Solvent-based two-component anticorrosive coating composition

The solvent-based two-part coating composition with polyhydroxyl-functional organic compounds addresses the inactivation and pH-dependent limitations of existing coatings by directly reacting with crosslinking agents, offering effective corrosion protection across various metals.

JP7567040B2Active Publication Date: 2024-10-15BASF COATINGS GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023514069
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-28
Filing Date
2021-08-26
Publication Date
2024-10-15
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

Existing anticorrosive coatings for aluminum and other metal substrates face challenges due to the inactivation of organic corrosion inhibitors during the curing process and limited effectiveness under varying pH conditions, necessitating encapsulation that complicates their use and alters coating properties.

Method used

A solvent-based two-part coating composition utilizing polyhydroxyl-functional aromatic organic compounds, such as quercetin and alizarin, which react with crosslinking agents without encapsulation, providing corrosion protection even at low pH values and across different metal substrates.

Benefits of technology

The composition effectively inhibits corrosion on aluminum and other metals without encapsulation, maintaining coating properties and ensuring corrosion protection under diverse environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567040000001
    Figure 0007567040000001
  • Figure 0007567040000002
    Figure 0007567040000002
  • Figure 0007567040000003
    Figure 0007567040000003
Patent Text Reader

Abstract

The present invention relates to (A) a masterbatch composition comprising: (a) one or more polymers and / or resins reactive with functional groups of one or more crosslinkers contained in the curing agent component (B); (b) one or more pigments and / or fillers; and (c) one or more species selected from the group consisting of species of formula (II): [Formula 1] TIFF2023539342000020.tif4879 (wherein the four residues R 1 Two of the residues are OH, and the other two residues are R 1 is H;R 2 = O; and R 3 -R 4 is C=C or HC-CH; R 5 is p-(OH)Ph(R 7 )(R 8 ) and R 6 =H or OH; R 2 =O;R 7 and R 8 is H or OH, with the proviso that R 7 and R 8 at least one of which is H), and / or a species of formula (III) [Case 2] TIFF2023539342000021.tif4671 (in the formula, R 1 is as defined above, and R 2 is C=O); and (B) a curing agent composition comprising one or more crosslinkers that contain functional groups reactive with functional groups of one or more polymers and / or resins; and, optionally, (C) a diluent composition. The present invention further relates to methods for making the coating composition, coating methods and resulting coatings, and methods for using compounds (II) and (III) as corrosion inhibitors.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solvent-borne, two-pack coating composition comprising at least a pigmented and / or filled masterbatch component (A) comprising at least one polyhydroxyl-functional aromatic organic compound and at least one polymer and / or resin having functional groups reactive to at least one crosslinker contained in the hardener component (B); (B) a hardener component, and optionally (C) a solvent component. The present invention further relates to a method for preparing the coating composition, a method for coating a metal substrate with the coating composition, the thus obtained coated substrates, in particular multi-layer coated substrates and their preparation, and a method for using the polyhydroxyl-functional aromatic organic compound in the solvent-borne, two-pack coating composition to impart corrosion protection to a cured coating formed from the coating composition. [Background technology]

[0002] In many areas of metal part painting, for example in the field of car repainting, commercial vehicle painting, aircraft painting, and also in the case of large technical machine systems such as wind power systems, it is usually necessary to protect the respective metal parts used, in particular those made of aluminum and / or aluminum alloys, against corrosion by means of anticorrosive coatings. The demands on corrosion protection are very high, especially since manufacturers often guarantee corrosion protection for many years.

[0003] However, the corrosion of aluminum is significantly different from the corrosion of iron-containing substrates, in particular, filiform corrosion is often observed in aluminum-based substrates, such as pure aluminum or aluminum alloys.

[0004] Anticorrosive pigments are often employed in coating compositions to protect metal substrates from corrosion, but the use of anticorrosive pigments often involves the use of environmentally problematic inorganic lead-based or chromate-based anticorrosive pigments, or particularly problematic organic corrosion inhibitors. Moreover, such pigments are generally used in large quantities, which can significantly alter the properties of the coating composition beyond their primary purpose of providing corrosion protection.

[0005] In particular, in two-component coating compositions, such as automotive refinish coating compositions, where highly reactive polymers, resins and / or crosslinkers are used, certain organic corrosion inhibitors are not considered to be effective because they are consumed by reaction with such polymers, resins and / or crosslinkers.

[0006] For example, in a scientific paper titled "Smart nanocontainer-based anticorrosive bio-coatings: Evaluation of quercetin for corrosion protection of aluminum alloys" (Progress in Organic Coatings 136(2019)105276), Ulaeto et al. propose encapsulating quercetin in mesoporous silica nanocontainers and using the encapsulated quercetin in a room temperature curing, solvent-free, two-part coating composition. The idea is that encapsulation protects quercetin from the reactive components of the coating composition, so that the encapsulated quercetin remains in the nanocontainer in the curing composition until the corrosion phenomenon caused by the increase in pH value to about 10 occurs. Thus, the use of organic corrosion inhibitors in coating compositions without prior protective nanoencapsulation generally results in the undesirable inactivation of such corrosion inhibitors during the curing process. However, although encapsulated organic corrosion inhibitors may not participate in the crosslinking reaction, their corrosion protection action is limited to pH changes to very high pH values ​​to become effective. However, corrosion of metal substrates, such as aluminum-containing substrates, may be caused by other mechanisms in addition to the increase in pH required to release the organic corrosion inhibitor from the mesoporous silica nanocontainers. In particular, corrosion under acidic conditions or environments may occur when the release mechanism of action of the encapsulated corrosion inhibitor is not effective.

[0007] There is a particular need to protect aluminium-based substrates from corrosion, but the coating material should also be suitable for providing corrosion resistance to other metal substrates, such as different types of steel. [Prior art documents] [Non-patent literature]

[0008] [Non-Patent Document 1] Ulaeto et al., “Smart nanocontainer-based anticorrosive bio-coatings: Evaluation of quercetin for corrosion protection of aluminum alloys” (Progress in Organic Coatings 136 (2019) 105276) Summary of the Invention [Problem to be solved by the invention]

[0009] While known techniques often utilize the crosslinking-promoting properties of some anticorrosive pigments or certain organometallic or metal-containing catalysts, the object of the present invention was to achieve excellent anticorrosive properties in primer and / or filler coating compositions by employing certain polyhydroxyl-functional organic compounds, even compounds that exist in nature and are therefore environmentally unproblematic. In particular, the corrosion inhibitors used in the coating materials of the present invention should be effective even in low pH value environments without the need for pH changes and without the need for protection from the components that form the matrix material of the cured coating. In other words, it should not be necessary to encapsulate the corrosion inhibitors used in the present invention, for example, in mesoporous silica nanocontainers. Moreover, if corrosion occurs without pH changes, the inhibitors thus encapsulated will be ineffective, since they will not be released from the encapsulating material.

[0010] The object of the present invention was to overcome the aforementioned drawbacks of the known art and to provide a two-component coating material that can be applied by spray application, in particular as used in automotive repainting, and that tends to provide corrosion protection to different metal and multi-metal substrates, in particular substrates containing aluminum, without pretreatment and without the need for encapsulation of the corrosion inhibitor, such as incorporation in mesoporous silica nanocontainers, etc. Furthermore, the corrosion inhibitor employed should already be effective at very low concentrations in the coating material, thus minimizing detrimental effects and changes on the overall properties of the coating material. [Means for solving the problem]

[0011] The problem to be solved by the present invention is as follows: (A) a. one or more polymers and / or resins containing functional groups reactive with the functional groups of one or more crosslinkers contained in the hardener component (B); b. one or more pigments and / or fillers; and c. one or more species containing a structural unit of formula (I); [ka] (wherein the four residues R 1 Two of the residues are OH and the other two residues are R 1 is H;R 2 ═O or C═O; and R 3 -R 4 is C=C or HC-CH; the asterisk * represents the residue R in formula (II) below. 5 and R 6 or a bond site to the residue CH-CH-CH-CH in formula (III) below), and one or more species selected from the group consisting of species of formula (II), [ka] (In the formula, R 5 teeth [ka] ;R 6 =H or OH, and the star * is R 4 indicates the binding site to; R 7 and R 8 is H or OH, where R 7 and R 8 At least one of is H; R 2 is O), and a species of formula (III) [ka] (In the formula, R 2 is C=O) A masterbatch component comprising: (B) a hardener component comprising one or more crosslinkers that contain functional groups that are reactive toward the functional groups of the one or more polymers and / or resins of masterbatch component (A); and, optionally, (C) Solvent components The problem has been solved by providing a solvent-based two-component coating composition comprising:

[0012] The present invention further provides a method for making the coating composition of the present invention.

