Light-reflecting thermosetting resin composition, optical semiconductor element mounting substrate, and optical semiconductor device
A thermosetting resin composition with epoxy resin, curing agents, and phosphorus-based accelerators, along with inorganic fillers, addresses the need for improved fluidity and heat resistance in LED reflectors, ensuring high light reflectance and optical stability.
Patent Information
- Application Number
- JP2020159593
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-24
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Thermosetting resin compositions used in forming LED reflectors require improved fluidity during molding and enhanced heat resistance to maintain optical properties under high temperatures.
A thermosetting resin composition comprising an epoxy resin, a curing agent, a phosphorus-based curing accelerator, an inorganic filler, and a white pigment, with specific components like phosphonium borate salts and inorganic hollow particles, to achieve high light reflectance and heat resistance.
The composition provides excellent fluidity and heat resistance, maintaining high light reflectance and optical properties even under prolonged high-temperature use.
Smart Images

Figure 0007567317000006 
Figure 0007567317000007 
Figure 0007567317000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-reflecting thermosetting resin composition, an optical semiconductor element mounting substrate, and an optical semiconductor device. [Background technology]
[0002] Optical semiconductor devices that combine optical semiconductor elements such as LEDs (Light Emitting Diodes) with phosphors have high energy efficiency and long life spans, and are therefore used in a variety of applications such as outdoor displays, mobile LCD backlights, and in-vehicle applications, and demand for such devices is expanding. Accordingly, LED devices are becoming increasingly bright, and there is a need to prevent deterioration of optical semiconductor devices due to an increase in junction temperature caused by an increase in the amount of heat generated by the elements or an increase in direct light energy.
[0003] Patent Document 1 discloses a substrate for mounting optical semiconductor elements using a thermosetting resin composition having a high reflectance in the visible to near-ultraviolet light range after the resin is cured, and Patent Document 2 discloses a member for mounting optical semiconductor elements with reduced light leakage. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-254633 A [Patent Document 2] JP 2010-287837 A Summary of the Invention [Problem to be solved by the invention]
[0005] In general, when a reflector for an LED is formed using a thermosetting resin composition, transfer molding is used. The thermosetting resin composition is required to have excellent flowability during molding. The cured product formed from the thermosetting resin composition is required to have not only high light reflectance but also heat resistance that can maintain optical properties even when used for a long time under high temperature.
[0006] An object of the present invention is to provide a light-reflecting thermosetting resin composition having excellent flowability and heat resistance, and an optical semiconductor element mounting substrate and an optical semiconductor device each using the same. [Means for solving the problem]
[0007] One aspect of the present invention is a curing agent that contains an epoxy resin, a curing agent, a phosphorus-based curing accelerator, an inorganic filler, and a white pigment, and the phosphorus-based curing accelerator is a phosphonium borate salt and a phosphonium cormorant The present invention relates to a light-reflecting thermosetting resin composition comprising a ruthenium phosphate salt.
[0008] In another aspect, the present invention relates to a substrate for mounting an optical semiconductor element comprising the cured product of the above-mentioned light-reflecting thermosetting resin composition. The substrate for mounting an optical semiconductor element according to the present invention has a recess having a bottom surface and a wall surface, and the bottom surface of the recess may be a mounting portion for the optical semiconductor element. In this case, at least a part of the wall surface of the recess is the cured product of the above-mentioned light-reflecting thermosetting resin composition.
[0009] In still another aspect, the present invention relates to an optical semiconductor device having the optical semiconductor element mounting board and an optical semiconductor element mounted on the optical semiconductor element mounting board. Effect of the Invention
[0010] According to the present invention, it is possible to provide a light-reflecting thermosetting resin composition having excellent flowability and heat resistance, and an optical semiconductor element mounting substrate and an optical semiconductor device using the same. [Brief description of the drawings]
[0011] [Figure 1] 1 is a perspective view showing one embodiment of an optical semiconductor element mounting board. [Diagram 2] 1A to 1C are schematic diagrams illustrating an embodiment of a process for producing an optical semiconductor element mounting board. [Diagram 3] 1 is a perspective view showing an embodiment of an optical semiconductor element mounted on an optical semiconductor element mounting substrate. FIG. [Figure 4] 1 is a schematic cross-sectional view showing one embodiment of an optical semiconductor device; [Diagram 5] FIG. 2 is a schematic cross-sectional view showing another embodiment of an optical semiconductor device. [Figure 6] FIG. 2 is a schematic cross-sectional view showing another embodiment of an optical semiconductor device. [Figure 7] FIG. 1 is a schematic cross-sectional view showing one embodiment of a copper-clad laminate. [Figure 8] FIG. 1 is a schematic cross-sectional view showing an example of an optical semiconductor device produced using a copper-clad laminate. [Figure 9] FIG. 2 is a schematic cross-sectional view showing another embodiment of an optical semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the drawings as necessary. However, the present invention is not limited to the following embodiment. In the drawings, the same elements are given the same reference numerals, and duplicated explanations will be omitted. Furthermore, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings, unless otherwise specified. Furthermore, the dimensional ratios of the drawings are not limited to the illustrated ratios.
[0013] In this specification, the numerical range indicated by "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range may be replaced with the upper limit or lower limit of the numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types. In addition, in this specification, (meth)acrylate means at least one of acrylate and its corresponding methacrylate.
