Gas barrier laminate

A gas barrier laminate with a paper base, aluminum vapor deposition, and a water-soluble polymer overcoat addresses folding-induced cracks, ensuring effective gas barrier performance and reduced plastic use.

JP7567332B2Active Publication Date: 2024-10-16TOPPAN HOLDINGS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020164881
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-16
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing gas barrier papers used in packaging materials suffer from deterioration of gas barrier properties when subjected to acute folds, and the overcoat layer cracks due to paper's elongation upon water absorption, leading to reduced performance.

Method used

A gas barrier laminate comprising a paper base material, an anchor coat layer, an aluminum vapor deposited layer, and an overcoat layer made of a water-soluble polymer, particularly polyvinyl alcohol, is developed to maintain gas barrier properties even after folding.

Benefits of technology

The laminate maintains crease retention and gas barrier properties, reducing plastic use and extending content preservation, suitable for packaging applications like gusset bags.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567332000004
    Figure 0007567332000004
  • Figure 0007567332000001
    Figure 0007567332000001
  • Figure 0007567332000002
    Figure 0007567332000002
Patent Text Reader

Abstract

To provide a gas barrier laminate which has crease-retaining properties that are features of paper and has sufficient gas barrier properties even after having been bent, and contributes to reduction in a used amount of a plastic material.SOLUTION: A gas barrier laminate has a paper base material, an anchor coat layer, an aluminum vapor-deposited layer, and an overcoat layer composed of a water-soluble polymer, in this order.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier laminate. [Background technology]

[0002] In many fields, such as food, beverages, pharmaceuticals, and chemicals, packaging materials are used according to the respective contents. Packaging materials are required to have a property of preventing the permeation of oxygen, water vapor, and the like, which cause deterioration of the contents (gas barrier property). Patent Document 1 discloses a gas barrier film in which a gas barrier coating layer is laminated on at least one side of a thermoplastic resin substrate film that has been subjected to a specific treatment. This gas barrier coating layer is made of specific flaky silica and polyvinyl alcohol resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-138289 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, the trend toward a plastic-free society has been growing due to growing environmental awareness triggered by the problem of marine plastic waste. From the viewpoint of reducing the amount of plastic materials used, the use of paper instead of plastic materials has been considered in various fields. If a part of the materials constituting packaging materials is changed from plastic films to paper, the amount of plastic materials used in the packaging material field can be reduced.

[0005] Paper has the characteristic of being easy to process because of its crease retention (also called dead hold property). Conventionally, studies have been made on imparting gas barrier properties to paper. For example, JP 2004-204366 A (hereinafter referred to as Patent Document 2) discloses a moisture-proof paper in which a vapor-deposited anchor layer, a vapor-deposited thin film layer, and an overcoat layer are provided in this order on the coated surface of paper or paperboard. Patent Document 2 discloses, as one embodiment of the overcoat layer, a layer made of a mixture of polyvinyl alcohol and an inorganic layered compound (e.g., montmorillonite, heclite, saponite) (see paragraph

[0039] of Patent Document 2). According to the description in paragraph

[0027] of Patent Document 2, this moisture-proof paper can be suitably used as packaging paper for copy paper, or paper packaging bags (soft type) or paper boxes (box type) for cigarettes.

[0006] However, according to the inventors' investigations, it has been found that when the moisture-proof paper described in Patent Document 2 is applied to packaging with sharper folds (for example, pillow packaging, three-sided sealed packaging, and gusset packaging), cracks occur in the evaporated thin film layer and overcoat layer, reducing the gas barrier properties, and there is still room for improvement. In addition, because paper has the property of expanding when it absorbs moisture, the overcoat layer cannot accommodate this expansion, which can reduce the gas barrier properties.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a gas barrier laminate that has the fold retention characteristic of paper, has sufficient gas barrier properties even after being folded, and contributes to reducing the amount of plastic materials used. [Means for solving the problem]

[0008] The present invention provides a gas barrier laminate comprising, in this order, a paper substrate, an anchor coat layer, an aluminum vapor deposition layer, and an overcoat layer made of a water-soluble polymer.

[0009] The water-soluble polymer may be polyvinyl alcohol.

[0010] The saponification degree of the polyvinyl alcohol may be 90 or more. Effect of the Invention

[0011] According to the present invention, it is possible to provide a gas barrier laminate that has the fold retention characteristic of paper and sufficient gas barrier properties even after being folded, and that contributes to reducing the amount of plastic materials used. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings where necessary. However, the present invention is not limited to the following embodiments.

[0014] <Gas barrier laminate> 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. The gas barrier laminate 10 according to one embodiment comprises, in this order, a paper substrate 1, an anchor coat layer 2, an aluminum vapor deposition layer 3, and an overcoat layer 4 made of a water-soluble polymer.

