Transfer sheet

The laminated transfer sheet with a polyester-PVA structure addresses high adhesion issues, enabling bubble-free and wrinkle-free transfer of materials like photoresists and metal films across temperatures, enhancing transfer efficiency and process compatibility.

JP7567135B2Active Publication Date: 2024-10-16AICELLO
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021529195
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-04
Filing Date
2020-07-03
Publication Date
2024-10-16
Estimated Expiration
2040-07-03

AI Technical Summary

Technical Problem

Existing transfer technologies struggle with transferring materials like curable resins, metal films, and inorganic oxides due to high adhesion, requiring different sheets for room-temperature and heat transfer, and face issues with peeling, wrinkling, and bubble formation during transfer.

Method used

A transfer sheet with a laminated structure of a polyester layer, a polyvinyl alcohol (PVA) layer containing specific diol and triol compounds, and a transfer layer, allowing for easy peeling of the polyester layer post-lamination, followed by PVA dissolution for smooth transfer without wrinkles or bubbles.

Benefits of technology

The solution enables reliable transfer of functional materials like photoresists and metal films onto substrates without damage, ensuring bubble-free and wrinkle-free results across various temperatures, facilitating processes like cutting and surface processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567135000006
    Figure 0007567135000006
  • Figure 0007567135000007
    Figure 0007567135000007
  • Figure 0007567135000008
    Figure 0007567135000008
Patent Text Reader

Abstract

The present invention provides a transfer sheet which enables the achievement of room temperature transfer and heating transfer by a single sheet in cases where a material that exhibits high adhesion to a material such as a polyester that constitutes a supporting body is transferred to a transfer-receiving substrate. The present invention specifically provides, as a solution, a transfer sheet which has a multilayer structure wherein a polyester layer serving as a supporting body layer, a polyvinyl alcohol (PVA) layer and a transfer layer are sequentially stacked in this order, said polyvinyl alcohol layer containing a diol compound and / or a triol compound wherein adjacent hydroxyl groups are in the δ-position or further away from each other, and which satisfies the condition (i) described below. (i) The T type peel strength between the polyester layer and the polyvinyl alcohol layer before the formation of the transfer layer as measured at a peeling rate of 100 mm / min. in an environment at 23°C at 50% RH after humidity control is 30 mN / 20 mm or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a transfer sheet for materials that are difficult to release by thermal transfer or the like, such as curable resins such as photoresists, metal films, inorganic oxides, etc., which have high adhesion to materials such as polyester constituting a support. [Background technology]

[0002] In the field of surface decoration of molded products, a technique is known in which a decorative layer is formed on a support layer on which a release layer has been formed, and the decorative layer is peeled off from the release layer by heating and pressing, etc., and transferred to the surface of an object, as described in Patent Document 1. Another technique is also used in which a decorative layer is formed on a water-soluble base material, the base material is swelled by the water surface, and the decorative layer is swelled with a solvent, and then the decorative layer is transferred to the object by water pressure. However, with this type of water pressure transfer, it is difficult to transfer metal films and some resins. Furthermore, the object and the decorative layer must be water resistant, and it is difficult to transfer objects and decorative layers made of a wider range of materials. As other transfer means, cold transfer and heat transfer are known, but for each transfer, separate transfer sheets are used for cold transfer and heat transfer. As a result, there has been no transfer sheet that can be used to perform cold transfer at one time and heat transfer at another time. As described in Patent Document 2, a thermal transfer sheet is known which comprises a base sheet, a primer layer made of water-soluble polyvinyl alcohol, and a transfer layer provided on the primer layer, and which is merely known to include a method in which after transfer, the base sheet is peeled off and the primer layer and transfer layer are removed by washing with water. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-077121 A [Patent Document 2] Japanese Patent Application Publication No. 10-166793 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, there has been a need to transfer not only decoration but also functions such as fine wiring patterns, metal films, inorganic oxide films, and functional resin films, and after transfer to the target substrate, further processes such as etching, sputtering, deposition, coating, surface processing, cutting, and joining may be carried out. Many of the layers (transfer materials) with such functions have high adhesion to the transfer sheet. Therefore, in order to perform the transfer smoothly, it is necessary to provide a release layer according to the transfer material. In addition, since there are transfer materials that cannot perform the specified function due to deterioration caused by heating, etc., it is desired to be able to achieve transfer under a wide range of temperatures with one type of transfer sheet depending on the type of transfer material and the substrate to be transferred. During transfer, the support layer must be attached to the substrate to prevent swelling and shrinkage of the polyvinyl alcohol (PVA) layer caused by atmospheric humidity, deformation of the transfer layer due to the conditions when laminating the substrate, and the substrate must be temporarily stored in the laminated state. In addition, when the substrate to be transferred is flexible, the substrate wound in a roll is unwound, and the transfer sheet is attached to the surface of the substrate, while the support of the transfer sheet is peeled off, and the transferred PVA layer is then dissolved in water to transfer the transfer layer to the substrate surface. Then, the substrate having the transfer layer on its surface is wound up in a roll, and continuous transfer processing by the roll-to-roll method may be performed. In both the sheet-fed method and the roll-to-roll method, in order to transfer the transfer layer to the substrate to be transferred without damaging it, it is important to peel off only the support layer cleanly from the substrate surface to be transferred without leaving any peeling marks after the transfer sheet is attached. Furthermore, in order to dissolve the PVA layer in water and form a transfer layer on the surface of the substrate without wrinkles or bubbles, it is necessary to prevent partial peeling between the support layer and the PVA layer, and between the PVA layer and the transfer layer in the process of forming the transfer layer on the PVA layer in advance and in the process of laminating the transfer layer to the substrate surface. Until now, it has been difficult to solve these problems. Therefore, an object of the present invention is to solve these problems. [Means for solving the problem]