[0014] [Thermosetting resin composition for light reflection] The light-reflecting thermosetting resin composition of this embodiment contains an epoxy resin, a curing agent, a phosphorus-based curing accelerator, an inorganic filler, and a white pigment. The phosphorus-based curing accelerator is a phosphonium borate salt and a phosphonium cormorant Contains phosphate salts.
[0015] (Epoxy resin) As the epoxy resin, an epoxy resin generally used in an epoxy resin molding material for sealing electronic components can be used. The thermosetting resin composition according to the present embodiment contains an epoxy resin, and thus can form a cured product having high hot hardness and bending strength and improved mechanical properties. Examples of the epoxy resin include epoxy resins obtained by epoxidizing novolac resins of phenols and aldehydes, such as phenol novolac epoxy resins and orthocresol novolac epoxy resins; diglycidyl ethers of bisphenol A, bisphenol F, bisphenol S, alkyl-substituted bisphenols, and the like; glycidylamine-type epoxy resins obtained by reacting polyamines such as diaminodiphenylmethane and isocyanuric acid with epichlorohydrin; linear aliphatic epoxy resins obtained by oxidizing olefin bonds with peracids such as peracetic acid; and alicyclic epoxy resins. The epoxy resins may be used alone or in combination of two or more.
[0016] Since the epoxy resin is less colored, it may contain a diglycidyl ester of dicarboxylic acid derived from diglycidyl isocyanurate, triglycidyl isocyanurate, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid or 1,4-cyclohexanedicarboxylic acid. For the same reason, the epoxy resin may also contain a diglycidyl ester of dicarboxylic acid such as phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, methyltetrahydrophthalic acid, nadic acid, methylnadic acid, etc. The epoxy resin may contain a glycidyl ester such as a nuclear hydrogenated trimellitic acid or a nuclear hydrogenated pyromellitic acid having an alicyclic structure in which an aromatic ring is hydrogenated. The epoxy resin may contain a polyorganosiloxane having an epoxy group, which is produced by heating a silane compound in the presence of an organic solvent, an organic base and water, and hydrolyzing and condensing it.
[0017] The epoxy resin may be a commercially available product. For example, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate may be obtained under the product names "Celloxide 2021", "Celloxide 2021A" and "Celloxide 2021P" from Daicel Corporation, and "ERL4221", "ERL4221D" and "ERL4221E" from Dow Chemical Japan Co., Ltd. For example, bis(3,4-epoxycyclohexylmethyl)adipate may be obtained under the product name "ERL4299" from Dow Chemical Japan Co., Ltd., and "EXA-7015" from DIC Corporation. As 1-epoxyethyl-3,4-epoxycyclohexane or limonene diepoxide, for example, Mitsubishi Chemical Corporation's product names "jER YX8000", "jER YX8034", and "jER YL7170", Daicel Corporation's product names "Celloxide 2081", "Celloxide 3000", "Epolead GT301", "Epolead GT401", and "EHPE3150" are available. As trisglycidyl isocyanurate, Nissan Chemical Industries, Ltd.'s product name "TEPIC-S" is available.
[0018] (hardening agent) As the curing agent, a curing agent generally used in epoxy resin molding materials for sealing electronic components can be used. The curing agent is not particularly limited as long as it reacts with the epoxy resin to obtain a cured product, but a curing agent with little coloring is preferable, and a colorless or pale yellow curing agent is more preferable. Examples of the curing agent include an acid anhydride-based curing agent, an isocyanuric acid derivative-based curing agent, and a phenol-based curing agent. The curing agent may be used alone or in combination of two or more types.
[0019] The curing agent according to the present embodiment may contain, as an acid anhydride curing agent, a tetracarboxylic dianhydride having a melting point of 180 to 400°C (hereinafter, may be simply referred to as "tetracarboxylic dianhydride"). By using such a tetracarboxylic dianhydride as a curing agent, the heat resistance of the thermosetting resin composition can be further improved. In order to disperse the tetracarboxylic dianhydride uniformly in the resin composition, the melting point of the tetracarboxylic dianhydride may be 200 to 380°C or 210 to 350°C.
[0020] In order to further improve heat resistance, the tetracarboxylic dianhydride may have an aromatic ring or an alicyclic ring. The tetracarboxylic dianhydride having an aromatic ring may be at least one selected from the group consisting of tetracarboxylic dianhydrides having two or more benzene rings and tetracarboxylic dianhydrides having a naphthalene ring.
[0021] The tetracarboxylic dianhydride having two or more benzene rings may be a compound represented by the following formula (1): In formula (1), R represents a single bond, an ether bond, a carbonyl group, a sulfonyl group, a hexafluoroisopropylidene group, or a fluorene group. [ka]
[0022] Examples of tetracarboxylic dianhydrides having an alicyclic ring include 1,2,3,4-cyclobutanetetracarboxylic dianhydride. Examples of tetracarboxylic dianhydrides having an aromatic ring include 4,4'-biphthalic anhydride, 4,4'-carbonyldiphthalic anhydride, 4,4'-sulfonyldiphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-oxydiphthalic anhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, and 2,3,6,7-naphthalenetetracarboxylic dianhydride.
