elastomer (B) (hereinafter sometimes abbreviated as "resin composition layer") and a layer made of polyethylene (hereinafter sometimes abbreviated as "polyethylene layer"). In the present invention, it is important that the inner pipe has a resin composition layer as a barrier layer. By having the inner pipe have a resin composition layer, the fuel barrier property is improved, and even if the fuel pipe is deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows), a decrease in the fuel barrier property is suppressed.

[0019] (EVOH(A)) The EVOH (A) used in the present invention is a copolymer having ethylene units and vinyl alcohol units. The EVOH (A) is usually obtained by saponifying an ethylene-vinyl ester copolymer. The production and saponification of the ethylene-vinyl ester copolymer can be carried out by known methods. Examples of vinyl esters used in the production of the ethylene-vinyl ester copolymer include fatty acid vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, and vinyl versatate, and among these, vinyl acetate is preferred.

[0020] The ethylene unit content of EVOH (A) is preferably 20 mol% or more, more preferably 25 mol% or more. If the ethylene unit content is less than 20 mol%, the thermal stability of EVOH (A) may decrease, or the flexibility may decrease, which may result in a decrease in fuel barrier property when the fuel pipe is deformed. On the other hand, the ethylene unit content of EVOH (A) is preferably 50 mol% or less, more preferably 35 mol% or less. If the ethylene unit content of EVOH (A) exceeds 50 mol%, the fuel barrier property may decrease. The ethylene unit content and saponification degree of EVOH (A) can be determined by a nuclear magnetic resonance (NMR) method.

[0021] The saponification degree of EVOH (A) is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more. When the saponification degree of EVOH (A) is 90 mol% or more, the fuel barrier property, thermal stability, and moisture resistance of the obtained fuel pipe are further improved. The saponification degree of EVOH (A) is usually 99.97 mol% or less, and preferably 99.94 mol% or less.

[0022] In addition, EVOH (A) may have units derived from other monomers other than ethylene, vinyl esters and their saponification products, within the scope of not impairing the object of the present invention. The content of units derived from other monomers in EVOH (A) is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less, based on the total monomer units in EVOH (A). When EVOH (A) has units derived from other monomers, the content thereof is preferably 0.05 mol% or more, more preferably 0.10 mol% or more, based on the total monomer units in EVOH (A). Examples of other monomers include unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, etc., or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile, methacrylonitrile, etc.; amides such as acrylamide, methacrylamide, etc.; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, methallylsulfonic acid, etc., or their salts; vinyl silane compounds such as vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tri(β-methoxy-ethoxy) silane, γ-methacryloxypropyl methoxy silane, etc.; alkyl vinyl ethers, vinyl ketones, N-vinyl pyrrolidone, vinyl chloride, vinylidene chloride, etc.

[0023] The MFR (melt flow rate) of EVOH (A) (measured at 190°C under a load of 2160 g) is preferably 0.1 to 100 g / 10 min. If the MFR of EVOH (A) exceeds 100 g / 10 min, the strength of the resin composition layer may decrease. The MFR of EVOH (A) is more preferably 50 g / 10 min or less, and even more preferably 30 g / 10 min or less. On the other hand, if the MFR of EVOH (A) is less than 0.1 g / 10 min, melt molding may become difficult. The MFR of EVOH (A) is more preferably 0.5 g / 10 min or more.

[0024] The EVOH (A) may be used alone or in combination of two or more kinds.

[0025] (Elastomer (B)) The resin composition layer contains an elastomer (B), which prevents the fuel barrier property from decreasing even when the fuel pipe is deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows). Examples of the type of elastomer (B) include acrylic elastomers, olefin elastomers such as ethylene-butene copolymers and ethylene-propylene copolymers, urethane elastomers, styrene elastomers such as styrene-ethylene / butylene-styrene block copolymers (SEBS), styrene-isobutylene-styrene block copolymers (SIBS), styrene-ethylene / propylene-styrene block copolymers (SEPS), styrene-butadiene-styrene block copolymers (SBS), and styrene-isoprene-styrene block copolymers (SIS), conjugated diene elastomers such as styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic acid ester-butadiene copolymers, and hydrogenated products thereof, silicone elastomers such as polyorganosiloxanes, ethylene ionomer copolymers, polybutadiene, polyisoprene, butadiene-isoprene copolymers, polychloroprene, and multilayered polymer particles having the above-mentioned components in the innermost layer. These may be used alone or in combination. Among these, the elastomer (B) is preferably at least one selected from the group consisting of acrylic elastomers, olefin elastomers, urethane elastomers, styrene elastomers, and conjugated diene elastomers, and more preferably an acrylic elastomer or a conjugated diene elastomer.

[0026] Acrylic elastomers are produced by polymerizing acrylic esters. Examples of acrylic esters used in the synthesis of the acrylic elastomers include alkyl acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and octyl acrylate. Among these, butyl acrylate or ethyl acrylate polymerized is preferred.

[0027] When synthesizing an acrylic elastomer, other monofunctional polymerizable monomers than acrylic esters may be copolymerized as necessary. Examples of other monofunctional polymerizable monomers to be copolymerized include methacrylic esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, amyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, octyl methacrylate, decyl methacrylate, dodecyl methacrylate, octadecyl methacrylate, phenyl methacrylate, benzyl methacrylate, naphthyl methacrylate, and isobornyl methacrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; and acrylonitrile. The content of other monofunctional monomer units relative to the total monomer units in the acrylic elastomer is preferably 20% by mass or less.

[0028] When producing a conjugated diene-based elastomer, other monofunctional polymerizable monomers than the conjugated diene may be copolymerized as necessary. Examples of other monofunctional polymerizable monomers to be copolymerized include those mentioned above as other monofunctional polymerizable monomers to be copolymerized with the acrylic acid ester when producing an acrylic elastomer. The content of other monofunctional polymerizable monomer units relative to the total monomer units in the conjugated diene-based elastomer is preferably 20 mass% or less.

[0029] The resin composition preferably contains multilayered polymer particles as the elastomer (B). The multilayered polymer particles more preferably have at least an outermost layer and an innermost layer. By containing the elastomer (B) in the resin composition as such multilayered particles, the deterioration of the fuel barrier property when the fuel pipe is deformed in a direction perpendicular to the longitudinal direction is further suppressed.