[0015] [Paper base material] The paper substrate 1 is not particularly limited and may be selected appropriately depending on the application of the packaging bag to which the gas barrier laminate 10 is applied, and may be paper whose main component is plant-derived pulp. Specific examples of the paper substrate 1 include wood-free paper, special wood-free paper, coated paper, art paper, cast-coated paper, imitation paper, kraft paper, glassine paper, etc. The thickness of the paper substrate 1 is, for example, 20 g / m 2 More than 500g / m 2 It is preferable that the thickness is less than 30 g / m 2 More than 100g / m 2 It is more preferable that:

[0016] The paper base material 1 may have a coating layer at least on the side in contact with the anchor coat layer 2 described below. By providing the coating layer, it is possible to prevent the anchor coat layer from penetrating into the paper, and it also plays a role of filling the unevenness of the paper, and the anchor coat layer can be formed uniformly without defects. For example, the coating layer may contain various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate copolymers, polyvinyl alcohol resins, cellulose resins, paraffin (WAX), etc. as binder resins, and may contain clay, kaolin, calcium carbonate, talc, mica, etc. as fillers.

[0017] The thickness of the coating layer is not particularly limited, but may be, for example, from 1 μm to 10 μm, or from 3 μm to 8 μm.

[0018] The weight of the paper is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the weight of the entire gas barrier laminate. If the weight of the paper is 50% by mass or more based on the weight of the entire gas barrier laminate, the amount of plastic material used can be sufficiently reduced, the gas barrier laminate as a whole can be said to be made of paper, and recyclability is excellent.

[0019] [Anchor coat layer] The anchor coat layer 2 is provided on the surface of the paper substrate to improve adhesion between the paper substrate 1 and the aluminum deposition layer 3 described below, and to improve the gas barrier properties of the gas barrier laminate. Examples of the anchor coat layer 2 include polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, polyimide, melamine, phenol, and polyolefin resins. Additives such as silane coupling agents and organic titanates may be mixed in.

[0020] The thickness of the anchor coat layer 2 may be, for example, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the anchor coat layer 2 is 1 μm or more, the unevenness of the paper base material described above can be efficiently filled, and the aluminum vapor deposition layer described below can be laminated uniformly. Also, if the thickness of the anchor coat layer 2 is 20 μm or less, the vapor deposition layer can be laminated uniformly while suppressing costs.

[0021] Examples of the solvent contained in the solution of the anchor coat layer 2 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Also, from the viewpoint of environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred. The method of providing the anchor coat layer 2 can be obtained by applying a coating liquid containing at least the above-mentioned solvent on a paper substrate and drying it.

[0022] [Aluminum vapor deposition layer] The aluminum deposition layer 3 is a layer formed by depositing metallic aluminum. Metallic aluminum has few polar groups, is impermeable to water vapor, and also has light blocking properties, making it preferable for the deposition layer according to this embodiment.

[0023] The thickness of the aluminum vapor-deposited layer 3 may be appropriately set depending on the application, but is preferably 10 to 300 nm, and more preferably 30 to 100 nm. By setting the thickness of the aluminum vapor-deposited layer 3 to 10 nm or more, the continuity of the aluminum vapor-deposited layer 3 can be easily ensured, and by setting the thickness to 300 nm or less, the occurrence of curling or cracking can be sufficiently suppressed, and sufficient gas barrier performance and flexibility can be easily achieved.

[0024] From the viewpoint of oxygen gas barrier performance and film uniformity, it is preferable to form the aluminum vapor deposition layer 3 by a vacuum deposition method. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its fast deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly effective because the deposition rate can be easily controlled by the irradiation area and electron beam current, and the temperature of the deposition material can be raised and lowered in a short time.

[0025] [Overcoat layer made of water-soluble polymer] The overcoat layer 4 made of a water-soluble polymer is provided on the surface of the aluminum vapor-deposited layer 3 so as to be in contact with the aluminum vapor-deposited layer 3. Such a water-soluble polymer has excellent flexibility, can suppress cracking of the aluminum vapor-deposited layer after bending (folding), and has excellent adhesion to the aluminum vapor-deposited layer. Not only does it make the vapor-deposited layer less likely to crack, but even if the vapor-deposited layer does crack, the hydroxyl groups of the water-soluble polymer keep it dense, so that the gas barrier property (oxygen barrier property) can be maintained.

[0026] The overcoat layer may contain, for example, 98% by mass or more of a water-soluble polymer, 99% by mass or more of a water-soluble polymer, or may contain only a water-soluble polymer. The overcoat layer may contain, as a material other than the water-soluble polymer, for example, 2% by mass or less, 1% by mass or less of inorganic materials such as metal alkoxides and their hydrolysates, silane coupling agents and their hydrolysates, silica particles, kaolin, mica, talc, montmorillonite, etc., or may not contain these materials.

