Wire rod forming method and wire rod forming device

The three-step wire forming method with controlled deformation and tension management effectively reduces warpage and improves mechanical properties by using driven and non-driven roller groups with urethane rubber rollers, achieving stable wire straightening.

JP7567023B2Active Publication Date: 2024-10-15ASTEMO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023502059
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-26
Filing Date
2021-10-18
Publication Date
2024-10-15
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

Existing wire rod forming methods fail to effectively reduce warpage caused by winding, as they do not adequately address the need for controlled deformation and tension management during the straightening process.

Method used

A three-step wire forming method involving driven and non-driven roller groups with controlled pushing amounts, where the first step applies significant deformation, the second step reduces tension, and the third step corrects warpage by using rotatably supported rollers with zero pushing amount, combined with urethane rubber rollers for improved followability.

Benefits of technology

The method stably reduces warpage and enhances mechanical properties by uniformly applying strain and correcting curvature, ensuring consistent wire quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567023000001
    Figure 0007567023000001
  • Figure 0007567023000002
    Figure 0007567023000002
  • Figure 0007567023000003
    Figure 0007567023000003
Patent Text Reader

Abstract

According to the present invention, a method for molding a wire material, carried out on a wire material moving from the upstream side to the downstream side, includes: a first step for feeding out the wire material while pressing the wire material by a first roller group, which is a plurality of rollers driven by a motor; and a second step for feeding out the wire material while pressing the wire material by a second roller group, which is a plurality of rotatably supported rollers. The first step is provided on the upstream side of the second step. The pressing-in amount, which is the difference between the outer dimensions of the wire material and the spacing between the rollers through which the wire material passes, is greater in the first step than in the second step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wire forming method and a wire forming device. [Background technology]

[0002] Metal wire is generally wound around a bobbin during the manufacturing process. When processing this wire, a process called "forming" or "straightening" is required to reduce the warping that occurs when the wire is wound. Patent Document 1 discloses a bar and wire straightening machine that easily improves the straightness of bar and wire rod, the straightening machine performing straightening by passing a metal bar and wire rod between a plurality of rolls, the straightening machine including at least one unit group including two or more adjacent units, the angle between the directions in which the two or more units straighten the bar and wire rod being ±15°, the unit including two or more fixed rolls and one movable roll less than the fixed rolls, the fixed roll and the movable roll being a fixed roll arranged on one side of the running bar and wire rod and a movable roll arranged on the opposite side of the fixed roll with respect to the bar and wire rod, the rolls being arranged in a staggered manner so as to sandwich the running bar and wire rod, the amount of pressure applied to the movable roll closest to the entrance side and the movable roll closest to the exit side of a unit can be set, and the amounts of pressure applied to adjacent units satisfy a predetermined relationship. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2018 / 174272 Summary of the Invention [Problem to be solved by the invention]

[0004] The invention described in Patent Document 1 leaves room for improvement in molding. [Means for solving the problem]

