Optical fiber fusion splicing device and optical fiber fusion splicing method

By employing a short discharge followed by a pause before an arc discharge, the method stabilizes ion distribution and discharge paths, enhancing the quality and consistency of optical fiber fusion splicing.

JP7567141B2Active Publication Date: 2024-10-16SUMITOMO ELECTRIC OPTIFRONTIER CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021524921
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-05
Filing Date
2020-06-05
Publication Date
2024-10-16
Estimated Expiration
2040-06-05

AI Technical Summary

Technical Problem

Existing optical fiber fusion splicing methods and devices face challenges in stabilizing the quality of spliced parts due to variations in discharge paths caused by non-uniform ion distribution between electrodes, leading to inconsistent fusion splicing results.

Method used

The method involves generating a short discharge followed by a pause, then an arc discharge, with the short discharge time being less than 200 milliseconds and the pause time being 100 milliseconds or less, to stabilize ion distribution and ensure a consistent discharge path.

Benefits of technology

This approach reduces variations in discharge paths and stabilizes the quality of spliced optical fibers by ensuring a uniform ion distribution, resulting in more consistent and reliable fusion splicing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567141000001
    Figure 0007567141000001
  • Figure 0007567141000002
    Figure 0007567141000002
  • Figure 0007567141000003
    Figure 0007567141000003
Patent Text Reader

Abstract

This optical fiber fusion splicing device fusion splices together, via arc discharge, a pair or a plurality of pairs of optical fibers that are arrayed with the end faces thereof abutting one another. This device comprises a pair of electrodes, an optical fiber disposition unit, and a control unit. The pair of electrodes generate the arc discharge. The optical fiber disposition unit positions the pair or plurality of pairs of optical fibers between the pair of electrodes. The control unit controls the voltage applied to the pair of electrodes. The control unit generates a first discharge between the pair of electrodes, and stops the first discharge between the pair of electrodes, after which the control unit generates an arc discharge between the pair of electrodes to fusion splice the pair or plurality of pairs of optical fibers together. The discharge time of the first discharge is 200 milliseconds or less. The time from the stopping of the first discharge to the starting of the arc discharge is 100 milliseconds or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an optical fiber fusion splicer and a method for fusion splicing optical fibers. This application claims priority to Japanese Application No. 2019-105103, filed on June 5, 2019, and incorporates by reference all of the contents of said Japanese application. [Background technology]

[0002] Patent Documents 1 to 5 describe techniques relating to optical fiber fusion splicing devices or optical fiber fusion splicing methods. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-122508 A [Patent Document 2] JP 2004-138650 A [Patent Document 3] JP 2001-66456 A [Patent Document 4] JP 2000-98170 A [Patent Document 5] Japanese Patent Application Publication No. 7-318742 Summary of the Invention

[0004] The optical fiber fusion splicing device of the present disclosure is a device that fusion splices one or more pairs of optical fibers arranged with their end faces butted against each other by arc discharge. The device includes a pair of electrodes, an optical fiber arrangement unit, and a control unit. The pair of electrodes generates an arc discharge. The optical fiber arrangement unit positions the pair or more pairs of optical fibers between the pair of electrodes. The control unit controls a voltage applied to the pair of electrodes. The control unit generates a first discharge between the pair of electrodes, pauses the first discharge between the pair of electrodes, and then generates an arc discharge between the pair of electrodes to fusion splice the pair or more pairs of optical fibers. The discharge time of the first discharge is 200 milliseconds or less. The time from pausing the first discharge to starting the arc discharge is 100 milliseconds or less.

