IGZO sputtering target
The IGZO sputtering target with controlled bulk resistance distribution addresses intermittent arcing and property changes by maintaining stable sputtering conditions and film properties throughout its life, enhancing production consistency.
Patent Information
- Application Number
- JP2022003203
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-13
- Filing Date
- 2022-01-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-01-12
AI Technical Summary
Sputtering targets with high bulk resistance in IGZO sintered bodies experience intermittent arcing and changes in film properties during use, necessitating adjustments in sputtering conditions based on target life, which is undesirable for stable film formation.
The IGZO sputtering target is designed with a specific range of bulk resistance distribution, where the minimum and maximum resistances (Rmin and Rmax) in the thickness direction satisfy Rmin≧50mΩ·cm, Rmax≦200mΩ·cm, and Rmax/Rmin≦1.3, ensuring stable sputtering conditions and film properties throughout the target's life.
This design stabilizes sputtering conditions and maintains consistent film properties by controlling the bulk resistance distribution, reducing the need for frequent adjustments during target use.
Smart Images

Figure 0007566804000001 
Figure 0007566804000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an IGZO sputtering target. [Background technology]
[0002] Traditionally, α-Si (amorphous silicon) has been used for the TFT (thin film transistor) of the backplane of FPD (flat panel display). However, α-Si does not provide sufficient electron mobility, and in recent years, research and development has been conducted on TFTs using In-Ga-Zn-O oxide (IGZO), which has higher electron mobility than α-Si. Some next-generation high-performance flat panel displays using IGZO-TFTs have been put into practical use and are attracting attention.
[0003] IGZO films can be obtained mainly by DC sputtering a sputtering target made from an IGZO sintered body. In DC sputtering, a target with low bulk resistance is preferred to enable stable DC sputtering (see, for example, Patent Document 1), and the bulk resistance of the sintered body is controlled to be, for example, 50 mΩ·cm or less by adjusting the oxide sintering temperature, the sintering atmosphere, etc. to control the amount of oxygen vacancy in the sintered body to be relatively high. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 136611 Summary of the Invention [Problem to be solved by the invention]
[0005] By the way, in sputtering targets having IGZO sintered bodies, the amount of oxygen vacancies (bulk resistance) is adjusted to a desired range according to the sputtering conditions used. Although the reason is unclear, it is known that when the oxygen partial pressure during sputtering is set high, it is preferable for the sintered body to have a small amount of oxygen vacancies, in other words, a relatively high bulk resistance. However, when the sputtering conditions of a sputtering target having an IGZO sintered body with a relatively high bulk resistance (e.g., 80 mΩ·cm or more) are the same from the beginning to the end of use, the frequency of arcing during sputtering may increase intermittently, or the film characteristics and device characteristics of the obtained IGZO may change. In addition, in order to prevent the film characteristics and device characteristics of the obtained IGZO from changing, it may be necessary to fine-tune the sputtering conditions according to the target life (progress of use) of the sputtering target.
[0006] Therefore, an object of the present invention is to provide an IGZO sputtering target that can suppress the effects of the target life during use on the sputtering conditions and the film properties of the obtained IGZO. [Means for solving the problem]
[0007] As a result of extensive research to solve the problems of the conventional technology described above, the inventors discovered that in a sputtering target including an IGZO sintered body having a relatively high bulk resistance, the sintered body has a distribution of bulk resistance in the thickness direction, which led to the completion of the present invention. That is, the present invention is as follows.
[0008] In one embodiment, the IGZO sputtering target of the present invention is a sputtering target having an oxide sintered body made of indium (In), gallium (Ga), zinc (Zn), oxygen (O) and unavoidable impurities, wherein the minimum value Rmin (mΩ·cm) and maximum value Rmax (mΩ·cm) of bulk resistance in the thickness direction of the oxide sintered body satisfy Rmin≧50 mΩ·cm, Rmax≦200 mΩ·cm, and Rmax / Rmin≦1.3. Effect of the Invention
[0009] According to one embodiment of the present invention, it is possible to provide an IGZO sputtering target that can suppress the effects of the target life during use on the sputtering conditions and the film properties of the obtained IGZO. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail, but the present invention is not limited to the present embodiment.