[0013] Furthermore, the present invention provides a method for coating a metal substrate, in particular an aluminium-containing metal substrate, with a coating composition according to the present invention, and the substrate thus coated.

[0014] Yet another object of the present invention is a multi-layer coated substrate and a method for producing the same. A further object of the present invention is the use of one or more species of formula (II) and (III) as defined above in a solvent-based two-component coating composition, in particular to impart corrosion protection properties to a cured coating formed from the coating composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The solvent-based two-component coating composition of the present invention The coating composition of the present invention is preferably in the form of a dispersion or solution, more particularly in the form of a dispersion.

[0016] The proportions expressed in % by weight of all components present in the coating composition of the invention, in other words of the components (A), (B), optionally (C) and optionally (D) described hereinafter, are based on the total weight of the coating composition of the invention and preferably in each case total 100% by weight.

[0017] The coating compositions of the present invention are solvent-based, that is, solvent-based or non-aqueous coating compositions.

[0018] The terms "solvent-based", "solvent-based" or "non-aqueous" in connection with the coating composition of the present invention preferably mean a coating composition which comprises as its liquid dilution medium, i.e. as liquid solvent and / or dispersion medium, at least one organic solvent as the main component (with respect to the dilution medium employed). The proportion of organic solvent in the coating composition of the present invention is preferably at least 95.0% by weight or at least 96.0% by weight or at least 97.0% by weight, most preferably at least 99% by weight or at least 99.5% by weight or at least 99.9% by weight, in each case based on the total proportion of the liquid dilution medium present in the coating composition. The liquid dilution medium can be present in the masterbatch component, the hardener component and / or the solvent component or in further constituents or components, if present.

[0019] The viscosity of the coating composition of the present invention is preferably suitable for spray application, for example with a spray gun as used in repainting automobiles. Preferably, the viscosity of the coating composition of the present invention, measured with DIN CUP 4 (according to DIN 53211:1987-06) at a temperature of 20° C., is less than 30 seconds, more preferably less than 25 seconds, particularly preferably 15 to 25 seconds, for example 17 to 23 seconds.

[0020] The coating composition of the invention preferably has a non-volatile fraction in the range of 30 to 90% by weight, more preferably in the range of 40 to 80% by weight, very preferably in the range of 45 to 75% by weight, more particularly 55 to 70% by weight and most preferably in the range of 60 to 65% by weight, in each case based on the total weight of the coating composition.

[0021] The term "non-volatile fraction" as used herein is the calculated total amount of all film-forming components, including all additives, pigments and fillers, as employed in each coating composition. Thus, the non-volatile fraction does not include solvent.

[0022] The term "two-part" or "two-component" in relation to coating compositions refers to such coating compositions in which the chemical reaction leading to crosslinking is initiated by mixing two components (masterbatch and hardener) in a ratio predetermined by the manufacturer (DIN 55945:1996-09) and hardening to form a durable coating. The individual components are not coating materials, since they are not suitable for film formation, are not capable of film formation, or do not form durable coatings. The mixture must be processed within a certain time (pot life or processing time), since after this time the processability or film-forming properties decrease. In two-component spray systems, this is generally not a problem, since mixing here only takes place immediately before application in the spray process (Roempp Lexikon, Lacke und Druckfarben, Georg Thieme Verlag 1998; Keyword: "Zweikomponenten-Lacke").

[0023] The solvent-based two-component coating composition of the present invention is preferably crosslinkable at a temperature in the range of 18°C ​​to 90°C.

[0024] The coating composition of the present invention is preferably a primer coating composition or a filler coating composition, i.e. a coating composition suitable for the production of a primer coating or a filler coating. The terms "primer (coating composition)" (German: "Primer") and "filler (coating composition)" (German: "Fueller") are known to the person skilled in the art and are defined, for example, in Roempp Lexikon, Lacke und Druckfarben, Georg Thieme Verlag 1998.

[0025] Masterbatch component (A) (A) a. Polymers and / or resins containing functional groups The masterbatch component (A) comprises one or more polymers and / or resins that contain functional groups that are chemically reactive with the functional groups of the one or more crosslinkers of the hardener component (B).

[0026] One preferred type of polymer and / or resin is a polyhydroxyl functional polymer and / or resin selected from the group consisting of polyesters, polyethers, polyether polyesters, polyurethanes and poly(meth)acrylates. In such polymers and resins, the functional groups that chemically react with the functional groups of one or more crosslinkers of the hardener component (B) contain at least two hydroxyl groups. However, the present invention does not exclude other functional groups, such as primary or secondary amine groups, that chemically react with the functional groups of one or more crosslinkers of the hardener component (B).

[0027] For the purposes of the present invention, the expressions "(meth)acryloyl" or "(meth)acrylate" encompass in each case the definitions "methacryloyl" and / or "acryloyl", or "methacrylate" and / or "acrylate". Poly(meth)acrylates can thus be obtained by polymerizing acrylate monomers, methacrylate monomers or both, optionally including other ethylenically unsaturated monomers.

[0028] A second preferred type of polymer and / or resin that chemically reacts with the functional groups of one or more crosslinkers of the hardener component (B) is one that contains at least two oxirane groups. Such polymers or resins are typically called epoxy resins. However, epoxy groups may be incorporated into poly(meth)acrylates by using oxirane group-containing ethylenically unsaturated monomers in the polymerization reaction.

[0029] Polyhydroxyl-functional polymers and / or resins Polyhydroxyl-functional polymers and / or resins have an average of at least two hydroxyl groups per polymer or resin molecule.

[0030] As polyhydroxyl-functional polymers and / or resins it is possible to use all compounds known to those skilled in the art which have an average of at least two hydroxyl groups per molecule and which are oligomeric and / or polymeric. As polyhydroxyl-functional polymers and / or resins it is also possible to use mixtures of different oligomeric and / or polymeric polyols.

[0031] Preferably, the polyhydroxyl-functional polymers and / or resins have a weight average molecular weight Mw, measured by means of gel permeation chromatography (GPC) against polystyrene standards, of more than 500 g / mol, in particular from 800 to 100,000 g / mol, more in particular from 1000 to 50,000 g / mol.

[0032] Particularly preferred polyhydroxyl-functional polymers and / or resins are selected from the group consisting of polyester polyols, polyurethane polyols, polysiloxane polyols and poly(meth)acrylate polyols.

[0033] Preferably, the polyhydroxyl-functional polymers and / or resins have a hydroxyl number of 30-400 mg KOH / g, more preferably 100-300 KOH / g. The hydroxyl number (OH number) indicates the number of mg of potassium hydroxide that corresponds to the amount of acetic acid bound when acetylating 1 g of substance. It is measured by boiling the sample with acetic anhydride-pyridine and titrating the acid formed with potassium hydroxide solution (DIN 53240-2). In the case of pure poly(meth)acrylates, the OH number can also be determined with sufficient accuracy by calculation based on the OH-functional monomers used.