[0005] The optical fiber fusion splicing method of the present disclosure is a method for fusion splicing one or more pairs of optical fibers arranged with their end faces butted against each other between a pair of electrodes by arc discharge generated between the pair of electrodes. This method includes a first step, a second step, and a third step. In the first step, discharge is generated between the pair of electrodes. In the second step, the discharge between the pair of electrodes is paused. In the third step, arc discharge is generated between the pair of electrodes to fusion splice one or more pairs of optical fibers together. The discharge time in the first step is 200 milliseconds or less. The time from pausing the discharge in the first step to starting the arc discharge in the third step is 100 milliseconds or less. [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a perspective view showing the appearance of a fusion splicing apparatus according to an embodiment. [Diagram 2] FIG. 2 is an enlarged perspective view of a fusion splicing section provided in the fusion splicing device. [Diagram 3] FIG. 3 is an enlarged cross-sectional side view showing a pair of electrodes and a first arrangement portion of the base. [Figure 4] FIG. 4 is a block diagram showing electrical connections within the fusion splicing device. [Diagram 5] FIG. 5 is a block diagram illustrating an example of a hardware configuration of the control unit. [Figure 6] FIG. 6 is a flow chart illustrating the operation of a fusion splicing device and a fusion splicing method of one embodiment. [Figure 7] FIG. 7 is a schematic diagram showing a state in which the discharge between the electrodes is paused. [Figure 8] FIG. 8 is a schematic diagram showing the state of discharge between electrodes. [Figure 9] FIG. 9 is a schematic diagram showing a state in which the discharge between the electrodes is paused. [Figure 10] FIG. 10 is a schematic diagram showing the state of discharge between electrodes. [Figure 11] FIG. 11 is a diagram for explaining problems with the conventional device and method. [Figure 12] FIG. 12 is a flowchart showing the operation of a fusion splicing device and a fusion splicing method according to one modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] [Problem that this disclosure aims to solve] As disclosed in Patent Documents 1 to 5, methods and devices are known for fusion splicing one or more pairs of optical fibers arranged with their end faces butted against each other by arc discharge between a pair of electrodes. In such fusion splicing methods and devices, when an arc discharge occurs, a discharge path with the smallest insulation resistance between the pair of electrodes is selected. Normally, the discharge path coincides with the shortest path between the pair of electrodes, but depending on the electrical conditions between the electrodes, such as the ion distribution conditions, a peculiar path that does not coincide with the shortest path and is not constant may be selected. For this reason, if the discharge path varies, it becomes difficult to achieve a fusion splice with stable quality.

[0008] Therefore, an object of the present disclosure is to provide an optical fiber fusion splicing device and an optical fiber fusion splicing method that can reduce the variation in the discharge path and stabilize the quality of the spliced ​​portion.

[0009] [Effects of this disclosure] According to the present disclosure, it is possible to provide an optical fiber fusion splicing device and an optical fiber fusion splicing method that can reduce variations in the discharge path and stabilize the quality of the spliced ​​portion.

[0010] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be listed and described. An optical fiber fusion splicing device according to one embodiment is a device that fusion splices one or more pairs of optical fibers arranged with their end faces butted against each other by arc discharge. This fusion splicing device includes a pair of electrodes, an optical fiber arrangement unit, and a control unit. The pair of electrodes generates an arc discharge. The optical fiber arrangement unit positions the pair or more pairs of optical fibers between the pair of electrodes. The control unit controls a voltage applied to the pair of electrodes. The control unit generates a first discharge between the pair of electrodes, pauses the first discharge between the pair of electrodes, and then generates an arc discharge between the pair of electrodes to fusion splice the one or more pairs of optical fibers to each other. The discharge time of the first discharge is 200 milliseconds or less. The time from pausing the first discharge to starting the arc discharge is 100 milliseconds or less.

[0011] A method for fusion splicing optical fibers according to one embodiment is a method for fusion splicing one or more pairs of optical fibers arranged with their end faces butted against each other between a pair of electrodes by arc discharge generated between the pair of electrodes. This method includes a first step, a second step, and a third step. In the first step, discharge is generated between the pair of electrodes. In the second step, the discharge between the pair of electrodes is paused. In the third step, arc discharge is generated between the pair of electrodes to fusion splice one or more pairs of optical fibers together. The discharge time in the first step is 200 milliseconds or less. The time from pausing the discharge in the first step to starting the arc discharge in the third step is 100 milliseconds or less.

[0012] The inventors have found through experiments that the quality of the spliced ​​portion can be stabilized by performing an extremely short discharge, i.e., 200 milliseconds or less, before the arc discharge for fusion splicing, and then performing an arc discharge after a short pause, i.e., 100 milliseconds or less. There are various possible reasons for this, but one possible explanation is as follows: If the ion distribution between a pair of electrodes changes and becomes uneven due to some cause, a unique path is selected during the arc discharge. In such a case, if an extremely short discharge is performed before the arc discharge, the discharge can make the ion distribution between the electrodes uniform. Therefore, the probability that a normal path, for example the shortest path between a pair of electrodes, is selected as the discharge path can be improved, and the variation in the discharge path can be reduced.

