Magnetic material for injection molding and its manufacturing method
A magnetic material composition with specific components and processing enhances wear resistance and reduces cracking in injection molding, addressing the issues of low wear resistance and dimensional mismatch in existing technologies, thus improving the durability and cost-effectiveness of water pump rotors.
Patent Information
- Application Number
- JP2022573718
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-06-30
AI Technical Summary
Injection molding materials for magnetic products, particularly those used in micro-electronic water pumps for turbochargers, suffer from low wear resistance and are prone to cracking due to mismatched dimensional shrinkage rates, leading to issues like motor shaking and noise.
A magnetic material composition comprising 80-85 parts of magnetic powder, 10-15 parts of polymer adhesive, 0.5-1 part of first coupling agent, 0.5-1 part of second coupling agent, and 2-5 parts of wollastonite, with specific mixing and extrusion processes to enhance bonding and wear resistance.
The solution improves wear resistance and reduces cracking, allowing for integral injection molding without secondary processes, thereby reducing manufacturing costs and enhancing the durability of water pump rotors.
Smart Images

Figure 0007567143000003 
Figure 0007567143000004 
Figure 0007567143000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of magnetic materials for injection molding, and in particular to magnetic materials for injection molding and methods for their manufacture. [Background technology]
[0002] Injection-molded magnetic products have the advantages of high dimensional accuracy, good processing performance, and ease of mass production, and are therefore widely used in the fields of automobiles, home appliances, power tools, and other fields. In recent years, with the focus on the development of turbocharged vehicles and the continuous popularization of new energy vehicles, micro electronic water pumps for turbochargers and battery pack liquid cooling systems have been rapidly developed. At present, the micro electronic water pump mainly adopts a permanent magnetic DC motor, and the rotor of the motor adopts an injection-molded magnetic material with high dimensional accuracy, high mechanical strength, long operating life, and high temperature (above 180°C) resistance. The rotor of water pumps needs to operate at high speed around the central shaft member during operation, and the inner circle of the rotor of the injection-molded magnetic material is easily worn out when rubbed at high speed, and the worn rotor is easily prone to problems with dynamic balance, resulting in problems such as motor shaking and abnormal noise.
[0003] The currently commonly used solution is to improve the wear resistance of the rotor by inserting wear-resistant materials, such as composite graphite inserts, PPS+30%GF inserts, etc., into the rotor magnetic body. However, this method requires secondary injection molding, and the insert materials, especially graphite inserts, are generally expensive, which also significantly increases the manufacturing cost of the water pump rotor. Moreover, this method also has the problem that the dimensional shrinkage rates of the insert and the injection-molded magnetic body are not consistent, which makes the magnetic body prone to cracking due to thermal shock. Summary of the Invention [Problem to be solved by the invention]
[0004] The main objective of the present invention is to provide a magnetic material for injection molding and a manufacturing method thereof, in order to solve the problems of the prior art that the injection molding material has low wear resistance and is prone to cracking. [Means for solving the problem]
[0005] In order to achieve the above object, according to one aspect of the present invention, A magnetic material for injection molding is provided, comprising, by weight, 80 to 85 parts of magnetic powder, 10 to 15 parts of polymeric adhesive, 0.5 to 1 part of a first coupling agent, 0.5 to 1 part of a second coupling agent, 2 to 5 parts of wollastonite, and 0.1 to 1 part of an auxiliary.
[0006] Furthermore, the magnetic powder is a ferrite magnetic powder and / or a rare earth magnetic powder for injection molding, preferably the ferrite magnetic powder is Sr ferrite and / or Ba ferrite magnetic powder, more preferably the ferrite magnetic powder is Sr ferrite, and preferably the average particle size D50 of the magnetic powder is 1.8 to 2.0 μm.
[0007] Furthermore, the polymer adhesive is polyphenylene sulfide, and preferably the polyphenylene sulfide has a melt flow rate of 500 to 3000 g / 10 min.