[0023] The curing agent according to the present embodiment may include an acid anhydride curing agent having a melting point of less than 180° C. Examples of acid anhydride curing agents having a melting point of less than 180° C. include phthalic anhydride, maleic anhydride, trimellitic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, methylnadic anhydride, nadic anhydride, glutaric anhydride, dimethylglutaric anhydride, diethylglutaric anhydride, succinic anhydride, methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, and tetracarboxylic dianhydride represented by the following formula (2).
[0024] [ka] In formula (2), Rx represents a divalent organic group, and n represents an integer of 1 to 10. The divalent organic group may be a divalent saturated hydrocarbon group having a saturated hydrocarbon ring, and examples of the saturated hydrocarbon include cyclobutane, cyclopentane, cyclohexane, cycloheptane, cyclooctane, norbornene, dicyclopentadiene, adamantane, hydrogenated naphthalene, and hydrogenated biphenyl.
[0025] Examples of isocyanuric acid derivatives include 1,3,5-tris(1-carboxymethyl)isocyanurate, 1,3,5-tris(2-carboxyethyl)isocyanurate, 1,3,5-tris(3-carboxypropyl)isocyanurate, and 1,3-bis(2-carboxyethyl)isocyanurate.
[0026] Examples of phenol-based curing agents include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene, and aldehydes such as formaldehyde, benzaldehyde, and salicylaldehyde, under an acidic catalyst; phenol-aralkyl resins synthesized from aryl groups; aralkyl-type phenolic resins such as biphenylene-type phenol-aralkyl resins and naphthol-aralkyl resins; dicyclopentadiene-type phenolic resins synthesized by copolymerization of phenols and / or naphthols with dicyclopentadiene; triphenylmethane-type phenolic resins; terpene-modified phenolic resins; paraxylylene- and / or metaxylylene-modified phenolic resins; melamine-modified phenolic resins; and phenolic resins obtained by copolymerization of two or more of these.
[0027] In the thermosetting resin composition according to this embodiment, the content of the curing agent may be 10 to 150 parts by mass, 50 to 130 parts by mass, or 60 to 120 parts by mass with respect to 100 parts by mass of the epoxy resin.
[0028] The mixing ratio of the curing agent may be 0.5 to 2.0 equivalents, 0.6 to 1.5 equivalents, or 0.7 to 1.2 equivalents of active groups (acid anhydride groups or hydroxyl groups) in the curing agent that can react with the epoxy groups per equivalent of the epoxy groups in the epoxy resin. When the active groups are 0.5 equivalents or more, the glass transition temperature of the cured product formed from the thermosetting resin composition becomes high, and it becomes easy to obtain a sufficient elastic modulus. On the other hand, when the active groups are 2.0 equivalents or less, the strength after curing is less likely to decrease.
[0029] (Cure accelerator) The thermosetting resin composition according to the present embodiment contains a phosphonium borate salt and a phosphonium cormorantWhen used in combination with ruthenium phosphate salt, it results in a molding material with an excellent balance of fluidity and heat resistance.
[0030] The phosphonium borate salt may be, for example, a compound represented by the following formula (3): [ka]
[0031] In formula (3), R 1 , R 2 , R 3 and R 4 R each independently represents a hydrocarbon group having 1 to 16 carbon atoms, and may be a hydrocarbon group having 1 to 8 carbon atoms or a hydrocarbon group having 1 to 6 carbon atoms. 5 , R 6 , R 7 and R 8 each independently represents a hydrocarbon group having 1 to 16 carbon atoms or a halogen atom, and may be a hydrocarbon group having 1 to 8 carbon atoms, a hydrocarbon group having 1 to 6 carbon atoms, or a fluorine atom.
[0032] Examples of phosphonium borate salts include tetra-n-butylphosphonium tetraphenylborate, tetra-n-butylphosphonium tetrafluoroborate, tetraphenylphosphonium tetraphenylborate, and tetraphenylphosphonium tetrafluoroborate.
[0033] The content of the phosphonium borate salt in the thermosetting resin composition may be 0.1 to 2.5 parts by mass, 0.4 to 2.2 parts by mass, or 0.6 to 2.0 parts by mass relative to 100 parts by mass of the epoxy resin, from the viewpoint of further improving the fluidity of the thermosetting resin composition during molding.
[0034] Phosphony cormorant The phosphate salt may be, for example, a compound represented by the following formula (4): [ka]
[0035] In formula (4), R 11 , R 12 , R 13 and R 14 R each independently represents a hydrocarbon group having 1 to 16 carbon atoms, and may be a hydrocarbon group having 1 to 8 carbon atoms or a hydrocarbon group having 1 to 6 carbon atoms. 15 and R 16 each independently represents a hydrocarbon group having 1 to 16 carbon atoms, and may be a hydrocarbon group having 1 to 8 carbon atoms, a hydrocarbon group having 1 to 6 carbon atoms, or a hydrocarbon group having 1 to 3 carbon atoms.
[0036] Phosphony cormorant Examples of methyl phosphate salts include tri-n-butylmethylphosphonium. cormorant dimethyl phosphate, tri-n-butyl methyl phosphonium cormorant Diethyl phosphate, Tetra-n-butyl phosphoni cormorant Dimethyl phosphate, triphenylmethylphosphonium cormorant Examples of suitable phenylphosphonium dimethyl phosphate include phenylphosphonium dimethyl phosphate, and tetraphenylphosphonium dimethyl phosphate.