[0005] A wire shaping method according to a first aspect of the present invention is a method for shaping a wire moving from an upstream side to a downstream side, and includes a first step of feeding the wire while pressing it with a first roller group which is a plurality of rollers driven by a motor, and a second step of feeding the wire while pressing it with a second roller group which is a plurality of rollers supported rotatably, the first step is provided upstream of the second step, a pressing amount which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes is larger in the first step than in the second step, and none of the rollers included in the second roller group are driven by an external power. In the second step, the pushing amount is gradually decreased from the upstream side to the downstream side until it reaches zero. . According to the second aspect of the present invention The wire rod shaping method is a method for shaping a wire rod moving from an upstream side to a downstream side, and includes a first step of feeding the wire rod while pressing it with a first roller group which is a plurality of rollers driven by a motor, and a second step of feeding the wire rod while pressing it with a second roller group which is a plurality of rollers supported rotatably, the first step is provided upstream of the second step, and a pressing amount, which is a difference between an outer dimension of the wire rod and a gap between rollers through which the wire rod passes, is larger in the first step than in the second step, none of the rollers included in the second roller group are driven by an external power, and the method further includes a third step of feeding the wire rod with a third roller group which is a plurality of rollers supported rotatably, the third step is provided downstream of the second step, and the pressing amount in the third step is zero. . According to the third aspect of the present invention The wire forming device includes a feed section that feeds out a wire, a first roller group that is a plurality of rollers that are driven by a motor and press the wire fed out by the feed section, and a second roller group that is a plurality of rollers that are rotatably supported and further press the wire pressed by the first roller group, and the first roller group has a larger pressing amount, which is the difference between the outer dimension of the wire and the gap between the rollers through which the wire passes, than the second roller group, and none of the rollers included in the second roller group is driven by an external power. First, the pushing amount of the second roller group gradually decreases from the first roller group side to the opposite side to zero. . A wire shaping device according to a fourth aspect of the present invention includes a feed-out section which feeds out a wire, a first roller group which is a plurality of rollers driven by a motor to press the wire fed out by the feed-out section, and a second roller group which is a plurality of rollers which are rotatably supported and which further press the wire pressed by the first roller group, wherein a pressing amount, which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes, is larger for the first roller group than for the second roller group, none of the rollers included in the second roller group are driven by an external power, and the device further includes a third roller group which is a plurality of rollers which are rotatably supported and which further press the wire pressed by the second roller group, and wherein the pressing amount in the third roller group is zero. . Effect of the Invention

[0006] According to the present invention, the warping of the wire can be stably reduced. [Brief description of the drawings]

[0007] [Figure 1] Schematic diagram of a wire processing system including a forming device [Diagram 2] Schematic diagram of the molding device [Diagram 3] Schematic diagram of the pushing amount in the molding device [Figure 4] FIG. 1 is a diagram showing an example of a configuration of a drive roller; [Diagram 5]Conceptual diagram of test results for determining arrangement angle θx DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] --Embodiment-- BEST MODE FOR CARRYING OUT THE DISCLOSURE Hereinafter, with reference to Figs. 1 to 5, an embodiment of a wire shaping device and a wire shaping method according to the present invention will be described.

[0009] (Overall configuration diagram) Fig. 1 is a schematic diagram of a wire processing system S including a forming device 1. For the purpose of explanation, Fig. 1 shows X, Y and Z axes which are perpendicular to each other. The X axis is parallel to the left-right direction of Fig. 1, with the right side in the figure being the positive direction. The Z axis is parallel to the up-down direction of Fig. 1, with the top in the figure being the positive direction. The Y axis is the depth direction of Fig. 1.

[0010] The wire processing system S includes a delivery device 700, a forming device 1, a peeling device 800, and a cutting device 900. The wire moves from left to right in the figure and is processed in that order. Hereinafter, the left side in the figure is also called "upstream" and the right side in the figure is also called "downstream".

[0011] A bobbin around which a wire is wound is placed in the delivery device 700 with its rotation axis parallel to the Y axis. The delivery device 700 delivers the wire wound around the bobbin to the molding device 1. The wire is warped in the Z direction in FIG. 1 after being wound around the bobbin. The molding device 1 corrects the warp in the Z direction of the wire delivered from the delivery device 700 and delivers it to the peeling device 800. Note that "warping" is also called "curving" or "curling."

[0012] The peeling device 800 peels off the insulating coating of the wire by cutting or laser irradiation. The cutting device 900 cuts the wire to a predetermined length. The configuration and operation of the forming device 1 will be described in detail below. Note that the wire is depicted in a straight line in FIG. 1 for convenience of drawing, and is not an essential component.