[0030] When the resin composition contains multilayered polymer particles as the elastomer (B), it is preferable that the elastomer (B) has a crosslinked molecular chain structure to exhibit rubber elasticity, and it is also preferable that the molecular chain of the polymer component constituting the innermost layer is grafted to the molecular chain in the adjacent layer by chemical bonding. For this purpose, it may be preferable to use a small amount of a polyfunctional polymerizable monomer as a crosslinking agent or grafting agent in the polymerization of the monomer for forming the polymer component constituting the innermost layer.

[0031] The polyfunctional polymerizable monomer used when forming the polymer component constituting the innermost layer is a monomer having two or more carbon-carbon double bonds in the molecule, and examples thereof include esters of unsaturated carboxylic acids such as acrylic acid, methacrylic acid, cinnamic acid, etc., with unsaturated alcohols such as allyl alcohol, methallyl alcohol, etc., or glycols such as ethylene glycol, butanediol, etc.; esters of dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, maleic acid, etc., with unsaturated alcohols, and the like. Specifically, examples include allyl acrylate, methallyl acrylate, allyl methacrylate, methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, and the like. The term "di(meth)acrylate" refers collectively to "diacrylate" and "dimethacrylate". These may be used alone or in combination. Among these, allyl methacrylate is preferably used.

[0032] The content of the polyfunctional polymerizable monomer unit relative to the total monomer units of the polymer component constituting the innermost layer is preferably 10% by mass or less. If the content of the polyfunctional polymerizable monomer unit is too high, the performance as an elastomer decreases, and the fuel barrier property may be easily decreased when the fuel pipe is deformed. When a monomer mainly composed of a conjugated diene compound is used, it does not necessarily have to be used in combination with a polyfunctional polymerizable monomer because the monomer itself functions as a crosslinking or grafting point.

[0033] From the viewpoint of further suppressing deterioration of the fuel barrier property due to deformation of the fuel pipe, it is preferable that the glass transition temperature (hereinafter sometimes abbreviated as Tg) of the polymer component constituting the innermost layer is -10°C or lower.

[0034] It is also preferable that the Tg of the polymer component constituting the outermost layer of the multilayered polymer particle is 30° C. or higher.

[0035] Examples of radical polymerizable monomers used in the synthesis of the polymer component constituting the outermost layer include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate; methacrylic acid esters having an alicyclic skeleton such as cyclohexyl methacrylate, isobornyl methacrylate, and adamantyl methacrylate; methacrylic acid esters having an aromatic ring such as phenyl methacrylate; aromatic vinyl compounds such as styrene and α-methylstyrene; and acrylonitrile. These monomers may be used alone or in combination. Preferred radical polymerizable monomers include methyl methacrylate or styrene alone or a combination of two or more radical polymerizable monomers having them as the main components.

[0036] The multilayered polymer particles may be composed of two or more layers, and examples of the layer structure include the following. Two-layer structure: innermost layer / outermost layer 3-layer structure: innermost layer / middle layer / outermost layer

[0037] It is preferable that the multilayered polymer particles have at least one functional group having reactivity or affinity to hydroxyl groups. This improves the dispersibility of the multilayered polymer particles in the matrix of EVOH (A) in the resulting resin composition, and further suppresses the deterioration of the fuel barrier property due to the deformation of the fuel pipe. Such multilayered polymer particles can be obtained by using a polymerizable compound having a functional group having reactivity or affinity to hydroxyl groups as a part of the monomer in the polymerization reaction for producing the multilayered polymer particles. Here, the functional group may be protected with a protecting group that does not hinder the object of the present invention and is removed when the EVOH (A) and the multilayered polymer particles are mixed.

[0038] Examples of radical polymerizable compounds having a functional group reactive or having affinity to hydroxyl groups include unsaturated compounds having a functional group capable of reacting with hydroxyl groups in EVOH (A) to form intermolecular bonds such as chemical bonds or hydrogen bonds when EVOH (A) and the multilayered polymer particles are mixed. Examples of functional groups reactive or having affinity to hydroxyl groups include hydroxyl groups, epoxy groups, isocyanate groups (-NCO), acid groups such as carboxyl groups, and acid anhydride groups such as maleic anhydride groups.

[0039] Examples of the unsaturated compound include polymerizable compounds having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxyethyl crotonate, 3-hydroxy-1-propene, 4-hydroxy-1-butene, cis-4-hydroxy-2-butene, and trans-4-hydroxy-2-butene; polymerizable compounds containing an epoxy group, such as glycidyl (meth)acrylate, allyl glycidyl ether, 3,4-epoxybutene, 4,5-epoxypentyl (meth)acrylate, 10,11-epoxyundecyl methacrylate, and p-glycidylstyrene; and carboxylic acids, such as (meth)acrylic acid, crotonic acid, cinnamic acid, itaconic acid, maleic acid, citraconic acid, aconitic acid, mezaconic acid, and methylenemalonic acid. The term "di(meth)acrylate" is a general term for "diacrylate" and "dimethacrylate," and "(meth)acrylic acid" is a general term for "acrylic acid" and "methacrylic acid."

[0040] The amount of the radical polymerizable compound having a functional group having reactivity or affinity to a hydroxyl group is preferably 0.01 to 75% by mass, more preferably 0.1 to 40% by mass, based on the total monomers used to produce the multilayered polymer particles. Examples of the radical polymerizable compound having a protected functional group include t-butyl methacrylocarbamate.

[0041] The functional group may be present in any layer of the multilayered polymer particles as long as it can substantially react with the hydroxyl group in EVOH (A) or form an intermolecular bond. A part of the multilayered polymer particles in the resin composition may form a chemical bond with EVOH (A), and it is particularly preferred that the functional group having reactivity or affinity to the hydroxyl group is present in the molecular chain in the outermost layer.

[0042] The content of the polymer component constituting the innermost layer in the multilayered polymer particle is preferably 50 to 90% by mass. If the content of the polymer component constituting the innermost layer is less than 50% by mass, the fuel barrier property may be significantly reduced when the fuel pipe is deformed. On the other hand, if the content of the polymer component constituting the innermost layer exceeds 90% by mass, the handleability of the multilayered polymer particle may be reduced.

[0043] The average primary particle diameter of the multilayered polymer particles is preferably 0.2 to 5 μm. When the average primary particle diameter of the multilayered polymer particles is less than 0.2 μm, when the multilayered polymer particles and the EVOH resin are dry-blended and the resin composition pellets are obtained by melt extrusion, the average secondary particle diameter of the multilayered polymer particles in the pellets tends to be too large. Here, the secondary particles refer to particles in which the primary particles are aggregated, and when the average secondary particle diameter is too large, the fuel barrier property may be significantly reduced when the fuel pipe is deformed. The average primary particle diameter is preferably 0.3 μm or more, more preferably 0.35 μm or more. On the other hand, when the average primary particle diameter exceeds 5 μm, the fuel barrier property may be significantly reduced when the fuel pipe is deformed. The average primary particle diameter is more preferably 3 μm or less, even more preferably 1 μm or less, particularly preferably 0.8 μm or less, and most preferably 0.6 μm or less.

