Composite, method for producing composite, laminate, and method for producing laminate

A nitride sintered body impregnated with a semi-cured thermosetting composition addresses the challenge of achieving both adhesion and insulation in heat dissipation composites, providing effective thermal conductivity and insulation for electronic components.

JP7566727B2Active Publication Date: 2024-10-15DENKA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021511882
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-25
Publication Date
2024-10-15
Estimated Expiration
2040-03-25

AI Technical Summary

Technical Problem

Existing composites used in electronic components for heat dissipation, such as those in LED lighting devices and automotive power modules, face challenges in achieving both excellent adhesion and insulation properties.

Method used

A composite comprising a nitride sintered body with a porous structure impregnated by a semi-cured thermosetting composition, which is heated and pressurized under specific conditions to achieve a dielectric breakdown voltage of over 5 kV, enhancing adhesion and insulation.

Benefits of technology

The composite exhibits excellent adhesion and insulation properties, making it suitable for use in applications requiring thermal conductivity and insulation, such as power module structures and LED light emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566727000001
    Figure 0007566727000001
  • Figure 0007566727000002
    Figure 0007566727000002
  • Figure 0007566727000003
    Figure 0007566727000003
Patent Text Reader

Abstract

The present disclosure provides a composite comprising: a nitride sintered body having a porous structure; and a semi-cured product, of a thermosetting composition, impregnated in the nitride sintered body, wherein when the composite is disposed between adherends, then the composite is heated and pressurized for 5 minutes under the conditions of 200°C and 10 MPa and further heated for 2 hours under the conditions of 200°C and atmospheric pressure, and the dielectric breakdown voltage of the composite is greater than 5 kV.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a composite, a method for producing a composite, a laminate, and a method for producing a laminate. [Background technology]

[0002] In electronic components such as LED lighting devices and in-vehicle power modules, efficient dissipation of heat generated during use is an issue. To address this issue, measures have been taken, such as a method of increasing the thermal conductivity of the insulating layer of the printed wiring board on which the electronic components are mounted, and a method of attaching the electronic components or printed wiring board to a heat sink via electrically insulating thermal interface materials. For such insulating layers and thermal interface materials, composites (heat dissipation members) made of resin and ceramics such as boron nitride are used.

[0003] Conventionally, such composites have been made by dispersing ceramic powder in resin. In recent years, composites in which a porous ceramic sintered body (e.g., boron nitride sintered body) is impregnated with resin have also been studied (e.g., Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2014 / 196496 Summary of the Invention [Problem to be solved by the invention]

[0005] In the above-mentioned composite, there is still room for improvement in terms of achieving both adhesiveness and insulating properties.

[0006] An object of the present disclosure is to provide a composite material having excellent adhesion to an adherend and excellent insulating properties after adhesion to the adherend, and a method for producing the same. [Means for solving the problem]

[0007] One aspect of the present disclosure provides a composite comprising a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body, the composite having a dielectric breakdown voltage of more than 5 kV after being placed between adherends, heated and pressurized for 5 minutes under conditions of 200°C and 10 MPa, and further heated for 2 hours under conditions of 200°C and atmospheric pressure.

[0008] The composite has excellent adhesion to an adherend because it includes a semi-cured product of a thermosetting composition. The composite has a specific dielectric breakdown voltage when bonded under the above-mentioned conditions, and therefore has excellent insulating properties after bonding to the adherend.

[0009] The semi-cured product may have at least one structural unit selected from the group consisting of a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group. When the semi-cured product contains the specific structural unit, the insulating property and adhesiveness of the composite to an adherend can be improved.

[0010] The semi-cured product may contain at least one curing agent selected from the group consisting of phosphine-based curing agents and imidazole-based curing agents. When the semi-cured product contains the specific curing agent, the composite can be bonded to the adherend in a shorter time.

[0011] The content of the semi-cured material may be 20 to 70% by volume or less. When the content of the semi-cured material is within the above range, the semi-cured material can be appropriately present at the interface when adhering to the adherend, and the adhesiveness of the composite to the adherend can be improved. Furthermore, when the content of the semi-cured material is within the above range, the insulating properties after adhering to the adherend can be improved.

[0012] One aspect of the present disclosure is a method for producing a composite having a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body, the method comprising: impregnating a nitride sintered body having a porous structure with a thermosetting composition; and heating the thermosetting composition to a heating temperature of 80 to 130 ° C. to semi-cure the composition. The impregnation step is a step of impregnating the thermosetting composition with a temperature higher than the heating temperature and not higher than the heating temperature + 20 ° C. The thermosetting composition is at least one compound selected from the group consisting of a compound having a cyanate group, a compound having a bismaleimide group, and a compound having an epoxy group, and at least one curing agent selected from the group consisting of a phosphine-based curing agent and an imidazole-based curing agent. The method for producing a composite is provided.

[0013] The method for producing the composite includes a step of impregnating a nitride sintered body having a porous structure with a thermosetting composition and a step of semi-curing the thermosetting composition, and the composite can be easily produced by impregnating the nitride sintered body with the thermosetting composition and then curing it. In addition, the obtained composite has excellent adhesion to the adherend since it includes a semi-cured product of the thermosetting composition. The composite has a specific dielectric breakdown voltage in adhesion under the above-mentioned conditions, and therefore has excellent insulation properties after adhesion to the adherend.

[0014] One aspect of the present disclosure provides a laminate comprising a first metal substrate, an intermediate layer, and a second metal substrate in this order, the first metal substrate and the second metal substrate being bonded together by the intermediate layer, and the intermediate layer being a cured product of the above-mentioned composite.