[0008] Furthermore, the auxiliary is a composition of a fluorine additive and a lubricant, preferably the fluorine additive is polyphthalamide, preferably the lubricant is erucamide, and more preferably the weight ratio of the fluorine additive to the lubricant is 2:3 to 3:2.
[0009] Furthermore, the wollastonite is ultrafine wollastonite, and more preferably the particle size of the wollastonite is 800 to 1200 mesh.
[0010] Further, the first coupling agent is a silane coupling agent, preferably the silane coupling agent is KH550 and / or KH560, and preferably the second coupling agent is a phosphate ester coupling agent.
[0011] Furthermore, the magnetic material for injection molding is By weight, it contains 83-85 parts of magnetic powder, 12-15 parts of polymeric adhesive, 0.5-1 part of a first coupling agent, 0.5-1 part of a second coupling agent, 2-5 parts of wollastonite, and 0.1-1 part of an auxiliary agent; More preferably, the magnetic material for injection molding comprises: It contains, by weight, 83 parts of magnetic powder, 12 parts of polymeric adhesive, 0.5 parts of first coupling agent, 0.5 parts of second coupling agent, 3 parts of wollastonite, and 1 part of auxiliary agent.
[0012] In order to achieve the above object, one aspect of the present invention is to The present invention provides a method for producing the magnetic material for injection molding, comprising step S1 of subjecting a magnetic powder, a first coupling agent, and a polymer adhesive to a first mixing to obtain a first mixture, step S2 of subjecting the first mixture to a first extrusion granulation to obtain a magnetic base material for injection molding, step S3 of subjecting the magnetic base material for injection molding, a second coupling agent, wollastonite, and an auxiliary to a second mixing to obtain a second mixture, and step S4 of subjecting the second mixture to a second extrusion granulation to obtain the magnetic material for injection molding.
[0013] Further, the temperature of the first mixing and the second mixing is independently 80 to 120° C., and the time of the first mixing and the second mixing is independently 30 to 60 minutes.
[0014] Furthermore, a twin-screw extruder is used for both the first extrusion granulation and the second extrusion granulation, and preferably the temperatures for the first extrusion granulation and the second extrusion granulation are independently 290 to 310°C.
[0015] Furthermore, in step S3, the first coupling agent and the second coupling agent are mixed with an organic solvent before use, preferably the organic solvent is isopropyl alcohol, and preferably the second coupling agent and the organic solvent are mixed in a weight ratio of 1:5 to 1:10. Effect of the Invention
[0016] According to the technical solution of the present invention, in the magnetic material for injection molding of the present application, the surface of the magnetic material for injection molding is filled with wollastonite, thereby effectively improving the bonding effect at the interface between each component, and the moldability and wear resistance of the magnetic material for injection molding are ensured by using the auxiliary and wollastonite, the first coupling agent improves the compatibility between the magnetic powder and the adhesive, and the second coupling agent improves the adhesion of the wollastonite and enhances the bonding force between the wollastonite and the magnetic powder, thereby improving the wear resistance of the magnetic material for injection molding. By the blending ratio of each component being within the above range, each component plays a synergistic effect, the bonding effect at the interface between each component is enhanced, and the wear resistance of the magnetic material for injection molding is further improved. [Brief description of the drawings]
[0017] The drawings in the specification which form a part of this application are provided for a further understanding of the present invention, and the illustrative examples of the present invention and the description thereof are intended to interpret the present invention and are not intended to unduly limit the present invention. The drawings are as follows: [Figure 1] 1 illustrates a magnetic device for use in one specific embodiment of the present invention. [Diagram 2] 1 shows a magnetic device used in Comparative Example 4 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In addition, unless contradictory, the embodiments and features of the embodiments of the present application may be combined with each other. Hereinafter, the present invention will be described in detail in combination with the embodiments with reference to the drawings.
[0019] As analyzed in the background art, the injection molding material according to the prior art has a problem of low wear resistance and easy cracking. To solve this problem, the present application provides a magnetic material for injection molding and a manufacturing method thereof.