[0005] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that the problems can be solved by the following means, and have arrived at the present invention. 1. A support layer has a structure in which a polyester layer, a polyvinyl alcohol (PVA) layer, and a transfer layer are laminated in this order, and the polyvinyl alcohol layer contains a diol compound and / or a triol compound in which an adjacent hydroxyl group is located at the δ position or later, A transfer sheet that satisfies the following condition (i). (i) After conditioning in an environment of 23°C and 50% RH before the formation of the transfer layer, the T-type peel strength between the polyester layer and the polyvinyl alcohol layer at a peel speed of 100 mm / min. is 30 mN / 20 mm or more. 2. The transfer sheet according to 1, wherein the polyester layer is not release-treated. 3. The transfer sheet according to 1 or 2, wherein the diol compound is a polyalkylene glycol having a number average molecular weight of 1,000 or more. 4. The transfer layer side of the transfer sheet described in any one of 1 to 3 is attached to the surface of a flat or three-dimensional substrate, The polyester layer is then peeled off. Furthermore, the transfer method includes dissolving the polyvinyl alcohol layer in water and removing it, thereby forming a transfer layer on the surface of the substrate. Effect of the Invention

[0006] The transfer sheet of the present invention uses a polyester layer having an appropriate range of peel strength with a polyvinyl alcohol (hereinafter sometimes referred to as "PVA") layer as a support layer, so that a transfer layer can be formed on the PVA layer formed thereon without wrinkles, and since no air bubbles are trapped between the polyester layer and the PVA layer, the transfer layer can be stored without being damaged. After the transfer sheet of the present invention is attached to the surface of the substrate to which the transfer is to be applied, the polyester layer can be easily peeled off, so that the PVA layer and the transfer layer are not damaged. Therefore, by dissolving the PVA layer in water, the transfer layer can be reliably transferred to the surface of the substrate. Even if the PVA layer and the transfer layer cannot be peeled off from the surface of the substrate to which the transfer is to be made, the PVA layer can be dissolved in water and removed to leave the transfer layer on the substrate, i.e., to transfer the layer. Therefore, it is not necessary to select and adopt a release layer according to the material of the transfer layer, and it is possible to prevent the components of the release layer from being mixed into the transfer layer. In addition, after the transfer sheet of the present invention is laminated to a substrate, the PVA layer does not peel off from the transfer layer, so the laminated state can be stored. Furthermore, if a light absorbent is contained in the PVA layer, the transfer layer can be prevented from being damaged by light. Furthermore, by using a laser beam corresponding to the wavelength of the light absorbent, cutting processing, surface processing, etc. can be performed before the PVA layer is dissolved in water. [Brief description of the drawings]

[0007] [Figure 1] Transfer sheet of the present invention [Diagram 2] Substrate formed by laminating a transfer sheet [Diagram 3] The polyester layer has been peeled off from the transfer sheet. [Figure 4] The PVA layer is hydrolyzed and the transfer layer is transferred to the substrate. [Explanation of symbols]

[0008] 1: Transfer sheet of the present invention 2: Polyester layer 3: Polyvinyl alcohol layer 4: Transfer layer 5: Substrate DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Preferred embodiments for carrying out the present invention will be described below, but the scope of the present invention is not limited to these embodiments. As shown in FIG. 1, the transfer sheet 1 of the present invention is a laminate comprising a polyester layer 2 as a support layer, a polyvinyl alcohol layer 3, and a transfer layer 4 in this order. Using this transfer sheet 1, as shown in FIG. 2, the surface on which the transfer layer 4 is to be transferred is adhered and bonded to a substrate 5 as the transfer target by a method such as heating, pressure, vacuum, compressed air, pressing, or the like, and then the polyester layer 2 is peeled off. The resulting state is one in which the substrate 5, the transfer layer 4 and the polyvinyl alcohol layer 3 are laminated in this order, as shown in FIG. Next, the polyvinyl alcohol layer 3 is dissolved and removed using cold water or hot water, and only the transfer layer 4 is transferred to the substrate 5, thereby obtaining a substrate 5 having the transfer layer 4 formed on the surface thereof, as shown in FIG. 4.