[0037] The content of the phosphonium phosphate salt in the thermosetting resin composition may be 0.05 to 2.0 parts by mass, 0.1 to 1.5 parts by mass, or 0.2 to 1.0 parts by mass relative to 100 parts by mass of the epoxy resin, from the viewpoint of further improving the heat resistance of the cured product.
[0038] The total amount of the curing accelerator in the thermosetting resin composition may be 0.15 to 4.5 parts by mass, 0.5 to 4.0 parts by mass, or 1.0 to 3.0 parts by mass, relative to 100 parts by mass of the epoxy resin. When the content of the curing accelerator is 0.1 part by mass or more, a sufficient curing acceleration effect is easily obtained, and when it is 5 parts by mass or less, discoloration of the cured product is easily suppressed.
[0039] (White pigment) The white pigment is used to impart a white color tone to the cured product (molded product) obtained from the thermosetting resin composition according to this embodiment. In particular, by imparting a high degree of whiteness to the color tone, the light reflectance of the molded product can be improved.
[0040] Examples of the white pigment include rare earth oxides such as yttrium oxide, titanium oxide, zinc oxide, aluminum oxide (alumina), magnesium oxide, antimony oxide, zinc sulfate, zirconium oxide, and zirconium oxide. These may be used alone or in combination of two or more. In order to further improve light reflectivity, the white pigment preferably contains at least one selected from the group consisting of titanium oxide, zinc oxide, alumina, magnesium oxide, antimony oxide, and zirconium oxide, and more preferably contains at least one selected from the group consisting of titanium oxide, antimony oxide, and zirconium oxide.
[0041] The median particle diameter of the white pigment may be 0.05 to 10 μm, 0.08 to 8 μm, or 0.1 to 5 μm. When the median particle diameter of the white pigment is 0.05 μm or more, the dispersibility is improved, and when it is less than 10 μm, the light reflection property of the cured product is improved. In this specification, the median particle diameter can be determined as the mass average value D50 (or median diameter) in particle size distribution measurement by laser light diffraction method.
[0042] (Inorganic filler) The thermosetting resin composition according to the present embodiment contains an inorganic filler from the viewpoint of improving moldability. Examples of the inorganic filler include quartz, fumed silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, ultrafine amorphous silica, barium sulfate, magnesium carbonate, barium carbonate, aluminum hydroxide, magnesium hydroxide, potassium titanate, calcium silicate, and inorganic hollow particles.
[0043] From the viewpoint of moldability, the inorganic filler may contain fused silica. The median particle size of the fused silica may be 1 to 100 μm, 1 to 50 μm, or 1 to 40 μm from the viewpoint of improving packing with the white pigment.
[0044] In order to further improve the grindability of the thermosetting resin composition, the inorganic filler may contain inorganic hollow particles having a median particle size of 1 to 25 μm. The inorganic hollow particles are particles having voids inside. Since the inorganic hollow particles refract and reflect incident light on the surface and inner wall, the inorganic hollow particles can be used in combination with a white pigment to form a cured product with further improved light reflectivity and mechanical properties.
[0045] Examples of inorganic hollow particles include soda silicate glass, aluminum silicate glass, soda borosilicate glass, and shirasu (white sand). From the viewpoint of heat resistance and pressure resistance, the shell of the inorganic hollow particle is preferably made of at least one material selected from the group consisting of soda silicate glass, aluminum silicate glass, soda borosilicate glass, shirasu, cross-linked styrene resin, and cross-linked acrylic resin, and more preferably made of at least one material selected from the group consisting of soda silicate glass, aluminum silicate glass, soda borosilicate glass, and shirasu.
[0046] Since the inorganic hollow particles can be easily uniformly dispersed when preparing a thermosetting resin composition, the inorganic hollow particles may have a median particle size of 1 μm or more, 5 μm or more, or 10 μm or more. Also, since the light reflection properties of the cured product to be formed are easily improved, the inorganic hollow particles may have a median particle size of 30 μm or less, 25 μm or less, or 22 μm or less.
[0047] In order to improve the mechanical properties of the thermosetting resin composition, the thickness of the outer shell of the inorganic hollow particles may be 0.4 to 1.5 μm, 0.45 to 1.2 μm, 0.5 to 1.1 μm, or 0.55 to 1.0 μm.
[0048] To improve light reflectivity, the bulk density of inorganic hollow particles is 0.20 to 0.38 g / cm 3 , 0.25~0.36g / cm 3, or 0.26 to 0.35 g / cm 3 The bulk density is a density calculated by filling a container having a certain volume with inorganic hollow particles and calculating the internal volume of the container.
[0049] Due to the excellent balance between light reflectivity and mechanical properties, the true density of inorganic hollow particles is 0.40 to 0.75 g / cm 3 , 0.45~0.70g / cm 3 , or 0.50 to 0.65 g / cm 3 The true density can be measured in accordance with ASTM D2840.
[0050] Since the strength of the cured product of the thermosetting resin composition is improved, the pressure resistance of the inorganic hollow particles may be 100 MPa or more, 110 MPa or more, 125 MPa or more, or 150 MPa or more at 25° C. Since the moldability of the thermosetting resin composition is improved, the pressure resistance of the inorganic hollow particles may be 500 MPa or less, 300 MPa or less, or 200 MPa or less at 25° C. The pressure resistance can be measured in accordance with ASTM D3102.