[0015] The laminate has an intermediate layer made of the cured product of the above-mentioned composite, and therefore has excellent adhesion to the first metal substrate and the second metal substrate, and has excellent insulating properties after bonding.

[0016] One aspect of the present disclosure provides a method for producing a laminate comprising a first metal substrate, an intermediate layer, and a second metal substrate in this order, the method comprising the steps of arranging the first metal substrate, the composite described above, and the second metal substrate in this order, and applying heat and pressure to harden the composite and form the intermediate layer.

[0017] The manufacturing method of the above laminate uses the above-mentioned composite as an intermediate layer, and therefore can provide a laminate that has excellent adhesion to the first metal substrate and the second metal substrate and has excellent insulating properties after bonding. Effect of the Invention

[0018] According to the present disclosure, it is possible to provide a composite material having excellent adhesion to an adherend and excellent insulating properties after adhesion to the adherend, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are merely examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents.

[0020] One embodiment of the composite is a composite including a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body. The composite has a dielectric breakdown voltage of more than 5 kV after the composite is placed between adherends, heated and pressurized for 5 minutes under conditions of 200°C and 10 MPa, and further heated for 2 hours under conditions of 200°C and atmospheric pressure.

[0021] In this specification, the "semi-cured" (also called B stage) state means that the material is in a state in which it can be further cured by a subsequent curing treatment. The material can be temporarily pressed onto an adherend by utilizing the semi-cured state, and then heated to adhere to the adherend. The semi-cured material is in a semi-cured state, and can be made into a "completely cured" (also called C stage) state by further curing treatment. Whether or not the semi-cured material in the composite is in a semi-cured state in which it can be further cured can be confirmed, for example, by a differential scanning calorimeter.

[0022] The composite is capable of adhering to an adherend since it comprises a semi-cured product of the thermosetting composition impregnated in the nitride sintered body. The composite comprises a nitride sintered body, and the pores of the nitride sintered body are filled with the semi-cured product of the thermosetting composition, so that the composite has a relatively high breakdown voltage and excellent insulation after adhering to the adherend. The composite also comprises a nitride sintered body, so that the thermal resistance is relatively low and the composite has excellent thermal conductivity. The composite of this embodiment is useful as an adhesive member (e.g., adhesive sheet, etc.) that requires thermal conductivity and insulation. Specifically, the composite of this embodiment can be used as an adhesive member that adheres a metal circuit board to other layers in a power module structure, an LED light emitting device, etc.

[0023] The shape of the composite may be, for example, a block shape, a sheet shape, or the like. When the composite is in a sheet shape, the thickness of the composite may be, for example, 0.1 mm or more, 0.2 mm or more, or 0.3 mm or more. When the thickness of the composite is within the above range, the insulation properties can be maintained even when used in applications where high voltage is applied. When the composite is in a sheet shape, the thickness of the composite may be, for example, 1.0 mm or less, 0.7 mm or less, or 0.4 mm or less. When the thickness of the composite is within the above range, the thermal resistance can be made smaller.

[0024] The nitride sintered body having a porous structure may be one in which primary particles of a nitride are sintered together. In this specification, the term "porous structure" refers to a structure having a plurality of fine holes (hereinafter also referred to as pores), and includes a structure in which at least a part of the pores are connected to form continuous pores. The average pore diameter of the pores may be, for example, 7 μm or less, 6 μm or less, or 5 μm or less. When the average pore diameter is within the above range, the thermal conductivity of the composite can be improved. The average pore diameter of the pores may be, for example, 0.3 μm or more, 0.5 μm or more, or 0.7 μm or more. When the average pore diameter is within the above range, the thermosetting composition can be easily filled into the pores, and the adhesiveness of the composite to the adherend can be further improved. In this specification, the "average pore diameter" refers to a value measured by mercury intrusion porosimetry.

[0025] A semi-cured product of a thermosetting composition (hereinafter, sometimes simply referred to as a "semi-cured product") means a product in which the curing reaction of the thermosetting composition has progressed to a certain degree, as described below. Therefore, the semi-cured product of a thermosetting composition may contain a thermosetting resin obtained by reaction of raw material components in the thermosetting composition (compounds contained in the thermosetting composition, etc.). The semi-cured product may contain, in addition to the thermosetting resin, unreacted compounds of the raw material components.

[0026] The semi-cured product of the thermosetting composition may have, for example, at least one structural unit selected from the group consisting of a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group, or may have at least two structural units selected from the group consisting of a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group, or may have a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group. By having the semi-cured product of the thermosetting composition have a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group, the production of the composite is facilitated and the adhesion between the composite and the adherend can be further improved.

[0027] The semi-cured product may have, for example, a structural unit derived from a cyanate group, a structural unit derived from a cyanate group, and at least one structural unit selected from the group consisting of a structural unit derived from a bismaleimide group and a structural unit derived from an epoxy group, or may have all of the structural units derived from a cyanate group, the structural units derived from a bismaleimide group, and the structural units derived from an epoxy group. By containing a certain amount or more of these structural units, the dielectric breakdown voltage described below can be further improved. When the semi-cured product has all of the structural units derived from a cyanate group, the structural units derived from a bismaleimide group, and the structural units derived from an epoxy group, it can exhibit excellent dielectric breakdown voltage even when the content of the semi-cured product in the composite is small.

[0028] An example of a structural unit having a cyanate group is a urethane bond (-NH-CO-). An example of a structural unit derived from a bismaleimide group is a structure represented by the following formula (1). An example of a structural unit derived from an epoxy group is a structure represented by the following general formula (2). These structural units are: 1 H-NMR and 13 It can be detected by using C-NMR. It can also be detected by using GPC (gel permeation chromatography). The above-mentioned structural units can be detected by either NMR or GPC.