[0013] In the above fusion splicing apparatus, the power of the first discharge may be greater than the power of the arc discharge. Similarly, in the above fusion splicing method, the discharge power of the first step may be greater than the arc discharge power of the third step. According to the inventor's experiments, for example, in such a case, the variation in the discharge path can be effectively reduced and the quality of the spliced ​​portion can be more stabilized.

[0014] In the above fusion splicing apparatus, the control unit may generate an arc discharge after alternately repeating the first discharge and pause multiple times. Similarly, in the above fusion splicing method, the third step may be performed after alternately repeating the first step and the second step multiple times. For example, even in such a case, the above-mentioned effect can be achieved.

[0015] In the above fusion splicing apparatus, the power of each first discharge may be equal to or less than the power of the arc discharge. Similarly, in the above fusion splicing method, the discharge power of each first step may be equal to or less than the arc discharge power of the third step. According to experiments by the present inventors, in such a case, for example, the variation in the discharge path can be effectively reduced, and the quality of the spliced ​​portion can be more stabilized.

[0016] In the above fusion splicing device, the control unit may perform sputter discharge for end face cleaning before the first discharge, and the time from pausing the sputter discharge to starting the first discharge may be longer than 100 milliseconds. Similarly, the above fusion splicing method may further include a step of performing sputter discharge for end face cleaning before the first step, and the time from pausing the sputter discharge to starting the discharge of the first step may be longer than 100 milliseconds. Conventionally, when fusion splicing optical fibers, sputter discharge for end face cleaning may be performed in advance. Usually, the discharge time of this sputter discharge is within a range of 50 milliseconds to 200 milliseconds. The first discharge and the discharge of the first step of the present disclosure have a completely different purpose from such sputter discharge, and the above-mentioned action and effect are achieved by setting the pause time to 100 milliseconds or less, which is shorter than that of the sputter discharge.

[0017] In the above fusion splicing apparatus, the discharge time of the first discharge may be 100 milliseconds or less. Similarly, in the above fusion splicing method, the discharge time of the first step may be 100 milliseconds or less. In this case, it is possible to effectively reduce the variation in the discharge path.

[0018] [Details of the embodiment of the present disclosure] Specific examples of the optical fiber fusion splicing device and the optical fiber fusion splicing method of the present disclosure will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims. In the following description, the same elements in the description of the drawings are given the same reference numerals, and duplicated descriptions are omitted. In the description, the XYZ Cartesian coordinate system shown in the drawings may be referenced.

[0019] Fig. 1 is a perspective view showing the appearance of a fusion splicing device 1 according to this embodiment. The fusion splicing device 1 is a device that melts and fusion-splices multiple pairs of optical fibers arranged with their end faces butted against each other by arc discharge. The optical fibers are, for example, glass fibers. The fusion splicing device 1 fusion-splices, for example, the ends of multiple optical fibers constituting a multi-core optical fiber cable to the ends of multiple optical fibers constituting another multi-core optical fiber cable.

[0020] As shown in FIG. 1, the fusion splicing device 1 includes a box-shaped housing 32. A fusion splicing section for fusing optical fibers together, which will be described later, and a heater 34 are provided on the upper part of the housing 32. The heater 34 heats and shrinks a fiber reinforcement sleeve that is placed over the fusion spliced ​​portion of the optical fiber. The fusion splicing device 1 further includes a monitor 35, a windshield cover 36, a power switch 37, and a connection start switch 38. The monitor 35 displays the fusion splicing status of the optical fibers captured by a camera (not shown) disposed inside the housing 32. The windshield cover 36 prevents wind from entering the fusion splicing section. The power switch 37 is a push button for switching the power of the fusion splicing device 1 on and off in response to a user's operation. The connection start switch 38 is a push button for starting an operation for fusing optical fibers together in response to a user's operation.

[0021] Fig. 2 is an enlarged perspective view of the fusion splicing unit 10 included in the fusion splicing apparatus 1. As shown in Fig. 2, the fusion splicing unit 10 has a pair of electrodes 5, 6 and a base 11. The pair of electrodes 5, 6 are arranged spaced apart from each other on the base 11. The tip 5a of the electrode 5 and the tip 6a of the electrode 6 face each other. In the illustrated example, the electrodes 5, 6 include approximately conical portions whose diameters decrease toward the tips 5a, 6a.