[0044] The average secondary particle diameter of the multilayered polymer particles in the resin composition is preferably 1.1 to 10 μm. By forming relatively small aggregates of multilayered polymer particles in the resin composition in this way, the deterioration of the fuel barrier property due to the deformation of the fuel pipe is further suppressed. The average secondary particle diameter is more preferably 1.5 μm or more, and even more preferably 2 μm or more. On the other hand, the average secondary particle diameter is more preferably 8 μm or less, even more preferably 6 μm or less, and particularly preferably 5 μm or less. As a method for adjusting the average secondary particle diameter of the multilayered polymer particles to a predetermined range, for example, the screw rotation speed during dry blending is set to 20 rpm or more.

[0045] The polymerization method for producing the multilayered polymer particles is not particularly limited, and for example, spherical multilayered polymer particles can be easily obtained by a normal emulsion polymerization method. The emulsion polymerization is carried out according to a means normally used by those skilled in the art, and a chain transfer agent such as octyl mercaptan or lauryl mercaptan can be used as necessary. After the emulsion polymerization, the multilayered polymer particles are separated and obtained from the copolymer latex according to a method normally used by those skilled in the art (for example, a method such as coagulation or drying).

[0046] (Resin composition) In the resin composition, the mass ratio (B / A) of the elastomer (B) to the EVOH (A) is preferably in the range of 1 / 99 to 40 / 60. When the mass ratio (B / A) is 1 / 99 or more, the deterioration of the fuel barrier property due to the deformation of the fuel pipe is further suppressed. The mass ratio (B / A) is more preferably 3 / 97 or more, and even more preferably 5 / 95 or more. On the other hand, when the mass ratio (B / A) is 40 / 60 or less, the fuel barrier property is further improved. The mass ratio (B / A) is more preferably 30 / 70 or less, and even more preferably 25 / 75 or less.

[0047] The total content of EVOH (A) and elastomer (B) in the resin composition is preferably 50 mass % or more, more preferably 70 mass % or more, further preferably 80 mass % or more, and particularly preferably 90 mass % or more.

[0048] (Antioxidant (C)) The resin composition preferably contains an antioxidant (C). The melting point of the antioxidant (C) is preferably, for example, 170° C. or less. If the melting point of the antioxidant (C) exceeds 170° C., the antioxidant (C) does not melt when the resin composition is produced by melt mixing, and the antioxidant (C) may be localized in the resin composition, causing coloration of high concentration portions.

[0049] The molecular weight of the antioxidant (C) is preferably 300 or more. If the molecular weight of the antioxidant (C) is less than 300, the antioxidant (C) may bleed out onto the surface of the resulting fuel pipe, which may reduce the thermal stability of the resin composition. The molecular weight of the antioxidant (C) is more preferably 400 or more, and even more preferably 500 or more. On the other hand, the upper limit of the molecular weight of the antioxidant (C) is preferably 8000 or less, more preferably 6000 or less, and even more preferably 4000 or less, from the viewpoint of dispersibility, for example.

[0050] A compound having a hindered phenol group is preferably used as the antioxidant (C). The compound having a hindered phenol group has excellent thermal stability by itself and has the ability to capture oxygen radicals, which are the cause of oxidative deterioration, and when blended as the antioxidant (C) in the resin composition, it has an excellent effect of preventing oxidative deterioration.

[0051] As the compound having a hindered phenol group, commercially available products can be used, and examples thereof include the following products. (1) BASF "IRGANOX 1010": melting point 110-125°C, molecular weight 1178, pentaerythritol tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (2) BASF "IRGANOX 1076": melting point 50-55°C, molecular weight 531, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (3) BASF "IRGANOX 1098": melting point 156-161°C, molecular weight 637, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] (4) BASF "IRGANOX 245": melting point 76-79°C, molecular weight 587, triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] (5) BASF "IRGANOX 259": melting point 104-108°C, molecular weight 639, 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (6) "Sumilizer MDP-s" manufactured by Sumitomo Chemical Co., Ltd.: melting point about 128°C, molecular weight 341, 2,2'-methylene-bis(4-methyl-6-tert-butylphenol) (7) "Sumilizer GM" manufactured by Sumitomo Chemical Co., Ltd.: melting point about 128°C, molecular weight 395, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate (8) "Sumilizer GA-80" manufactured by Sumitomo Chemical Co., Ltd.: melting point about 110°C, molecular weight 741, 3,9-bis[2-{3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane

[0052] It is also preferable to use a compound having a hindered amine group as the antioxidant (C). The compound having a hindered amine group not only suppresses the thermal deterioration of EVOH (A), but also captures the aldehyde generated by the thermal decomposition of EVOH (A). This reduces the generation of decomposition gas, thereby suppressing the generation of voids and bubbles during molding.

[0053] As the compound having a hindered amine group, a piperidine derivative is preferred, and among them, a 2,2,6,6-tetraalkylpiperidine derivative having a substituent at the 4-position is more preferred. The substituent at the 4-position may be a carboxyl group, an alkoxy group, or an alkylamino group. In addition, the N-position of the hindered amine group of the compound having a hindered amine group may be substituted with an alkyl group.

[0054] As the compound having a hindered amine group, commercially available products can be used, and examples thereof include the following products. (9) BASF "TINUVIN 770": melting point 81-85°C, molecular weight 481, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate (10) BASF "TINUVIN 765": liquid compound, molecular weight 509, bis(1,2,2,6,6-pentamethyl-4-piperidyl) sebacate and 1,2,2,6,6-pentamethyl-4-piperidyl sebacate (mixture) (11) BASF "TINUVIN 622LD": melting point 55-70°C, molecular weight 3100-4000, polycondensation product of dimethyl succinate and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine (12) BASF "CHIMASSORB 119FL": melting point 130-140°C, molecular weight 2000 or more, N,N'-bis(3-aminopropyl)ethylenediamine-2,4-bis[N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate (13) BASF "CHIMASSORB 944LD": melting point 100-135°C, molecular weight 2000-3100, poly[[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl][2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene(2,2,6,6-tetramethyl-4-piperidine)imino]] (14) BASF "TINUVIN 144": melting point 146-150°C, molecular weight 685, bis(1,2,2,6,6-pentamethyl-4-piperidyl) [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate (15) BASF "UVINUL 4050H": melting point 157°C, molecular weight 450, N,N'-1,6-hexanediylbis{N-(2,2,6,6-tetramethyl-4-piperidinyl)-formamide}

[0055] (16) "UVINUL 5050H" manufactured by BASF: a compound having a melting point of 104-112°C, a molecular weight of about 3500, and the following structural formula:

[0056] [ka]

[0057] These compounds having a hindered phenol group or a hindered amine group may be used alone or in combination of two or more kinds.