[0029] [ka]

[0030] [ka]

[0031] In the above general formula (2), R 1 represents a hydrogen atom or another functional group. The other functional group may be, for example, an alkyl group.

[0032] The semi-cured product may have a structural unit other than the structural unit derived from a cyanate group, the structural unit derived from a bismaleimide group, and the structural unit derived from an epoxy group.

[0033] The semi-cured product may contain a thermosetting resin, or may contain at least one resin selected from the group consisting of a cyanate resin, a bismaleimide resin, and an epoxy resin. In addition to the thermosetting resin, the semi-cured product may contain, for example, a phenol resin, a melamine resin, a urea resin, an alkyd resin, etc.

[0034] The semi-cured product may contain at least one curing agent selected from the group consisting of phosphine-based curing agents and imidazole-based curing agents. The phosphine-based curing agent may promote a triazine-producing reaction by trimerization of a compound having a cyanate group. Examples of the phosphine-based curing agent include tetraphenylphosphonium tetra-p-tolylborate. The imidazole-based curing agent produces oxazoline and promotes the curing reaction of a compound having an epoxy group. Examples of the imidazole-based curing agent include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole. The semi-cured product may be a cured product formed by curing a polymerizable compound (e.g., a compound having a cyanate group, a compound having an epoxy group, etc.) contained in the thermosetting composition with these curing agents.

[0035] The degree of curing of the semi-cured product may be, for example, the curing rate of the thermosetting composition, where the curing rate when the product is completely cured is 100%. The curing rate of the semi-cured product may be, for example, 70% or less, 65% or less, or 60% or less. When the curing rate of the semi-cured product is within the above range, the adhesiveness of the composite to the adherend can be improved. Furthermore, the semi-cured product moves within the resin composite, filling voids within the resin composite and improving the dielectric breakdown voltage. Furthermore, the curing rate of the resin semi-cured product may be, for example, 5% or more, 15% or more, 30% or more, or 40% or more. When the curing rate of the semi-cured product is within the above range, the semi-cured product is prevented from flowing out of the resin composite, and the semi-cured product can be sufficiently retained within the pores of the nitride sintered body.

[0036] The above-mentioned curing rate can be determined by measurement using a differential scanning calorimeter. First, the amount of heat Q generated when 1 g of the uncured thermosetting composition is completely cured is measured. Next, 1 g of a semi-cured product is sampled from the composite to be measured, and the amount of heat R generated when the sampled semi-cured product is completely cured is measured. A differential scanning calorimeter is used for the measurement. Then, the curing rate of the semi-cured product can be calculated according to the following formula (A). Whether or not the semi-cured product is completely cured can be confirmed by the end of heat generation in the heat generation curve obtained by differential scanning calorimetry.

[0037] Cure rate of semi-cured material [%] = [(QR) / R] × 100 (A)

[0038] The curing rate may be calculated as follows. That is, the curing rate of the semi-cured material impregnated in the nitride sintered body can be obtained by the following method. First, the amount of heat Q2 generated when the uncured thermosetting composition is heated and completely cured is obtained. Then, the amount of heat R2 generated when a sample taken from the semi-cured material included in the composite is heated in the same manner and completely cured is obtained. At this time, the mass of the sample used for the measurement by the differential scanning calorimeter is the same as that of the thermosetting composition used for measuring the amount of heat Q2. If the semi-cured material contains c (mass%) of a thermosetting component, the curing rate of the thermosetting composition impregnated in the composite can be obtained by the following formula (B).

[0039] Cure rate of impregnated semi-cured material (%) = {1 - [(R2 / c) × 100] / Q2} × 100 (B)

[0040] The content of the semi-cured product may be, for example, 20% by volume or more, 25% by volume or more, 30% by volume or more, 35% by volume or more, or 40% by volume or more based on the composite. When the content of the thermosetting composition is within the above range, the adhesiveness can be further improved when the product is bonded to an adherend by heating and pressing. The content of the thermosetting composition may be, for example, 70% by volume or less, 65% by volume or less, 60% by volume or less, or 55% by volume or less based on the composite. When the content of the thermosetting composition is within the above range, the adhesiveness and the insulating property of the composite can be compatible at a higher level. In addition, when the content of the thermosetting composition is within the above range, the decrease in the heat dissipation property of the laminate obtained using the composite can be sufficiently suppressed. The content of the thermosetting composition can be adjusted within the above range, and may be, for example, 20 to 70% by volume. The content of the semi-cured product is obtained by heating the resin composite at about 600°C to volatilize the semi-cured product, and measuring the weight difference before and after the volatilization.

[0041] The content of the thermosetting composition in the composite can be regarded as the porosity of the nitride sintered body, and can be calculated from the following formula (C). The true density of the nitride sintered body is, for example, 2.28 g / cm for boron nitride. 3 It is.

[0042] Content of thermosetting composition [volume %] = porosity of nitride sintered body = [1-(D / true density of nitride sintered body)] (C)

[0043] In the above formula (C), D means the bulk density of the nitride sintered body represented by the following formula (D).

[0044] Bulk density of sintered nitride [g / cm 3 ] = mass of sintered nitride compact / volume of sintered nitride compact (D)

[0045] In the above formula (C), when the nitride sintered body is obtained from a plurality of nitrides, the true density of each nitride is multiplied by the compounding ratio (mass ratio) of each nitride. For example, when nitride A and nitride B are mixed in a mass ratio of a:b, the true density of the nitride sintered body is calculated by the following formula (D).