[0013] (Configuration of molding device) FIG. 2 is a schematic diagram of the forming device 1. The forming device 1 includes a first roller group 11, a second roller group 12, and a third roller group 13. The wire is first formed by the first roller group 11, then by the second roller group 12, and finally by the third roller group 13. Hereinafter, forming of the wire by the first roller group 11 will be referred to as a "first step", forming of the wire by the second roller group 12 will be referred to as a "second step", and forming of the wire by the third roller group 13 will be referred to as a "third step". Both the first step and the second step plastically deform the wire.

[0014] In this embodiment, the difference between the outer dimension of a given wire and the gap between the rollers through which the wire passes is called the "push-in amount." For example, if the outer dimension of a given wire is "1.000 mm" and the roller interval is "0.998 mm," the push-in amount is "0.002 mm."

[0015] Each of the first roller group 11, the second roller group 12, and the third roller group 13 has rollers arranged in two rows, one above the other, and the wire passes through approximately the center of the rows. Each of the first roller group 11, the second roller group 12, and the third roller group 13 includes at least three rollers. The number of rollers included in each of the first roller group 11, the second roller group 12, and the third roller group 13 may be different. Note that in FIG. 2, all of the rollers in the lower row of the first roller group 11, the second roller group 12, and the third roller group 13 are arranged in a straight line, but this is merely one example of the configuration.

[0016] Each of the first roller group 11 is a drive roller whose outer circumference is molded with urethane rubber and driven by a motor as described below. The direction in which the rollers are driven is the direction along the movement of the wire material, specifically, the upper roller in the figure is driven counterclockwise, and the lower roller in the figure is driven clockwise. The gap between the rollers in the first roller group 11 through which the wire material passes is set so that the pressing amount decreases sequentially from the upstream side to the downstream side. In the following, the gap between the rollers through which the wire material passes is also called the "roller interval."

[0017] Each of the second roller group 12 and the third roller group 13 is made of metal and is not driven by an external power. The spacing between the rollers in the second roller group 12 is set so that the amount of pressure gradually decreases from the upstream side to the downstream side, and the final amount of pressure in the second roller group 12 is set to zero. The amount of pressure at the most upstream position in the second roller group 12 is smaller than the amount of pressure at the most downstream position in the first roller group 11. The amounts of pressure in the third roller group 13 are all set to zero.

[0018] The second roller group 12 is configured such that a plurality of rollers in an upper row are fixed together and can rotate around the rearmost roller in the upper row. The position of the rearmost roller in the upper row is determined in advance so that the final pushing amount in the second roller group 12 is zero, and the position of this roller is not readjusted unless the wire material is changed. In this embodiment, the angle formed by the line connecting the centers of the upper row rollers in the second roller group 12 and the line connecting the centers of the lower row rollers in the second roller group 12 is called the "arrangement angle θx". Although this can only occur during the adjustment process described below, if the arrangement angle θx is zero degrees, the upper row and the lower row are parallel and all the pushing amounts in the second roller group 12 are zero. The arrangement angle θx of the second roller group 12 in the state in which the adjustment is completed and the wire material is being formed is set so that the pushing amount becomes larger on the upstream side.

[0019] FIG. 3 is a schematic diagram of the amount of pushing in the molding device 1. The vertical axis in FIG. 3 indicates the amount of pushing, with the upward direction indicating a larger positive value, and the minimum value being zero. The horizontal axis in FIG. 3 indicates the X-coordinate value of the position where the pushing in the molding device 1 is performed, with the left side indicating the upstream side and the right side indicating the downstream side. In the first roller group 11 and the second roller group as a whole, the amount of pushing decreases sequentially from the upstream side to the downstream side and reaches zero. The amount of pushing in the third roller group 13 is zero in both cases. In FIG. 3, the ratio of the minimum amount of pushing in the first roller group 11 to the maximum amount of pushing in the second roller group 12 is several times, but it may be 10 times or more or 50 times or more.