[0010] The transfer sheet 1 of the present invention will now be described. <Transfer sheet> (polyester layer) The polyester layer 2 used in the transfer sheet 1 of the present invention is a support layer, which holds the transfer layer 4 via the polyvinyl alcohol layer 3 laminated thereon with an appropriate peel strength, and is a layer that is peeled off from the polyvinyl alcohol layer 3 in the transfer step. As a result, the transfer layer 4 can be accurately adhered to the surface of the transfer target substrate 5 without causing wrinkles. Examples of such polyester layers include sheets of polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and the like. In addition, the surface of the polyester layer may be subjected to a release treatment (hydrophobic treatment) or may be subjected to a hydrophilic treatment by a known means such as a corona discharge treatment, but an untreated surface that has not been subjected to either a release treatment or a hydrophilic treatment is preferable. When the surface of the polyester layer is subjected to a release treatment such as silicone or fluorine, the peel strength with the polyvinyl alcohol layer 3 is too low, so that the polyvinyl alcohol layer 3 may be partially peeled off from the polyester layer 2 by heating, pressing, etc. in the process of producing the transfer layer 4. As a result, air bubbles may be trapped between the polyester layer 2 and the polyvinyl alcohol layer 3, and the air bubble marks may be transferred to the transfer layer 4, damaging the appearance after transfer. In addition, a small amount of the component of the release treatment agent such as silicone may be mixed into the transfer layer 4, adversely affecting the process following the transfer or impairing the device performance of the transfer target substrate 5. If the peel strength is increased more than necessary as a result of hydrophilization treatment such as corona discharge treatment, it becomes difficult to peel the polyester layer 2 from the polyvinyl alcohol layer 3, and the transfer layer may be damaged. As such a polyester layer 2, a commercially available polyester film can be used, for example, Emblet S (manufactured by Unitika Ltd., untreated PET), Toyobo Ester Film (manufactured by Toyobo Co., Ltd., untreated PET), Teonex (manufactured by Teijin Ltd., PEN), and the like. In the present invention, when a polyester layer 2 that has not been subjected to a surface treatment is used, the polyester layer 2 has not been subjected to a treatment that renders the surface hydrophilic or hydrophobic. Furthermore, the polyester layer 2 is a layer that has not been subjected to a treatment that affects the hydrophilic or hydrophobic properties of the surface by blending an additive or the like in the polyester layer 2 or modifying the polyester resin itself. As long as the effects of the present invention are exhibited, the above-mentioned treatments for improving the hydrophobicity or hydrophilicity to a certain degree are not excluded.

[0011] The polyester layer 2 may be either stretched or unstretched. Its thickness is preferably 10 to 188 μm. If it is less than 10 μm, it may be difficult to provide a trigger portion that is a starting point when peeling off the polyester layer 2, and if it exceeds 188 μm, the rigidity of the polyester layer 2 may become too high, which may deteriorate the workability during peeling. It is also possible to provide irregularities on the surface of the polyvinyl alcohol layer 3 by blending a filler or roughening the surface. However, it is necessary to provide the irregularities within a range that does not reduce the releasability of the polyester layer 2 or does not cause irregularities on the surface of the polyvinyl alcohol layer 3 reflecting the roughened surface.

[0012] (Polyvinyl alcohol layer) In the transfer sheet 1 of the present invention, the polyvinyl alcohol (PVA) resin used in the polyvinyl alcohol layer 3 preferably has a degree of saponification of 60 mol % or more, more preferably 70 to 95 mol %. If the degree of saponification is less than 60 mol %, the PVA layer cannot be sufficiently hydrolyzed (dissolved and removed with water) during the transfer step, which may cause problems in the subsequent steps. The PVA resin may be modified and / or unmodified. In the case of modification, other monomers may be copolymerized in the main chain within a range that does not impair the effects of the present invention, for example, 10 mol % or less, preferably 7 mol % or less.

[0013] Examples of such monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or their salts or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or their salts; alkyl vinyl ethers; polyoxyalkylene (meth)allyl ethers such as polyoxyethylene (meth)allyl ether and polyoxypropylene (meth)allyl ether; polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate; Examples of the monomers include polyoxyalkylene (meth)acrylates, polyoxyethylene (meth)acrylamides such as polyoxyethylene (meth)acrylamide and polyoxypropylene (meth)acrylamide, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) esters, polyoxyethylene vinyl ethers, polyoxypropylene vinyl ethers, polyoxyethylene allylamines, polyoxypropylene allylamines, polyoxyethylene vinylamines, polyoxypropylene vinylamines, diacrylacetamides, N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, dimethyldiallylammonium chloride, dimethylallylvinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, etc. These other monomers may be used alone or in combination.