[0022] The base 11 includes an electrode arrangement section 13 and an optical fiber arrangement section 15. As an example, the material of the base 11 may be zirconia. The electrode arrangement section 13 is a section where the pair of electrodes 5, 6 are arranged. The electrode arrangement section 13 has contact surfaces 13a, 13b corresponding to the pair of electrodes 5, 6, respectively. The contact surfaces 13a, 13b are formed by two planes so that their cross sections are substantially V-shaped. The electrode 5 contacts the contact surface 13a, thereby determining the position of the electrode 5 in the Y direction and the Z direction. The electrode 6 contacts the contact surface 13b, thereby determining the position of the electrode 6 in the Y direction and the Z direction. The positions of the electrodes 5, 6 in the X direction can be adjusted in a state where the electrodes 5, 6 contact the contact surfaces 13a, 13b. The positioned electrodes 5, 6 can be fixed to the electrode arrangement section 13 by a fixing member (not shown). Furthermore, the base 11 has an opening 11a. The opening 11a penetrates the base 11 in the Z direction in a region between the contact surfaces 13a and 13b in the X direction. The tips 5a and 6a of the pair of electrodes 5 and 6 face each other within the opening 11a.

[0023] The optical fiber arrangement section 15 is located between the pair of electrodes 5, 6 in the X direction. The optical fiber arrangement section 15 has a first arrangement section 16 and a second arrangement section 17. In the Y direction, the first arrangement section 16 is located on one side of a center line C1 connecting the tips 5a, 6a of the pair of electrodes 5, 6. The second arrangement section 17 is located on the other side of the center line C1. That is, the first arrangement section 16 and the second arrangement section 17 are spaced apart from each other in the Y direction across the center line C1. The first arrangement section 16 has a plurality of grooves 16a for accommodating and positioning the plurality of one-side optical fibers. The number of the one-side optical fibers is 12 in the illustrated example. The shape of a cross section perpendicular to the extension direction of the groove 16a is, for example, V-shaped. The grooves 16a are arranged at equal intervals in the X direction and extend linearly along the Y direction. Similarly, the second arrangement section 17 has a plurality of grooves 17a for accommodating and positioning the plurality of other-side optical fibers. The number of the other optical fibers is also 12 in the illustrated example. The cross section perpendicular to the extending direction of the groove 17a is, for example, V-shaped. The grooves 17a are arranged at equal intervals in the X direction and extend linearly along the Y direction. Each of the grooves 16a of the first arrangement section 16 and each of the grooves 17a of the second arrangement section 17 are located on a common straight line. As a result, the optical fibers positioned by the grooves 16a of the first arrangement section 16 and the optical fibers positioned by the grooves 17a of the second arrangement section 17 are butted against each other in the region between the first arrangement section 16 and the second arrangement section 17. The region between the first arrangement section 16 and the second arrangement section 17 is an opening 11a of the base 11.

[0024] Fig. 3 is an enlarged cross-sectional side view of the pair of electrodes 5, 6 and the first arrangement section 16 of the base 11. Fig. 3 is a cross-sectional view looking at the first arrangement section 16 side along the XZ plane including the center line C1, and also shows the multiple optical fibers 3 arranged in the first arrangement section 16. The configuration in which the multiple optical fibers are arranged in the second arrangement section 17 is similar to the configuration in which the multiple optical fibers 3 are arranged in the first arrangement section 16, and therefore a description thereof will be omitted.

[0025] As shown in FIG. 3, the optical fibers 3 are positioned between the pair of electrodes 5, 6 in the X direction, and are housed in the corresponding grooves 16a. The axial direction of each optical fiber 3 coincides with the Y direction. The optical fibers 3 are arranged spaced apart from each other in the X direction. The pitch between adjacent optical fibers 3 is uniform. As an example, the diameter of each optical fiber 3 is 125 μm, and the optical fibers 3 are arranged in the X direction at a pitch of 250 μm, which is twice the diameter. The position at which the optical fibers 3 are arranged is shifted in the Z direction from the center line C1 of the electrodes 5, 6.

[0026] Fig. 4 is a block diagram showing electrical connections within the fusion splicing apparatus 1. As shown in Fig. 4, the fusion splicing apparatus 1 further includes a voltage generating unit 19 that applies a voltage to the pair of electrodes 5, 6, and a control unit 20 that controls the voltage output from the voltage generating unit 19. The voltage generating unit 19 is electrically connected to the electrodes 5, 6 via wiring within the fusion splicing apparatus 1, and applies a voltage for discharge to the electrodes 5, 6. The control unit 20 is electrically connected to the voltage generating unit 19, and controls the magnitude and application timing of the voltage.