[0058] The content of the antioxidant (C) in the resin composition is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the EVOH (A). If the content of the antioxidant (C) is less than 0.01 parts by mass, the above-mentioned effects may not be obtained. The content of the antioxidant (C) is more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more. On the other hand, if the content of the antioxidant (C) exceeds 5 parts by mass, poor dispersion of the antioxidant (C) may occur. The content of the antioxidant (C) is more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the EVOH (A).

[0059] The resin composition may contain additives other than the EVOH (A), the elastomer (B) and the antioxidant (C) as long as the effects of the present invention are not impaired. Examples of such additives include resins other than the EVOH (A) and the elastomer (B), metal salts, acids, boron compounds, plasticizers, fillers, antiblocking agents, lubricants, stabilizers, surfactants, colorants, ultraviolet absorbers, antistatic agents, drying agents, crosslinking agents, fillers, reinforcing materials such as various fibers, etc., and among these, metal salts and acids are preferred from the viewpoints of the thermal stability of the resin composition and adhesion to other resins.

[0060] As the metal salt, an alkali metal salt is preferred from the viewpoint of further increasing interlayer adhesion, and an alkaline earth metal salt is preferred from the viewpoint of thermal stability. When the resin composition contains a metal salt, the content is preferably 1 to 10,000 ppm in terms of metal element. The content of the metal salt is more preferably 5 ppm or more, even more preferably 10 ppm or more, and particularly preferably 20 ppm or more, in terms of metal element. On the other hand, the content of the metal salt is more preferably 5,000 ppm or less, even more preferably 1,000 ppm or less, and particularly preferably 500 ppm or less, in terms of metal element. As a method for measuring the content of the metal salt, for example, a method in which a sample obtained by freeze-pulverizing a dried EVOH pellet is quantified using an ICP emission spectrometer can be mentioned.

[0061] As the acid, from the viewpoint of increasing the thermal stability during melt molding, a carboxylic acid compound and a phosphoric acid compound are preferred. When the resin composition contains a carboxylic acid compound, the content is preferably 1 to 10,000 ppm. The content of the carboxylic acid compound is more preferably 10 ppm or more, and even more preferably 50 ppm or more. On the other hand, the content of the carboxylic acid compound is more preferably 1,000 ppm or less, and even more preferably 500 ppm or less. For example, a neutralization titration method can be used as a method for measuring the content of the acid.

[0062] When the resin composition contains a phosphoric acid compound, the content is preferably 1 to 10,000 ppm. The content of the phosphoric acid compound is more preferably 10 ppm or more, and even more preferably 30 ppm or more. On the other hand, the content of the phosphoric acid compound is more preferably 1,000 ppm or less, and even more preferably 300 ppm or less. The method for measuring the content of the phosphoric acid compound includes, for example, a method in which a sample obtained by freeze-pulverizing a dried EVOH pellet is quantified using an ICP emission spectrometer.

[0063] When the resin composition contains a boron compound, the content is preferably 1 to 2000 ppm. The content of the boron compound is more preferably 10 ppm or more, and even more preferably 50 ppm or more. On the other hand, the content of the boron compound is more preferably 1000 ppm or less, and even more preferably 500 ppm or less. When the content of the boron compound in the resin composition is within the above range, the thermal stability during melt molding is further improved. The content of the boron compound can be measured by the same method as that of the phosphoric acid compound described above.

[0064] As a method for incorporating the phosphoric acid compound, carboxylic acid or boron compound into the resin composition, for example, a method of adding the compound to the EVOH composition and kneading when producing pellets of the resin composition is preferably adopted. As a method for adding the compound to the EVOH composition, for example, a method of adding a dry powder, a method of adding a paste impregnated with a solvent, a method of adding a suspension in a liquid, a method of adding a solution dissolved in a solvent, and a method of immersing EVOH pellets in a solution can be mentioned. Among them, from the viewpoint of uniformly dispersing the phosphoric acid compound, carboxylic acid or boron compound, a method of adding a solution dissolved in a solvent or a method of immersing EVOH pellets in a solution is preferred. As the solvent, for example, water is preferably used from the viewpoints of the solubility of the additive, the viewpoint of cost, the ease of handling, the safety of the working environment, and the like.

[0065] The resin composition can be obtained by mixing EVOH (A), elastomer (B), and, if necessary, antioxidant (C) and other additives described above. As a method for mixing these, a known method for mixing resins can be used. When using a melt-kneading method, EVOH (A), elastomer (B), and, if necessary, antioxidant (C), stabilizer, dye, pigment, plasticizer, lubricant, filler, other resin, etc. are added, and then melt-kneaded, for example, at 200 to 300°C using a screw-type extruder, etc.

[0066] The multilayered polymer particles to be used for producing the resin composition may be, for example, those in which the outermost layers of the multilayered polymer particles are fused to each other to form pellets, so long as they can be sufficiently dispersed in particle form when mixed with EVOH (A).

[0067] Examples of polyethylene used in the polyethylene layer of the inner tube of the fuel pipe of the present invention include polyethylenes such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene; and ethylene-based copolymers obtained by copolymerizing ethylene with α-olefins such as 1-butene, 1-hexene, and 4-methyl-1-pentene. One type of polyethylene may be used alone, or two or more types may be used in combination. Among these, high-density polyethylene is preferred as the polyethylene used in the polyethylene layer of the inner tube.

[0068] The MFR (melt flow rate, 190°C, under a load of 2160 g) of the polyethylene used in the polyethylene layer of the inner tube is preferably 0.01 to 10 g / 10 min. If the MFR of the polyethylene is less than 0.01 g / 10 min, melt molding may be difficult. On the other hand, if the MFR of the polyethylene is more than 10 g / 10 min, the strength of the polyethylene layer may decrease or extrusion molding may be difficult. The MFR of the polyethylene is more preferably 5 g / 10 min or less, further preferably 3 g / 10 min or less, and particularly preferably 2 g / 10 min or less.