[0014] The polyvinyl alcohol layer 3 is required to contain at least one diol compound and / or triol compound in which adjacent hydroxyl groups are located at the δ-position or later. In order to facilitate smooth transfer, the diol compound preferably has a number average molecular weight of 400 or more, more preferably 800 or more, and even more preferably 1000 or more. Also preferred is a polyalkylene glycol having a number average molecular weight of 20000 or less. Also, it is most preferable that the composition contains a polyalkylene glycol having a number average molecular weight of 1000 or more and a triol compound in which the adjacent hydroxyl group is located at the δ position or later. In this case, it is more preferable that the composition contains a polyalkylene glycol having a number average molecular weight of 1000 or more and a triol compound in which the adjacent hydroxyl group is located at the δ position or later in a weight ratio of 1:9 to 9:1. Here, a triol compound in which adjacent hydroxyl groups are located at the δ position or higher is a compound that has three hydroxyl groups, and when any one of the hydroxyl groups is taken as a reference and the carbon element bonded to it is taken as the α position, the shortest distance between the reference hydroxyl group and each of the remaining two hydroxyl groups is four or more atoms with a valence of two or more, such as carbon or oxygen. In addition, in all combinations of any two hydroxyl groups out of the three hydroxyl groups, it is necessary that four or more atoms with a valence of two or more are bonded. For example, in 1,4,8-octanetriol shown in Chemical formula 1 below, when the hydroxyl group bonded to the carbon atom at position 4 is taken as the reference, the positions of the hydroxyl groups at positions 1 and 8 adjacent to it are δ and ε, respectively. Similarly, in oxyethylene glyceryl ether shown in Chemical formula 2 below, when the hydroxyl group located in the middle of the molecule is taken as the reference, the adjacent hydroxyl groups are each located at θ positions. The triol compound in which adjacent hydroxyl groups are located at the δ-position or later in the present invention is a compound in which all of the hydroxyl groups in the triol compound are located at the δ-position or later relative to one another. A compound in which the space between two adjacent hydroxyl groups is located at the δ position or later, but the combination of another two adjacent hydroxyl groups is located up to the γ position, such as 1,2,8-octanetriol shown in Chemical Formula 3 below, is not a triol compound in which adjacent hydroxyl groups are located at the δ position or later in the present invention.

[0015] [ka]

[0016] [ka]

[0017] [ka]

[0018] In addition, the diol compound and the triol compound having adjacent hydroxyl groups at the δ-position or later are preferably added in a total amount of 1 part by weight or more, more preferably 1 to 20 parts by weight, even more preferably 1 to 15 parts by weight, and most preferably 3 to 12 parts by weight, per 100 parts by weight of the polyvinyl alcohol resin. Furthermore, the diol compound is preferably added in an amount of 1 part by weight or more, more preferably 1 to 15 parts by weight, even more preferably 1 to 10 parts by weight, and most preferably 3 to 10 parts by weight, per 100 parts by weight of the polyvinyl alcohol resin. The triol compound having adjacent hydroxyl groups at the δ-position or later is preferably added in an amount of 1 part by weight or more, more preferably 1 to 18 parts by weight, even more preferably 1 to 13 parts by weight, and most preferably 3 to 10 parts by weight, per 100 parts by weight of the polyvinyl alcohol resin. If the polyester layer 2 contains a triol compound having adjacent hydroxyl groups at the α-, β-, and γ-positions, or a polyhydric alcohol compound having tetrahydric or higher hydroxyl groups, peeling the polyester layer 2 after bonding to the substrate 5 during the transfer process becomes so difficult that peeling marks are left, which may damage the transfer layer 4.

[0019] Furthermore, the T-peel strength at a peel speed of 100 mm / min between the polyester layer 2 before the transfer layer is formed and the polyvinyl alcohol layer 3, which have been conditioned in an environment of 23°C and 50% RH, must be 30 mN / 20 mm or more, and is preferably 30 to 400 mN / 20 mm, further preferably 30 to 300 mN / 20 mm, further preferably 40 to 100 mN / 20 mm, and most preferably 45 to 70 mN / 20 mm. If the T-peel strength is less than 30 mN / 20 mm, the polyvinyl alcohol layer 3 may partially peel off from the polyester layer 2 due to heating and pressure during the process of forming the transfer layer 4 on the polyvinyl alcohol layer 3, causing air bubbles to accumulate. These air bubbles may be transferred to the transfer layer 4 and may impair the appearance. If the T-peel strength exceeds 400 mN / 20 mm, it may be difficult to initiate peeling when peeling the polyester layer after bonding to the substrate 5 during the transfer process. Also, if the T-peel strength exceeds 300 mN / 20 mm, it may be difficult to initiate peeling.

[0020] The diol compound in the present invention must be soluble in water, and examples thereof include ethylene glycol, trimethylene glycol, 1,4-butanediol, 1,3-butylene glycol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 2-methylpentane-2,4-diol, polyethylene glycol, polypropylene glycol, a copolymer of ethylene glycol and propylene glycol, a copolymer of propylene glycol and butylene glycol, and a terpolymer of ethylene glycol, propylene glycol and butylene glycol.

[0021] In the present invention, the triol compound in which the adjacent hydroxyl groups are located at the δ-position or higher must also be soluble in water. Examples of such compounds include triethylolpropane, polyoxyethylene glyceryl ether, polyoxypropylene glyceryl ether, and diglycerin monoalkylate.

[0022] The means for providing the polyvinyl alcohol layer is not particularly limited, and the polyvinyl alcohol layer may be provided by coating and drying a solution obtained by dissolving the composition of the polyvinyl alcohol layer 3 in a solvent by a known means, or the polyvinyl alcohol layer 3 formed on a separately prepared peelable film may be transferred onto the polyester layer 2 by a known means. The polyvinyl alcohol layer 3 has a thickness of 5 to 100 μm.