[0027] FIG. 5 is a block diagram showing an example of a hardware configuration of the control unit 20. As shown in FIG. 5, the control unit 20 may be configured as a computer including a central processing unit (CPU) 20a, a random access memory (RAM) 20b, and a read only memory (ROM) 20c. The control unit 20 reads and executes a program previously stored in the ROM 20c, and reads and writes data from the RAM 20b and the ROM 20c under the control of the CPU 20a. In this way, the control unit 20 can realize each function of the fusion splicing unit 10, including butting the optical fibers 3 together and discharging the electrodes 5 and 6. The operating status of the control unit 20 is always displayed on the monitor 35 during the operation of the fusion splicing apparatus 1. The control unit 20 is electrically connected to a connection start switch 38 and receives an electric signal from the connection start switch 38.

[0028] Here, the operation of the fusion splicing apparatus 1 will be described together with the fusion splicing method of this embodiment. Fig. 6 is a flowchart showing the operation of the fusion splicing apparatus 1 and the fusion splicing method of this embodiment. Figs. 7 to 10 are schematic diagrams showing the state of discharge between the electrodes 5 and 6.

[0029] 6, in step S1, one optical fiber 3 to be spliced ​​is accommodated in each groove 16a of the base 11 of the fusion splicer 1. The other optical fiber 3 to be spliced ​​is accommodated in each groove 17a of the base 11. Next, the end face of the optical fiber 3 accommodated in the groove 16a and the end face of the optical fiber 3 accommodated in the groove 17a are made to face each other at the opening 11a.

[0030] Next, in step S2, a predetermined voltage is applied between the electrodes 5 and 6 from the voltage generating unit 19 to perform sputter discharge for end face cleaning. The discharge time of the sputter discharge is longer than 50 milliseconds and shorter than 200 milliseconds. In one example, the discharge time of the sputter discharge is 100 milliseconds. The discharge power applied between the electrodes 5 and 6 during the sputter discharge is, for example, within a range of 50% to 200% of the arc discharge power during fusion splicing, which will be described later. After this sputter discharge, the voltage applied between the electrodes 5 and 6 from the voltage generating unit 19 is lowered, and the discharge is suspended until step S4. During this period, the operator can check through the monitor 35 whether dust or the like is attached to the optical fiber end face. This suspension period is longer than 100 milliseconds, typically about one second to several seconds. FIG. 7 shows this suspension period.

[0031] In step S3, the end face of the optical fiber 3 housed in the groove 16a and the end face of the optical fiber 3 housed in the groove 17a are butted against each other at the opening 11a. This butting is performed by controlling the control unit 20 so that the parts holding the optical fibers 3 approach each other in the Y direction.

[0032] Next, in step S4, a voltage is applied from the voltage generating unit 19 between the electrodes 5 and 6 instantaneously, and an extremely short-time discharge P1 shown in FIG. 8 is generated between the electrodes 5 and 6. This step S4 is the first step in this embodiment, and this discharge is the first discharge in this embodiment. Specifically, for example, a voltage of several kV to several tens of kV is applied between the electrodes 5 and 6, and a high-frequency discharge is generated with a frequency of about 100 kHz and a current of several tens of mA. The discharge time may be 200 milliseconds or less, 100 milliseconds or less, 50 milliseconds or less, 30 milliseconds or less, or 10 milliseconds or less. The arc discharge time during fusion splicing is 1 second or more, and usually several seconds to several tens of seconds, so the discharge time in step S3 is extremely short compared to the arc discharge time during fusion splicing. The discharge time in step S4 is equal to or shorter than the sputter discharge time in the above step S2.

[0033] The discharge power in step S4 may be greater than the arc discharge power during fusion splicing, may be the same as the arc discharge power during fusion splicing, or may be less than the arc discharge power during fusion splicing. In one example, the discharge power in step S4 may be 30% or less, or 300% or more, of the arc discharge power during fusion splicing.

[0034] Next, in step S5, the discharge P1 between the electrodes 5 and 6 is paused as shown in Fig. 9. Specifically, the voltage applied between the electrodes 5 and 6 from the voltage generating unit 19 is set to a voltage at which no discharge occurs or less. This pause time, that is, the time from pausing the discharge P1 to starting the next arc discharge, may be 100 milliseconds or less, 50 milliseconds or less, 30 milliseconds or less, or 10 milliseconds or less. This step S5 is the second step in this embodiment.