[0011] The IGZO sputtering target of this embodiment (hereinafter also referred to as "sputtering target") is a sputtering target having an oxide sintered body consisting of indium (In), gallium (Ga), zinc (Zn), oxygen (O) and unavoidable impurities. The sputtering target of this embodiment can be used to form a semiconductor film, specifically, it can be used to form TFTs (thin film transistors) for FPDs (flat panel displays) such as organic electroluminescence (EL) and flexible displays.
[0012] Here, the oxide sintered body of the sputtering target of this embodiment is mainly composed of In2O3-Ga2O3-ZnO and mainly composed of composite oxides of indium (In), gallium (Ga), and zinc (Zn). Note that it may contain a single oxide of indium oxide, gallium oxide, or zinc oxide. More specifically, for example, in a composition with a target Ga content of 100 and a target Zn content of 100 when the In content in the oxide sintered body is taken as 100, the atomic ratios of Ga and Zn are preferably 100±20 and 100±20, more preferably 100±10 and 100±10, and even more preferably 100±3 and 100±3. The contents of In, Ga, and Zn in the oxide sintered body can be measured by a method such as fluorescent X-rays or ICP-AES.
[0013] In this embodiment, the oxide sintered body may further contain other additive elements as oxides in addition to indium (In), gallium (Ga), and zinc (Zn). Specifically, it may contain at least one oxide selected from the group consisting of Sn, Zr, Mg, Al, Si, Y, and Ti. The total amount of these other additive elements is preferably 50 to 1000 mass ppm in terms of metal amount, and more preferably 100 to 500 mass ppm. By making the total amount of these other additive elements 1000 mass ppm or less, the bulk resistance value can be adjusted, and by making it 50 mass ppm or more, the effect of adding the additive elements can be sufficiently obtained. The additive elements here also include the inclusion as inevitable impurities due to grinding media wear. In this embodiment, when the oxide sintered body further contains other additive elements as oxides, it is preferable that the oxide sintered body contains at least tin (Sn), which makes it possible to relatively increase the bulk resistance of the oxide sintered body. When the oxide sintered body contains at least tin, the tin content is preferably 1000 mass ppm or less, more preferably 500 ppm or less.
[0014] In addition, inevitable impurities are generally those that are present in raw materials or are inevitably mixed in the manufacturing process of metal or metal oxide products, such as media used in grinding raw powder. Although they are essentially unnecessary, they are permitted because they are present in trace amounts and do not affect the properties of metal or metal oxide products. In the sputtering target according to this embodiment, the total amount of inevitable impurities is generally 1000 ppm by mass or less, typically 500 ppm by mass or less, and more typically 200 ppm by mass or less.
[0015] In the oxide sintered body of the sputtering target of this embodiment, the minimum value of the bulk resistance in the thickness direction of the oxide sintered body is Rmin (mΩ·cm), and the maximum value is Rmax (mΩ·cm). In this case, in this embodiment, Rmin (mΩ·cm) and Rmax (mΩ·cm) are Rmin≧50mΩ·cm, Rmax≦200mΩ·cm, Rmax / Rmin≦1.3 It meets the following criteria. In this embodiment, the minimum value Rmin (mΩ·cm) and maximum value Rmax (mΩ·cm) of the bulk resistance in the thickness direction of the oxide sintered body have the above relationship, so that the target life during use of the sputtering target can suppress the influence on the sputtering conditions and the film properties of the obtained IGZO. Specifically, since the minimum value Rmin of the bulk resistance in the thickness direction is 50 mΩ·cm or more, a sputtering target having an oxide sintered body with a small amount of oxygen deficiency can be obtained, and the oxygen partial pressure during sputtering can be set high. In addition, since the maximum value Rmax of the bulk resistance in the thickness direction is 200 mΩ·cm or less, the sputtering target can be DC sputtered. Furthermore, since Rmax / Rmin≦1.3, the distribution of the bulk resistance in the thickness direction can be suppressed, and therefore, the influence on the sputtering conditions and the film properties of the obtained IGZO can be suppressed due to the target life during use of the sputtering target.
[0016] The minimum bulk resistance Rmin (mΩ·cm) of the oxide sintered body in the thickness direction is preferably Rmin≧80 mΩ·cm from the viewpoint of reducing the amount of oxygen vacancies in the sputtering target. Moreover, the maximum value Rmax (mΩ·cm) of the bulk resistance in the thickness direction of the oxide sintered body is preferably Rmax≦180 mΩ·cm from the viewpoint of effective DC sputtering of the sputtering target. Furthermore, from the viewpoint of further reducing the distribution of bulk resistance in the thickness direction, Rmax / Rmin≦1.2 is preferable.