[0027] Examples of the water-soluble polymer include polyvinyl alcohol and its modified products, starch, and celluloses. Among these, polyvinyl alcohol (hereinafter also referred to as PVA) is preferable because it can provide excellent gas barrier properties. The PVA referred to here is generally obtained by saponifying polyvinyl acetate, and can be, for example, a so-called partially saponified PVA in which several tens of percent of acetate groups remain, or a fully saponified PVA in which only a few percent of acetate groups remain. As the PVA, for example, a partially saponified PVA having a saponification degree of 70 or more may be used, but from the viewpoint of maintaining sufficient water vapor barrier properties even after the gas barrier laminate is folded, it is preferable to use a fully saponified PVA, and the saponification degree of the PVA may be, for example, 90 or more, or 95 or more. In addition, a part of the hydroxyl groups of the PVA may be modified into a hydrophobic group.

[0028] The thickness of the overcoat layer made of a water-soluble polymer may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the overcoat layer 4 made of a water-soluble polymer is 0.05 μm or more, the initial barrier properties are good, and cracking of the deposition layer due to bending of the gas barrier laminate can be prevented. In addition, if the thickness of the overcoat layer 4 made of a water-soluble polymer is 20 μm or less, the cost and curling of the substrate can be suppressed.

[0029] The gas barrier laminate described above can maintain sufficient gas barrier properties even after being folded, and can therefore be used, for example, in gusset bags. This makes it possible to sufficiently prevent deterioration of the contents for a long period of time. In addition, the amount of plastic used can be reduced compared to containers entirely made of plastic materials. EXAMPLES

[0030] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0031] The following materials were prepared:

[0032] [Water-soluble polymer] PVA1: Polyvinyl alcohol (saponification degree: 98-99, polymerization degree: 500) PVA2: Polyvinyl alcohol (saponification degree: 87-89, polymerization degree: 500) PVA3: Modified PVA (Exceval, manufactured by Kuraray Co., Ltd.)

[0033] [Preparation of gas barrier laminate] Example 1 A solution of PVA1 (solid content: 5% by mass, solvent: water / IPA = 90 / 10 (mass ratio)) was prepared as a solution of fully saponified polyvinyl alcohol. 2 An anchor coat layer (a mixed solution of acrylic polyol, γ-isocyanatopropyltrimethoxysilane, and aliphatic xylene diisocyanate, thickness: 1 μm) was formed on the surface of the anchor coat layer, and then an aluminum vapor deposition layer (50 nm) was formed on the surface of the anchor coat layer. The above PVA1 solution was applied onto the surface of the aluminum vapor deposition layer with a bar coater, and the coating was dried in an oven at 120°C for 1 minute to form a layer containing a water-soluble polymer (thickness: 1 μm). Through these steps, a gas barrier laminate (layer structure: paper / anchor coat layer / aluminum vapor deposition layer / overcoat layer (PVA1) consisting of a water-soluble polymer) was obtained.

[0034] Example 2 A solution of PVA2 (solid content: 5% by mass, solvent: water / IPA=90 / 10 (mass ratio)) was prepared as a solution of partially saponified polyvinyl alcohol. A gas barrier laminate (layer structure: paper / anchor coat layer / aluminum vapor deposition layer / overcoat layer (PVA2) made of water-soluble polymer) was prepared in the same manner as in Example 1, except that the PVA2 solution was applied with a bar coater.

[0035] Example 3 A solution of PVA3 (5% by mass, solvent: water / IPA=90 / 10 (mass ratio)) was prepared as a modified PVA solution. A gas barrier laminate (layer structure: paper / anchor coat layer / aluminum vapor deposition layer / overcoat layer made of water-soluble polymer (PVA3)) was prepared in the same manner as in Example 1, except that the PVA3 solution was applied with a bar coater.

[0036] Comparative Example 1 TEOS (10.4 g of tetraethoxysilane was added with 89.6 g of hydrochloric acid (0.05N), and then the mixture was stirred for 30 minutes to prepare a solution with a solid content of 3% by mass (SiO2 equivalent)). A solution of PVA1 (solid content: 5% by mass, solvent: water / IPA = 90 / 10 (mass ratio)) mixed with the above TEOS hydrolyzate at a ratio of 70 / 30 (solid content ratio) was prepared. Paper (thickness: 55 g / m 2 The anchor coat layer (thickness: 1 μm) described in Example 1 was formed on the surface of the laminate, and then an aluminum vapor deposition layer (50 nm) was formed on the surface of the anchor coat layer. A solution of the above PVA1 and TEOS hydrolyzate mixed at 70 / 30 (solid content ratio) was applied to the surface of the aluminum vapor deposition layer with a bar coater, and the coating was dried in an oven at 120° C. for 1 minute to form an overcoat layer (thickness: 1 μm), and a gas barrier laminate was obtained.