[0035] 10 is generated between the electrodes 5 and 6, and the arc discharge P2 is overlapped with the portion where the ends of the optical fibers 3 are butted together, thereby melting the ends of one optical fiber 3 and the other optical fiber 3 to fusion splice them together. Specifically, a voltage of, for example, several kV to several tens of kV is applied between the electrodes 5 and 6, and a high-frequency discharge is generated with a frequency of about 100 kHz and a current of several tens of mA. The discharge time of the arc discharge P2 is 1 second or more.

[0036] The effects obtained by the fusion splicing apparatus 1 and the fusion splicing method of the present embodiment having the above configuration will be described. FIG. 11 is a diagram for explaining the problems in the conventional apparatus and method. When an arc discharge P2 for fusion splicing occurs, a discharge path with the smallest insulation resistance between the electrodes 5 and 6 is selected. Usually, the discharge path coincides with the shortest path A1 between the electrodes 5 and 6, but depending on the electrical condition between the electrodes 5 and 6, for example, the distribution condition of ions C which are discharge carriers, a unique path that does not coincide with the shortest path and is not constant may be selected. In the figure, the path A2 is shown as an example of such a path. If the discharge path varies as a result, it becomes difficult to perform fusion splicing of stable quality.

[0037] The inventors have found through experiments that it is possible to reduce the variation in the discharge path and stabilize the quality of the spliced ​​portion by performing an extremely short discharge P1 before the arc discharge P2 for fusion splicing, and then performing the arc discharge P2 after a short pause. There are various possible reasons for this, but one idea is that if an extremely short discharge P1 is performed before the arc discharge P2, the discharge P1 can homogenize the distribution of ions C between the electrodes 5 and 6. Therefore, it is possible to improve the probability that a normal path, for example the shortest path A1 between the electrodes 5 and 6, is selected as the discharge path, and to reduce the variation in the discharge path.

[0038] As described above, the power of the discharge P1 may be greater than the power of the arc discharge P2. According to the inventor's experiments, for example, in such a case, the variation in the discharge path can be effectively reduced and the quality of the connection portion can be more stabilized.

[0039] As in this embodiment, the control unit 20 performs a sputter discharge for end face cleaning before the discharge P1, and the time from pausing the sputter discharge to starting the discharge P1 may be longer than 100 milliseconds. Conventionally, when fusion splicing optical fibers, a sputter discharge for end face cleaning may be performed in advance. Usually, the discharge time of this sputter discharge is within a range of 50 milliseconds to 200 milliseconds. The discharge P1 of this embodiment has a completely different purpose from such a sputter discharge, and by setting the pause time to 100 milliseconds or less, which is shorter than that of the sputter discharge, the above-mentioned action and effect are achieved.

[0040] As described above, the discharge time of the discharge P1 may be 100 milliseconds or less, which can effectively reduce the variation in the discharge path.

[0041] (Modification) FIG. 12 is a flowchart showing the operation of the fusion splicing apparatus 1 and the fusion splicing method according to a modification of the above embodiment. In the above embodiment, the short-time discharge P1 is performed only once, but in this modification, the discharge P1 is performed multiple times. That is, step S4 and step S5 in the above embodiment are alternately repeated multiple times, and then step S6 is performed. The details of steps S4 and S5 are the same as in the above embodiment. Steps S4 and S5 may be repeated two times, three times, or any number of times equal to or greater than four times. In this modification, the same effects as in the above embodiment can be achieved.

[0042] In this modification, the discharge power in each step S4 may be set to be equal to or lower than the arc discharge power in step S6. According to the inventor's experiments, in such a case, for example, the variation in the discharge path can be effectively reduced and the quality of the connection portion can be further stabilized.

[0043] (Example) In order to confirm the effects of the fusion splicing method according to the above embodiment and modified example, the inventors performed experiments while setting the discharge time of discharge P1 to 10 milliseconds, the pause time after discharge P1 to several tens of milliseconds, and varying the discharge power and number of discharges of discharge P1. Then, they investigated the relative occurrence rate of abnormal discharge when the occurrence rate of abnormal discharge in the conventional method in which arc discharge P2 is performed without discharge P1 after sputter discharge for cleaning was set to 1.0.