[0017] The bulk resistance in the thickness direction of the oxide sintered body in the sputtering target was measured by a four-probe method at three arbitrary points on each of the seven surfaces (seven surfaces ground) that appeared after grinding k (mm) (k = an integer from 1 to 7) from the outermost surface of the oxide sintered body, and the arithmetic average value was taken as the bulk resistance value for the thickness direction position (specific surface). The minimum value Rmin and maximum value Rmax of the bulk resistance were taken as the minimum value Rmin and the maximum value Rmax, respectively, of the bulk resistance values of the seven surfaces. The average value Rave of the bulk resistance of the oxide sintered body means the arithmetic average of the bulk resistance values for the seven surfaces. The bulk resistance was measured by a four-probe method.
[0018] In this embodiment, the minimum bulk resistance Rmin (mΩ·cm) in the thickness direction of the oxide sintered body, the maximum bulk resistance Rmax (mΩ·cm), the bulk resistance ratio Rmax / Rmin, and the average bulk resistance Rave (mΩ·cm) described below can be controlled by sintering the raw material molded body to obtain the oxide sintered body under a high oxygen partial pressure, adjusting the sintering temperature, sintering time, sintering atmosphere, and temperature increase / decrease rate, annealing treatment after sintering, fine adjustment of the composition, and the like. Specifically, the bulk resistance can be set in a desired range by adjusting these conditions in a complex manner. More specifically, depending on the maximum firing temperature during the formation of the oxide sintered body, the degree of oxygen adsorption from the firing atmosphere to metal atoms during the formation of the InZnGaO4 phase changes, and the degree of oxygen vacancies caused by oxygen sublimation from the surface of the sintered body also changes. More specifically, in the region where the firing temperature during the formation of the oxide sintered body is relatively low, oxygen vacancies are easily formed during the formation of the InZnGaO4 phase (bulk resistance is easily reduced), and in the region where the firing temperature is relatively medium, oxygen is easily adsorbed from the firing atmosphere to metal atoms (oxygen vacancies are not easily formed and bulk resistance is easily increased). On the other hand, from the viewpoint of oxygen sublimation from the surface of the sintered body, oxygen sublimation is not easily caused in the region where the firing temperature is relatively low, and therefore oxygen vacancies are not easily formed (bulk resistance is large). In addition, as the firing temperature becomes relatively high, oxygen sublimation becomes more easily caused, and therefore oxygen vacancies are easily formed (bulk resistance is small). In addition, the degree of oxygen distribution (degree of penetration) from the surface of the sintered body to the entire sintered body also changes depending on the holding time of the maximum firing temperature when forming the oxide sintered body. In the relatively low temperature and medium temperature firing temperature ranges where oxygen component sublimation is difficult to occur, the longer the holding time, the easier it is for oxygen to distribute from the surface of the sintered body to the entire sintered body and for the degree of oxygen deficiency to reach an equilibrium state (the bulk resistance ratio Rmax / Rmin approaches 1). Conditions for making the oxide sintered body of the sputtering target of this embodiment have a desired bulk resistance are exemplified by the examples described in the Examples section below.
[0019] Furthermore, in the prior art (JP Patent Publication No. 2015-189630), it has been reported that the bulk resistance of the oxide sintered body can be made uniform throughout the target by subjecting the oxide sintered body obtained in the firing process to a reduction treatment (heat treatment) in an inert gas. However, as shown in the comparative examples described in the Examples section below, no significant effect was confirmed in the sputtering target of this embodiment.
[0020] The average bulk resistance Rave (mΩ·cm) of the oxide sintered body is preferably 55 to 180 mΩ·cm, more preferably 60 to 130 mΩ·cm, and further preferably 80 to 120 mΩ·cm. By setting the average bulk resistance Rave (mΩ·cm) to 55mΩ·cm or more, it is possible to obtain a sputtering target having an oxide sintered body with a small amount of oxygen vacancy, i.e., a relatively large amount of oxygen content, and the oxygen partial pressure during sputtering can be set low. In addition, by setting the average Rave (mΩ·cm) to 180mΩ·cm or less, the sputtering target can be DC sputtered.