[0051] In order to further improve the light reflectance, the content of the inorganic hollow particles is preferably 10 to 200 parts by mass, more preferably 30 to 180 parts by mass, and even more preferably 60 to 150 parts by mass, relative to 100 parts by mass of the epoxy resin.
[0052] (Coupling Agent) A coupling agent may be added to the thermosetting resin composition to improve the adhesion between the inorganic filler and the epoxy resin. The coupling agent is not particularly limited, but may be, for example, a silane coupling agent or a titanate coupling agent. The silane coupling agent may be, for example, an epoxy silane compound, an amino silane compound, a cationic silane compound, a vinyl silane compound, an acrylic silane compound, and a mercapto silane compound. The content of the coupling agent may be 5% by mass or less based on the total amount of the thermosetting resin composition.
[0053] If necessary, additives such as an antioxidant, a release agent, and an ion scavenger may be added to the thermosetting resin composition according to the present embodiment.
[0054] The thermosetting resin composition according to the present embodiment can be prepared by uniformly dispersing and mixing the various components described above. The preparation means, conditions, etc. are not particularly limited. A general method for preparing a thermosetting resin composition includes a method in which each component is kneaded with a kneader, roll, extruder, mortar and pestle, or a planetary mixer that combines rotation and revolution. When each component is kneaded, it is preferable to knead it in a molten state from the viewpoint of improving dispersibility.
[0055] The kneading conditions may be appropriately determined depending on the type or amount of each component. For example, kneading is preferably performed at 15 to 100°C for 5 to 40 minutes, and more preferably at 20 to 100°C for 10 to 30 minutes. When the kneading temperature is 15°C or higher, each component can be easily kneaded, and dispersibility can be improved. When the kneading temperature is 100°C or lower, the epoxy resin can be prevented from being polymerized and hardened during kneading. When the kneading time is 5 minutes or longer, a sufficient dispersion effect can be easily obtained. When the kneading time is 40 minutes or less, the epoxy resin can be prevented from being polymerized and hardened during kneading.
[0056] The thermosetting resin composition according to the present embodiment is useful in various applications requiring high light reflectivity and heat resistance, such as substrate materials for mounting optical semiconductor elements, electrical insulating materials, optical semiconductor sealing materials, adhesive materials, coating materials, epoxy resin molding materials for transfer molding, etc. Hereinafter, an example of using the thermosetting resin composition according to the present embodiment as an epoxy resin molding material for transfer molding will be described.
[0057] In terms of mechanical properties, the thermosetting resin composition according to this embodiment has a bending strength of preferably 70 MPa or more, more preferably 75 MPa or more, at 25° C. when transfer molded under conditions of a molding die temperature of 180° C., a molding pressure of 6.9 MPa, and a curing time of 90 seconds. A bending strength of 70 MPa or more provides excellent toughness.
[0058] From the viewpoint of improving the brightness of the optical semiconductor device, the initial light reflectance at a wavelength of 460 nm of the cured product of the thermosetting resin composition according to the present embodiment is preferably 91% or more, more preferably 92% or more, and even more preferably 93% or more. From the viewpoint of improving the heat coloration resistance, the light reflectance at a wavelength of 460 nm after the cured product is heat-treated at 150° C. for 168 hours is preferably 88% or more, more preferably 89% or more, and even more preferably 90% or more.
[0059] [Optical semiconductor device mounting board] The optical semiconductor element mounting substrate of this embodiment has a recess having a bottom surface and wall surfaces. The bottom surface of the recess is an optical semiconductor element mounting portion (optical semiconductor element mounting region), and the wall surfaces of the recess, i.e., at least a part of the inner peripheral side surface of the recess, are made of a cured product of the light-reflecting thermosetting resin composition of this embodiment.
[0060] FIG. 1 is a perspective view showing one embodiment of an optical semiconductor element mounting substrate. The optical semiconductor element mounting substrate 110 includes metal wiring 105 (first and second connection terminals) on which Ni / Ag plating 104 is formed, an insulating resin molded body 103' provided between the metal wiring 105 (first and second connection terminals), and a reflector 103, and has an optical semiconductor element mounting region (recess) 200 formed by the metal wiring 105 on which Ni / Ag plating 104 is formed, the insulating resin molded body 103', and the reflector 103. The bottom surface of the recess 200 is composed of the metal wiring 105 on which Ni / Ag plating 104 is formed, and the insulating resin molded body 103', and the wall surface of the recess 200 is composed of the reflector 103. The reflector 103 and the insulating resin molded body 103' are molded bodies made of a cured product of the light-reflecting thermosetting resin composition according to the present embodiment described above.
[0061] The method for producing the optical semiconductor element mounting substrate is not particularly limited, but it can be produced, for example, by transfer molding using a light-reflecting thermosetting resin composition. FIG. 2 is a schematic diagram showing one embodiment of the process for producing the optical semiconductor element mounting substrate. The optical semiconductor element mounting substrate can be produced, for example, by a process of punching out a metal foil, forming a metal wiring 105 by a known method such as etching, and applying Ni / Ag plating 104 by electroplating (FIG. 2(a)), then arranging the metal wiring 105 in a mold 151 of a predetermined shape, injecting a light-reflecting thermosetting resin composition from a resin injection port 150 of the mold 151, and performing transfer molding under predetermined conditions (FIG. 2(b)), and then removing the mold 151 (FIG. 2(c)). In this way, an optical semiconductor element mounting region (recess) 200 surrounded by a reflector 103 made of a cured product of the light-reflecting thermosetting resin composition is formed in the optical semiconductor element mounting substrate. The bottom surface of the recess 200 is composed of a metal wiring 105 serving as a first connection terminal, a metal wiring 105 serving as a second connection terminal, and an insulating resin molded body 103' made of a cured product of a light-reflecting thermosetting resin composition provided between them. The conditions for the transfer molding are preferably a mold temperature of 170 to 200°C, more preferably 170 to 190°C, a molding pressure of 0.5 to 20 MPa, more preferably 2 to 8 MPa, for 60 to 120 seconds, and an after-cure temperature of 120°C to 180°C for 1 to 3 hours.