[0020] Fig. 4 is a diagram showing an example of the configuration of each roller constituting the first roller group 11, i.e., the drive roller. The drive roller 22 is driven by power energy obtained from the motor 31 shown in the lower right of Fig. 4. The rotational energy generated by the motor 31 is transmitted to the shaft 27 via the timing pulley 30, the timing belt 29, and the timing pulley 28. As described above, the position of the drive roller 22 can be adjusted, and in Fig. 4, the position can be adjusted in the Z direction by the shaft slide screw 25 and the shaft slide box 24. To accommodate this position adjustment, a universal joint 26 is interposed between the shaft 27 and the drive roller 22.

[0021] (Roller position) The procedure for determining the amount of compression for the first roller group 11 and the second roller group 12, in other words, the procedure for determining the spacing between the rollers, will be described. As for the third roller group 13, as described above, all of the compression amounts are zero, and the roller spacing is the same as the specified dimension of the wire, so the description will be omitted here. As described below, the first roller group 11 is adjusted first, and then the second roller group 12 is adjusted. The adjustments described below may be performed, for example, by an operator, or may be calculated by a computer.

[0022] The amount of pressing in the first roller group 11 is determined by first identifying the strain corresponding to the "tensile strength" that is the maximum stress in the wire from the composition of the wire. For example, a physical property table or a database can be used for this identification. Next, the product of the identified strain and a predetermined ratio, for example, "0.6", is calculated and named the "target strain". Then, the amount of pressing in of each roller in the first roller group 11 is determined so that the amount of pressing in decreases gradually and reaches the "target strain" when the first process is completed. For this determination, the results of calculations using simulation software or the results of one or more experiments using the forming device 1 can be used.

[0023] Once the amount of pressure applied to each roller in the first roller group 11 can be determined by the above procedure, the position of the first roller group 11 can be determined according to a predetermined policy. For example, the predetermined policy is to fix the positions of the lower rollers in the first roller group 11 and adjust the positions of the upper rollers to set the roller spacing to a determined value. The first roller group 11 is set at the determined position of the first roller group 11, and the process proceeds to the next process of determining the amount of pressure applied to the second roller group 12.

[0024] The amount of pressing in the second roller group 12 is determined by the arrangement angle θx. The optimal arrangement angle θx is determined, for example, by an operator changing xx in multiple ways and measuring the processing results of the second step. A specific example will be described below.

[0025] FIG. 5 is a conceptual diagram of the test results for determining the arrangement angle θx. In FIG. 5, the vertical axis indicates the amount of warping, and the horizontal axis indicates the arrangement angle θx. Note that FIG. 5 shows eight arrangement angles θx, S1 to S8, but these eight are merely examples and may be more or less than eight. A positive amount of warping means warping on the positive side of the Z axis, and a negative amount of warping means warping on the negative side of the Z axis. FIG. 5 shows two independent test results, with triangular plots indicating a case where the wire output from the first process was significantly biased to the positive side, and square plots indicating a case where the wire output from the first process was significantly biased to the negative side.

[0026] When the wire rod output from the first process is significantly biased to the positive side, as shown by the triangular plot, it indicates that when the arrangement angle θx is small (S1), the warpage correction in the second process is not very effective and the value remains large and positive. The larger the arrangement angle θx is, the smaller the warpage becomes, and in the example shown in Figure 5, when the arrangement angle θx is S4, the warpage becomes almost zero. When the arrangement angle θx is further increased from S4, the warpage starts to increase and continues to increase. When the result of the triangular plot shown in Figure 5 is obtained, the operator selects S4, which has the smallest absolute value of the warpage, as the arrangement angle θx.

[0027] When the wire rod output from the first process is significantly biased toward the negative side, as shown by the square plot, it indicates that when the arrangement angle θx is small (S1), the warpage correction in the second process does not work well, and the value remains a large negative value. As the arrangement angle θx is increased, the amount of warpage approaches zero, and in the example shown in Figure 5, when the arrangement angle θx is S5, the amount of warpage is almost zero. When the arrangement angle θx is further increased from S5, the amount of warpage continues to increase and reaches a large positive value. When the result of the square plot shown in Figure 5 is obtained, the operator selects S5, which has the smallest absolute value of the amount of warpage, as the arrangement angle θx.