[0046] True density of sintered nitride body [g / cm 3 ]=(A×a+B×b)÷(a+b)···(D)

[0047] The adhesiveness of the composite can be evaluated using as an index the cohesive failure area ratio (area %) at the peeled surface when a sample is peeled according to JIS K 6854-1:1999 "Adhesive-Peel Adhesion Strength Test Method." The cohesive failure area ratio at the peeled surface of the composite can be, for example, 40 area % or more, 50 area % or more, or 60 area % or more relative to the total area of ​​the adhesive surface of the adherend.

[0048] The dielectric breakdown voltage between the adherends after the adhesion of the composite is, for example, more than 5 kV, and can be 5.5 kV or more, 6 kV or more. The dielectric breakdown voltage between the adherends after the adhesion of the composite may be, for example, 12 kV or less, or 10 kV or less. The dielectric breakdown voltage of the composite can be adjusted, for example, by the composition of the thermosetting composition and the content of the semi-cured material. In this specification, the "dielectric breakdown voltage" means a value measured by a voltage tester (manufactured by Kikusui Electronics Co., Ltd., device name: TOS-8700) according to JIS C2110-1:2016.

[0049] The test specimen used for measuring the breakdown voltage is prepared by the following method. First, the composite is placed between two copper plates, heated and pressurized for 5 minutes under conditions of 200°C and 10 MPa, and further heated for 2 hours under conditions of 200°C and atmospheric pressure to prepare a laminate. Pressure is applied between the two copper plates and in the lamination direction of the composite. An etching resist agent is screen-printed on one side of the laminate so as to form a circle with a diameter of 20 mm, and an etching resist agent is screen-printed on the entire surface (so-called solid pattern) of the other side of the laminate. After printing, the etching resist agent is irradiated with ultraviolet light to harden it and form a resist. After forming the resist, the copper plate on the side on which the circular resist is formed is etched with cupric chloride solution to form a circular copper circuit with a diameter of 20 mm on one side of the laminate. The laminate on which the circular copper circuit is formed is the measurement target.

[0050] The thermal resistance of the composite after adhesion can be, for example, 0.50 K / W or less, 0.40 K / W or less, 0.37 K / W or less, or 0.35 K / W or less. The thermal resistance of the composite can be adjusted, for example, by the composition of the thermosetting composition, the content of the semi-cured material, and the density of the nitride sintered body. In this specification, the term "thermal resistance" refers to a value measured by a resin material thermal resistance measuring device (manufactured by Hitachi Technology and Services Co., Ltd.) in accordance with ASTM D5470. The thermal resistance measurement is performed by placing the composite between two copper plates (both copper plates having a thickness of 1 mm), heating and pressing the composite for 5 minutes under conditions of 200°C and 10 MPa, and further heating the composite for 2 hours under conditions of 200°C and atmospheric pressure, to obtain a laminate as the measurement object.

[0051] The above-mentioned composite can be manufactured, for example, by the following manufacturing method. One embodiment of the manufacturing method of the composite is a manufacturing method of a composite having a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body, and includes a step of impregnating the nitride sintered body having a porous structure with the thermosetting composition (hereinafter also referred to as an impregnation step), and a step of heating the thermosetting composition to a heating temperature of 80 to 130 ° C. to semi-cure the composition (hereinafter also referred to as a semi-curing step). The impregnation step is a step of impregnating the thermosetting composition by setting the temperature of the thermosetting composition to be higher than the heating temperature in the semi-curing step and not higher than the heating temperature + 20 ° C. The thermosetting composition contains at least one compound selected from the group consisting of a compound having a cyanate group, a compound having a bismaleimide group, and a compound having an epoxy group, and at least one curing agent selected from the group consisting of a phosphine-based curing agent and an imidazole-based curing agent.

[0052] The nitride sintered body having a porous structure may be one obtained by sintering primary particles of a nitride. The nitride sintered body having a porous structure may be a commercially available nitride sintered body, or may be one prepared by sintering a powder containing a nitride. That is, the method for producing a composite may include a step of sintering a powder containing a nitride (hereinafter also referred to as a nitride powder) to obtain a nitride sintered body having a porous structure. The nitride sintered body may be prepared by subjecting a slurry containing a nitride powder to a spheroidizing treatment using a spray dryer or the like, further molding the slurry, and then sintering the slurry. A mold may be used for molding, or a cold isostatic pressing (CIP) method may be used.

[0053] The nitride may contain at least one nitride selected from the group consisting of boron nitride, aluminum nitride, and silicon nitride, and preferably contains boron nitride. As the boron nitride, either amorphous boron nitride or hexagonal boron nitride can be used. The thermal conductivity of the nitride may be, for example, 40 W / (m·K) or more, 50 W / (m·K) or more, or 60 W / (m·K) or more. When the nitride having excellent thermal conductivity as described above is used as the nitride, the thermal resistance of the obtained composite can be further reduced.

[0054] A sintering aid may be used when sintering the nitride powder. The sintering aid may be, for example, an oxide of a rare earth element such as yttria oxide, alumina oxide, or magnesium oxide, an alkali metal carbonate such as lithium carbonate or sodium carbonate, or boric acid. When a sintering aid is blended, the amount of the sintering aid added may be, for example, 0.01 parts by mass or more or 0.1 parts by mass or more relative to 100 parts by mass of the total of the nitride and the sintering aid. The amount of the sintering aid added may be, for example, 20 parts by mass or less, 15 parts by mass or less, or 10 parts by mass or less relative to 100 parts by mass of the total of the nitride and the sintering aid. By setting the amount of the sintering aid added within the above range, it becomes easy to adjust the average pore size of the nitride sintered body to the above range.