[0069] In the inner pipe, the resin composition layer may be directly bonded to another layer such as a polyethylene layer, but is preferably bonded via an adhesive resin layer.

[0070] Resins used in the adhesive resin layer include, for example, polyurethane-based or polyester-based one-component or two-component curable adhesives; and polyolefins having carboxyl groups, carboxylic anhydride groups, or epoxy groups. Among these, polyolefins having carboxyl groups, carboxylic anhydride groups, or epoxy groups are more preferred because of their excellent adhesion to both EVOH (A) and polyethylene.

[0071] Examples of polyolefins containing carboxyl groups include polyolefins copolymerized with acrylic acid or methacrylic acid, and as typified by ionomers, all or part of the carboxyl groups contained in the polyolefin may be present in the form of metal salts. Examples of polyolefins having carboxylic anhydride groups include polyolefins graft-modified with maleic anhydride or itaconic acid. Examples of polyolefin resins containing epoxy groups include polyolefins copolymerized with glycidyl methacrylate. Among these polyolefins having carboxyl groups, carboxylic anhydrides, or epoxy groups, polyolefins modified with carboxylic anhydrides such as maleic anhydride, particularly polyethylene, are preferred in terms of excellent adhesiveness.

[0072] The polyethylene content in the polyethylene layer of the inner tube is usually 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more.

[0073] The polyethylene layer of the inner tube may contain additives other than polyethylene as long as the effects of the present invention are not impaired. Examples of such additives include those mentioned above as additives other than the EVOH (A) and the elastomer (B) contained in the resin composition.

[0074] The polyethylene layer of the inner tube may be made of recycled inner tubes or outer tubes (described later).

[0075] The inner pipe used in the fuel pipe of the present invention is a multi-layer pipe having a resin composition layer and a polyethylene layer, and examples of the layer structure include the following: In this example, the left is the inner side and the right is the outer side. 2 layers (inner) resin composition layer / polyethylene layer (outer), polyethylene layer / resin composition layer 3 layers: resin composition layer / adhesive resin layer / polyethylene layer, polyethylene layer / adhesive resin layer / resin composition layer, polyethylene layer / resin composition layer / polyethylene layer 4 layers: polyethylene layer / resin composition layer / adhesive resin layer / polyethylene layer 5 layers: polyethylene layer / adhesive resin layer / resin composition layer / adhesive resin layer / polyethylene layer

[0076] The thickness of the inner pipe must be 5 mm or more. If the thickness of the inner pipe is less than 5 mm, the flattening strength of the fuel pipe of the present invention decreases. On the other hand, the thickness of the inner pipe is usually 50 mm or less, and preferably 20 mm or less. Here, the flattening strength refers to the compressive strength of the fuel pipe against compression from a direction perpendicular to the longitudinal direction of the fuel pipe (the direction in which the fuel flows).

[0077] The ratio of the thickness of the resin composition layer to the thickness of the inner tube (resin composition layer / inner tube) must be 0.02 to 0.2. If the thickness ratio (resin composition layer / inner tube) is less than 0.02, the fuel barrier properties become insufficient. On the other hand, from the viewpoint of suppressing the deterioration of the fuel barrier properties after deformation and from the viewpoint of cost, the thickness ratio (resin composition layer / inner tube) is preferably 0.1 or less.

[0078] In the inner pipe, by disposing the resin composition layer at a position closer to the inside with respect to the overall thickness, a pipe having superior fuel barrier properties can be obtained compared to a case where the resin composition layer is disposed at the center with respect to the overall layer thickness. The effect becomes greater the further away from the center.

[0079] The inner tube can be manufactured by, for example, melt molding or solution coating. In the case of melt molding, co-extrusion molding, co-injection molding, extrusion coating, etc. are used. In addition, a multi-layer molding method such as dry lamination is also used.

[0080] In the case of melt molding, for example, a step of cooling the inner pipe immediately after molding with water at 10 to 70 ° C. is preferably included. That is, after melt molding, it is preferable to solidify the resin composition layer by cooling the resin composition layer with water at 10 to 70 ° C. If the temperature of the cooling water is too low, cracks may easily occur when the fuel pipe is deformed. Although the details of the cause of the cracks being easily generated are not clear, it is presumed that the residual stress in the molded product has an influence. From this viewpoint, the temperature of the cooling water is more preferably 15 ° C. or higher, and more preferably 20 ° C. or higher. On the other hand, if the temperature of the cooling water is too high, cracks may easily occur when the fuel pipe is deformed. Although the details of the cause of the cracks are not clear, it is presumed that the crystallization degree of the resin composition becomes too high. From this viewpoint, the temperature of the cooling water is more preferably 60 ° C. or lower, and more preferably 50 ° C. or lower.

[0081] The multi-layer pipe obtained by the above method may be subjected to secondary processing. As the secondary processing method, a known secondary processing method can be appropriately used, for example, a method in which the multi-layer pipe is heated to 80 to 160°C, deformed into a desired shape, and then fixed for 1 minute to 2 hours.

[0082] The fuel pipe of the present invention has a layer made of polyethylene in the outer pipe. The polyethylene layer of the outer pipe can be the same as the polyethylene layer of the inner pipe described above. The outer pipe may have a layer other than the polyethylene layer, and examples of the other layer include layers similar to the resin composition layer and adhesive resin layer used in the inner pipe described above. From the viewpoint of cost, it is preferable that the outer pipe is a single-layer pipe consisting of only a polyethylene layer.

[0083] The thickness of the outer tube is not particularly limited as long as the effects of the present invention are not impaired, but is preferably 1 mm or more, more preferably 2 mm or more, in order to further improve the flattening strength. On the other hand, the thickness of the outer tube is usually 50 mm or less, preferably 20 mm or less. The outer diameter of the outer tube is also not particularly limited as long as the effects of the present invention are not impaired, but is usually 20 to 400 mm.

[0084] The outer tube can be manufactured by a known method such as a melt molding method, for example, an extrusion molding method, an injection molding method, or the like.

[0085] The fuel pipe of the present invention is obtained by inserting the inner pipe into the outer pipe thus obtained. The fuel pipe of the present invention has high flattening strength by forming such a double pipe. Furthermore, even if a crack or the like occurs in one pipe due to deformation or the like, the other pipe prevents the fuel from leaking out to the outside. As long as such an effect is not hindered, the difference between the inner diameter of the outer pipe and the outer diameter of the inner pipe (inner diameter of the outer pipe - outer diameter of the inner pipe) is not particularly limited, and is usually 0.5 to 10 mm. In addition, in the fuel pipe of the present invention, a part of the inner surface of the outer pipe and a part of the outer surface of the inner pipe may be bonded. As a method for bonding the inner surface of the outer pipe and the outer surface of the inner pipe, a bonding wire made of an electric heating wire is wound in a coil shape around the outer surface of the inner pipe, the inner pipe is inserted into the outer pipe, and then a voltage is applied to the wire to fuse the inner surface of the outer pipe and the outer surface of the inner pipe.