[0028] According to the above-described embodiment, the following advantageous effects can be obtained. (1) The forming device 1 forms the wire moving from the upstream side, which is the left side of FIG. 2, to the downstream side, which is the right side of FIG. 2, as follows. The forming of the wire by the forming device 1 includes the following first and second steps. In the first step, the wire is fed out while being pressed by the first roller group 11, which is a plurality of rollers driven by the motor 31. In the second step, the wire is fed out while being pressed by the second roller group 12, which is a plurality of rollers supported rotatably. The first step is provided upstream of the second step, i.e., on the left side of FIG. 2. The amount of pressing, which is the difference between the outer dimensions of the wire and the gap between the rollers through which the wire passes, is larger in the first step than in the second step. Therefore, in the first step, the tension generated in the wire is reduced by using the driven first roller group 11 to feed the wire, thereby suppressing elongation and reducing warping, and in the second step, the amount of pressing is set lower than in the first step, thereby stably reducing warping of the wire. In other words, the forming method by the forming device 1 stably reduces warping of the wire.

[0029] (2) In the first process, the amount of pushing is gradually decreased from the upstream side to the downstream side, so that the warping of the wire can be reduced more stably.

[0030] (3) In the second process, the amount of pushing is gradually decreased from the upstream side to the downstream side until it reaches zero, so that the warpage of the wire can be reduced more stably.

[0031] (4) The minimum indentation amount in the first step is at least 10 times the maximum indentation amount in the second step. Therefore, a large strain is imparted to the wire in the first step, and the mechanical properties can be made uniform by work hardening.

[0032] (5) In addition to the first and second steps, the forming of the wire by the forming device 1 also includes a third step in which the wire is fed by a third roller group 13, which is a plurality of rotatably supported rollers. This third step is provided downstream of the second step, i.e., on the right side in the figure. The pushing amount in the third step is zero. Therefore, by using the third roller group 13, which has a pushing amount of zero, the warping of the wire itself is corrected, and variation can be suppressed.

[0033] (6) The surface of each roller in the first roller group 11 is made of urethane rubber, which improves the ability of the wire to follow each drive roller, thereby further reducing warping of the wire.

[0034] (Variation 1) The above-described embodiment is as follows: <1> ~ <5> It may be modified as follows. <1> ~ <5> may be combined in any way. <1> ~ <4> All the above variations may be added. <1> ~ <5> Any one or more of the above modifications may be applied.

[0035] <1> The forming device 1 does not necessarily have to include the third roller group 13, and the forming of the wire rod does not necessarily have to include the third step. <2> The ratio between the minimum amount of pushing in the first step and the maximum amount of pushing in the second step may be several times. <3> In the first step, the pushing amount does not have to decrease gradually from the upstream side to the downstream side. <4> In the second step, the pushing amount does not have to decrease gradually from the upstream side to the downstream side. <5> The rollers constituting the first roller group 11 may not have urethane rubber molded on the outer periphery, and may have a metal surface.

[0036] According to this modification 1, although there are disadvantages such as insufficient reduction of warping and lack of stability compared to the above-mentioned embodiment, it is easier to adjust the roller position. Even if these disadvantages exist, it is acceptable as long as the required precision is satisfied.

[0037] (Variation 2) The method of determining the amount of pressing in the second roller group 12 described in the above embodiment is merely an example. For example, the positions of the upper rollers in the second roller group 12 may be individually adjustable, and the position of each roller may be changed little by little while measuring the amount of warping to determine the roller position at which the amount of warping is smallest. In this case, the number of times the roller position is adjusted and the number of times the amount of warping is measured will be significantly greater than in the embodiment, but it may be possible to reduce the absolute value of the amount of warping compared to the embodiment.