[0055] The sintering temperature of the nitride may be, for example, 1600° C. or more or 1700° C. or more. The sintering temperature of the nitride may be, for example, 2200° C. or less or 2000° C. or less. The sintering time of the nitride may be, for example, 1 hour or more and 30 hours or less. The sintering atmosphere may be, for example, an inert gas atmosphere such as nitrogen, helium, and argon.

[0056] For the sintering, for example, a batch furnace or a continuous furnace can be used. Examples of the batch furnace include a muffle furnace, a tubular furnace, and an atmosphere furnace. Examples of the continuous furnace include a rotary kiln, a screw conveyor furnace, a tunnel furnace, a belt furnace, a pusher furnace, and a koto-shaped continuous furnace.

[0057] Before the impregnation step, the nitride sintered body may be shaped, for example, by cutting into a desired shape and thickness, if necessary.

[0058] In the impregnation step, a solution containing a thermosetting composition is prepared in an impregnation device, and the nitride sintered body is immersed in the solution to impregnate the pores of the nitride sintered body with the thermosetting composition. The solution containing the thermosetting composition may contain a solvent in addition to the thermosetting composition, or may contain only the thermosetting composition. Examples of the solvent include aliphatic alcohols, ether alcohols, glycol ethers, ketones, and hydrocarbons.

[0059] The thermosetting composition contains at least one compound selected from the group consisting of a compound having a cyanate group, a compound having a bismaleimide group, and a compound having an epoxy group, and at least one curing agent selected from the group consisting of a phosphine-based curing agent and an imidazole-based curing agent.

[0060] Examples of the compound having a cyanate group include dimethylmethylenebis(1,4-phenylene)biscyanate and bis(4-cyanatephenyl)methane. Dimethylmethylenebis(1,4-phenylene)biscyanate is commercially available as, for example, TACN (trade name, manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0061] Examples of compounds having a bismaleimide group include N,N'-[(1-methylethylidene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide and 4,4'-diphenylmethane bismaleimide. N,N'-[(1-methylethylidene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide is commercially available as, for example, BMI-80 (trade name, manufactured by K.I. Chemicals Co., Ltd.).

[0062] Examples of the compound having an epoxy group include 1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene and a compound represented by the following general formula (3). In general formula (3), the value of n is not particularly limited, but can be an integer of 0 or 1 or more, and is usually 1 to 10, and preferably 2 to 5. 1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene is commercially available, for example, as HP-4032D (trade name, manufactured by DIC Corporation).

[0063] [ka]

[0064] In the thermosetting composition, the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group may be 50 mass% or more, 70 mass% or more, 80 mass% or more, or 90 mass% or more, based on the total amount of the thermosetting composition.

[0065] The content of the compound having a cyanate group in the thermosetting composition may be, for example, 50 parts by mass or more, 60 parts by mass or more, or 70 parts by mass or more, based on 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. When the content of the compound having a cyanate group in the thermosetting composition is within the above range, the curing reaction when adhering the obtained composite to the adherend proceeds quickly, and the dielectric breakdown voltage after adhesion to the adherend is superior. When the adhesion conditions to the adherend are the adhesion conditions in the examples, the effect of improving the dielectric breakdown voltage can be more remarkable.

[0066] The content of the compound having a bismaleimide group in the thermosetting composition may be, for example, 15 parts by mass or more, 20 parts by mass or more, or 25 parts by mass or more, relative to 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. When the content of the compound having a bismaleimide group in the thermosetting composition is within the above range, the water absorption rate of the semi-cured product is reduced, and the reliability of the product can be improved.

[0067] The content of the compound having an epoxy group in the thermosetting composition may be, for example, 10 parts by mass or more, 20 parts by mass or more, or 30 parts by mass or more, based on 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. The content of the compound having an epoxy group in the thermosetting composition may be, for example, 70 parts by mass or less, or 60 parts by mass or less, based on 100 parts by mass of the total amount of the compound having a cyanate group and the compound having a bismaleimide group. When the content of the compound having an epoxy group in the thermosetting composition is within the above range, the decrease in the heat curing initiation temperature of the thermosetting composition can be suppressed, and it becomes easier to impregnate the nitride sintered body with the thermosetting composition.

[0068] The curing agent may include a phosphine-based curing agent and an imidazole-based curing agent.

[0069] Phosphine-based curing agents can promote the triazine-producing reaction by trimerization of a compound having a cyanate group or a cyanate resin. Examples of phosphine-based curing agents include tetraphenylphosphonium tetra-p-tolylborate and tetraphenylphosphonium tetraphenylborate. Tetraphenylphosphonium tetra-p-tolylborate is commercially available as, for example, TPP-MK (trade name, manufactured by Hokko Chemical Industry Co., Ltd.).

[0070] Imidazole-based curing agents generate oxazoline and promote the curing reaction of compounds having epoxy groups or epoxy resins. Examples of imidazole-based curing agents include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole and 2-ethyl-4-methylimidazole. 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole is commercially available, for example, as 2E4MZ-CN (manufactured by Shikoku Chemical Industry Co., Ltd., trade name).

[0071] The content of the phosphine-based curing agent may be, for example, 5 parts by mass or less, 4 parts by mass or less, or 3 parts by mass or less, based on 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. The content of the phosphine-based curing agent may be, for example, 0.1 parts by mass or more, or 0.5 parts by mass or more, based on 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. When the content of the phosphine-based curing agent is within the above range, the production of the composite is easy, and the time required for adhesion of the adherend using the composite can be further shortened.