[0023] A light absorbent may be added to the polyvinyl alcohol layer 3 as necessary to impart light resistance and laser light absorption. For example, to impart light absorption in the UV region of 300 to 400 nm, benzotriazole compounds, triazine compounds, benzophenone compounds, benzoate compounds, hindered amine compounds, etc. may be added, such as Adekanol UC (manufactured by ADEKA Corporation) and New Coat UVA (manufactured by Shin-Nakamura Chemical Co., Ltd.). To impart light absorption in the near infrared region of 1100 nm, such as diimonium salt compounds or aminium salt compounds, etc. may be added, such as NIR-IM1 (manufactured by Nagase Chemtex Corporation). To prevent foaming during hydrolysis in the transfer process, a defoaming agent may be added to the polyvinyl alcohol layer 3. The defoaming agent is preferably a non-silicone type, such as SN DEFORMER (manufactured by SAN NOPCO LTD.) or SY GLYSTAR (manufactured by SAKAMOTO YAKINKOGYO CO., LTD.). Such a polyvinyl alcohol layer 3 can be produced by coating an aqueous solution of PVA on the polyester layer 2 using a slot die or the like, followed by drying.

[0024] The polyvinyl alcohol layer 3 can be colored by adding known dyes or pigments for the purpose of blocking light or for indicating the presence or absence of polyvinyl alcohol resin before and after removal with water. Such dyes and pigments are preferably water-soluble or water-dispersible, and examples of such dyes and pigments include food colorings such as Blue No. 1 and Yellow No. 4, and titanium oxide.

[0025] (Transfer layer) The transfer layer 4 in the transfer sheet 1 of the present invention can be made of known materials that can be transferred, such as thermoplastic resins, curable resins, metal films, and inorganic oxide films that can be formed on the polyvinyl alcohol layer 3. Examples of such materials include photocurable resin compositions such as negative resists such as epoxy-based photocurable resins, positive resists such as novolak-naphthoquinone diazide-based resists, and chemically amplified resists such as polyhydroxystyrene-based resists; various printing layers; inorganic compounds such as silicon dioxide (SiO2) and metal oxides such as indium tin oxide (ITO); and metals such as copper and gold. The transfer layer 4 can be produced by a method suited to the material of the transfer layer 4, such as coating, sputtering, vapor deposition, adhesion, or transfer onto the polyvinyl alcohol layer 3. In order to improve adhesion to the surface of the substrate 5 to be transferred, the surface of the transfer layer 4 can be provided with an adhesive layer or a pressure-sensitive adhesive layer, or coated with a silane coupling agent or the like. In addition, a cover film may be provided on the surface of the transfer layer 4 to prevent the transfer layer 4 from being damaged or stained during storage.

[0026] (substrate) The substrate 5 is an object onto which the transfer layer 4 is transferred, and may be either flat or three-dimensional, and may be made of plastic moldings, glass, ceramics, metals, semiconductors, rubber, etc. To improve adhesion with the transfer layer, it is also possible to provide an adhesive layer or coat with a silane coupling agent, etc. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples. Note that the examples show one embodiment of the present invention, and the present invention is not limited thereto. <Preparation of transfer sheet 1> Example 1 A polyethylene terephthalate (PET) film having an untreated surface (manufactured by Unitika Ltd., untreated SD-75, thickness 75 μm) was used as the support layer. A polyvinyl alcohol layer was prepared on the support layer by bar coating using an aqueous solution of a resin composition consisting of 100 parts by weight of polyvinyl alcohol (PVA) (PXP-05, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol%, polymerization degree 600), 9 parts by weight of polyethylene glycol (PEG) 1540 (number average molecular weight 1540) as a diol compound, and 1 part by weight of polyoxypropylene glyceryl ether 300 (polyoxypropylene chains bonded to all three hydroxyl groups of glycerin (same below), number average molecular weight 300) as a triol compound in which adjacent hydroxyl groups are located at the δ position or later, using a bar coating method to form a polyvinyl alcohol layer with a dry thickness of 15 μm. Then, photocurable resin AZ1500 (Clariant, novolac resin system) was bar coated onto the polyvinyl alcohol layer as a transfer layer to a dry thickness of 3 μm, and after drying at 90°C for 5 minutes, it was irradiated with ultraviolet light with an exposure of 300 mJ to produce a transfer sheet.

[0028] Example 2 A transfer sheet was prepared in the same manner as in Example 1, except that a polyvinyl alcohol layer was obtained from an aqueous solution of a resin composition consisting of 100 parts by weight of PVA (PXP-05, manufactured by Japan Vinyl Acetate & Poval, saponification degree 88 mol%, polymerization degree 600), 1 part by weight of PEG1540 as a diol compound, and 9 parts by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the δ position or later.

[0029] Example 3 A PET film having an untreated surface (Unitika Ltd., untreated SD-75, thickness 75 μm) was used as the support layer. A polyvinyl alcohol layer was prepared on the support layer by bar coating using an aqueous solution of a resin composition consisting of 100 parts by weight of PVA (Japan Vinyl Acetate & Poval Corporation, JR-05, saponification degree 70 mol%, polymerization degree 600), 5 parts by weight of PEG1540 as a diol compound, and 5 parts by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the δ position or later, so that the dry thickness was 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0030] Example 4 A PET film having an untreated surface (Unitika Ltd., untreated S-50, thickness 50 μm) was used as the support layer. An aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol%, polymerization degree 1000), 5 parts by weight of PEG1540 as a diol compound, and 5 parts by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the δ position or later was applied to the support layer by bar coating to prepare a polyvinyl alcohol layer with a dry thickness of 15 μm. Then, a Cr film (1000 Å) was prepared as a transfer layer on the polyvinyl alcohol layer by sputtering, and an adhesive resin (acrylic resin, DIC Corporation, Acrydic A-811-BE) was coated on the Cr film using a bar coater to a dry thickness of 3 μm, and the film was dried at 80°C for 5 minutes to prepare a transfer sheet.