[0034] Preferably, the glass transition temperature of the polyhydroxyl functional polymers and / or resins, determined by DSC measurement according to DIN EN ISO 11357-2, is between -150°C and 100°C, more preferably between -120°C and 80°C.

[0035] Suitable polyester polyols are described, for example, in EP-A-0 994 117 and EP-A-1 273 640. In one or more embodiments, polyurethane polyols are prepared by reaction of polyester polyol prepolymers with suitable di- or polyisocyanates, as described, for example, in EP-A-1 273 640. Suitable polysiloxane polyols are described, for example, in WO-A-01 / 09260, the polysiloxane polyols described therein may preferably be used in combination with other polyols, more particularly those having a high glass transition temperature.

[0036] The most preferred polyhydroxyl-functional polymers and / or resins include one or more poly(meth)acrylate polyols. In addition to the poly(meth)acrylate polyol(s), polyhydroxyl-functional polymers and / or resins can be employed, examples of which include polyester polyols, polyurethane polyols, and polysiloxane polyols, especially polyester polyols.

[0037] Preferably, the poly(meth)acrylate polyols which can be used are copolymers and have a weight-average molecular weight Mw of 1000 to 20,000 g / mol, more particularly 1500 to 10,000 g / mol, measured by means of gel permeation chromatography (GPC) in each case against polystyrene standards.

[0038] Preferably, the glass transition temperature of the poly(meth)acrylate polyol copolymer is from −100 to 100° C., more in particular from −60 to less than 20° C. (determined by DSC measurement according to DIN-EN-ISO 11357-2).

[0039] Preferably, the poly(meth)acrylate polyol copolymer has an OH number of 60 to 300 mg KOH / g, more particularly 70 to 200 KOH / g, and an acid number of 0 to 30 mg KOH / g.

[0040] The hydroxyl number (OH number) is determined as described above (DIN 53240-2). The acid number here indicates the number of mg of potassium hydroxide consumed to neutralize 1 g of the compound in question (DIN EN ISO 2114).

[0041] Preferably, as hydroxyl-functional monomeric building blocks, hydroxyalkyl (meth)acrylates are used, such as more particularly 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0042] As further monomeric building blocks of the poly(meth)acrylate polyol copolymers, alkyl(meth)acrylates are used, such as, preferably, ethyl(meth)acrylate, propyl(meth)acrylate, isopropyl(meth)acrylate, butyl(meth)acrylate, isobutyl(meth)acrylate, tert-butyl(meth)acrylate, amyl(meth)acrylate, hexyl(meth)acrylate, ethylhexyl(meth)acrylate, 3,3,5-trimethylhexyl(meth)acrylate, stearyl(meth)acrylate or lauryl(meth)acrylate; cycloalkyl(meth)acrylates, such as, for example, cyclopentyl(meth)acrylate, isobornyl(meth)acrylate or cyclohexyl(meth)acrylate.

[0043] As further monomeric constituents of the poly(meth)acrylate polyol copolymers, it is also possible to use vinyl aromatic hydrocarbons, such as vinyl toluene, alpha-methylstyrene, or in particular styrene, amides or nitriles of acrylic or methacrylic acid, vinyl esters or vinyl ethers, and also, preferably in particular small amounts of acrylic acid and / or methacrylic acid.

[0044] Epoxy Resin Epoxy resins contain two or more oxirane rings, and can be converted to epoxy resins cured with crosslinkers by reaction of the oxirane rings. Common epoxy resins are prepared by reaction of reactive phenols, alcohols, acids, and amines with epichlorohydrin, and contain oxirane rings in the form of glycidyl groups. There are a virtually infinite number of reactive structures that can be reacted with epichlorohydrin to form epoxy resins, so there are many resins available industrially. In addition, unsaturated aliphatic and alicyclic compounds have been directly epoxidized, for example, with peracetic acid.

[0045] For the purposes of the present invention, in principle, all epoxy resins commonly used in formulating solvent-based two-component coating compositions can be used.The epoxy resins that can be used according to the present invention are preferably selected from the group consisting of glycidyl ethers, such as bisphenol-A-diglycidyl ether, bisphenol-F-diglycidyl ether, epoxide-novalac, epoxide-o-cresol-novalac, 1,3-propane-, 1,4-butane- or 1,6-hexane-diglycidyl ether and polyalkylene oxide glycidyl ethers; glycidyl esters, such as diglycidyl hexahydrophthalate; glycidyl amines, such as diglycidyl aniline or tetraglycidyl methylene dianiline; cycloaliphatic epoxides, such as 3,4-epoxycyclohexyloxyethane or 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; and glycidyl isocyanurates, such as trisglycidyl isocyanurate.

[0046] (A)b. Pigments and / or fillers The masterbatch component (A) further comprises one or more pigments and / or fillers.

[0047] The term "pigment" is known to the skilled person, for example from DIN 55945 (date: October 2001). "Pigments" in the sense of the present invention preferably refer to powder- or platelet-like compounds that are substantially, preferably completely insoluble in the medium that surrounds them, for example in the coating composition of the present invention. Pigments as defined herein differ from "fillers" at least in their refractive index, the refractive index of pigments being 1.7 or higher.

[0048] Suitable pigments are preferably selected from the group consisting of organic and inorganic color-imparting pigments (including black and white pigments), effect pigments and mixtures thereof.

[0049] Examples of suitable inorganic color-imparting pigments include white pigments, such as zinc white, zinc sulfide or lithopone; black pigments, such as carbon black, iron manganese black or spinel black; chromatic pigments, such as chromium oxide, chromium oxide hydrate green, cobalt green or ultramarine green, cobalt blue, ultramarine blue or manganese blue, ultramarine violet or cobalt violet and manganese violet, red iron oxide, cadmium sulfoselenium, molybdate red or ultramarine red; brown iron oxide, mixed brown, spinel phase and corundum phase or chrome orange; or yellow iron oxide, nickel titanium yellow, chrome titanium yellow, cadmium sulfide, cadmium zinc sulfide, chrome yellow or bismuth vanadate. Examples of further inorganic color-imparting pigments are, for example, aluminum oxide, aluminum oxide hydrate, in particular boehmite, titanium dioxide, zirconium oxide, cerium oxide, and mixtures thereof. Examples of suitable organic color-imparting pigments include monoazo pigments, disazo pigments, anthraquinone pigments, benzimidazole pigments, quinacridone pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, dioxazine pigments, indanthrone pigments, isoindoline pigments, isoindolinone pigments, azomethine pigments, thioindigo pigments, metal complex pigments, perinone pigments, perylene pigments, phthalocyanine pigments, or aniline black. Effect pigments include metallic effect pigments, but also pearlescent pigments, and the like.

[0050] The term "filler" is known to the skilled person, for example from DIN 55945 (date: October 2001). "Filler" in the sense of the present invention preferably refers to a substance that is substantially insoluble, preferably completely insoluble, in the coating composition of the present invention and is more particularly used to increase the volume. "Filler" in the sense of the present invention differs from "pigments" at least in its refractive index, the refractive index of the filler being less than 1.7. Any conventional filler known to the skilled person can be used. Examples of suitable fillers include kaolin, dolomite, calcite, chalk, calcium sulfate, barium sulfate, graphite, silicates, such as magnesium silicate, more particularly corresponding phyllosilicates, such as hectorite, bentonite, montmorillonite, talc and / or mica, silica, in particular fumed silica, hydroxides, such as aluminum hydroxide or magnesium hydroxide, or organic fillers, such as textile fibers, cellulose fibers, polyethylene fibers, or polymer powders. For further details, see Römpp Lexikon Lacke und Druckfarben, Georg Thieme Verlag, 1998, pp. 250 ff., "Fillers".

[0051] The above-mentioned pigments and fillers can be suitably employed in the coating composition of the present invention, but pigments containing environmentally problematic elements such as Pb, Cd, Cr, Cu, Mo, Hg, Se or Zn are less preferred, and it is most preferable that they are not included in the coating composition of the present invention.