[0062] [Optical semiconductor device] The optical semiconductor device according to this embodiment includes the optical semiconductor element mounting substrate and an optical semiconductor element mounted on the optical semiconductor element mounting substrate. A more specific example is an optical semiconductor device including the optical semiconductor element mounting substrate, an optical semiconductor element provided in a recess of the optical semiconductor element mounting substrate, and a phosphor-containing sealing resin part that fills the recess to seal the optical semiconductor element.
[0063] FIG. 3 is a perspective view showing an embodiment of a state in which an optical semiconductor element 100 is mounted on an optical semiconductor element mounting substrate 110. As shown in FIG. 3, the optical semiconductor element 100 is mounted at a predetermined position in an optical semiconductor element mounting region (recess) 200 of the optical semiconductor element mounting substrate 110, and is electrically connected to the metal wiring 105 by a bonding wire 102. FIGS. 4 and 5 are schematic cross-sectional views showing an embodiment of an optical semiconductor device. As shown in FIGS. 4 and 5, the optical semiconductor device includes an optical semiconductor element mounting substrate 110, an optical semiconductor element 100 provided at a predetermined position in the recess 200 of the optical semiconductor element mounting substrate 110, and a sealing resin part made of a transparent sealing resin 101 containing a phosphor 106 that fills the recess 200 to seal the optical semiconductor element, and the optical semiconductor element 100 and the metal wiring 105 on which Ni / Ag plating 104 is formed are electrically connected to each other by a bonding wire 102 or a solder bump 107.
[0064] Fig. 6 is also a schematic cross-sectional view showing one embodiment of an optical semiconductor device. In the optical semiconductor device shown in Fig. 6, an LED element 300 is disposed at a predetermined position on a lead 304 on which a reflector 303 is formed, via a die bond material 306, and the LED element 300 and the lead 304 are electrically connected by a bonding wire 301. The LED element 300 is sealed with a transparent sealing resin 302 containing a phosphor 305.
[0065] Although the preferred embodiment of the present invention has been described above, the present invention is not limited thereto. For example, the light-reflecting thermosetting resin composition of the present embodiment can be used as a light-reflecting coating agent. As this embodiment, a copper-clad laminate, a substrate for mounting an optical semiconductor element, and an optical semiconductor element will be described.
[0066] The copper-clad laminate according to this embodiment includes a light-reflecting resin layer formed using the above-mentioned light-reflecting thermosetting resin composition, and a copper foil laminated on the light-reflecting resin layer.
[0067] Fig. 7 is a schematic cross-sectional view showing a preferred embodiment of a copper-clad laminate. As shown in Fig. 7, a copper-clad laminate 400 includes a substrate 401, a light-reflecting resin layer 402 laminated on the substrate 401, and a copper foil 403 laminated on the light-reflecting resin layer 402. Here, the light-reflecting resin layer 402 is formed using the above-mentioned thermosetting resin composition for light reflection.
[0068] As the substrate 401, any substrate used for a copper-clad laminate can be used without any particular limitation, and examples thereof include a resin laminate such as an epoxy resin laminate, and a substrate for mounting an optical semiconductor.
[0069] Copper-clad laminate 400 can be produced, for example, by applying the light-reflecting thermosetting resin composition of this embodiment to the surface of substrate 401, layering copper foil 403, and curing the composition under heat and pressure to form light-reflecting resin layer 402 made of the thermosetting resin composition.
[0070] The thermosetting resin composition can be applied to the substrate 401 by, for example, a printing method, a die coating method, a curtain coating method, a spray coating method, a roll coating method, or the like. In this case, the thermosetting resin composition may contain a solvent to facilitate application. When a solvent is used, it is preferable to set the total amount excluding the solvent when the blending ratio of each component described above is based on the total amount of the thermosetting resin composition.
[0071] The conditions for the heating and pressing are not particularly limited, but it is preferable to perform the heating and pressing under conditions of, for example, 130 to 180° C., 0.5 to 4 MPa, and 30 to 600 minutes.
[0072] The above copper-clad laminate can be used to prepare a printed wiring board for optical components such as LED mounting. The copper-clad laminate 400 shown in FIG. 7 is a laminate in which a light-reflecting resin layer 402 and a copper foil 403 are laminated on one side of a substrate 401, but the copper-clad laminate may be a laminate in which a light-reflecting resin layer 402 and a copper foil 403 are laminated on both sides of the substrate 401. The copper-clad laminate may be composed of only the light-reflecting resin layer 402 and the copper foil 403 without using the substrate 401. In this case, the light-reflecting resin layer 402 plays the role of the substrate. In this case, for example, the light-reflecting resin layer 402 can be obtained by impregnating a glass cloth or the like with the thermosetting resin composition and curing the same.