[0020] In an exemplary embodiment of the present application, A magnetic material for injection molding is provided, comprising, by weight, 80 to 85 parts of magnetic powder, 10 to 15 parts of polymeric adhesive, 0.5 to 1 part of a first coupling agent, 0.5 to 1 part of a second coupling agent, 2 to 5 parts of wollastonite, and 0.1 to 1 part of an auxiliary.
[0021] In the magnetic material for injection molding of the present application, the surface of the magnetic material for injection molding is filled with wollastonite, thereby effectively improving the bonding effect at the interface between each component, and the moldability and wear resistance of the magnetic material for injection molding are ensured by using an auxiliary and wollastonite, the first coupling agent improves the compatibility between the magnetic powder and the adhesive, and the second coupling agent improves the adhesive force of the wollastonite and increases the bonding force between the wollastonite and the magnetic powder, thereby improving the wear resistance of the magnetic material for injection molding. By having the compounding ratio of each component within the above range, each component acts synergistically, the bonding effect at the interface between each component is increased, and the wear resistance of the magnetic material for injection molding is further improved.
[0022] Of the above components, the higher the content of the polymer adhesive and wollastonite, the lower the viscosity of the magnetic material for injection molding and the more the fluidity deteriorates, resulting in a decrease in the performance of the magnetic material for injection molding.
[0023] In the prior art, the dimensional shrinkage mismatch mainly occurs between dissimilar materials, for example, when a magnetic body is injection molded in addition to a graphite insert, the graphite insert and the magnetic body will experience different degrees of shrinkage. In contrast, in the present application, the components are thoroughly mixed and kneaded to improve the wear resistance of the magnetic material for injection molding, which solves the problem of dimensional shrinkage mismatch when used in the manufacture of water pump rotors.
[0024] The magnetic material for injection molding of the present application can be integrally injection molded into the rotor of a water pump rotor, which has high wear resistance, and does not require the use of wear-resistant fitted secondary injection molding, thereby significantly reducing the manufacturing costs due to secondary injection molding and inserts, while reducing the risk of cracks occurring in the product due to the dimensional shrinkage rate of the insert and the injection molded magnetic material not matching.
[0025] In the present application, the type of magnetic powder is not particularly limited, and any magnetic powder commonly used in this field can be applied to the present application. In some embodiments, the magnetic powder is a ferrite magnetic powder or a rare earth magnetic powder for injection molding, preferably the ferrite magnetic powder is Sr ferrite and / or Ba ferrite magnetic powder, more preferably the ferrite magnetic powder is Sr ferrite. If the average particle size of the magnetic powder is too large, the flowability of the magnetic material for injection molding decreases, and in order to achieve both the flowability and mechanical strength of the magnetic material for injection molding, the average particle size D50 of the magnetic powder is preferably 1.8 to 2.0 μm.
[0026] The type of polymer adhesive is specifically selected according to the needs of the injection molded magnetic device. In consideration of cost and to maintain the flowability of the magnetic material for injection molding, in some embodiments, the polymer adhesive is polyphenylene sulfide, preferably the polyphenylene sulfide has a melt flow rate of 500-3000g / 10min, more preferably 1100-2500g / 10min. The melt flow rate is measured at 316°C and 5Kg according to ISO1133.
[0027] In order to ensure the moldability and wear resistance of the magnetic material for injection molding, in some embodiments, the auxiliary is a composition of a fluorine additive and a lubricant, preferably the fluorine additive is polyphthalamide (PPA), preferably the model number of the fluorine additive is DA310ST, preferably the lubricant is erucamide, and more preferably the weight ratio of the fluorine additive to the lubricant is 2:3 to 3:2.
[0028] In some embodiments, the wollastonite is ultrafine wollastonite, and more preferably, the particle size of the wollastonite is 800-1200 mesh. By making the particle size of the wollastonite in this range, the wear resistance of the magnetic material for injection molding is greatly improved; if the particle size of the wollastonite is too high, the powder becomes finer than necessary, and more adhesive is required, which reduces the flowability of the magnetic material for injection molding and negatively affects the wear resistance of the magnetic material for injection molding; if the particle size of the wollastonite is too low, the powder falls off.