[0052] Although the pigments and / or fillers as described above may contain silica, it is expressly stated here that mesoporous silica nanocontainers or silica containing encapsulated species of formula (II) and (III) are preferably not included in the coating composition of the present invention. The mere simultaneous presence of silica and any of the species of formula (II) and (III) should not be confused with the rather elaborate formation of mesoporous silica nanocontainer encapsulated corrosion inhibitors as taught by Uleato et al. (see above). As stated above, one object of the present invention was to avoid the need for encapsulation of corrosion inhibitors, i.e., encapsulation of any of the species of formula (II) and (III).

[0053] The mass ratio of the pigment and / or filler (A)b. to (A)a., i.e., the one or more polymers and / or resins containing functional groups reactive towards the functional groups of the one or more crosslinkers contained in the hardener component (B), is preferably 6:1 to 1:6, more preferably 5:1 to 1:5, even more preferably 5:1 to 1:2 or 5:1 to 1:1, for example 4:1 to 2:1.

[0054] (A)c. A species containing a structural unit of formula (I) The masterbatch composition (A) further comprises one or more species containing structural units of formula (I): [ka] (wherein the four residues R 1 Two of the residues are OH and the other two residues are R 1 is H;R 2 ═O or C═O; and R 3 -R 4 is C=C or HC-CH; the asterisk * represents the residue R in formula (II) below. 5 and R 6 or a bond site to the residue CH-CH-CH-CH in formula (III) below), and one or more species selected from the group consisting of species of formula (II), [ka] (In the formula, R 5 teeth [ka] ;R 6 =H or OH, and the star * is R 4 indicates the binding site to; R 7 and R 8 is H or OH, where R 7 and R 8 At least one of is H; R 2 =O), and a species of formula (III) [ka] (In the formula, R 2 is C=O) Further includes:

[0055] Species of formulas (II) and (III) above, and particularly preferred ones described below, can be incorporated in the coating compositions of the invention to provide cured coatings with corrosion inhibiting properties.

[0056] Of the species of formula (II), preferred are species selected from the group consisting of flavonols, such as quercetin and morin; and flavanones, such as naringenin.

[0057] Particularly preferred species of formula (II) are those of formula (IIa) [ka] (In the formula, R 7 and R 8 is defined as above; and aR 6 is OH and R 3 -R 4 is C=C (flavonol); or bR 6 is H and R 3 -R 4 is HC-CH (flavanone).

[0058] In the most preferred species of formula (IIa), R 3 -R 4 is C=C, and R 6 and R 8 is OH and R 7 is H (i.e., quercetin).

[0059] Of the species represented by formula (III), those selected from the group consisting of dihydroxyanthraquinones are preferred, most preferred being 1,4-dihydroxyanthraquinone and 1,2-dihydroxyanthraquinone (i.e. alizarin).

[0060] This species has been employed in coating compositions without being encapsulated or otherwise associated with mesoporous silica nanocontainers, as described by Ulaeto et al. Surprisingly, despite the fact that these species of formulae (II) and (III) contain some hydroxy groups and thus are in principle susceptible to reaction with epoxy resins in the same manner as crosslinkers containing free isocyanate groups, coating compositions containing the respective species provide excellent corrosion protection when applied onto and subsequently cured on metal substrates, particularly aluminum-containing metal substrates.

[0061] The total amount of species of formula (II) and / or (III) employed in the coating composition of the present invention is preferably in the range of 1 ppm to 15 wt.%, more preferably 0.1 to 5 wt.%, most preferably 0.5 to 2.5 wt.%, based on the total weight of the masterbatch component (A). If this amount is below the lower limit, no mitigation of the corrosive effect is detected; if this amount exceeds the upper limit, film formation may be inhibited or the curing reaction may be poisoned.

[0062] Hardener component (B) The coating composition, which is a two-part coating composition, comprises at least one crosslinker in the hardener component (B), such as: a polyisocyanate crosslinker having free isocyanate groups that can react with the hydroxyl and active hydrogen-containing groups (e.g., primary or secondary amino groups) of one or more polymers and / or resins contained in the masterbatch component (A); or a polyamine that can react with, for example, an epoxy resin that may be contained in the masterbatch component (A).

[0063] Since it is the nature of the two-part composition that the crosslinking component (B) is stored separately from the masterbatch composition (A) to avoid premature crosslinking, the hardener component (B) does not contain any components that are reactive towards the crosslinker. However, the crosslinking component may contain further inert components, such as a solvent or solvent mixture in which the crosslinker is dissolved or dispersed, or further inert additives as described below.

[0064] Crosslinking Agents for Polyhydroxyl-Functional Polymers and / or Resins When the functional groups of the at least one polymer and / or resin in the masterbatch component (A) are selected from hydroxyl groups, primary and secondary amino groups, it is particularly preferred to use one or more polyisocyanates (as that term is used herein to include diisocyanates) having free isocyanate groups as crosslinking agents.

[0065] Examples of suitable polyisocyanate crosslinking agents include, but are not limited to, alkylene polyisocyanates such as hexamethylene diisocyanate, 4- and / or 2,4,4-trimethylhexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-diisocyanatocyclohexane, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate), 2,4'- and / or 4,4'-diisocyanatodicyclohexylmethane, 3-isocyanatomethyl-3,5,5-trimethylcyclohexylisocyanate, aromatic polyisocyanates such as 2,4'- and / or 4,4'-diisocyanatodiphenylmethane, 2,4- and / or 2,6-diisocyanatotoluene, naphthylene diisocyanate, and mixtures of these polyisocyanates. Generally, polyisocyanates having an average of three or more isocyanate groups are used, which may be derivatives or adducts of diisocyanates. Useful polyisocyanates are obtained by reacting an excess of isocyanates with water, polyols (e.g., ethylene glycol, propylene glycol, 1,3-butylene glycol, neopentyl glycol, 2,2,4-trimethyl-1,3-pentanediol, hexamethylene glycol, cyclohexanedimethanol, hydrogenated bisphenol A, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, glycerin, sorbitol or pentaerythritol), or by reacting the isocyanates with themselves to obtain isocyanurates.Examples include polyisocyanates containing biuret groups, such as those described in U.S. Pat. Nos. 3,124,605 ​​and 3,201,372 or DE-OS 1,101,394; polyisocyanates containing isocyanurate groups, such as those described in U.S. Pat. No. 3,001,973, DE-PS 1,022,789, 1,222,067 and 1,027,394, and DE-OS 1,929,034 and 2,004,048; polyisocyanates containing urethane groups, such as those described in DE-OS 953,012, BE-PS 752,261 or U.S. Pat. Nos. 3,394,164 and 3,644,457; polyisocyanates containing carbodiimide groups, such as those described in DE-PS Nos. 1,092,007, 3,152,162, and DE-OS 2,504,400, 2,537,685, and 2,552,350; allophanate group-containing polyisocyanates, such as those described in GB-PS 994,890, BE-PS 761,626, and NL-05 7,102,524; and uretdione group-containing polyisocyanates, such as those described in EP-A 0,377,177, each of which is incorporated herein by reference.

[0066] Such isocyanate crosslinkers are typically stored separately and combined with the polyhydroxyl functional polymer and / or resin immediately prior to application.

[0067] The coating composition may use a curing catalyst for the urethane reaction, such as a tin catalyst. Representative examples are tin and bismuth compounds, including, but not limited to, dibutyltin dilaurate, dibutyltin oxide, and bismuth octoate. If used, the catalyst is typically present in an amount of about 0.05 to 2% by weight tin, based on the weight of total solids.