[0021] In this embodiment, the grain size of the oxide sintered body measured by the cord method is preferably 1.7 μm to 15 μm, more preferably 3.0 μm to 10 μm. If the grain size is large and exceeds 15 μm, there is a concern that coarse particles will be generated during sputtering. If the grain size is less than 1.7 μm, there is a concern that sintering will be insufficient and sufficient density will not be obtained.
[0022] In addition, the grain size of the microstructure measured by the code method was determined by first cutting a sample for observation from the target, mirror-polishing the surface of the cut sample, taking a microstructure photograph of the surface of the mirror-polished sample at 1000x magnification using a scanning electron microscope (SEM) in five fields of view, drawing two straight lines on the photographed image, and measuring the arithmetic mean grain size of the lengths at which each line intersects with the crystal grains. The arithmetic mean grain size was determined as the grain size of the microstructure (crystal grain size). The grain size of the oxide sintered body measured by the cord method can be controlled by adjusting the maximum sintering temperature, sintering holding time, sintering atmosphere, and the like.
[0023] The oxide sintered body of the sputtering target of this embodiment preferably has a relative density of 97% or more. By having a relative density of 97% or more, the generation of nodules during sputtering can be suppressed. The relative density is determined by the ratio of the Archimedes density to the theoretical density, which is determined by the composition.
[0024] Here, the theoretical density is a density value calculated from the theoretical density of the oxide of each of the constituent elements of the oxide sintered body of the sputtering target, excluding oxygen. The oxide sintered body is subjected to a component analysis, and the theoretical density is calculated using the oxide mass ratio (mass%) calculated by converting the atomic ratio (at%) of each of the constituent elements In, Ga, and Zn to the total of 100 at% of In, Ga, and Zn, obtained by the analysis, and the simple substance densities of In2O3, Ga2O3, and ZnO. Specifically, the simple substance density of In2O3 is set to 7.18 (g / cm 3 ), and the density of Ga2O3 is 5.95 (g / cm 3 ), and the density of ZnO is 5.61 (g / cm 3 ) and the mass ratio of In2O3 is W In2O3 (mass%), the mass ratio of Ga2O3 is W Ga2O3 (mass%), the mass ratio of ZnO is W ZnO (mass%), theoretical density (g / cm 3 )=(7.18×W In2O3 +5.95×W Ga2O3 +5.61×W ZnO ) / 100.
[0025] Note that this relative density is based on the theoretical density calculated by assuming that the sintered body of the sputtering target is a mixture of In2O3, Ga2O3, and ZnO. Since the true density of the target sintered body may be higher than the theoretical density, the relative density referred to here may exceed 100%.
[0026] The relative density of the oxide sintered body of the sputtering target of this embodiment can be controlled within the above range by adjusting the maximum sintering temperature, sintering holding time, sintering atmosphere, and the like.
[0027] Here, in this embodiment, the oxide sintered body can be a part of a sputtering target, and can be bonded to a backing plate with a bonding material as necessary, and the oxide sintered body in the sputtering target can be in the shape of a circular plate, a rectangular plate, or a cylindrical shape. The thickness of the oxide sintered body of the sputtering target can be 20 mm or less, preferably 3.0 to 15 mm, and more preferably 6.0 to 12 mm. If the target is too thick, sufficient density cannot be obtained during sintering, and the ratio of the maximum and minimum values of the bulk resistance tends to be difficult to fall within a predetermined range, so the thickness is preferably 20 mm or less. Furthermore, by making the thickness 3.0 mm or more, the service life of the target can be extended, the downtime of the sputtering device can be reduced, and productivity can be improved.
[0028] Next, a method for producing the sputtering target of this embodiment will be described. The sputtering target of this embodiment can be produced through the steps of mixing and pulverizing raw materials, a granulating step, a molding step, and a firing step. In the mixing and grinding process, indium oxide (In2O3) powder, gallium oxide (Ga2O3) powder, and zinc oxide (ZnO) powder are prepared as raw material powders. The indium oxide powder as raw material powder has a median diameter (D50): 0.5 to 3.0 μm and a specific surface area: 4.0 to 10 m 2 / g, and the gallium oxide powder has a median diameter (D50): 0.5 to 4.0 μm and a specific surface area: 6.0 to 30 m 2 / g, and the zinc oxide powder has a median diameter (D50): 0.1 to 2.0 μm and a specific surface area: 2.0 to 20 m 2 It is preferred to use / g.