[0037] Comparative Example 2 A solution of PVA1 (solid content: 5% by mass, solvent: water / IPA = 90 / 10 (mass ratio)) was mixed with a layered compound (Sunlovely HN-050, manufactured by AGC Si-Tech Co., Ltd.) so that the ratio of PVA1 to the layered compound was 70 / 30 (solid content ratio). 2On the surface of the laminate, the anchor coat layer (thickness: 1 μm) described in Example 1 was formed, and then an aluminum vapor deposition layer (50 nm) was formed on the surface of the anchor coat layer. On the surface of the aluminum vapor deposition layer, a solution of the above PVA1 and the layered compound mixed at 70 / 30 (solid content ratio) was applied with a bar coater, and the coating was dried in an oven at 120° C. for 1 minute to form an overcoat layer (thickness: 1 μm), and a gas barrier laminate was obtained.

[0038] Comparative Example 3 The same procedure as in Example 1 was carried out, except that the aluminum vapor deposition layer was replaced with a silica (SiO2) vapor deposition layer.

[0039] Comparative Example 4 The same procedure as in Comparative Example 1 was carried out, except that the aluminum vapor deposition layer was replaced with a silica (SiO2) vapor deposition layer.

[0040] Comparative Example 5 The same procedure as in Comparative Example 2 was carried out, except that the aluminum vapor deposition layer was replaced with a silica (SiO2) vapor deposition layer.

[0041] Comparative Example 6 The same procedure as in Example 1 was carried out, except that the aluminum vapor-deposited layer was replaced with an alumina (Al2O3) vapor-deposited layer.

[0042] Comparative Example 7 The same procedure as in Comparative Example 1 was carried out, except that the aluminum vapor-deposited layer was replaced with an alumina (Al2O3) vapor-deposited layer.

[0043] Comparative Example 8 The same procedure as in Comparative Example 2 was carried out, except that the aluminum vapor-deposited layer was replaced with an alumina (Al2O3) vapor-deposited layer.

[0044] [Measurement of water vapor permeability] The water vapor permeability of the gas barrier laminates according to the examples and comparative examples was measured by the MOCON method. The measurement conditions were a temperature of 40°C and a relative humidity of 90%. A 600g roller was rolled at a speed of 300mm / min to make a crease in the gas barrier laminate, and the water vapor permeability of the gas barrier laminate after opening was also measured in the same manner. For each of the examples and comparative examples, the water vapor permeability is shown after the gas barrier laminate was folded in a mountain shape as viewed from the paper substrate side. The results are shown in Tables 1 to 3 below in units of [g / m 2 ·day].

[0045] [Table 1]

[0046] [Table 2]

[0047] [Table 3] [Explanation of symbols]

[0048] 1...paper substrate, 2...anchor coat layer, 3...aluminum vapor deposition layer, 4...overcoat layer made of water-soluble polymer, 10...gas barrier laminate.

Claims

1. A paper substrate, an anchor coat layer, an aluminum vapor deposition layer, and an overcoat layer made of a water-soluble polymer, in this order; the water-soluble polymer is polyvinyl alcohol; the anchor coat layer contains a resin selected from the group consisting of polyacrylic resins, polyester resins, polyurethane resins, polycarbonate resins, polyurea resins, polyamide resins, polyimide resins, melamine resins, phenolic resins, and polyolefin resins, The paper base material and the anchor coat layer are in direct contact with each other, A gas barrier laminate, in which the anchor coat layer and the aluminum vapor-deposited layer are in direct contact with each other (however, this excludes gas barrier laminates in which the anchor coat layer contains an aliphatic polyester resin).

2. A gas barrier laminate as described in claim 1, having a coating layer provided on the side of the paper base material that contacts the anchor coating layer.

3. A gas barrier laminate as described in claim 2, wherein the coating layer contains at least one binder resin selected from the group consisting of styrene-butadiene resins, styrene-acrylic resins, ethylene-vinyl acetate resins, polyvinyl alcohol resins, cellulose resins and paraffin.

4. A gas barrier laminate as described in claim 2 or 3, wherein the coating layer contains at least one filler selected from the group consisting of clay, kaolin, calcium carbonate, talc and mica.

5. A gas barrier laminate described in any one of claims 1 to 4, wherein the mass of the paper is 50 mass% or more based on the total mass of the gas barrier laminate.

Citation Information

Patent Citations

  • Cylindrical paper container

    JP1998139032A

  • Laminated material

    JP2003291296A

  • Paper for printer

    JP2004225213A

  • Gas barrier film

    JP2005138289A

  • Electromagnetic wave shielding paper, paper packaging material and laminated material for paper container using the same

    JP2005187969A