[0086] In the fuel pipe of the present invention, the ratio of the thickness of the outer pipe to the thickness of the inner pipe (outer pipe / inner pipe) must be 0.1 to 5, and within this range, a fuel pipe with high flattening strength can be obtained. The ratio (outer pipe / inner pipe) is preferably 0.2 or more. On the other hand, the ratio (outer pipe / inner pipe) is preferably 3 or less, more preferably 2 or less, and even more preferably 1.5 or less.

[0087] The fuel pipe of the present invention has high flattening strength, and further prevents a decrease in fuel barrier properties even when deformed in a direction perpendicular to the longitudinal direction (the direction in which the fuel flows). The fuel pipe of the present invention does not use steel material and is light, so that construction efficiency during installation is high. A fuel transportation method in which fuel is transported using such a fuel pipe is a preferred embodiment of the present invention. It is preferable that the fuel pipe of the present invention is a fuel pipe for underground burial. The fuel pipe of the present invention is buried underground and is not easily deformed even when a force is applied from the ground, and even if it is deformed, fuel leakage is unlikely to occur. A fuel transportation method in which the fuel pipe of the present invention is buried underground and then used to transport fuel is a more preferred embodiment of the present invention. EXAMPLES

[0088] The present invention will now be described in more detail with reference to examples.

[0089] (1) Average primary particle size of multilayer structure polymer particles The resin composition pellets obtained in each Example and Comparative Example were cut using a Leica ultramicrotome (model: Ultracut S / FC-S) to prepare ultrathin sections for observation under a transmission electron microscope. The cutting conditions were as follows: Sample: -100℃ Knife: -100℃ Cutting speed: 0.4~1.0mm / s Cutting thickness setting: 85nm Thickness: 85 nm The obtained ultrathin sections were collected on a copper mesh (1000 mesh) and subjected to electron staining using a phosphomolybdic acid solution.

[0090] The structure of the obtained ultrathin sections was observed under the following conditions: A Hitachi High-Technologies Corporation transmission electron microscope (model: HT7700, 3DTEM compatible) equipped with a LaB6 electron gun was used for the structure observation. Accelerating voltage: 100 kV LaB6 electron beam irradiation amount: 10μA Electron beam spot size: 1μm Condenser aperture diameter: 0.1mm (No.2) 3D objective movable aperture hole diameter: 0.16mm (No.3)

[0091] The CCD camera used for recording images was an AMT bottom mount camera (model: XR81B, 8 megapixel camera), and the average values ​​of the long and short diameters of the particles in the images of the obtained ultrathin sections were calculated. The average values ​​were calculated in the same manner for 20 particles, and the average value of all of these was taken as the average primary particle size of the multilayer structure polymer particles.

[0092] (2) Average secondary particle size of multilayer structure polymer particles The average long and short diameters of the multilayered polymer particle aggregates were calculated in the same manner as for the average primary particle diameter. The average was calculated for 20 aggregates in the same manner, and the average was taken as the average secondary particle diameter of the multilayered polymer particle.

[0093] (3) Fuel barrier properties One end of the double-walled pipe cut to a length of 100 mm was sealed with aluminum tape (FP Kako Co., Ltd. "Aluminum Seal" (gasoline permeability: 0 g / m 2 ·day). The double-walled pipe was filled with 500 ml of CE10 (toluene 45% by volume, isooctane 45% by volume, ethanol 10% by volume) as model gasoline, and the other end was sealed with aluminum tape. The double-walled pipe filled with the model gasoline was left in an explosion-proof constant temperature and humidity chamber (40°C, 65% RH), and the mass of the double-walled pipe was measured every 7 days for 3 months. The amount of fuel permeation was calculated from the change in mass of the double-walled pipe, and the fuel barrier properties of the double-walled pipe were evaluated according to the following criteria. A: Less than 0.01g / day B: 0.01g / day or more and less than 0.1g / day C: 0.1g / day or more

[0094] (4) Flattening strength measurement The double-walled pipe was cut to a length of 100 mm. Using a compressor (AYS-type benchtop test press manufactured by Shinto Metal Industries Co., Ltd.), the double-walled pipe was compressed perpendicular to the longitudinal direction (the direction of fuel flow) at a speed of 30 mm / min. The compressive strength at which the dimensional change rate of the double-walled pipe reached 10% was taken as the flattened compressive strength of the double-walled pipe, and was evaluated according to the following criteria. A:1kN / 100mm or more B: 0.5kN / 100mm or more, less than 1kN / 100mm C: Less than 0.5kN / 100mm

[0095] The dimensional change rate was calculated by the following formula using the outer diameter D of the double-walled pipe before deformation (before compression) and the minor axis d (perpendicular to the longitudinal direction) of the double-walled pipe after deformation. Dimensional change rate (%) = (1-d / D) x 100

[0096] (5) Fuel barrier properties of double-walled pipes after deformation As in the above "(4) Flattening strength measurement," the double-walled pipe was compressed so that the dimensional change rate was 10%, and was kept in that state for 24 hours. The pressure was released, the double-walled pipe was removed, and its gasoline permeation amount was measured in the same manner as in the above "(3) Fuel barrier property." The ratio of the gasoline permeation amount of the double-walled pipe before and after deformation (fuel permeation amount of the double-walled pipe after deformation / fuel permeation amount of the double-walled pipe before deformation) was calculated, and the change in the fuel barrier property of the double-walled pipe due to deformation was evaluated according to the following criteria. A: Less than 1.3 B: 1.3 or more and less than 3 C:3 or more

[0097] [Production of EVOH-1] 2 kg of EVOH resin with ethylene unit content of 32 mol% and saponification degree of 99.8 mol% was placed in 18 kg of a mixed solvent of water / methanol = 40 / 60 (mass ratio) and stirred at 60 ° C for 6 hours to completely dissolve. This solution was continuously extruded from a nozzle with a diameter of 4 mm into a coagulation bath of water / methanol = 90 / 10 (mass ratio) adjusted to 0 ° C, and the EVOH was coagulated into strands. The strands were introduced into a pelletizer to obtain porous EVOH chips.