[0029] Next, the raw material powders are weighed to obtain the desired composition ratio, and then mixed and pulverized. There are various pulverization methods depending on the desired particle size and the material to be pulverized, and wet or dry ball mills, vibration mills, bead mills, etc. can be used. To obtain uniform and fine crystal particles, the bead mill mixing method is preferred, which has high efficiency in disintegrating aggregates in a short time and also provides good dispersion of additives.
[0030] Next, in the granulation process, the finely ground slurry is granulated. This is to improve the fluidity of the powder by granulation, so that the powder can be filled evenly into a mold during the next process of press molding, and a homogeneous molded body can be obtained. There are various methods for granulation, but one method for obtaining granulated powder suitable for press molding is to use a spray drying device (spray dryer). This method makes the powder into a slurry, disperses it as droplets in hot air, and dries it instantly, and it is possible to continuously obtain spherical granulated powder of 10 to 500 μm.
[0031] When drying with a spray dryer, it is important to control the inlet and outlet temperatures of the hot air. If the temperature difference between the inlet and outlet is large, the amount of dry material per unit time increases, improving productivity. However, if the inlet temperature is too high, the powder and added binder may be altered by the heat, and the desired characteristics may not be obtained. Also, if the outlet temperature is too low, the granulated powder may not be dried sufficiently.
[0032] In addition, the strength of the molded body can be improved by adding a binder such as polyvinyl alcohol (PVA) to the slurry and incorporating it into the granulated powder. The amount of PVA added can be 50 to 250 cc / kg of an aqueous solution containing 6% by mass of PVA relative to the raw material powder. Furthermore, the crushing strength of the granulated powder during press molding can be adjusted by adding a plasticizer suitable for the binder. There is also a method of improving the strength of the molded body by adding a small amount of water to the obtained granulated powder to moisten it.
[0033] Next, in the molding process, the granulated powder is pressed by a mold or cold isostatic press (CIP) at a pressure of, for example, 1 ton / cm 2The pressure is maintained at the above level for 1 to 3 minutes to form the mixture into a molded product.
[0034] In the subsequent sintering step, for example, an electric furnace may be used, and in addition to atmospheric sintering, pressure sintering methods such as hot pressing, oxygen pressure, and hot isostatic pressing may also be used. However, from the viewpoints of reducing manufacturing costs, the possibility of mass production, and the ease of manufacturing large sintered bodies, it is preferable to use atmospheric sintering.
[0035] In addition, the firing atmosphere in the firing step preferably contains oxygen, and more preferably is an oxygen atmosphere. By containing oxygen (by increasing the oxygen partial pressure), the bulk resistance of the oxide sintered body can be made relatively large and can be easily set within a desired range. In the normal pressure sintering method, the molded body is usually sintered by firing in the air, and when oxygen is introduced for firing, the flow rate of oxygen is preferably 5.0 to 2000 L / min.
[0036] The maximum firing temperature in the firing step can be 1200 to 1500° C., and preferably 1220 to 1360° C. By setting the maximum firing temperature within this range, it is possible to easily set the minimum value Rmin (mΩ·cm), maximum value Rmax (mΩ·cm) of the bulk resistance of the oxide sintered body, and the bulk resistance ratio Rmax / Rmin within the desired ranges. The holding time at the maximum firing temperature can be 10 to 100 hours, and is preferably 20 to 80 hours. By setting the holding time at the maximum firing temperature within this range, it is possible to easily set the minimum bulk resistance Rmin (mΩ·cm), maximum bulk resistance Rmax (mΩ·cm), and bulk resistance ratio Rmax / Rmin of the oxide sintered body within the desired range while maintaining the grain size of the sintered body within the desired range.
[0037] Furthermore, the heating rate during sintering is preferably 0.1 to 5.0°C / min, more preferably 0.3 to 3.0°C / min, and even more preferably 0.5 to 2.0°C / min in a temperature range of 1000°C or higher. A heating rate of more than 5.0°C / min in this temperature range is not preferred from the viewpoint of process stability during mass production. Also, a heating rate of less than 0.1°C / min in this temperature range is not preferred from the viewpoint of productivity. Furthermore, the rate of temperature increase outside the above-mentioned predetermined temperature range is not particularly limited and can be any rate of temperature increase.