[0073] Fig. 8 is a schematic cross-sectional view showing an example of an optical semiconductor device produced using a copper-clad laminate. As shown in Fig. 8, optical semiconductor device 500 is a surface-mount type light-emitting diode including optical semiconductor element 410 and transparent sealing resin 404 provided so as to seal optical semiconductor element 410. In optical semiconductor device 500, optical semiconductor element 410 is bonded to copper foil 403 via adhesive layer 408, and is electrically connected to copper foil 403 by bonding wire 409.
[0074] Another embodiment of the optical semiconductor element mounting substrate is a substrate having a light reflecting resin layer formed between a plurality of conductive members (connection terminals) on a substrate using the above-mentioned light reflecting thermosetting resin composition. Another embodiment of the optical semiconductor device is a substrate having an optical semiconductor element mounted on the above-mentioned optical semiconductor element mounting substrate.
[0075] Fig. 9 is a schematic cross-sectional view showing a preferred embodiment of an optical semiconductor device. As shown in Fig. 9, an optical semiconductor device 600 is a surface-mounted light-emitting diode in which an optical semiconductor element 610 is mounted on an optical semiconductor element mounting substrate including a base material 601, a plurality of conductor members 602 formed on the surface of the base material 601, and a light-reflecting resin layer 603 formed between the plurality of conductor members (connection terminals) 602 and made of the above-mentioned thermosetting resin composition for light reflection, and a transparent sealing resin 604 is provided to seal the optical semiconductor element 610. In the optical semiconductor device 600, the optical semiconductor element 610 is bonded to the conductor member 602 via an adhesive layer 608 and is electrically connected to the conductor member 602 by a bonding wire 609.
[0076] As the substrate 601, any substrate used for an optical semiconductor device mounting board can be used without any particular limitation, and examples thereof include a resin laminate such as an epoxy resin laminate.
[0077] The conductive member 602 functions as a connection terminal, and can be formed by a known method, for example, a method of photoetching a copper foil.
[0078] The substrate for mounting optical semiconductor elements can be produced by applying the above-mentioned light-reflecting thermosetting resin composition between a plurality of conductive members 602 on a substrate 601, and heating and curing the composition to form a light-reflecting resin layer 603 made of the light-reflecting thermosetting resin composition.
[0079] The light-reflecting thermosetting resin composition can be applied to the substrate 601 by, for example, a printing method, a die coating method, a curtain coating method, a spray coating method, a roll coating method, or the like. In this case, the light-reflecting thermosetting resin composition can contain a solvent to facilitate application. When a solvent is used, it is preferable to set the total amount excluding the solvent as the total amount of the resin composition based on the blending ratio of each component described above.
[0080] The heating conditions for heat curing the coating film of the light-reflecting thermosetting resin composition are not particularly limited, but may be, for example, heating at 130 to 180° C. for 30 to 600 minutes.
[0081] Thereafter, excess resin components adhering to the surface of the conductor member 602 are removed by buffing or the like to expose the circuit made of the conductor member 602, thereby forming a substrate for mounting optical semiconductor elements. In order to ensure adhesion between the light reflecting resin layer 603 and the conductor member 602, the conductor member 602 may be subjected to a roughening treatment such as an oxidation-reduction treatment or a CZ treatment (manufactured by MEC Co., Ltd.).
[0082] An optical semiconductor element mounting substrate and an optical semiconductor device having a cured product of the light-reflecting thermosetting resin composition according to this embodiment have high light reflectance and can maintain their optical properties even when used for long periods of time at high temperatures. EXAMPLES
[0083] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.
[0084] [Preparation of light-reflecting thermosetting resin composition] In order to prepare the thermosetting resin compositions of the Examples and Comparative Examples, the following components were prepared.
[0085] (Epoxy resin) Nissan Chemical Industries, Ltd.'s product name "TEPIC-S" (trisglycidyl isocyanurate, epoxy equivalent: 100) (hardening agent) Tetracarboxylic dianhydride of formula (2) (Rx: cyclohexane ring, melting point: 40°C) "Rikacid HH" (Hexahydrophthalic anhydride, melting point: 35°C) manufactured by New Japan Chemical Co., Ltd. Manac Corporation's product name "ODPA-C" (4,4'-oxydiphthalic anhydride, melting point: 229°C) (Phosphorus-based curing accelerator) Product name "PX-4PB" (Tetrabutylphosphonium tetraphenylborate) manufactured by Nippon Chemical Industry Co., Ltd. Nippon Chemical Industry Co., Ltd.'s product name "PX-4MP" (tri-n-butylmethylphosphonium cormorant (Dimethyl Phosphate) (Coupling Agent) Epoxysilane compound (3-glycidoxypropyltrimethoxysilane) (Release agent) Product name "ZNST" (Zinc Stearate) manufactured by NOF Corporation (Additives) "ADEKA STAB AO-60" (hindered phenol-based antioxidant) manufactured by ADEKA Corporation ADEKA STAB PEP-36A (a phosphite antioxidant) manufactured by ADEKA Corporation Gelest product name "DBL-C32" (silicone wax dispersant) (Inorganic hollow particles) "iM30K" (product name: 3M Japan Ltd.) (center particle size: 18 μm, shell layer thickness: 0.61 μm, bulk density: 0.33 g / cm 3 , Compressive strength: 186MPa) (silica) Denka Company Ltd.'s product name "FB-950" (fused silica) Product name "SO-25R" (fused silica), manufactured by Admatechs Co., Ltd. "Silohobic 702" (hydrophobic fine silica powder) manufactured by Fuji Silysia Chemical Co., Ltd. (White pigment) Titanium oxide (median particle size 0.2 μm)
[0086] The components were mixed according to the mixing ratio (parts by mass) shown in Table 1, thoroughly kneaded with a mixer, and then melt-kneaded with a mixing roll at 40° C. for 15 minutes to obtain a kneaded mixture. The kneaded mixture was cooled and pulverized to prepare the thermosetting resin compositions of the examples and comparative examples.