[0029] The coupling agent can provide good dispersibility for the magnetic powder in the system, good compatibility with the magnetic material for injection molding, and enhance the binding strength of each component. In order to obtain a better coupling effect, in some embodiments, the first coupling agent is a silane coupling agent, preferably the silane coupling agent is KH550 and / or KH560, and preferably the second coupling agent is a phosphate ester coupling agent.
[0030] In order to further enhance the synergistic effect between the components and improve the wear resistance of the magnetic material for injection molding, in some embodiments, the magnetic material for injection molding comprises: More preferably, the magnetic material for injection molding comprises, by weight, 83-85 parts of magnetic powder, 12-15 parts of polymeric adhesive, 0.5-1 part of first coupling agent, 0.5-1 part of second coupling agent, 2-5 parts of wollastonite, and 0.1-1 part of auxiliary agent. It contains, by weight, 83 parts of magnetic powder, 12 parts of polymeric adhesive, 0.5 parts of first coupling agent, 0.5 parts of second coupling agent, 3 parts of wollastonite, and 1 part of auxiliary agent.
[0031] In another representative embodiment of the present application, a method for producing the above-mentioned magnetic material for injection molding is provided, and the method includes a step S1 of subjecting a magnetic powder, a first coupling agent, and an adhesive to a first mixing to obtain a first mixture, a step S2 of subjecting the first mixture to a first extrusion granulation to obtain a magnetic base material for injection molding, a step S3 of subjecting the magnetic base material for injection molding, a second coupling agent, wollastonite, and an auxiliary agent to a second mixing to obtain a second mixture, and a step S4 of subjecting the second mixture to a second extrusion granulation to obtain a magnetic material for injection molding.
[0032] In the present application, the raw materials are weighed out in the above-mentioned ratio of each component, and the compatibility between the magnetic powder and the adhesive is improved by carrying out the first coupling treatment, and the adhesive strength of the wollastonite is improved by carrying out the second coupling treatment, thereby improving the wear resistance of the magnetic material for injection molding. The magnetic material for injection molding manufactured by the manufacturing method of the present application has excellent wear resistance and is less susceptible to cracking.
[0033] In some embodiments, to perform a coupling process on the magnetic powder, step S1 includes subjecting the magnetic powder and a first coupling agent to a third mixture to obtain a third mixture, and subjecting the third mixture and an adhesive to a first mixture to obtain the first mixture.
[0034] In some embodiments, to perform a coupling process on the magnetic base material for injection molding, step S3 includes subjecting the magnetic base material for injection molding and a second coupling agent to a fourth mixture to obtain a fourth mixture, and subjecting the fourth mixture, wollastonite, and an auxiliary agent to a second mixture to obtain a second mixture.
[0035] The temperatures of the third and fourth mixtures are independently 80 to 120° C., and the times of the first and second mixtures are independently 30 to 60 minutes.
[0036] In the present application, the mixing conditions are not particularly limited, and in some embodiments, the temperatures of the first mixing and the second mixing are independently 80 to 120° C., and the times of the first mixing and the second mixing are independently 30 to 60 minutes.
[0037] All extrusion granulation conditions commonly used in this field can be applied to the present application. In some embodiments, the first extrusion granulation and the second extrusion granulation are both performed using a twin-screw extruder, and preferably the temperatures of the first extrusion granulation and the second extrusion granulation are independently 290 to 310°C.
[0038] In order to mix the magnetic base material for injection molding and the second coupling agent more uniformly, in some embodiments, in step S3, the first coupling agent and the second coupling agent are mixed with an organic solvent before use, preferably the organic solvent is isopropyl alcohol, and preferably the second coupling agent and the organic solvent are mixed in a weight ratio of 1:5 to 1:10.
[0039] In some embodiments, the first and second mixing may all be mixed at high speed in a high speed mixer, and the speed of the first and second mixing is independently 600 to 1000 rpm.