[0038] Furthermore, the temperature of the molded body (sintered body) after sintering can be decreased at a rate of 10°C / min or less in a temperature range of 600°C or more. By decreasing the rate of temperature decrease to 10°C / min or less, cracking of the sintered body due to thermal stress can be suppressed. The reason why the temperature range for which the rate of temperature decrease is 10°C / min or less is set to 600°C or more is that thermal stress tends to increase in sintered bodies at 600°C or more when the temperature of the sintered body is decreased. The temperature drop rate is preferably 5.0° C. / min or less, more preferably 3.0° C. / min or less, and from the viewpoint of productivity, is preferably 0.1° C. / min or more, more preferably 0.5° C. / min or more. Furthermore, the temperature decreasing rate outside the above-mentioned predetermined temperature range is not particularly limited and can be any desired temperature decreasing rate.
[0039] In the method for producing a sputtering target of this embodiment, the sintered body obtained through the above-mentioned firing process can be processed into a desired shape by a processing machine such as a surface grinder, a cylindrical grinder, or a machining machine, as necessary, to produce a sputtering target. There is no particular restriction on the shape of the sputtering target. For example, it can be disk-shaped, rectangular, cylindrical, etc. The sputtering target may be bonded to a backing plate using a bonding material as necessary.
[0040] Although the embodiments of the present invention have been described above, the sputtering target of the present invention is not limited to the above examples and can be modified as appropriate. EXAMPLES
[0041] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0042] (Sputtering target production) As raw material powders of oxide sintered bodies for the sputtering targets of Examples 1 to 22 and Comparative Examples 1 to 17, indium oxide (In2O3) powder, gallium oxide (Ga2O3) powder, and zinc oxide (ZnO) powder were prepared. In the sputtering targets of Examples 1 to 3, 6, 8, 14, 18 to 22 and Comparative Examples 3, 8, and 15 to 17, the indium oxide powder had a median diameter (D50): 1.6 μm and a specific surface area: 4.2 m 2 / g, as gallium oxide powder, median diameter (D50): 1.7 μm, specific surface area: 11.7 m 2 / g, as zinc oxide powder, median diameter (D50): 0.6 μm, specific surface area: 3.9 m 2 / g was used. In the sputtering targets of Examples 4, 5, 7, 9 to 13, and 15 to 17 and Comparative Examples 1, 2, 4 to 7, and 9 to 14, the indium oxide powder had a median diameter (D50): 1.4 μm and a specific surface area: 5.0 m 2 / g, as gallium oxide powder, median diameter (D50): 1.7 μm, specific surface area: 11.7 m 2 / g, as zinc oxide powder, median diameter (D50): 0.6 μm, specific surface area: 3.9 m 2 In Examples 4, 5, 7, 9 to 13, 15 to 17 and Comparative Examples 1, 2, 4 to 7, 9 to 14, tin oxide (SnO2) powder was also used as a raw material in the amount shown in Table 1 (Table 1 shows the content of tin atoms). The tin oxide powder had a median diameter (D50): 1.5 μm and a specific surface area: 5.7 m 2 / g was used.
[0043] Next, each raw material powder was weighed to have the composition ratio (atomic ratio) shown in Table 1, and then wet mixed and pulverized in a bead mill. Note that the particle size of each raw material powder in the slurry after pulverization was 0.6 μm. Next, the pulverized slurry was granulated. In the granulation, the powder was made into a slurry, dispersed as droplets in hot air using a spray dryer, and instantly dried to continuously obtain 49 μm spherical granulated powder.