[0098] The obtained porous EVOH chips were washed with an aqueous solution of acetic acid and ion-exchanged water, and then immersed in an aqueous solution containing acetic acid, potassium dihydrogen phosphate, sodium acetate, and orthoboric acid. The aqueous solution for treatment and the EVOH chips were separated and dehydrated, then placed in a hot air dryer and dried at 80°C for 4 hours, and then further dried at 100°C for 16 hours to obtain dried EVOH pellets (EVOH-1). The acetic acid content of EVOH-1 was 150 ppm, the sodium ion content was 140 ppm, the phosphoric acid compound content was 45 ppm in terms of phosphoric acid radical, and the boron compound content was 260 ppm in terms of boron. The MFR of EVOH-1 (ASTM-D1238, 190°C, 2160g load) was 1.6 g / 10 min.

[0099] [Production of multilayered polymer particles P-1] In a nitrogen atmosphere, 600 parts by mass of distilled water, 0.168 parts by mass of sodium lauryl sarcosinate as an emulsifier, and 2.1 parts by mass of sodium stearate were added to a polymerization vessel equipped with a stirring blade, a cooling tube, and a dropping funnel, and the mixture was heated to 70°C to dissolve uniformly. Next, at the same temperature, 150 parts by mass of butyl acrylate (BA) and 0.15 parts by mass of allyl methacrylate as a polyfunctional polymerizable monomer were added, and the mixture was stirred for 30 minutes, after which 0.15 parts by mass of potassium peroxodisulfate was added to start polymerization. After 4 hours, it was confirmed by gas chromatography that all of the monomers had been consumed.

[0100] Next, 0.3 parts by mass of potassium peroxodisulfate was added to the obtained copolymer latex, and then a mixture of 50 parts by mass of methyl methacrylate and 10 parts by mass of glycidyl methacrylate (GMA) was dropped from the dropping funnel over 2 hours. After the dropping was completed, the reaction was continued for another 30 minutes at 70°C, and the polymerization was terminated after confirming that the monomers had been consumed. The particle diameter of the obtained copolymer latex was 0.4 μm. This was cooled to -20°C for 24 hours to cause coagulation, and the coagulation was taken out and washed three times with hot water at 80°C. Furthermore, it was dried under reduced pressure at 50°C for 2 days to obtain multilayer structure polymer particles P-1. The obtained multilayered polymer particles P-1 were polymer particles (average primary particle diameter 0.4 μm) with a two-layer structure (core-shell structure) having an innermost layer (core, 70 mass%) consisting of a polymer component (Tg = -39 ° C) mainly composed of butyl acrylate (BA) and an outermost layer (shell, 30 mass%) consisting of polymethyl methacrylate (PMMA, Tg = 106 ° C) modified with glycidyl methacrylate (GMA, content 25 mol%).

[0101] [Production of multilayered polymer particles P-2, P-4, and P-5] Multilayer structure polymer particles (P-2: 0.8 μm, P-4: 0.2 μm, P-5: 4 μm) were produced in the same manner as multilayer structure polymer particles P-1, except that the average primary particle diameter of the polymer particles was changed by adjusting the polymerization reaction time of butyl acrylate.

[0102] [Production of multilayered polymer particles P-3] Multilayer structure polymer particles P-3 were produced in the same manner as multilayer structure polymer particles P-1, except that 50 parts by mass of styrene (St) was used instead of methyl methacrylate. The obtained multilayer structure polymer particles P-3 were polymer particles (average primary particle diameter 0.4 μm) with a two-layer structure (core-shell structure) having an innermost layer (core, 70 mass%) made of a polymer component (Tg = -39 ° C) mainly composed of butyl acrylate, and an outermost layer (shell, 30 mass%) made of polystyrene (Tg = 98 ° C) modified with glycidyl methacrylate (content 25 mol%).

[0103] Example 1 90 parts by mass of EVOH-1 as EVOH (A), 10 parts by mass of multilayer structure polymer particles P-1 as elastomer (B), and 0.5 parts by mass of N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide] as antioxidant (C) were dry blended at a screw rotation speed of 50 rpm, and the resulting mixture was pelletized at an extrusion temperature of 200°C using a 30 mmφ co-rotating twin-screw extruder ("TEX-30N" manufactured by Japan Steel Works, Ltd.) to obtain resin composition pellets.

[0104] The obtained resin composition pellets were put into the first extruder, maleic anhydride modified polyethylene into the second extruder, and pellets of high density polyethylene [density 0.96 g / cc, MFR (measured at 190 ° C. under a load of 2160 g) 0.5 g / 10 min] into the third extruder, and a multi-layer pipe for an inner tube having an outer diameter of 100 mm and a thickness of 6 mm was extruded using a three-kind, three-layer circular die, and immediately after that, it was cooled and solidified through a cooling water tank adjusted to 40 ° C. The layer structure of the obtained multi-layer pipe was high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 5640 μm / 180 μm / 180 μm.

[0105] Separately, the above-mentioned high-density polyethylene pellets were placed in an extruder, and a single-layer pipe for an outer tube with an inner diameter of 105 mm and a thickness of 6 mm was extruded using a single-layer circular die, and immediately thereafter, the pipe was cooled and solidified through a cooling water tank adjusted to 40° C. In the subsequent double-walled pipe manufacturing process, the inner diameter of the outer tube was made larger than the outer diameter of the inner tube so that the inner tube with a bonding wire wound around its outer surface could be inserted into the outer tube.

[0106] A bonding wire made of an electric heating wire coated with high density polyethylene was wound in a coil shape around the outer surface of the obtained multi-layer pipe for the inner pipe, and the multi-layer pipe was then inserted into the single-layer pipe for the outer pipe. A voltage was applied to the bonding wire to fuse a part of the outer surface of the inner pipe to a part of the inner surface of the outer pipe, obtaining a double pipe. The obtained double pipe was evaluated. The results are shown in Table 1.

[0107] Example 2 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 6580 μm / 210 μm / 210 μm, and the thickness of the single-layer pipe for the outer pipe was changed to 7 mm. The results are shown in Table 1.

[0108] Example 3 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 5400 μm / 300 μm / 300 μm. The results are shown in Table 1.

[0109] Example 4 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 7520 μm / 240 μm / 240 μm, and the thickness of the single-layer pipe for the outer pipe was changed to 4 mm. The results are shown in Table 1.

[0110] Example 5 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 4700 μm / 150 μm / 150 μm, and the thickness of the single-layer pipe for the outer pipe was changed to 7 mm. The results are shown in Table 1.