[0040] The present application will be described in more detail below in conjunction with specific examples, but these examples do not limit the scope of protection of the present application.
[0041] In the present invention, unless otherwise specified, all the equipment and materials may be commercially available or commonly used in the art, and the methods described in the following examples are common methods in the art, unless otherwise specified.
[0042] Average particle size of permanent magnetic Sr ferrite magnetic powder (Fisher air permeability method) D50: 1.8-2.0μm; Polyphenylene sulfide I: Melt index (316℃, Kg) 500g / 10min; Polyphenylene sulfide II: Melt index (316℃, Kg) 1100g / 10min; Polyphenylene sulfide III: Melt index (316℃, Kg) 2500g / 10min; Wollastonite A: particle size 500 mesh; Wollastonite B: grain size 800 mesh; Wollastonite C: grain size 1200 mesh; Wollastonite D: grain size 1500 mesh; Auxiliary agent A: Fluorine additive PPA 0.5 parts, erucamide 0.5 parts; Auxiliary agent B: Fluorine additive PPA 0.6 parts, erucamide 0.4 parts; Auxiliary agent C: Fluorine additive PPA 0.4 parts, erucamide 0.6 parts; Auxiliary agent D: Fluorine additive PPA 0.05 parts, Erucamide 0.05 parts.
[0043] Test Method: Dumbbell-shaped strength test specimens and strips were injection molded at a temperature of 330°C, and then A Universal 6633 testing machine is used to evaluate the tensile and flexural strength of the materials.
[0044] The magnetic material for injection molding in each of the following examples was injection molded to form the magnetic device shown in FIG. 1, and the magnetic material for injection molding in Comparative Example 4 was injection molded to form the magnetic device shown in FIG. 2. The magnetic device was attached to a water pump motor and operated at high speed for 300 hours at a rotation speed of 1000 rpm, and the rate of change in the dimension of the inner hole before and after operation was tested.
[0045] The flowability of the examples and comparative examples of each group is tested according to ISO 1133 at 330° C. and a pressure of 10 kg.
[0046] Example 1 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100°C and 800 rpm for 40 minutes to obtain a fourth mixture.
[0047] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 500 g / 10 min was added to the fourth mixture, and the mixture was further blended at a rotation speed of 800 rpm for 30 minutes to obtain a first mixture.
[0048] (3) The first mixture was extrusion-granulated at a granulation temperature of 300° C. in a twin-screw extruder to obtain a magnetic base material for injection molding.
[0049] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base material particles for injection molding, and the mixture was blended at high speed at 100°C and 800 rpm for 40 minutes to obtain a third mixture.
[0050] (5) Mix 3 parts of 500 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.5 parts of ethyl acetate and 0.5 parts of erucamide was added, and the mixture was mixed at high speed for an additional 20 minutes at a rotation speed of 800 rpm to obtain a second mixture.
[0051] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0052] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to obtain the magnetic device shown in FIG. 1, where a was a magnet.
[0053] Example 2 Step (5) was the same as in Example 1, except that 3 parts of 800 mesh ultrafine wollastonite was mixed into the third mixture.
[0054] Example 3 Step (5) was the same as in Example 1, except that 3 parts of 1200 mesh ultrafine wollastonite was mixed into the third mixture.
[0055] Example 4 Step (5) was the same as in Example 1, except that 3 parts of 1500 mesh ultrafine wollastonite was mixed into the third mixture.
[0056] Example 5 In step (5), the compounding agent is the fluorine additive PPA. The same as Example 2, except that the glycerol was 0.6 parts and erucamide was 0.4 parts.
[0057] Example 6 In step (5), the compounding agent is the fluorine additive PPA. The results were the same as in Example 2, except that the glycerol was 0.4 parts and erucamide was 0.6 parts.