[0044] Next, for Examples 1, 2, 9 to 13, 15 to 18, 20 to 22 and Comparative Examples 3, 6 to 9, 11 to 17, the granulated powder was filled into a mold, cold pressed, and then subjected to a pressure of 1800 kgf / cm 2 The pressure was maintained for 1 minute to obtain a disk-shaped molded body having a diameter of 130 mm and a thickness of 21 mm. In addition, in Examples 14 and 19 and Comparative Examples 4 and 10, the granulated powder was filled into a rubber mold and a pressure of 1800 kgf / cm was applied. 2 The pressure was maintained for 1 minute to form the molded product, and then cutting was performed to obtain a cylindrical molded product having an axial length of 1600 mm, an outer diameter of 197 mm, and an inner diameter of 157 mm. In addition, for Examples 3 to 8 and Comparative Examples 1, 2, and 5, the granulated powder was filled into a mold and cold pressed, and then the molded product was subjected to a pressure of 1800 kgf / cm. 2 The pressure was maintained for 1 minute to form a rectangular molded body having a width of 550 mm, a length of 595 mm, and a thickness of 16 mm. These molded bodies were then fired in an electric furnace under the atmosphere of Table 1 to obtain oxide sintered bodies. Specifically, the molded bodies were heated under the conditions shown in Table 1, and then fired at the sintering temperature and time shown in Table 1. The heating rate from 1000°C to the maximum temperature was 1°C / min, and after the maximum temperature was maintained, the temperature was lowered to 600°C at a rate of 1.5°C / min.
[0045] The obtained oxide sintered bodies were processed into disks having a diameter of 100 mm and a thickness of 15 mm for Examples 1, 2, 9-13, 15-18, 20-22 and Comparative Examples 3, 6-9, 11-17, and into cylindrical shapes having an axial length of 50 mm, an outer diameter of 153 mm, and an inner diameter of 135 mm for Examples 14, 19, and Comparative Examples 4 and 10. Moreover, in Examples 3-8 and Comparative Examples 1, 2, and 5, they were processed into rectangular shapes having a width of 450 mm, a length of 450 mm, and a thickness of 10 mm. Each oxide sintered body was subjected to the evaluation described below.
[0046] In Comparative Example 13, the sintered body obtained in Comparative Example 12 was subjected to a reduction treatment at 600°C for 5 hours in a nitrogen atmosphere, and in Comparative Example 14, the sintered body obtained in Comparative Example 12 was subjected to a heat treatment at 600°C for 5 hours in an oxygen atmosphere. The electric furnace used to sinter each molded body had a furnace volume of 2.2 m. 3 (in Table 1, it is referred to as "large furnace"), with a furnace volume of 0.06 m 3 (referred to as small furnace in Table 1) was used.
[0047] [Table 1]
[0048] The obtained oxide sintered body was evaluated as follows. The evaluation results are shown in Table 2. (1) Density and relative density of oxide sintered bodies In accordance with JIS R 1634, the bulk density was calculated from the volume and dry weight of the sintered body calculated by the Archimedes method using the following formula, and the bulk density was divided by the theoretical density to obtain the relative density. Volume of sintered body = (weight of sintered body containing water - weight of sintered body in water) / density of water The theoretical density of the sintered body is the mass ratio W of In2O3 calculated from the atomic ratio (at%) of each of the constituent elements In, Ga, and Zn to 100 at%. In2O3 (mass%), mass ratio of Ga2O3 W Ga2O3 (mass%), mass ratio of ZnO W ZnO (mass%), and the density of In2O3 is 7.18 (g / cm 3 ), and the density of Ga2O3 is 5.95 (g / cm 3 ), and the density of ZnO is 5.61 (g / cm 3 ) was used to calculate the following formula: Theoretical density (g / cm 3 )=(7.18×W In2O3 +5.95×W Ga2O3 +5.61×WZnO ) / 100
[0049] (2) Grain size of oxide sintered body measured by cord method The grain size of the oxide sintered body measured by the code method was obtained by cutting out a sample for observation from the oxide sintered body after surface finishing with an abrasive, and mirror-polishing the surface of the cut sample. Photographs of the grain size of the mirror-polished sample surface were taken in five fields of view at 1000x magnification using a scanning electron microscope (SEM), and the crystal grain size (grain size of the grain) of the multiple fields (five fields) was calculated as the arithmetic average value using the code method evaluation method. In the code method, two straight lines of arbitrary length were drawn on each surface grain photograph, the length of the lines was divided by the number of grains that the lines crossed, and this value was converted by applying it to the scale of the surface grain photograph, and the arithmetic average grain size was calculated based on the value obtained from the total of 10 straight lines. In addition, "-" in the grain size column of Table 2 means that there is no measurement result.