[0111] Example 6 A fuel pipe was produced and evaluated in the same manner as in Example 1, except that the multilayer structure polymer particles P-2 were used as the elastomer (B) and the dry blending was performed at a screw rotation speed of 100 rpm. The results are shown in Table 1.

[0112] Example 7 Except for dry blending at a screw rotation speed of 150 rpm, a fuel pipe was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0113] Example 8 Except for dry blending at a screw rotation speed of 25 rpm, a fuel pipe was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0114] Example 9 Except for using the multilayer structure polymer particles P-3 as the elastomer (B), a fuel pipe was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0115] Example 10 A fuel pipe was produced and evaluated in the same manner as in Example 1, except that the content of EVOH (A) was changed to 70 parts by mass and the content of the multilayered polymer particles was changed to 30 parts by mass. The results are shown in Table 1.

[0116] Examples 11 and 12 Fuel pipes were produced and evaluated in the same manner as in Example 1, except that the ethylene content of the EVOH used as EVOH (A) was changed as shown in Table 1 (Example 11: EVOH-2, Example 12: EVOH-3). The results are shown in Table 1.

[0117] Examples 13 and 14 A fuel pipe was produced and evaluated in the same manner as in Example 1, except that the multilayer structure polymer particles P-4 (Example 13) or the multilayer structure polymer particles P-5 (Example 14) were used as the elastomer (B). The results are shown in Table 1.

[0118] Example 15 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to resin composition layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / high density polyethylene layer (innermost layer) = 180 μm / 180 μm / 5640 μm. The results are shown in Table 2.

[0119] Examples 16 to 18 The fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that a maleic anhydride-modified ethylene-butene copolymer (EB, Mitsui Chemicals, Inc. "Tafmer MH7020": Example 16), a polyurethane (TPU, BASF, Inc. "ET890": Example 17), or a maleic anhydride-modified styrene-ethylene / butylene-styrene block copolymer (SEBS, Asahi Kasei Corporation "Tuftec M1943": Example 18) was used instead of the multilayered polymer particles P-1. The results are shown in Table 2.

[0120] Comparative Example 1 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 2820 μm / 90 μm / 90 μm, and the thickness of the single-layer pipe for the outer pipe was changed to 3 mm. The results are shown in Table 2.

[0121] Comparative Example 2 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the thickness of the single-layer pipe for the outer pipe was changed to 0.48 mm. The results are shown in Table 2.

[0122] Comparative Example 3 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 940 μm / 30 μm / 30 μm. The results are shown in Table 2.

[0123] Comparative Example 4 A fuel pipe was manufactured and evaluated in the same manner as in Example 1, except that the layer structure of the multi-layer pipe for the inner pipe was changed to high density polyethylene layer (outermost layer) / maleic anhydride modified polyethylene (adhesive resin layer) / resin composition layer (innermost layer) = 5880 μm / 60 μm / 60 μm. The results are shown in Table 2.

[0124] Comparative Example 5 A multi-layer pipe for an inner pipe was produced in the same manner as in Example 1, and was evaluated without covering it with an outer pipe. The results are shown in Table 2.

[0125] Comparative Example 6 A multi-layer pipe for an inner tube was produced in the same manner as in Example 1, except that the thickness was 12 mm, and evaluation was carried out without covering it with an outer tube. The results are shown in Table 2.

[0126] Comparative Example 7 Except for not adding the multilayered polymer particles, a fuel pipe was produced and evaluated in the same manner as in Example 1. The results are shown in Table 2.

[0127] Comparative Examples 8 and 9 A fuel pipe was produced and evaluated in the same manner as in Example 1, except that the multilayered polymer particles were not added and the ethylene content of the EVOH used as EVOH (A) was changed as shown in Table 2. The results are shown in Table 2.

[0128] Comparative Example 10 A fuel pipe was produced and evaluated in the same manner as in Example 1, except that the multilayered polymer particles were not added and nylon-6 (PA6, "ULTRAMID A3K" manufactured by BASF) was used instead of EVOH (A). The results are shown in Table 2.

[0129] [Table 1]

[0130] [Table 2]

Claims

1. A fuel pipe consisting of a double pipe having an inner pipe and an outer pipe disposed outside the inner pipe, the inner tube has a layer made of a resin composition containing an ethylene-vinyl alcohol copolymer (A) and an elastomer (B) and a layer made of polyethylene; the outer tube has a layer made of polyethylene; the thickness of the inner tube is 5 mm or more, and the ratio of the thickness of the layer made of the resin composition to the thickness of the inner tube (resin composition layer / inner tube) is 0.02 to 0.2; A fuel pipe, wherein the ratio of the thickness of the outer pipe to the thickness of the inner pipe (outer pipe / inner pipe) is 0.1 to 5.

2. 2. The fuel pipe according to claim 1, wherein the elastomer (B) is at least one selected from the group consisting of acrylic elastomers, olefin elastomers, urethane elastomers, styrene elastomers, and conjugated diene elastomers.

3. 3. The fuel pipe according to claim 1, wherein the resin composition contains multilayer structure polymer particles as the elastomer (B).

4. 4. The fuel pipe according to claim 3, wherein the average primary particle size of the multilayered polymer particles is 0.2 to 1 μm.

5. 5. The fuel pipe according to claim 3, wherein the multilayer structure polymer particles have an average secondary particle size of 1.1 to 10 μm.

6. 6. The fuel pipe according to claim 3, wherein the multi-layered polymer particle has at least an outermost layer and an innermost layer.

7. 7. The fuel pipe according to claim 6, wherein the polymer component constituting the outermost layer has a glass transition temperature of 30° C. or higher, and the polymer component constituting the innermost layer has a glass transition temperature of -10° C. or lower.

8. 8. The fuel pipe according to claim 1, wherein the ethylene-vinyl alcohol copolymer (A) has an ethylene content of 20 to 50 mol %.

9. 9. The fuel pipe according to claim 1, wherein a mass ratio (B / A) of the elastomer (B) to the ethylene-vinyl alcohol copolymer (A) is 1 / 99 to 40 / 60.

10. A fuel pipe for underground burial, comprising the fuel pipe according to any one of claims 1 to 9.

11. A method for transporting fuel, comprising transporting fuel using the fuel pipe according to any one of claims 1 to 9.

12. A fuel transportation method, comprising burying the fuel pipe according to claim 10 in the ground and then transporting fuel using the fuel pipe.

Citation Information

Patent Citations

  • Fuel container and fuel pipe

    JP1998024505A

  • Method for manufacturing molded product with excellent barrier property

    JP2002096016A

  • Piping for fuel oil

    JP2006062734A