[0058] Example 7 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0059] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 1100 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0060] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0061] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0062] (5) Mix 3 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0063] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0064] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0065] Example 8 (1) 85 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0066] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 1100 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0067] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0068] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0069] (5) Mix 1 part of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0070] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0071] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0072] Example 9 (1) 81 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0073] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 1100 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0074] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0075] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0076] (5) Mix 5 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0077] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0078] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0079] Example 10 (1) 81 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0080] (2) 14 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 1100 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0081] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0082] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0083] (5) Mix 3 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0084] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0085] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0086] Example 11 (1) 85 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0087] (2) 10 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 1100 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0088] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0089] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0090] (5) Mix 3 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0091] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0092] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0093] Example 12 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0094] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 2500 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0095] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0096] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0097] (5) Mix 3 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.6 parts of cellulose acetate and 0.4 parts of erucamide was added and mixed at high speed for another 20 minutes to obtain a second mixture.
[0098] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0099] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0100] Example 13 (1) 80 parts of Ba ferrite magnetic powder (D50 of 2.0 μm) and 1 part of KH560 coupling agent (a 1:10 mixture of coupling agent and isopropyl alcohol by weight) were blended at high speed at 120° C. and 600 rpm for 30 minutes to obtain a fourth mixture.
[0101] (2) 10 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 500 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0102] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 290° C. to obtain a magnetic base material for injection molding.
[0103] (4) The above magnetic base material particles for injection molding were mixed with one part of a phosphate ester coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6), and then high-speed blended at 100°C and 800 rpm for 40 minutes to obtain a third mixture.
[0104] (5) Mix 2 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. 0.1 parts of a compounding agent containing 0.05 parts of cellulose acetate and 0.05 parts of erucamide was added, and the mixture was mixed at high speed for another 20 minutes to obtain a second mixture.
[0105] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 290° C. to obtain a magnetic material for injection molding.
[0106] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to produce the magnetic device shown in FIG.
[0107] Example 14 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 80° C. and 1,000 rpm for 60 minutes to obtain a fourth mixture.
[0108] (2) 15 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 500 g / 10 min was added to the fourth mixture, and the mixture was further blended for 60 minutes to obtain a first mixture.
[0109] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 310° C. to obtain a magnetic base material for injection molding.
[0110] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 80°C for 60 minutes to obtain a third mixture.
[0111] (5) Mix 3 parts of 1200 mesh ultrafine wollastonite into the third mixture, and add fluorine additive PPA. One part of a composite auxiliary containing 0.5 parts of cellulose acetate and 0.5 parts of erucamide was added, and the mixture was mixed at a high speed of 1000 rpm for an additional 20 minutes to obtain a second mixture.
[0112] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0113] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0114] Comparative Example 1 (1) 87 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 1 part of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a mixture.
[0115] (2) 12 parts of polyphenylene sulfide having a melt index (316°C, Kg) of 500g / 10min was added to the mixture and blended for an additional 30 minutes to obtain a high-speed mixture.
[0116] (3) The high-mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic material for injection molding.
[0117] (4) The above magnetic material for injection molding was injection molded at 335° C. to form the magnetic device shown in FIG.
[0118] Comparative Example 2 (1) 87 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 1 part of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a mixture.
[0119] (2) 12 parts of polyphenylene sulfide having a melt index (316°C, Kg) of 1100 g / 10 min was added to the mixture and blended for an additional 30 minutes to obtain a high-speed mixture.
[0120] (3) The high-mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic material for injection molding.
[0121] (4) The above magnetic material for injection molding was injection molded at 335° C. to form the magnetic device shown in FIG.
[0122] Comparative Example 3 (1) 87 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 1 part of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a mixture.
[0123] (2) 12 parts of polyphenylene sulfide having a melt index (316°C, Kg) of 2500 g / 10 min was added to the mixture and blended for an additional 30 minutes to obtain a high-speed mixture.
[0124] (3) The high-mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic material for injection molding.
[0125] (4) The above magnetic material for injection molding was injection molded at 335° C. to form the magnetic device shown in FIG.