[0072] The content of the imidazole-based curing agent may be, for example, 0.1 parts by mass or less, 0.05 parts by mass or less, or 0.03 parts by mass or less, based on 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. The content of the imidazole-based curing agent may be, for example, 0.001 parts by mass or more, or 0.005 parts by mass or more, based on 100 parts by mass of the total amount of the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group. When the content of the imidazole-based curing agent is within the above range, the production of the composite is easy, and the time required for adhesion of the adherend using the composite can be further shortened.

[0073] The thermosetting composition may contain other components other than the compound having a cyanate group, the compound having a bismaleimide group, and the compound having an epoxy group, as well as the curing agent. The other components may further contain, for example, other resins such as phenolic resins, melamine resins, urea resins, and alkyd resins, silane coupling agents, leveling agents, defoamers, surface conditioners, and wetting and dispersing agents. The content of these other components may be 20% by mass or less, 10% by mass or less, or 5% by mass or less, based on the total amount of the thermosetting composition.

[0074] The viscosity of the solution containing the thermosetting composition at 100°C may be 50 mPa·s or less, 30 mPa·s or less, 20 mPa·s or less, 10 mPa·s or less, or 5 mPa·s. When the viscosity of the solution at 150°C is within the above range, the preparation of the composite is easier. The viscosity of the solution at 100°C may be 3 mPa·s or more. The viscosity of the solution at 100°C is preferably kept at 50 mPa·s or less for 5 hours or more while maintaining the temperature of the solution at 100°C. The viscosity of the solution at 100°C means a value measured using a rotational viscometer under the condition of a shear rate of 10 (1 / sec).

[0075] The impregnation step may be performed under reduced pressure or under pressurized conditions, or may be performed by combining impregnation under reduced pressure and impregnation under pressurized conditions. When the impregnation step is performed under reduced pressure, the pressure in the impregnation device may be, for example, 1000 Pa or less, 500 Pa or less, 100 Pa or less, 50 Pa or less, or 20 Pa or less. When the impregnation step is performed under pressurized conditions, the pressure in the impregnation device may be, for example, 1 MPa or more, 3 MPa or more, 10 MPa or more, or 30 MPa or more.

[0076] In the impregnation step, the solution containing the thermosetting composition is heated. By heating the solution within the following temperature range, the viscosity of the solution is adjusted and the impregnation of the resin is promoted, resulting in an excellent composite. The temperature to which the solution is heated is higher than the heating temperature for semi-curing. The upper limit of the temperature to which the solution is heated is equal to or lower than the heating temperature for semi-curing + 20°C.

[0077] In the impregnation step, the nitride sintered body is immersed in a solution containing a thermosetting composition and held for a predetermined time, which may be, for example, 5 hours or more, 10 hours or more, 100 hours, or 150 hours or more.

[0078] The semi-curing step is a step of heating the thermosetting composition impregnated in the nitride sintered body to semi-cure it. The semi-curing step allows the semi-cured state of the thermosetting composition in the composite to be adjusted. The heating temperature in this step is 80 to 130°C.

[0079] The semi-cured product obtained by the semi-curing step may contain at least one thermosetting resin selected from the group consisting of cyanate resins, bismaleimide resins, and epoxy resins, and a curing agent. In addition to the above-mentioned thermosetting resins and curing agents, the semi-cured product may contain other resins such as phenolic resins, melamine resins, urea resins, and alkyd resins, as well as components derived from silane coupling agents, leveling agents, defoamers, surface conditioners, and wetting and dispersing agents. The total content of the other resins and components may be 20% by mass or less, 10% by mass or less, or 5% by mass or less based on the total amount of the semi-cured product.

[0080] In the above embodiment, the impregnation step and the semi-curing step are described as separate steps. In another embodiment, the two steps do not necessarily have to be distinguishable from each other, and each step may have the desired effect. That is, the heating conditions may be adjusted during the impregnation step to semi-cure the thermosetting composition impregnated in the nitride sintered body. From the viewpoint of sufficiently impregnating the nitride sintered body with the thermosetting composition, it is preferable to provide the impregnation step and the semi-curing step separately.

[0081] The above-mentioned composite can be used, for example, to manufacture a laminate such as a thermally conductive adhesive sheet. One embodiment of the laminate, for example, comprises a first metal substrate, an intermediate layer, and a second metal substrate in this order. The first metal substrate and the second metal substrate are bonded by the intermediate layer, and the intermediate layer is a cured product of the above-mentioned composite.

[0082] The first metal substrate and the second metal substrate may be the same metal substrate or may be different metal substrates. The first metal substrate and the second metal substrate may be, for example, copper, aluminum, etc. The thickness of the first metal substrate and the second metal substrate may be, for example, 0.035 mm or more or 10 mm or less, independently of each other. The first metal substrate and the second metal substrate may form, for example, a circuit.

[0083] The above-mentioned laminate can be manufactured, for example, by the following method. One embodiment of the method for manufacturing a laminate is a method for manufacturing a laminate including a first metal substrate, an intermediate layer, and a second metal substrate in this order, and includes a step of arranging the first metal substrate, the above-mentioned composite, and the second metal substrate in this order, and applying heat and pressure to harden the composite to form the intermediate layer.

[0084] In the method for producing the laminate, since the composite is used, the first metal substrate and the second metal substrate can be bonded together in a short time, and the bonding time can be 2 hours or less, 1 hour or less, or 0.5 hours or less.