[0038] Although various embodiments and modifications have been described above, the present invention is not limited to these. Other embodiments that are conceivable within the scope of the technical idea of ​​the present invention are also included within the scope of the present invention. [Explanation of symbols]

[0039] 1…Forming equipment 11...First roller group 12...Second roller group 13…Third roller group 31…Motor

Claims

1. A method for forming a wire moving from an upstream side to a downstream side, comprising the steps of: a first step of pressing and feeding the wire rod by a first roller group which is a plurality of rollers driven by a motor; a second step of pressing and feeding the wire rod by a second roller group that is a plurality of rollers supported rotatably, The first step is provided upstream of the second step, a pressing amount, which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes, is larger in the first process than in the second process; None of the rollers included in the second roller group are driven by an external power source, In the second step, the pushing amount gradually decreases from the upstream side to the downstream side until it reaches zero.

2. A method for forming a wire moving from an upstream side to a downstream side, comprising the steps of: a first step of pressing and feeding the wire rod by a first roller group which is a plurality of rollers driven by a motor; a second step of pressing and feeding the wire rod by a second roller group that is a plurality of rollers supported rotatably, The first step is provided upstream of the second step, a pressing amount, which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes, is larger in the first process than in the second process; None of the rollers included in the second roller group are driven by an external power source, The method further includes a third step of feeding the wire by a third roller group that is a plurality of rollers supported rotatably, The third step is provided downstream of the second step, The method for forming a wire, wherein the pushing amount in the third step is zero.

3. The method for forming a wire according to claim 1 or 2, The method for forming a wire, wherein in the first step, the pushing amount gradually decreases from the upstream side to the downstream side.

4. The method for forming a wire according to claim 1 or 2, A method for forming a wire, wherein the minimum amount of pushing in the first step is at least 10 times the maximum amount of pushing in the second step.

5. The wire forming method according to claim 1 or 2, A method for forming a wire, wherein each of the rollers constituting the first roller group has a surface made of urethane rubber.

6. a feed-out section that feeds out a wire rod; a first roller group that is a plurality of rollers that are driven by a motor and press the wire rod fed out by the feed-out section; and a second roller group that is a plurality of rollers that are rotatably supported and further press the wire rod pressed by the first roller group, a pressing amount, which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes, is larger in the first roller group than in the second roller group; None of the rollers included in the second roller group are driven by an external power source, The pressing amount in the second roller group gradually decreases from the first roller group side to the opposite side until it reaches zero.

7. a feed-out section that feeds out a wire rod; a first roller group that is a plurality of rollers that are driven by a motor and press the wire rod fed out by the feed-out section; and a second roller group that is a plurality of rollers that are rotatably supported and further press the wire rod pressed by the first roller group, a pressing amount, which is a difference between an outer dimension of the wire and a gap between rollers through which the wire passes, is larger in the first roller group than in the second roller group; None of the rollers included in the second roller group are driven by an external power source, a third roller group which is a plurality of rollers and is rotatably supported to further press the wire rod pressed by the second roller group; The wire forming apparatus, wherein the pushing amount in the third roller group is zero.

8. The wire forming apparatus according to claim 6 or 7, the first roller group is disposed between the delivery section and the second roller group, The pressing amount in the first roller group gradually decreases from the delivery section side to the second roller group side.

9. The wire forming apparatus according to claim 6 or 7, A wire forming apparatus, wherein the minimum pushing amount of the first roller group is at least 10 times the maximum pushing amount of the second roller group.

10. The wire forming apparatus according to claim 6 or 7, A wire forming apparatus, wherein each of the rollers constituting the first roller group has a surface made of urethane rubber.

Citation Information

Patent Citations

  • JP1971009935Y1

  • JP1974004665A

  • Method for correcting residual stress and straightness in metal wire rod

    JP1993104181A

  • Method and device for correcting wire rope

    JP1994246380A

  • Device for straightening wire rod and device for assembling and wiring solar cell

    JP2007044734A