[0044] As a result, when the number of discharges of the discharge P1 was set to 1 and the discharge power of the discharge P1 was set to 300% of the discharge power of the arc discharge P2, the relative occurrence rate of abnormal discharge was 0.5. When the number of discharges of the discharge P1 was set to 2 and the discharge power of the discharge P1 was set to 100% of the discharge power of the arc discharge P2, the relative occurrence rate of abnormal discharge was 0.6. When the number of discharges of the discharge P1 was set to 3 and the discharge power of the discharge P1 was set to 30% of the discharge power of the arc discharge P2, the relative occurrence rate of abnormal discharge was 0.9. In this way, it was confirmed that the above embodiment and modified example can effectively reduce the variation in the discharge path.

[0045] The optical fiber fusion splicing device and the optical fiber fusion splicing method according to the present invention are not limited to the above-mentioned embodiment, and various other modifications are possible. For example, although the above-mentioned embodiment and modification perform fusion splicing on a plurality of pairs of optical fibers at once, it is also possible to perform fusion splicing on a single pair of optical fibers. Even in this case, it is possible to reduce the variation in the discharge path and stabilize the quality of the spliced ​​portion. [Explanation of symbols]

[0046] 1...Fusion splicer 3…Optical fiber 5,6...electrode 5a,6a…Tip 10…Fusion splice 11…Pedestal 11a...Opening 13...Electrode placement part 13a, 13b…Abutment surface 15...Optical fiber placement section 16...First placement part 16a...Groove 17…Second placement part 17a...Groove 19...Voltage generating section 20...Control section 20a…CPU 20b…RAM 20c…ROM 32…Housing 34…heater 35…Monitor 36…Windshield cover 37…Power switch 38…Connection start switch C...Ion C1…center line P1…discharge P2…Arc discharge

Claims

1. An apparatus for fusion splicing a plurality of pairs of optical fibers arranged with their end faces butted together by arc discharge, comprising: A pair of electrodes for generating an arc discharge; an optical fiber positioning unit that positions the pairs of optical fibers between the pair of electrodes; A control unit that controls a voltage applied to the pair of electrodes; Equipped with the control unit generates a first discharge between the pair of electrodes, stops the first discharge between the pair of electrodes, and then generates an arc discharge between the pair of electrodes to fusion-splice the plurality of pairs of optical fibers to each other; a discharge time of the first discharge is 200 milliseconds or less, and a time from the cessation of the first discharge to the start of the arc discharge is 100 milliseconds or less (but excluding 100 milliseconds); An optical fiber fusion splicing apparatus, wherein the power of the first discharge is greater than the power of the arc discharge.

2. the control unit performs a sputter discharge for cleaning an end surface before the first discharge, 2. The optical fiber fusion splicing apparatus according to claim 1, wherein the time between stopping the sputter discharge and starting the first discharge is longer than 100 milliseconds.

3. 3. The optical fiber fusion splicing device according to claim 1, wherein a discharge time of the first discharge is 100 milliseconds or less.

4. A method for fusion splicing a plurality of pairs of optical fibers arranged with their end faces butted against each other between a pair of electrodes by arc discharge generated between the pair of electrodes, comprising the steps of: a first step of generating a discharge between the pair of electrodes; a second step of pausing the discharge between the pair of electrodes; a third step of generating the arc discharge between the pair of electrodes to fusion-splice the pairs of optical fibers together; Including, a discharge time of the first step is 200 milliseconds or less, and a time from when the discharge of the first step is stopped to when the arc discharge of the third step is started is 100 milliseconds or less (excluding 100 milliseconds); a discharge power in the first step being greater than an arc discharge power in the third step;

5. The method further includes a step of performing sputter discharge for edge surface cleaning before the first step, 5. The method for fusion splicing optical fibers according to claim 4, wherein the time from stopping the sputtering discharge to starting the discharge in the first step is longer than 100 milliseconds.

6. 6. The method for fusion splicing optical fibers according to claim 4, wherein the discharge time in the first step is 100 milliseconds or less.

Citation Information

Patent Citations

  • Process and device for the heat treatment of at least one optical fibre

    EP0831347A2

  • Terminal processing for optical fiber strand in fusion-splicing method of optical fiber

    JP1987099704A

  • Fusion splicing method for optical fiber

    JP1987184403A

  • Fusion splicing method for optical fiber