[0031] Example 5 A transfer sheet was prepared in the same manner as in Example 4, except that a corona discharge-treated PET film (manufactured by Unitika Ltd., one-sided treatment SD-75, thickness 75 μm) was used as the support layer.

[0032] Example 6 A PET film having an untreated surface (Unitika Ltd., untreated S-38, thickness 38 μm) was used as the support layer. An aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-15, manufactured by Japan Vinyl Acetate & Poval, saponification degree 88 mol%, polymerization degree 1500) and 5 parts by weight of PEG400 (polyethylene glycol, number average molecular weight 400) as a diol compound was bar coated on the support layer to produce a polyvinyl alcohol layer with a dry thickness of 15 μm. Then, a thermoplastic resin (urethane resin, Toyo Ink Co., Ltd., Rio Alpha S) was coated on the polyvinyl alcohol layer as a transfer layer using a bar coater to a dry thickness of 3 μm, and then dried at 80°C for 5 minutes to prepare a transfer sheet.

[0033] Example 7 A transfer sheet was prepared in the same manner as in Example 6, except that the diol compound was 5 parts by weight of PEG1000 (polyethylene glycol, number average molecular weight 1000).

[0034] Example 8 A transfer sheet was prepared in the same manner as in Example 6, except that the diol compound was 5% by weight of trimethylene glycol.

[0035] Example 9 A transfer sheet was prepared in the same manner as in Example 6, except that the diol compound was 5 wt.

[0036] Example 10 A PET film having an untreated surface (Unitika Ltd., untreated SD-75, thickness 75 μm) was used as the support layer. A polyvinyl alcohol layer was prepared on the support layer 2 by bar coating using an aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-05, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol%, polymerization degree 600) and 15 parts by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the δ position or later, so that the dry thickness was 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0037] Example 11 A transfer sheet was prepared in the same manner as in Example 10, except that PVA with a saponification degree of 70 mol % (manufactured by Japan Vinyl Acetate & Poval Corporation, JR-05, polymerization degree 600) was used.

[0038] Example 12 A PET film having an untreated surface (Unitika Ltd., untreated SD-75, thickness 75 μm) was used as the support layer. A polyvinyl alcohol layer was prepared on the support layer by bar coating using an aqueous solution of a resin composition consisting of 100 parts by weight of PVA (manufactured by Japan Vinyl Acetate & Poval Corporation, JR-05, saponification degree 70 mol%, polymerization degree 600) and 10 parts by weight of PEG1540 as a diol compound, so that the dry thickness was 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0039] (Example 13) A transfer sheet was prepared in the same manner as in Example 12, except that PEG6000 (polyethylene glycol, number average molecular weight 6000) was used as the diol compound.

[0040] Comparative Example 1 A PET film (manufactured by Unitika Ltd., SD-75, thickness 75 μm) having an untreated surface was used as the support layer. An aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol%, polymerization degree 1000) and 5 parts by weight of glycerin as a triol compound in which adjacent hydroxyl groups are located at the β-position was used to bar coat the support layer to produce a polyvinyl alcohol layer with a dry thickness of 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0041] Comparative Example 2 Instead of the triol compound in Comparative Example 1 in which adjacent hydroxyl groups are located at the β-position, 5 parts by weight of trimethylolpropane was used as the triol compound in which adjacent hydroxyl groups are located at the γ-position to prepare a transfer sheet.

[0042] Comparative Example 3 A transfer sheet was prepared using 5 parts by weight of 1,2,6-hexanetriol as a triol compound in which adjacent hydroxyl groups are located at the ε and β positions, instead of the triol compound in which adjacent hydroxyl groups are located at the β position in Comparative Example 1.

[0043] Comparative Example 4 A transfer sheet was prepared using 5 parts by weight of diglycerol as a tetraol compound in place of the triol compound in Comparative Example 1 in which adjacent hydroxyl groups were located at the β-position.

[0044] Comparative Example 5 Instead of the triol compound in Comparative Example 1 in which adjacent hydroxyl groups were located at the β-position, a transfer sheet was prepared using 5 parts by weight of polyoxyethylene diglyceryl ether (number average molecular weight 450) as a tetraol compound.

[0045] Comparative Example 6 A transfer sheet was prepared using 5 parts by weight of sorbitol as a hexaol compound in place of the triol compound in Comparative Example 1 in which adjacent hydroxyl groups are located at the β-position.

[0046] Comparative Example 7 A transfer sheet was prepared using 10 parts by weight of polypropylene glycol (PPG) 400 (number average molecular weight 400) as a diol compound in place of the triol compound in which adjacent hydroxyl groups were located at the β-position in Comparative Example 1.