[0068] Crosslinking Agent for Epoxy Resins Below, we will explain the crosslinking agents that are usually used for curing epoxy resins, which can be used in the masterbatch component (A) as resins that contain functional groups that are reactive to the functional groups present in the crosslinking agent contained in the hardener component (B). Crosslinking agents of this type are referred to as "epoxide crosslinking agents" in their function according to the relevant literature (for example: Kittel, "Lehrbuch der Lacke und Beschichtungen", Vol. 2, 2nd edition, 1998, pp. 267-318).

[0069] An epoxide crosslinker is a compound having a functionality of 2 or more, in which the functional group can react with an oxirane group (a compound having an active hydrogen, especially a hydrogen bonded to nitrogen or oxygen). Preferably, the crosslinker is employed substantially stoichiometrically with respect to the epoxy resin. The concentration of oxirane rings in the epoxy resin can be determined, for example, by titration. The amount of crosslinker required can be calculated from the equivalent of active hydrogen ("H active equivalent") of the crosslinker.

[0070] The crosslinking agent that can be used according to the present invention is preferably one selected from the group consisting of polyamines (including here diamines) and polyamides. Particularly preferred are polyamines. Thus, in its most preferred embodiment, the curing agent may be referred to as an amine-based crosslinking agent.

[0071] Particularly preferred polyamines may be selected from the group of aliphatic amines, such as diethylenetriamine, triethylenetetramine or 3,3',5-trimethylhexamethylenediamine; cycloaliphatic amines, such as 1,2-cyclohexyldiamine, isophoronediamine and its isomeric mixtures, or m-xylylenediamine; aromatic amines, such as methylenedianiline or 4,4-diaminodiphenylsulfone; modified amines, such as Mannich bases (e.g. diethylenetriamine-phenol Mannich base), or the amine adduct of 3,3',5-trimethylhexamethylenediamine and bisphenol A diglycidyl ether.

[0072] Particularly preferred epoxide crosslinkers of the polyamide type are, for example, polyaminoamides or dicyandiamide.

[0073] Solvent component (C) The coating composition according to the invention comprises, as component (C), at least one organic solvent. The concept of "organic solvent" is familiar to the person skilled in the art, for example from the European Directive 1999 / 13 / EC of 11 March 1999.

[0074] As component (C) of the coating composition of the present invention, all organic solvents known to those skilled in the art are suitable, as long as the solvent is not reactive with the constituents of the component in which it is used. Most preferred are aprotic organic solvents.

[0075] The at least one organic solvent is preferably selected from the group consisting of aliphatic hydrocarbons, aromatic hydrocarbons such as toluene and / or xylene, ketones such as acetone, N-methylpyrrolidone, N-ethylpyrrolidone, methyl isobutyl ketone, isophorone, cyclohexanone, and methyl ethyl ketone, esters such as methoxypropyl acetate, ethyl acetate, butyl glycol acetate, and butyl acetate, amides such as dimethylformamide, and mixtures thereof.

[0076] Further optional components of the coating composition of the present invention The coating composition of the present invention may optionally contain at least one further component, such as a typical additive used in two-component coating compositions.

[0077] The at least one further component or additive is preferably selected from the group consisting of antioxidants, antistatic agents, moisture-resistant and dispersing agents, antisettling agents, emulsifiers, flow control aids, solubilizers, defoamers, wetting agents, stabilizers, UV and / or light stabilizers, light protection agents, degassing agents, inhibitors, catalysts, waxes, flexibilizers, flame retardants, hydrophobizing agents, hydrophilizing agents, thixotropic agents, impact modifiers, processing aids, plasticizers, and mixtures of the aforementioned components. The amount of the preferably at least one further component in the coating composition of the invention can vary very widely depending on the intended use. The total amount of such components is preferably 0.01 to 10.0% by weight, more preferably 0.05 to 8.0% by weight, very preferably 0.1 to 6.0% by weight, particularly preferably 0.1 to 5.0% by weight, in each case based on the total weight of the coating composition of the invention.

[0078] The additional components may be part of the masterbatch component (A), the hardener component (B) and the solvent component (C) or may alternatively be added in the form of a separate component (D). The additional components are preferably chemically inert to the components of the respective components in which they are utilized.

[0079] Method for producing the coating composition according to the present invention The present invention further provides a method for making the coating composition of the present invention.

[0080] The method for producing the coating composition of the present invention preferably comprises the steps of: i. first, mixing (A)a. one or more polymers and / or resins containing functional groups reactive to functional groups of one or more crosslinkers contained in the hardener component (B) with at least a portion of (A)b. one or more pigments and / or fillers, wherein (A)a. one or more polymers and / or resins containing functional groups reactive to functional groups of one or more crosslinkers contained in the hardener component (B) are optionally and preferably pre-dissolved and / or pre-dispersed in at least a portion of the organic solvent contained in the final coating composition; ii. adding the remainder of A(b). one or more pigments and / or fillers (if not fully added in step i.) while mixing, and adding, while mixing, one or more species of formula (II) and / or (III) as defined above; iii. milling the mixture thus obtained, preferably using a bead mill, until the Hegman fineness is determined to be preferably less than 25 μm, more preferably less than 23 μm, and most preferably less than 20 μm; and iv. adding hardener component (B), optionally solvent component (C), and optionally component (D) under mixing conditions to achieve a homogenous coating composition. and preferably maintaining the temperature during all mixing steps at less than 50°C.

[0081] Step iv. is preferably carried out with a spray gun, such as those used for example in car repainting.

[0082] Method for coating a substrate with a coating composition according to the present invention The present invention further provides a method of coating a metal substrate with a coating composition according to the present invention, wherein the method comprises at least the step (i) of contacting the metal substrate with the coating composition of the present invention.

[0083] The term "contacting" in the sense of the present invention preferably refers to spraying the coating composition of the present invention onto a substrate to form a coating layer on the substrate.

[0084] Such spraying is preferably carried out by electrostatic spraying, air spray coating or airless spray coating. The dry thickness of the obtained coating film is preferably in the range of 25 to 100 μm, more preferably 30 to 90 μm, and most preferably 40 to 80 μm, when dried at 23° C. for 60 minutes. The coating film may be cured by heating at a temperature preferably in the range of 18 to 90° C., more preferably 30 to 80° C., and most preferably 50 to 70° C., for 5 to 120 minutes.

[0085] However, if the thus coated substrate, preferably at least partially dried, is further coated with a subsequent coating composition, such as a topcoat coating composition or a clearcoat coating composition, and fully cured together with such subsequently applied coating layer, the curing step to full curing of the coating layer can be at least partially omitted. This possibility of a wet-on-wet coating method is further explained below when describing a method for coating a substrate with a multi-layer coating.

[0086] metal base material The substrates used according to the invention are preferably selected from the group consisting of iron, steel, aluminum or alloys thereof, more preferably aluminum-based alloys, which alloys can optionally comprise at least one further metal and / or metalloid, for example copper. Preferably, the substrates here each have at least one surface of iron, steel, aluminum or alloys thereof, more preferably they are entirely composed of iron, steel, aluminum or alloys thereof. Suitable steels are preferably steels selected from the group consisting of cold-rolled steel, hot-rolled steel, high-strength steel, galvanized steel, for example dipping galvanized steel, alloy galvanized steel (for example Galvalume®, Galvannealed® or Galfan®), and aluminized steel. Examples of suitable alloys include alloys of aluminum and copper. Particularly preferred are substrates made of aluminum or aluminum-containing alloys.

[0087] The substrates used here may in particular be metal bodies of automobiles and commercial vehicles, but also of aircraft, ships, etc.

[0088] Before being coated with the coating composition of the present invention, the metal substrate used according to the method for coating a substrate according to the present invention may be pretreated with a suitable, preferably aqueous, pretreatment composition. Such pretreatment compositions are known to the skilled person and are commercially available. For example, substrates based on aluminum, aluminum or aluminum-containing alloys may be pretreated by tartaric-sulfuric anodizing (TSA) according to DIN EN 4704 (date: May 2012). Steel substrates or steel-based substrates may be pretreated by pretreatment, for example, according to DIN EN ISO 12944-4 (date: July 1998). The grade of the steel substrates or steel-based substrates used is preferably at least 2.5. The grade of the steel may be determined according to DIN EN ISO 8501-1 (date: December 2007).