[0085] From the viewpoint of reducing the energy required for manufacturing the power module structure and the LED light emitting device, there is a demand for shortening the bonding time required for manufacturing the power module structure and the LED light emitting device, particularly for bonding the metal circuit and the metal fin for heat dissipation. In order to shorten the above-mentioned bonding time using a composite in which a conventional porous ceramic sintered body is impregnated with a resin, for example, a method of manufacturing an adhesive sheet in which the polymerization degree of the resin is increased in advance is considered. However, in this method, it becomes difficult to impregnate the ceramic sintered body with the resin due to the increase in the solution viscosity accompanying the increase in the polymerization degree of the resin. As a result, it is not possible to impregnate a sufficient amount of resin, and there is a risk that the adhesiveness and insulating properties of the resulting composite will be insufficient.

[0086] Compared with conventional composites, the composite of the present disclosure can be selected such that the breakdown voltage exceeds 5 kV when cured under specific conditions, thereby shortening the bonding time required for bonding, for example, a metal circuit and a metal fin for heat dissipation. When the composite of the present disclosure is produced using a specific thermosetting composition, the production of the composite becomes easier and the bonding time with the adherend can be shortened. By using a combination of a specific thermosetting resin and a specific curing agent, the conditions for impregnating the nitride sintered body with the thermosetting composition can be made relatively mild, and the curing time for the obtained composite to be brought to the C stage can be shortened even if the impregnation is performed under a condition where the viscosity of the solution is low.

[0087] Although several embodiments have been described above, the present disclosure is not limited to the above-described embodiments. In addition, the descriptions of the above-described embodiments can be mutually applied. EXAMPLES

[0088] The present disclosure will be described in more detail below with reference to examples and comparative examples. However, the present disclosure is not limited to the following examples.

[0089] Example 1 [Preparation of nitride sintered bodies with porous structures] Amorphous boron nitride powder (manufactured by Denka Company Limited, oxygen content: 1.5%, boron nitride purity: 97.6%, average particle size: 6.0 μm) was weighed out to a container so that the content was 40.0 mass%, and hexagonal boron nitride powder (manufactured by Denka Company Limited, oxygen content: 0.3%, boron nitride purity: 99.0%, average particle size: 30.0 μm) was 60.0 mass%. Sintering aids (boric acid, calcium carbonate) were added, followed by the addition of an organic binder and water, which were then mixed. The mixture was then dried and granulated to prepare a nitride mixed powder.

[0090] The mixed powder was filled into a mold and press molded at a pressure of 5 MPa to obtain a molded body. Next, the molded body was compressed at a pressure of 20 to 100 MPa using a cold isostatic pressing (CIP) device (manufactured by Kobe Steel, Ltd., product name: ADW800). The compressed molded body was sintered at 2000°C for 10 hours using a batch-type high-frequency furnace (manufactured by Fuji Electric Industrial Co., Ltd., product name: FTH-300-1H) to prepare a nitride sintered body. The sintering was performed by flowing nitrogen into the furnace at a flow rate of 10 L / min under standard conditions, while adjusting the inside of the furnace to a nitrogen atmosphere.

[0091] [Preparation of Thermosetting Composition] 80 parts by mass of a compound having a cyanate group, 20 parts by mass of a compound having a bismaleimide group, and 50 parts by mass of a compound having an epoxy group were weighed out and placed in a container, and 1 part by mass of a phosphine-based curing agent and 0.01 part by mass of an imidazole-based curing agent were added to a container for a total of 100 parts by mass of the above three compounds, and mixed. Since the epoxy resin was in a solid state at room temperature, it was mixed while heated to about 80°C. The viscosity of the obtained thermosetting composition at 100°C was 10 mPa·s.

[0092] The following compounds were used in preparing the thermosetting compositions:

[0093] <Compounds with specific functional groups> Compound having a cyanate group: dimethylmethylenebis(1,4-phenylene)biscyanate (manufactured by Mitsubishi Gas Chemical Company, Inc., product name: TA-CN) Compound having a bismaleimide group: N,N'-[(1-methylethylidene)bis[(p-phenylene)oxy(p-phenylene)]]bismaleimide (manufactured by K.I. Chemicals Co., Ltd., product name: BMI-80) Compound having an epoxy group: 1,6-bis(2,3-epoxypropan-1-yloxy)naphthalene (manufactured by DIC Corporation, product name: HP-4032D) Compound having a benzoxazine group: Bisphenol F-type benzoxazine (manufactured by Shikoku Chemical Industry Co., Ltd., product name: Fa-type benzoxazine)

[0094] <Hardening agent> Phosphine-based curing agent: Tetraphenylphosphonium tetra-p-tolylborate (manufactured by Kagaku Co., Ltd., product name: TPP-MK) Imidazole curing agent: 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole (manufactured by Shikoku Chemical Industry Co., Ltd., product name: 2E4MZ-CN) Metal catalyst: bis(2,4-pentanedionato)zinc(II) (Tokyo Chemical Industry Co., Ltd.)

[0095] [Preparation of the complex] The nitride sintered body prepared as described above was impregnated with the thermosetting composition prepared as described above by the following method. First, the nitride sintered body and the thermosetting composition contained in a container were placed in a vacuum heating impregnation device (manufactured by Kyoshin Engineering Co., Ltd., product name: G-555AT-R). Next, the inside of the device was degassed for 10 minutes under conditions of temperature: 100°C and pressure: 15 Pa. After degassing, while maintaining the same conditions, the nitride sintered body was immersed in the thermosetting composition for 40 minutes, and the thermosetting composition was impregnated into the nitride sintered body.

[0096] Thereafter, the container containing the nitride sintered body and the thermosetting composition was taken out and placed in a pressurized heating impregnation device (manufactured by Kyoshin Engineering Co., Ltd., product name: HP-4030AA-H45), and held for 120 minutes under conditions of temperature: 130°C and pressure: 3.5 MPa, thereby further impregnating the nitride sintered body with the thermosetting composition. Thereafter, the nitride sintered body was taken out of the device and heated for 8 hours under conditions of temperature: 120°C and atmospheric pressure, thereby semi-curing the thermosetting composition to prepare a composite. The content of the semi-cured material was 25 to 68% by volume.