[0047] Comparative Example 8 A PET film having an untreated surface (Unitika Ltd., untreated SD-75, thickness 75 μm) was used as the support layer. An aqueous solution of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol %, polymerization degree 1000) was bar-coated onto the support layer to produce a dry thickness of 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0048] Comparative Example 9 A transfer sheet was prepared in the same manner as in Comparative Example 8, except that a release-treated PET film (FT-50, manufactured by Unitika Ltd., thickness 50 μm) was used as the support layer.

[0049] Comparative Example 10 A transfer sheet was prepared in the same manner as in Comparative Example 8, except that a corona discharge-treated PET film (manufactured by Unitika Ltd., one-sided treatment SD-75, thickness 75 μm) was used as the support layer.

[0050] Comparative Example 11 A transfer sheet was prepared in the same manner as in Comparative Example 8, except that a corona discharge-treated polypropylene film (manufactured by Futamura Chemical Co., Ltd., FOH, thickness 50 μm) was used as the support layer.

[0051] Comparative Example 12 A release-treated PET film (FT-50, thickness 50 μm, manufactured by Unitika Ltd.) was used as the support layer. An aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval, saponification degree 88 mol%, polymerization degree 1000) and 5 parts by weight of glycerin was bar coated on the support layer to produce a polyvinyl alcohol layer with a dry thickness of 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0052] Comparative Example 13 A transfer sheet was prepared in the same manner as in Comparative Example 12, except that a corona discharge-treated polypropylene film (manufactured by Futamura Chemical Co., Ltd., FOH, thickness 50 μm) was used as the support layer.

[0053] Comparative Example 14 As the support layer, release-treated PET (FT-50, manufactured by Unitika Ltd., thickness 50 μm) was used. An aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval Co., Ltd., saponification degree 88 mol%, polymerization degree 1000), 9 parts by weight of PEG1540 as a diol compound, and 1 part by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the δ position or later was applied to the support layer by bar coating to prepare a polyvinyl alcohol layer with a dry thickness of 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0054] Comparative Example 15 A polyvinyl alcohol layer was prepared by casting using an aqueous solution of a resin composition consisting of 100 parts by weight of PVA (JP-10, manufactured by Japan Vinyl Acetate & Poval, saponification degree 88 mol%, polymerization degree 1000), 5 parts by weight of PEG1540 as a diol compound, and 5 parts by weight of polyoxypropylene glyceryl ether 300 as a triol compound in which adjacent hydroxyl groups are located at the γ-position or later, so that the dry thickness of the polyvinyl alcohol layer was 15 μm. Thereafter, a transfer layer was formed on the polyvinyl alcohol layer in the same manner as in Example 1 to prepare a transfer sheet.

[0055] [Table 1]

[0056] <Transfer of transfer layer to substrate> The transfer sheets of Examples 1 to 13 and Comparative Examples 1 to 15 were attached with the transfer layer side to a 5 cm square polycarbonate plate with a thickness of 3 mm and a silicon wafer with a thickness of 0.38 mm as a substrate, and pressure treatment was performed for 5 minutes at 0.2 MPa and temperatures of 30° C., 80° C., and 130° C. using a precision heating and pressing device (CYPT-50, manufactured by Shinto Kogyo Co., Ltd.). Next, the support layer was peeled off from the polyvinyl alcohol layer, and the polyvinyl alcohol layer was dissolved and removed with pure water, and the transfer layer was transferred to the substrate. Note that only the cases where the substrate was polycarbonate are shown in Table 2. However, the results of the following evaluations when the silicon wafer was used as the substrate were the same in all examples as when the polycarbonate plate was used.

[0057] <Evaluation of the transfer layer production process> (Rating A: T-type peel strength between support layer and PVA layer) For the transfer sheets of Examples 1 to 13 and Comparative Examples 1 to 14, the support layer / PVA layer films before preparing the transfer layer were conditioned in an environment of 23°C and 50% RH, and then the T-type peel strength between the support layer / PVA layer was measured using a tensile tester (TG-5kN, manufactured by MinebeaMitsumi Inc.).

[0058] (Evaluation B: State after preparation of transfer sheet) After the transfer layer was formed, the appearance of the transfer sheets of Examples 1 to 13 and Comparative Examples 1 to 15 was judged according to the following criteria. ◯: There is no partial peeling between the support layer and the PVA layer, and no wrinkles in the transfer layer. do not have ×: Air bubbles are present due to partial peeling between the support layer and the PVA layer. ××: The transfer layer has wrinkles

[0059] <Transfer process evaluation> (Evaluation C: Peeling state of the support layer during the transfer process) For the transfer sheets of Examples 1 to 13 and Comparative Examples 1 to 14 after lamination with the substrate in the transfer step, cellophane tape was applied to the support layer to create a peel trigger, and then the support layer was peeled off at 90°. The state of the process was evaluated according to the following criteria. When no trigger was created, an incision was made with a cutter to allow peeling. ◎ : Cellophane tape can be used to easily create a peeling trigger, allowing for clean peeling ○: Cellophane tape is difficult to peel off, but it can be peeled off cleanly. ×: The cellophane tape did not trigger the peeling, and the support layer and the PVA layer were left with peeling marks when peeled off.