[0089] All preferred embodiments described herein in relation to the inventive coating composition are also preferred embodiments of the inventive coating composition to be used in the inventive method for coating a substrate.

[0090] Method for coating a substrate with a multi-layer coating The present invention further comprises at least the following steps: (i) contacting a metal substrate with the coating composition of the present invention for application of the coating composition to the substrate, particularly preferably by spray coating; and (ii) applying a further coating composition, preferably a topcoat coating composition or a clearcoat coating composition, to the coating layer formed by applying the coating composition in step (i), preferably by spray coating. The present invention provides a method for coating a substrate with a multi-layer coating, comprising:

[0091] All preferred embodiments described herein in relation to the inventive coating composition are also preferred embodiments of the inventive coating composition used in the inventive method for coating a substrate with a multi-layer coating. The same applies to metal substrates for which the method for coating a substrate with a primer and / or filler coat has been described.

[0092] A further coating composition, more particularly a topcoat coating composition or a clearcoat coating composition, most preferably a topcoat coating composition, is usually applied to the coating layer formed in step (i). The coating layer formed in step (i) is preferably dried before the application of a further coating composition according to step (ii). The term "drying" in the context of the present invention preferably refers to the removal of at least a portion of the solvent from the applied coating material. Drying may first be performed at 15-30°C for 10-120 minutes. Some curing may occur during drying, but it is preferred that the layer formed in step (i) does not cure, or at least does not cure completely (wet-on-wet method).

[0093] The general techniques for application of the further coating composition according to step (ii) are similar to those described above for the coating layer formed from the coating composition according to the invention. The further coating composition, e.g. the topcoat coating composition, is applied at a conventional and known film thickness, e.g. a dry film thickness after curing in the range of 15 to 100 μm, more particularly 40 to 80 μm or 50 to 75 μm.

[0094] Curing is carried out according to conventional and known techniques, for example by heating in a forced air oven or by irradiation with infrared lamps. Photocuring by UV irradiation is also possible in the case of radiation curing systems. Curing may be carried out at elevated temperatures, for example in the range of about 15° C. to 90° C., preferably at 40-80° C., for example in the range of 50-70° C. The duration of the curing step is likewise individually selected. For example, curing may be carried out over a period of 5 to 120 minutes, preferably 15 to 45 minutes. Curing can also be optionally preceded by a flashing or pre-drying step, for example for a period of 1 to 60 minutes, preferably at room temperature (i.e. 23° C. in the context of the present invention). After step (ii) has been carried out, it is particularly preferred to dry or cure for a period of 15 minutes to 2 hours, preferably at 40 to 80° C., more preferably at 50 to 70° C.

[0095] Further provided by the present invention are multi-layer coatings obtainable by the method of the present invention.

[0096] The present invention further provides a metal substrate coated with the coating composition of the present invention. The present invention further provides a part or article manufactured from at least one substrate thus coated. Suitable substrates for use in this method are the same as those described herein above.

[0097] Method of using species according to formulae (II) and (III) to provide corrosion protection The present application also relates to the use of one or more species of formula (II) and (III) as defined above in solvent-based two-component coating compositions, in particular for providing corrosion protection to cured coatings formed from the coating compositions.

[0098] All embodiments of the preferred species according to formulae (II) and (III) and all embodiments relating to the part of the solvent-based two-part coating compositions described herein in relation to the coating compositions of the invention are also preferred embodiments of the method of use of the invention.

[0099] The present invention will now be described more specifically with reference to experimental data. EXAMPLES

[0100] test Acid Salt Spray Test (AASS) The Acid Salt Spray Mist Test (AASS) is used to determine the corrosion resistance of coatings on substrates. According to DIN EN ISO 9227 (date: June 2017), the Acid Salt Spray Mist Test was carried out on a coated conductive substrate, namely aluminium. Here, the investigated samples were in a chamber where they were continuously sprayed with a 5% common salt solution with a controlled pH in the range of 3.1-3.3 at a temperature of 35°C for a duration of 1008 hours. This spray deposited on the investigated samples and covered them with a corrosive film of salt water.

[0101] Since the substrate corrodes along the score lines during the DIN EN ISO 9227 AASS salt spray test, the coating on the investigated samples was cut down to the substrate with a knife before the acid salt spray test according to DIN EN ISO 9227 AASS in order to be able to investigate the level of undermining according to DIN EN ISO 4628-8 (date: 01.03.2013). As a result of the corrosion process, the coating is more or less damaged during the test. The degree of undermining (in mm) is an indicator of the corrosion resistance of the coating. Note that the average undermining level stated in the results below is the average of the individual values ​​evaluated for 3-5 panels, and the individual value for a panel is the average of the undermining level at 11 measurement points on the panel.

[0102] Gloss, blister, adhesiveness The gloss and adhesion were determined before and after a constant weather test with an exposure time of 240 h. After the constant weather test, the formation of blisters was also evaluated. The constant weather test was carried out according to EN ISO 6270-2 (April 2018) with an exposure time of 240 h.

[0103] The gloss was evaluated at an angle of 60° on ten different spots on one coated specimen before and after a constant climate test according to DIN EN 13523-2 (August 2014). The average values ​​with one-digit accuracy are reported in the results.

[0104] The blister grade was assessed according to DIN EN ISO 4628-2 (July 2016) according to the density of the blisters and their size. The assessment was carried out directly after the constant climate test and subsequent relaxation periods of 1 h and 24 h at ambient conditions (22°C, 50% rh).

[0105] The adhesion was evaluated by a cross-cut test according to ISO 2409. A cross-hatch pattern was made from the coating to the substrate using a multi-blade cutting tool. The delaminated areas of the coating were removed by brushing with a soft brush. Then adhesive tape was applied over the cross-hatch and all delaminated areas of the coating were removed. Classification was done according to table 1 of ISO 2409. The cross-hatch test was performed before and after the constant climate test. After the climate-controlled test, the cross-hatch test was performed after 1 hour and 24 hour recovery times. During the climate-controlled test, the cross-hatch was covered with adhesive tape to avoid corrosion of the prepared cross-hatch.

[0106] Filler Coating Composition Solvent-based two-part hydroxyl / isocyanate filler coating composition Table 1 lists the ingredients (parts by weight) of comparative filler coating compositions C1 and C2, and filler coating compositions E1-E4 of the present invention. Masterbatch composition (A) ("A pack") contains a hydroxyl group-containing polymer (polyacrylate polyol), a pigment, and a filler (TiO 2 and BaSO 4), solvents (xylene and butyl acetate), and 0.50 or 1.00 parts by weight of corrosion inhibitors (I1, I3, and I4) for the inventive examples and 1 part by weight of 3-methylanthraquinone (I2) for comparative composition C2. The hardener component (B) ("B pack") contains an isocyanate group-containing aliphatic hardener and a solvent mixture.

[0107] Positions 1-7 and 10 in Table 1 are parts by weight based on 100% solids. However, the polyacrylate polyol in position 1 was used pre-dispersed in butyl acetate / xylene (3:1; w / w) as a dispersion with 65% solids by weight. The solvent content of this dispersion was assigned to positions 8 and 9, and only the solids of this dispersion was assigned to position 1. Furthermore, the isocyanate hardener in position 10 was used pre-dissolved in the solvent mixture in position 11.