[0126] Comparative Example 4 A673 (PPS+30%GF) material manufactured by Japan Toray Industries, Inc. was injection molded into an insert, and then the material manufactured in Comparative Example 1 was secondarily injection molded into a magnet, and finally the device shown in FIG. 2 was injection molded, where b was the insert and c was the magnet.
[0127] Comparative Example 5 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0128] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 500 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0129] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0130] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0131] (5) Fluorine additive PPA in the third mixture One part of a compounding agent containing 0.5 parts of cellulose acetate and 0.5 parts of erucamide was added, and the mixture was mixed at high speed for another 20 minutes to obtain a second mixture.
[0132] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0133] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0134] Comparative Example 6 (1) 83 parts of Sr ferrite magnetic powder (D50 of 1.8 μm) and 0.5 parts of KH550 coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) were blended at high speed at 100° C. for 40 minutes to obtain a fourth mixture.
[0135] (2) 12 parts of polyphenylene sulfide having a melt index (316° C., Kg) of 500 g / 10 min was added to the fourth mixture, and the mixture was further blended for 30 minutes to obtain a first mixture.
[0136] (3) The first mixture was extrusion-granulated in a twin-screw extruder at a granulation temperature of 300° C. to obtain a magnetic base material for injection molding.
[0137] (4) 0.5 parts of a phosphate coupling agent (a mixture of coupling agent and isopropyl alcohol in a weight ratio of 1:6) was mixed with the above magnetic base particles for injection molding, and high-speed blended at 100°C for 40 minutes to obtain a third mixture.
[0138] (5) 7 parts of 500 mesh ultrafine wollastonite are mixed into the third mixture, and fluorine additive PPA is added. One part of a compounding agent containing 0.5 parts of cellulose acetate and 0.5 parts of erucamide was added, and the mixture was mixed at high speed for another 20 minutes to obtain a second mixture.
[0139] (6) The second mixture was added to a twin-screw extruder and granulated at a granulation temperature of 310° C. to obtain a magnetic material for injection molding.
[0140] (7) The above magnetic material particles for injection molding were injection molded at 335° C. to form the magnetic device shown in FIG.
[0141] The components and proportions of each of the above-mentioned Examples and Comparative Examples are shown in Table 1, and the test results of each of the above-mentioned Examples and Comparative Examples are shown in Table 2.
[0142] [Table 1]
[0143] [Table 2] In Example 10, the abrasion resistance was inferior to that of Example 3 because the proportion of the adhesive PPS was high.
[0144] In Example 11, the flowability was 0 because the proportion of adhesive was low.
[0145] In Example 12, the adhesive used had a low viscosity, so the strength and abrasion resistance of the magnetic material were reduced.
[0146] In Comparative Example 6, the proportion of wollastonite was too high, so that the wollastonite could not be repeatedly covered with the adhesive, and as a result, slight powder shedding was observed.
[0147] As can be seen from the above description, the above-mentioned embodiments of the present invention provide the following technical effects. In the magnetic material for injection molding of the present application, the surface of the magnetic material for injection molding is filled with wollastonite, thereby effectively improving the bonding effect at the interface between each component, and the moldability and wear resistance of the magnetic material for injection molding are ensured by using an auxiliary and wollastonite, the first coupling agent improves the compatibility between the magnetic powder and the adhesive, and the second coupling agent improves the adhesion of the wollastonite and increases the bonding force between the wollastonite and the magnetic powder, thereby improving the wear resistance of the magnetic material for injection molding. By using the above-mentioned range of the blending ratio of each component, each component has a synergistic effect, the bonding effect at the interface between each component is increased, and the wear resistance of the magnetic material for injection molding is further improved.
[0148] The above is merely a preferred embodiment of the present invention, and does not limit the present invention. Those skilled in the art can make various modifications and changes to the present invention. All modifications, equivalent replacements, improvements, etc. made without departing from the spirit and principle of the present invention shall be included in the patent scope of the present invention.