[0050] (3) Minimum and maximum bulk resistance values Rmin (mΩ cm) and Rmax (mΩ cm), and average value Rave (mΩ cm) in the thickness direction The bulk resistance in the thickness direction of the oxide sintered body was measured by a four-probe method at three arbitrary points on each of the seven faces that were revealed by grinding k (mm) (k = an integer from 1 to 7) from the outermost surface of the oxide sintered body, and the arithmetic average value was taken as the bulk resistance value of the face. The minimum value Rmin and maximum value Rmax of the bulk resistance were taken as the minimum value Rmin and the maximum value Rmax, respectively, of the bulk resistance values of the seven faces. The average value Rave of the bulk resistance of the oxide sintered body was taken as the arithmetic average value of the bulk resistance values of the seven faces.
[0051] (4) Sputtering evaluation The sintered bodies obtained in Examples 3, 7, and 8 and Comparative Example 5 were each processed to a size of 127 mm x 254 mm, and two of these were combined to produce a sputtering target of 127 mm x 508 mm. Using this sputtering target, a DC sputtering device (Shinchron, model number: BSC-7011) was used in an Ar+O2 10 vol% atmosphere, a total gas flow rate of 300 sccm, a sputtering pressure of 0.6 Pa, and a power of 2.3 W / cm. 2 Sputtering was performed under the following conditions. It was confirmed that stable discharge occurred in the sputtering targets obtained from the sintered bodies of Examples 3, 7, and 8, whereas it was confirmed that the number of intermittent arcing events rapidly increased in the sputtering target obtained from the sintered body of Comparative Example 5. In other words, it is understood that by setting the bulk resistance ratio to Rmax / Rmin≦1.3, it is possible to suppress the effects of the target life during use of the sputtering target on the sputtering conditions and the film properties of the obtained IGZO.
[0052] [Table 2]
[0053] As shown in Table 2, the minimum bulk resistance Rmin (mΩ cm), maximum bulk resistance Rmax (mΩ cm), and bulk resistance ratio Rmax / Rmin in the thickness direction of the oxide sintered body can be adjusted to within the desired range by sintering the raw material molded body to obtain the oxide sintered body under a high oxygen partial pressure, adjusting the sintering temperature, sintering time, sintering atmosphere, and temperature increase / decrease rate, annealing treatment after sintering, fine-tuning the composition, etc. The oxide sintered bodies of Comparative Examples 12 to 14 were obtained by subjecting the sintered body obtained in Comparative Example 1 to the heat treatment as described above. It can be seen that the minimum bulk resistance Rmin (mΩ cm), the maximum bulk resistance Rmax (mΩ cm), and the bulk resistance ratio Rmax / Rmin fell outside the desired ranges as a result of the heat treatment. [Industrial Applicability]
[0054] According to the present invention, it is possible to provide an IGZO sputtering target that can suppress the effects of the target life during use on the sputtering conditions and the film properties of the obtained IGZO.
Claims
1. A sputtering target having an oxide sintered body composed of indium (In), gallium (Ga), zinc (Zn), oxygen (O) and unavoidable impurities, The minimum value Rmin (mΩ cm) and the maximum value Rmax (mΩ cm) of the bulk resistance in the thickness direction of the oxide sintered body are Rmin≧50mΩ・cm, Rmax≦200mΩ・cm, Rmax / Rmin≦1.3 IGZO sputtering targets that meet these requirements.
2. The IGZO sputtering target according to claim 1, wherein the grain size of the oxide sintered body measured by the cord method is 1.7 to 15 μm and the relative density is 97% or more.
3. The IGZO sputtering target according to claim 1 or 2, wherein the oxide sintered body has a circular plate shape, a rectangular plate shape, or a cylindrical shape.
4. The IGZO sputtering target according to any one of claims 1 to 3, wherein when the In content in the oxide sintered body is 100, Ga is 100 ± 20 and Zn is 100 ± 20 in terms of atomic ratio.
5. The IGZO sputtering target according to any one of claims 1 to 4, wherein the average bulk resistance Rave (mΩ cm) of the oxide sintered body is 55 to 180 mΩ cm.
6. The IGZO sputtering target according to any one of claims 1 to 5, wherein the oxide sintered body has a thickness of 15 mm or less.
Citation Information
Patent Citations
In-Ga-Zn-O BASED OXIDE SINTERED COMPACT SPUTTERING TARGET HAVING EXCELLENT STABILITY UPON LONG TERM FILM DEPOSITION
JP2011106003A
Oxide sintered body and sputtering target comprising oxide sintered body
WO2016136611A1