[0108] To prepare inventive filler coating compositions E1-E4 containing different corrosion inhibitors I1, I3 and I4 and comparative filler coating composition C2 (containing substance I2), the amounts of positions 1, 2, 3, 8 and 9 used in comparative filler coating composition C1 were reduced to maintain the same pigment to polyacrylate polyol weight ratio of 74:26 in masterbatch component (A) and solvent content of about 21% by weight of masterbatch component (A) for all filler coating compositions. The amount of isocyanate curing agent in hardener component (B) was selected to provide a molar ratio of OH groups (from polyacrylate polyol) to NCO groups (from isocyanate curing agent) of 1:1.08.

[0109] For all filler coating compositions, positions 1 and 2 were fed into a mixing vessel and positions 3-9 were added while mixing at about 1000-1500 rpm. The resulting mixture was then mixed for a further 30 minutes at about 1500 rpm using a dissolver (VMA Getzmann, Dispermat CN20) while maintaining the temperature below 50° C. (C1: about 47° C.; E1-E5: about 36° C.). For composition C1, the determined Hegman fineness was about 23 μm (DIN EN ISO 1524, June 2013). Inventive filler coating compositions E1-E4 and comparative filler coating composition C2 were further milled in a bead mill (0.5 L grinding vessel; 200 g Siliquarzit® pearls 1.8-2.2 mm per 400 g masterbatch component (A)) at about 2000-2100 rpm under maximum cooling for various times (C2: 45 min; E1: 90 min; E2: 300 min; E3: 50 min; and E4: 60 min) to obtain a Hegman fineness of less than about 23 μm (C2: 23 μm; E1: 20 μm; E2: 20 μm; E3: <23 μm; and E4: <23 μm).

[0110] To obtain the final filler coating compositions C1, C2 and E1-E4 for application to aluminum alloy panels, the masterbatch component (A) and the hardener component (B) were thoroughly mixed and diluted with the solvent composition S (1-methoxypropyl acetate, 2-butyl acetate and xylol; in C1: 0 wt %; in C2, E1-E4: about 10 wt %) to a DIN Cup 4 spray application viscosity at 20° C. of about 19 seconds to about 22 seconds.

[0111] [Table 1]

[0112] 1 Polyacrylate polyol (solid; OH number: 149 mg KOH / g, hydroxyl equivalent: 378), 2 1,4-Dihydroxyanthraquinone 33-Methylanthraquinone (not of the present invention) 4 Alizarin (1,2-dihydroxyanthraquinone) 5 Quercetin 6. Mixture of aliphatic polyisocyanate oligomers based on IPDI and HDI 7 A mixture of the following solvents is used to dilute position 10:

[0113] Solvent-based, two-part epoxy / amine filler coating composition Table 2 lists the ingredients (parts by weight) of comparative filler coating compositions C3 and C4, and filler coating compositions E5-E8 of the present invention. Masterbatch composition (A) ("A pack") is a mixture of epoxy resin, wetting and dispersing additive, pigment (TiO 2 , BaSO 4 and platelet talc) and solvents (xylene, methoxypropanol, isobutanol), and in the case of the examples of the present invention, 0.50 or 1.00 parts by weight of corrosion inhibitors (I1, I3, and I5). The hardener component (B) ("B pack") contains an amine group-containing hardener mixture and a solvent mixture.

[0114] Positions 1-9 and 17 in Table 2 are parts by weight based on 100% solids. However, the epoxy resin mixture in position 1 was pre-dispersed in the solvent in positions 10 and 11 and used, and wetting and dispersing agents were pre-dissolved in positions 12 and 13. Additionally, the amine hardener mixture in position 17 was pre-dissolved in the solvent mixture in position 18 and used.

[0115] To prepare inventive filler coating compositions E5-E8 and comparative filler coating composition C4 containing different corrosion inhibitors I1, I3 and I4 and non-inventive compound I2, the amounts of positions 1-5, 14 and 15 used in the comparative filler coating compositions were reduced to maintain the same pigment to epoxy resin weight ratio of 70:30 and solvent content of about 24 wt% in masterbatch component A for all filler coating compositions. The amount of amine hardener mixture in hardener component (B) was selected to provide a molar ratio of epoxy groups (from the epoxy resin mixture) to amine groups (from the amine hardener mixture) of 100:16.45.

[0116] For all filler coating compositions, positions 1, 10 and 11 were fed into a mixing vessel and position 2 (premixed with positions 12 and 13) was added. This mixture was mixed for 10 minutes at 1500 rpm using a dissolver (VMA Getzmann, Dispermat CN20) followed by the addition of 15, 4, 5 and 14 in that order, then positions 6-9 and finally 3. The resulting mixture was then mixed for an additional 30 minutes at approximately 1500 rpm while maintaining a temperature of 33-36°C. The filler coating compositions were further milled in a bead mill (0.5 L milling vessel; 202 g Siliquarzit® pearls 1.8-2.2 mm per 400 g masterbatch component A) at about 2000 rpm under cooling for various times (C3: 70 min; C4: 70 min; E5: 60 min; E6: 60 min; E7: 70 min; and E8: 90 min) to obtain Hegman finenesses of less than about 23 μm (after 4:1 dilution with butyl glycol acetate) (C3: 10 μm; C4: 20 μm; E5: <20 μm; E6: 20 μm; E7: 20 μm; and E8: 23 μm), where the Hegman finenesses were determined as described above.

[0117] To obtain the final filler coating compositions C3, C4, and E5-E8 to be applied to aluminum alloy panels, Masterbatch A and Hardener Composition B were thoroughly mixed and diluted with Solvent Composition S (1-methoxypropyl acetate, 2-butyl acetate, and xylol; in C3: about 5 wt. %; in C4, E5, E7, and E8: about 15 wt. %; and in E6: about 13 wt. %) to a DIN Cup 4 spray application viscosity at 20° C. of about 19 seconds to about 22 seconds.

[0118] [Table 2]

[0119] 7 Epoxy resin mixture (84% by mass of epoxy resin A: epoxy group content: 3800-4250 mmol / kg; 16% by mass of epoxy resin B: Beckopox EM 460 (solvent-free)) 8 1,4-Dihydroxyanthraquinone 9 3-Methylanthraquinone (not of the present invention) 10 Alizarin 11 Quercetin 12 Used to disperse the epoxy resin mixture in position 1 13 Used to dissolve the wetting and dispersing agent in position 2, 14 Proprietary mixture of oligomeric and polymeric amines (amine value: approx. 270±20mg KOH / g) 15 A proprietary solvent mixture used to dissolve the amine hardener mixture at position 16.

[0120] Application of the coating composition Application of a two-part hydroxyl / isocyanate system and topcoat with a topcoat The filler coating compositions E1-E4 of the invention and the comparative filler coating compositions C1 and C2 were applied by spraying (spray gun: SATA3000RP, nozzle 1.3 mm, pressure 2.5 bar) onto aluminum alloy panels (AA6014 for AASS tests, AlMgMn4.5 for other tests). After application, the resulting films were dried at room temperature (23° C.) for 60 minutes (dry film thickness of filler coating: 58±9 μm, except for coating composition E3: 39 μm).

[0121] The filler coated film thus obtained was overcoated by spray application (spray gun: SATA 3000 RP, nozzle: 1.4 mm, pressure: 2.5 bar) by spraying with a white topcoat (Masterbatch: Series 68 CV, product number: 68-RAL 9010; Hardener: Hardener CV, product number: 922-138; Thinner: product number: 352-216; 4:1:1 (v / v / v); all available from BASF Coatings GmbH) and dried at 60° C. for 30 minutes to obtain a dry film thickness of 66 μm.

[0122] Application of a two-part epoxy / amine system and topcoat application Filler coating compositions E5 to E8 according to the invention and comparative filler coating compositions C3 and C4 were applied by spraying (spray gun: SATA 100BF RP, nozzle: 1.6 mm, pressure: 2.5 bar). After application, the films obtained were dried at room temperature (23° C.) for 60 minutes (dry film thickness of filler coating: 52±6 μm, except for coating composition C2: 71 μm).