Claims
1. A magnetic material for injection molding, comprising, by weight, 80 to 85 parts of magnetic powder, 10 to 15 parts of polymeric adhesive, 0.5 to 1 part of a first coupling agent, 0.5 to 1 part of a second coupling agent, 2 to 5 parts of wollastonite, and 0.1 to 1 part of an auxiliary.
2. The magnetic powder is a ferrite magnetic powder and / or a rare earth magnetic powder for injection molding, preferably the ferrite magnetic powder is Sr ferrite and / or Ba ferrite magnetic powder, more preferably the ferrite magnetic powder is Sr ferrite, and preferably the average particle size D50 of the magnetic powder is 1.8 μm to 2.0 μm. The magnetic material for injection molding according to claim 1, characterized in that
3. The polymer adhesive is polyphenylene sulfide, The magnetic material for injection molding according to claim 1, further preferably characterized in that the polyphenylene sulfide has a melt flow rate of 500 g / 10 min to 3000 g / 10 min.
4. The auxiliary is a composition of a fluorine additive and a lubricant, preferably the fluorine additive is a polyphthalamide, and preferably the lubricant is an erucamide; The magnetic material for injection molding according to any one of claims 1 to 3, further preferably, the weight ratio of said fluorine additive to said lubricant is 2:3 to 3:
2.
5. The magnetic material for injection molding according to any one of claims 1 to 3, characterized in that the wollastonite is ultrafine wollastonite, more preferably the particle size of the wollastonite is between 800 mesh and 1200 mesh.
6. The magnetic material for injection molding according to any one of claims 1 to 3, characterized in that the first coupling agent is a silane coupling agent, preferably the silane coupling agent is KH550 and / or KH560, and preferably the second coupling agent is a phosphate ester coupling agent.
7. By weight, it comprises 83-85 parts of magnetic powder, 12-15 parts of polymeric adhesive, 0.5-1 part of a first coupling agent, 0.5-1 part of a second coupling agent, 2-5 parts of wollastonite, and 0.1-1 part of an auxiliary agent; More preferably, the magnetic material for injection molding according to claim 1 contains, by weight, 83 parts of magnetic powder, 12 parts of polymeric adhesive, 0.5 parts of a first coupling agent, 0.5 parts of a second coupling agent, 3 parts of wollastonite, and 1 part of an auxiliary agent.
8. A step S1 of subjecting a magnetic powder, a first coupling agent, and a polymer adhesive to a first mixing to obtain a first mixture; Step S2 of subjecting the first mixture to a first extrusion granulation to obtain a magnetic base material for injection molding; Step S3 of subjecting the magnetic base material for injection molding, the second coupling agent, the wollastonite, and the auxiliary agent to a second mixing to obtain a second mixture; The method for producing a magnetic material for injection molding according to any one of claims 1 to 7, further comprising a step S4 of subjecting the second mixture to a second extrusion granulation to obtain the magnetic material for injection molding.
9. 9. The method of claim 8, wherein the temperature of the first mixing and the second mixing are independently 80° C. to 120° C., and the time of the first mixing and the second mixing are independently 30 min to 60 min.
10. The manufacturing method according to claim 8 or 9, characterized in that the first extrusion granulation and the second extrusion granulation are both performed using a twin-screw extruder, and preferably the temperatures of the first extrusion granulation and the second extrusion granulation are independently 290 ° C to 310 ° C.
11. 10. The method according to claim 8 or 9, wherein in step S3, the first coupling agent and the second coupling agent are mixed with an organic solvent before use, preferably the organic solvent is isopropyl alcohol, and preferably the second coupling agent and the organic solvent are mixed in a weight ratio of 1:5 to 1:10.
Citation Information
Patent Citations
Nano-modified magnet composite material and application in inductive component
CN106409453A
Aromatic polyesters, polyesteramides, and compositions thereof
EP0271929B1
Alloy powder for bond magnet and bond magnet
JP1994010100A
Ni-Zn FERRITE MATERIAL AND METHOD FOR MANUFACTURING Ni-Zn FERRITE MATERIAL
JP2017197417A
Method for injection-molding thermosetting resin composition
WO2016171099A1