[0060] (Evaluation D: Peelability between PVA layer and transfer layer during transfer process) After peeling off the support layer during the transfer process, a 2 cm square was cut with a cutter from the PVA layer side, cellophane tape was attached to the square, and the tape was peeled off to evaluate the peelability of the PVA layer and the transfer layer. 〇: The PVA layer does not peel off. ×: The PVA layer peels off.

[0061] (Evaluation E: State of the transfer layer after hydrolysis of the PVA layer during the transfer process) The state of the transfer layer after the PVA layer was hydrolyzed during the transfer process was evaluated according to the following criteria. 〇: The transfer layer was transferred neatly to the substrate without any air bubbles, peeling marks, or wrinkle marks. ×: There are air bubbles, peeling marks, and wrinkle marks on the transfer layer.

[0062] [Table 2]

[0063] According to each of the examples according to the present invention, good results were obtained in each evaluation. In particular, good results were obtained for evaluations C to E at all of the transfer process temperatures of 30° C., 80° C., and 130° C. In contrast, Comparative Examples 1 to 6 and 8, which do not satisfy the requirements of the present invention in the composition of the polyvinyl alcohol layer 3, gave poor results in many of the evaluations C and E. In particular, Comparative Example 3, which uses 1,2,6-hexanetriol, did not give good results because all of the hydroxyl groups were not located at the δ position. In Comparative Example 7, the composition of the polyvinyl alcohol layer 3 meets the requirements of the present invention, but the T-peel strength is less than 30 mN / 20 mm, so partial peeling occurs between the support layer 2 and the polyvinyl alcohol layer 3, causing air bubble marks in the transfer layer 4, and therefore good results were not obtained. Furthermore, Comparative Examples 9 and 10, which used surface-treated PET and had a layer made only of polyvinyl alcohol, Comparative Example 11, which used surface-treated polypropylene and had a layer made only of polyvinyl alcohol, Comparative Examples 12 and 13, which used a surface-treated PET layer or polypropylene layer and had a polyvinyl alcohol layer that did not satisfy the requirements of the present invention, and Comparative Example 14, which used a surface-treated PET layer and met the requirements for the polyvinyl alcohol layer of the present invention but did not meet the T-peel strength requirements, all had similar results to Comparative Examples 1 to 7. Furthermore, Comparative Example 15, which did not use a polyester layer, did not have a support layer 2 and therefore showed a poor result in evaluation B, and also did not show a good result in evaluation E. The above results show that by using transfer sheet 1 of the present invention, transfer can be smoothly carried out at room temperature or under heating. [Industrial Applicability]

[0064] The transfer sheet of the present invention can transfer not only patterns but also functional materials such as photoresist and other hardening resins, metal films, and inorganic oxides to a target substrate without air bubbles or wrinkles, both at room temperature and under heated conditions. It can be used as a process member for molding processes using transfer for automobile parts, electronic parts, metal surface processing, etc.

Claims

1. The support layer has a structure in which a polyester layer, a polyvinyl alcohol (PVA) layer, and a transfer layer are laminated in this order, and the polyvinyl alcohol layer contains a triol compound in which an adjacent hydroxyl group is located at the δ position or later, A transfer sheet that satisfies the following condition (i): (i) After humidity conditioning in an environment of 23° C. and 50% RH before the formation of the transfer layer, the polyester layer and the polyvinyl alcohol layer have a T-peel strength of 30 mN / 20 mm or more at a peel speed of 100 mm / min.

2. (delete)

3. (delete)

4. (delete)

5. The transfer sheet according to claim 1 , wherein the polyvinyl alcohol layer contains a diol compound.

6. 6. The transfer sheet according to claim 1, wherein the diol compound is a polyalkylene glycol having a number average molecular weight of 1,000 or more.

7. 7. The transfer sheet according to claim 1, wherein the polyvinyl alcohol layer has a thickness of 5 to 100 μm.

8. 8. The transfer sheet according to claim 1, wherein the polyester layer is not subjected to a release treatment.

9. 9. The transfer sheet according to claim 1, wherein the transfer layer is made of at least one material selected from the group consisting of thermoplastic resins, metal films, and inorganic oxides.

10. 9. The transfer sheet according to claim 1, wherein the transfer layer is made of a curable resin.

11. A transfer layer side of the transfer sheet according to claim 9 is attached to a surface of a flat or three-dimensional substrate, The polyester layer is then peeled off. Furthermore, the transfer method includes dissolving the polyvinyl alcohol layer in water and removing it, thereby forming a transfer layer on the surface of the substrate.

12. After the curable resin is cured, the transfer layer side of the transfer sheet according to claim 10 is attached to a surface of a flat or three-dimensional substrate, The polyester layer is then peeled off. Furthermore, the transfer method includes dissolving the polyvinyl alcohol layer in water and removing it, thereby forming a transfer layer on the surface of the substrate.

Citation Information

Patent Citations

  • Water transfer printing process

    CN106394047A

  • Heat developing photo sensitive material

    JP1986193142A

  • Original plate of waterless planographic printing plate

    JP1996305009A

  • Thermal transfer sheet

    JP1998166793A

  • Aminoplast resin-photochromic coating compositions and photochromic articles