[0123] The filler coated film thus obtained was overcoated by spray application (spray gun: SATA 3000 RP, nozzle: 1.4 mm, pressure: 2.5 bar) by spraying with a white topcoat (Masterbatch: Series 68 CV, product number: 68-RAL 9010; Hardener: Hardener CV, product number: 922-138; Thinner: product number: 352-216; 4:1:1 (v / v / v); all available from BASF Coatings GmbH) and dried at 60° C. for 30 minutes to obtain a dry film thickness of 58 μm.

[0124] Corrosion test results

[0125] [Table 3]

[0126] As shown in Table 3, in AASS testing, filler coating compositions E1-E4 of the present invention were significantly superior to comparative filler coating composition C1, which contained no corrosion inhibitor, and comparative filler coating composition C2, which was 3-methylanthraquinone without hydroxyl groups. Coating composition E3 also still showed good corrosion inhibition, despite the reduced dry film thickness of this example compared to the other examples.

[0127] Furthermore, the results of the cross-cut test, gloss (60°) test and determination of the number / size of blisters on aluminium alloy panels (AlMgMn4.5) subjected to a constant climate test (CCT; 240 h) were very satisfactory, with no adverse effect of the corrosion inhibitors observed in any of the test parameters.

[0128] [Table 4]

[0129] As shown in Table 4, in AASS testing, filler coating compositions E5-E8 of the present invention were significantly superior to comparative filler coating composition C3, which did not contain a corrosion inhibitor, even though comparative filler coating composition C3 was applied at a high dry film thickness. Comparative filler coating composition C4, which is 3-methylanthraquinone without a hydroxyl group, was found to be significantly less effective than the corrosion inhibitors used in filler coating compositions E5-E8 of the present invention.

Claims

1. (A) a. one or more polymers and / or resins that contain functional groups that are reactive with the functional groups of one or more crosslinkers contained in the hardener component (B); b. one or more pigments and / or fillers; and c. one or more species containing a structural unit of formula (I); 【Chemistry 1】 (wherein the four residues R 1 Two of the residues are OH and the other two residues R 1 is H; R 2 ═O or C═O; and R 3 -R 4 is C=C or HC-CH; the asterisk * represents the residue R in formula (II) below. 5 and R 6 or a bond site to the residue CH-CH-CH-CH in formula (III) below), and one or more species selected from the group consisting of species of formula (II): 【Chemistry 2】 (In the formula, R 5 teeth 【Chemistry 3】 and R 6 = H or OH, and the star * is R 4 indicates the binding site to 2 = O; R 7 and R 8 is H or OH, where R 7 and R 8 is H), and / or a species of formula (III) 【Chemistry 4】 (In the formula, R 2 is C=O) wherein the compounds of formula (II) and (III) are not encapsulated in mesoporous silica nanocontainers; and (B) a hardener composition comprising one or more crosslinkers that contain functional groups that are reactive towards the functional groups of the one or more polymers and / or resins; and, optionally, (C) Diluent Composition 1. A solvent-based two-part coating composition comprising:

2. The species of formula (II) is a species of formula (IIa) 【Chemistry 5】 (In the formula, R 7 and R 8 is defined in claim 1; and a.R 6 is OH, R 3 -R 4 is C=C, or b. R 6 is H, and R 3 -R 4 is HC-CH), the solvent-based two-part coating composition of claim 1.

3. 2. The solvent-based two-part coating composition of claim 1, wherein the species of formula (II) is selected from the group consisting of quercetin, morin and naringenin, and / or the species of formula (III) is selected from 1,2-dihydroxyanthraquinone and 1,4-dihydroxyanthraquinone.

4. 4. A solvent-based two-part coating composition according to claim 1, wherein the species containing the structural unit of formula (I) is quercetin.

5. 5. The solvent-based two-component coating composition according to any one of claims 1 to 4, wherein the one or more polymers and / or resins comprising functional groups reactive towards functional groups of the one or more crosslinkers comprised in the hardener component (B) are polyhydroxy-functional polymers and / or resins, the one or more crosslinkers being polyisocyanates having free isocyanate groups or the one or more polymers and / or resins comprising functional groups reactive towards functional groups of the one or more crosslinkers comprised in the hardener component (B) are epoxy resins, the one or more crosslinkers being selected from the group consisting of polyamines and polyamidines.

6. The solvent-based two-component coating composition according to any one of claims 1 to 5, wherein the mass ratio of the total of (A)b. pigment and filler to (A)a. one or more polymers and / or resins having functional groups reactive to the functional groups of one or more crosslinkers contained in the hardener component (B) is 1:5 to 5:

1.

7. 7. The solvent-based two-part coating composition of claim 1 which is a primer coating composition or a filler composition or both.

8. 8. The solvent-based two-component coating composition of any one of claims 1 to 7, having a DIN Cup 4 viscosity (DIN 53211:1987-06) of less than 30 seconds.

9. 9. The solvent-based two-component coating composition according to any one of claims 1 to 8, wherein the one or more species of formula (II) and / or (III) are contained in said masterbatch composition (A) in a total amount of from 1 ppm to 15 wt.-%, based on the total weight of said masterbatch composition (A).

10. i. first, (A)a. one or more polymers and / or resins containing functional groups reactive to functional groups of one or more crosslinkers contained in the hardener component (B) are mixed with at least a portion of (A)b. one or more pigments and / or fillers, wherein (A)a. one or more polymers and / or resins containing functional groups reactive to functional groups of one or more crosslinkers contained in the hardener component (B) are optionally and preferably pre-dissolved and / or pre-dispersed in at least a portion of the organic solvent contained in the final coating composition; ii. adding, while mixing, the remaining A(b). one or more pigments and / or fillers if not fully added in step i., and adding, while mixing, one or more species of formula (II) and / or (III) as defined in any one of claims 1 to 9; iii. milling the mixture thus obtained, preferably using a bead mill, until the Hegman fineness is preferably determined to be less than 25 μm, more preferably less than 23 μm, and most preferably less than 20 μm; iv. adding hardener component (B), and optionally solvent component (C), under mixing conditions to achieve a homogenous coating composition. A method for producing the solvent-based two-part coating composition of any one of claims 1 to 9, comprising:

11. 10. A method for coating a metal substrate with the coating composition of any one of claims 1 to 9, comprising at least step (i) of contacting the metal substrate with the coating composition of the present invention.

12. 12. A method of coating a metal substrate with the coating composition of claim 11, wherein the metal substrate is or contains aluminum.

13. A coated metal substrate obtainable by the method according to claim 11 or 12.

14. At least the following steps: (i) for application of the coating composition to the substrate, particularly preferably by spray coating, contacting a metal substrate with a coating composition according to any one of claims 1 to 9; and (ii) applying a further coating composition, preferably a topcoat coating composition or a clearcoat coating composition, to the coating layer formed by applying the coating composition in step (i), preferably by spray coating.

1. A method for coating a substrate with a multi-layer coating, comprising:

15. 15. The method of coating a substrate with a multi-layer coating according to claim 14, wherein the metal substrate is aluminum or contains aluminum.

16. A multi-layer coated metal substrate obtainable by the method according to claim 14 or 15.

17. To provide corrosion protection to a cured coating formed from the coating composition, (A) a masterbatch composition comprising (A)a. and (A)b. as defined in any one of claims 1 to 9, and (B) a hardener composition as defined in any one of claims 1 to 9, and optionally (C) Diluent Composition 10. The use of one or more species of formula (II) and (III) as defined in any one of claims 1 to 9 in a solvent-based two-component coating composition comprising

Citation Information

Patent Citations

  • Rust preventive coating composition

    JP1980127470A

  • Magnetic recording medium

    JP1987172526A

  • Two-pack type polyurethane coating composition

    JP2013203952A

  • Method for forming multilayer film

    JP2017087164A

  • Antifreeze solution, and rust inhibitor capable of being used as component thereof

    WO2004074397A1