[0097] [Measurement of dielectric breakdown voltage] The composite obtained as described above was placed between two copper plates, heated and pressed for 5 minutes under conditions of 200°C and 10 MPa, and further heated for 2 hours under conditions of 200°C and atmospheric pressure to prepare a laminate. An etching resist agent was screen-printed on one side of the obtained laminate so as to have a circular shape with a diameter of 20 mm, and an etching resist agent was screen-printed on the entire surface of the other side of the laminate. After printing, the etching resist agent was irradiated with ultraviolet light to harden it and form a resist. Next, the copper plate on the side on which the circular resist was formed was etched with a cupric chloride solution, and a circular copper circuit with a diameter of 20 mm was formed on one side of the laminate. In this way, the laminate on which the circular copper circuit was formed, which was the measurement target, was obtained. The dielectric breakdown voltage was measured for the obtained laminate using a voltage tester (manufactured by Kikusui Electronics Co., Ltd., device name: TOS-8700) according to JIS C2110-1:2016. From the measurement results, the insulation was evaluated according to the following criteria. The results are shown in Table 1. A: Dielectric breakdown voltage is 10kV or more B: Breakdown voltage is 5 kV or more and less than 10 kV C: Breakdown voltage is less than 5 kV

[0098] [Evaluation of 90° peelability and adhesion] The composite obtained as described above was placed between two copper plates, heated and pressed at 200°C and 10 MPa for 5 minutes, and further heated at 200°C and atmospheric pressure for 2 hours to prepare a laminate, which was used as the measurement subject. A 90° peel test was performed according to JIS K 6854-1:1999 "Adhesive-Peel Adhesion Strength Test Method" to measure the area of ​​the cohesive failure portion. From the measurement results, the adhesion was evaluated according to the following criteria. The results are shown in Table 1. A: The area of ​​the cohesive failure part is 70% or more B: The area of ​​the cohesive failure portion is 30% or more and less than 70%. C: The area of ​​the cohesive failure portion is less than 30%.

[0099] [Measurement of thermal resistance and evaluation of heat dissipation] The composite obtained as described above was placed between two copper plates, heated and pressed at 200°C and 10 MPa for 5 minutes, and further heated at 200°C and atmospheric pressure for 2 hours to prepare a laminate, which was used as the measurement subject. Thermal resistance was measured according to ASTM-D5470. From the measurement results, heat dissipation was evaluated according to the following criteria. The results are shown in Table 1. A: Thermal resistance is less than 0.40K / W B: Thermal resistance is 0.40K / W or more and less than 0.50K / W C: Thermal resistance is 0.50K / W or more

[0100] (Examples 2 to 7, Comparative Examples 1 to 3) Composites were prepared in the same manner as in Example 1, except that the types and blending ratios of the compound having a specific functional group and the curing agent, and the content of the semi-cured product were changed as shown in Table 1, and the dielectric breakdown voltage, insulating properties, 90° peelability, adhesion, thermal resistance, and heat dissipation properties were evaluated.

[0101] [Table 1] [Industrial Applicability]

[0102] According to the present disclosure, it is possible to provide a composite material having excellent adhesion to an adherend and excellent insulating properties after adhesion to the adherend, and a method for producing the same.

Claims

1. A composite body comprising a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body, the semi-cured product has a structural unit derived from a cyanate group, a structural unit derived from a bismaleimide group, and a structural unit derived from an epoxy group, The composite has a dielectric breakdown voltage of more than 5 kV after the composite is placed between adherends, heated and pressed at 200°C and 10 MPa for 5 minutes, and further heated at 200°C and atmospheric pressure for 2 hours.

2. The composite according to claim 1 , wherein the semi-cured product contains at least one curing agent selected from the group consisting of a phosphine-based curing agent and an imidazole-based curing agent.

3. The composite according to claim 1 or 2, wherein the content of the semi-cured product is 20 to 70 volume %.

4. A method for producing a composite having a nitride sintered body having a porous structure and a semi-cured product of a thermosetting composition impregnated into the nitride sintered body, comprising the steps of: A step of impregnating a nitride sintered body having a porous structure with a thermosetting composition; and heating the thermosetting composition to a heating temperature of 80 to 130° C. to semi-cure the composition. The impregnation step is a step of impregnating the thermosetting composition at a temperature higher than the heating temperature and not higher than the heating temperature + 20°C, The thermosetting composition contains a compound having a cyanate group, a compound having a bismaleimide group, and a compound having an epoxy group, as well as a phosphine-based curing agent and an imidazole-based curing agent.

5. A first metal substrate, an intermediate layer, and a second metal substrate in this order; the first metal substrate and the second metal substrate are bonded to each other by the intermediate layer; A laminate, wherein the intermediate layer is a cured product of the composite according to any one of claims 1 to 3.

6. A method for producing a laminate including a first metal substrate, an intermediate layer, and a second metal substrate in this order, comprising: A method for producing a laminate, comprising the steps of: arranging a first metal substrate, the composite according to any one of claims 1 to 3, and a second metal substrate in this order; and applying heat and pressure to harden the composite to form the intermediate layer.

Citation Information

Patent Citations

  • Thermally conductive insulating sheet, power module, and manufacturing method for same

    WO2014142123A1

  • Resin-impregnated boron nitride sintered body and use for same

    WO2014196496A1

  • Ceramic resin composite body

    WO2017155110A1