[0087] [evaluation] (Spiral Flow) Using a spiral flow measurement die conforming to the EMMI-1-66 standard, the thermosetting resin composition was transfer molded under the conditions of a molding die temperature of 180°C, a molding pressure of 6.9 MPa, and a curing time of 90 seconds. The flow distance (inch) of the thermosetting resin composition during transfer molding was measured.
[0088] (light reflectance) The thermosetting resin composition was transfer molded under the conditions of a mold temperature of 180°C, a molding pressure of 6.9 MPa, and a curing time of 90 seconds, and then post-cured at 150°C for 2 hours to prepare a test piece having a thickness of 3.0 mm. The light reflectance of the test piece at a wavelength of 460 nm was measured using a spectrophotometer "CM-600d" (manufactured by Konica Minolta, Inc.). The test piece was then left in a thermostatic chamber set at 150°C for 1000 hours, after which the light reflectance was measured.
[0089] [Table 1]
[0090] From Table 1, it can be seen that the light-reflecting thermosetting resin compositions of the Examples have excellent fluidity and can form cured products (molded articles) with high heat resistance. [Explanation of symbols]
[0091] 100...optical semiconductor element, 101...encapsulating resin, 102...bonding wire, 103...reflector, 103'...insulating resin molded body, 104...Ni / Ag plating, 105...metal wiring, 106...phosphor, 107...solder bump, 110...substrate for mounting optical semiconductor element, 150...resin injection port, 151...mold, 200...optical semiconductor element mounting area, 300...LED element, 301...bonding wire, 302...encapsulating resin, 303...reflector , 304...lead, 305...phosphor, 306...die bond material, 400...copper-clad laminate, 401...substrate, 402...light-reflecting resin layer, 403...copper foil, 404...sealing resin, 408...adhesive layer, 409...bonding wire, 410...optical semiconductor element, 500, 600...optical semiconductor device, 601...substrate, 602...conductor member, 603...light-reflecting resin layer, 604...sealing resin, 608...adhesive layer, 609...bonding wire, 610...optical semiconductor element.
Claims
1. Contains epoxy resin, hardener, phosphorus-based hardening accelerator, inorganic filler, and white pigment, the phosphorus-based curing accelerator comprises a phosphonium borate salt and a phosphonium phosphate salt; A light-reflecting thermosetting resin composition, wherein the content of the phosphonium borate salt is 0.4 to 2.2 parts by mass relative to 100 parts by mass of the epoxy resin, and the content of the phosphonium phosphate salt is 0.2 to 1.0 part by mass relative to 100 parts by mass of the epoxy resin.
2. The light-reflecting thermosetting resin composition according to claim 1 , wherein the curing agent comprises an acid anhydride curing agent.
3. 3. The light-reflecting thermosetting resin composition according to claim 1, wherein the inorganic filler comprises inorganic hollow particles having a median particle size of 1 to 25 μm.
4. The light-reflecting thermosetting resin composition according to any one of claims 1 to 3, wherein the white pigment comprises at least one selected from the group consisting of titanium oxide, zinc oxide, alumina, magnesium oxide, antimony oxide, and zirconium oxide.
5. A substrate for mounting an optical semiconductor element, comprising a cured product of the light-reflecting thermosetting resin composition according to any one of claims 1 to 4.
6. a recess having a bottom surface and a wall surface, the bottom surface of the recess being a mounting portion for an optical semiconductor element; 5. A substrate for mounting optical semiconductor elements, wherein at least a portion of the wall surface of the recess is made of a cured product of the light-reflecting thermosetting resin composition according to claim 1.
7. A substrate, and a first connection terminal and a second connection terminal provided on the substrate, A substrate for mounting optical semiconductor elements, comprising a cured product of the light-reflecting thermosetting resin composition according to any one of claims 1 to 4 between the first connection terminal and the second connection terminal.
8. 8. An optical semiconductor device comprising: the optical semiconductor element mounting substrate according to claim 5; and an optical semiconductor element mounted on the optical semiconductor element mounting substrate.
Citation Information
Patent Citations
Thermosetting resin composition, substrate for loading photosemiconductor element using the same, method for producing the substrate, and photosemiconductor device
JP2010047740A
Member for mounting optical semiconductor element, and optical semiconductor device
JP2010287837A
Thermosetting resin composition for light reflection, method for manufacturing the resin composition, optical semiconductor element-mounting substrate, and optical semiconductor device using the resin composition
JP2012254633A
Epoxy resin composition for optical semiconductor device and lead frame for optical semiconductor device obtained by using the same, sealed optical semiconductor element and optical semiconductor device
JP2015130476A
Resin composition, cured product of same, and reflective material for optical semiconductors using said cured product
WO2013146081A1