Insulated circuit board and method for manufacturing the same
The insulated circuit board with a copper plate laminate and high thermal conductivity bonding material addresses the challenge of balancing heat dissipation and pattern refinement, achieving efficient heat transfer and precise circuit patterns.
Patent Information
- Application Number
- JP2020207670
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-15
AI Technical Summary
Existing insulated circuit boards face challenges in balancing improved heat dissipation characteristics with the refinement of circuit patterns as the thickness of the circuit layer increases, making it difficult to form fine patterns while maintaining effective heat dissipation.
The insulated circuit board features a copper plate laminate with multiple copper plates laminated together, each with specific thickness ranges, and a bonding material with high thermal conductivity to enhance heat dissipation and allow for fine circuit patterns.
The configuration results in improved heat dissipation characteristics with reduced thermal resistance and the ability to form precise circuit patterns, achieved through a manufacturing method that stabilizes the production of thick copper plate laminates without excessive thickness.
Smart Images

Figure 0007567432000002 
Figure 0007567432000003 
Figure 0007567432000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulating circuit board and a method for manufacturing an insulating circuit board. [Background technology]
[0002] Power modules, LED modules and thermoelectric modules are constructed in such a way that elements such as power semiconductor elements, LED elements and thermoelectric elements are bonded to an insulating circuit board having a circuit layer made of a conductive material formed on one side of an insulating layer. In insulating circuit boards, increasing the thickness of the circuit layer is being considered in order to improve the heat dissipation characteristics of heat generated by elements.
[0003] Patent Document 1 describes an insulating circuit board in which a circuit layer is made of a metal material and has a thickness in the range of 0.05 mm to 2.0 mm. Patent Document 1 describes a method for forming a circuit layer in which a plurality of metal pieces are arranged in a circuit pattern on one side of an insulating layer. Patent Document 1 also describes a punching process as a method for manufacturing the metal pieces that make up the circuit layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-169540 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, with the increasing integration and output of elements such as power semiconductor elements, LED elements, and thermoelectric elements, it is desired to improve the heat dissipation characteristics of an insulating circuit board. Furthermore, with the increasing integration of elements, there is also a demand for finer circuit patterns. In order to improve the heat dissipation characteristics of an insulating circuit board, it is effective to increase the thickness of the circuit layer, particularly the circuit layer in the element mounting area where the element that is the heat source is mounted. However, in the punching process described in Patent Document 1, it tends to become difficult to form a fine circuit pattern as the thickness of the circuit layer increases. For this reason, it has been difficult to satisfy both the improvement of heat dissipation characteristics and the finer circuit pattern.
[0006] The present invention has been made in view of the above circumstances, and provides an insulating circuit board having a circuit layer which has excellent heat dissipation characteristics and on which a fine circuit pattern can be formed, and a method for manufacturing the insulating circuit board. [Means for solving the problem]
[0007] In order to solve the above problems, an insulating circuit board according to one aspect of the present invention is an insulating circuit board including a metal substrate, an insulating layer provided on one surface of the metal substrate, and a circuit layer provided on a surface of the insulating layer opposite to the metal substrate, the insulating layer is formed of an insulating resin or an insulating resin composition containing an insulating resin and an inorganic filler, The circuit layer has a circuit pattern, and the circuit pattern includes a copper plate laminate in which two or more copper plates are stacked, and the copper plate laminate is characterized in that the thickness of the copper plate located on the side opposite the insulating layer is in the range of 0.5 mm or more and 3.0 mm or less.
[0008] According to the insulating circuit board of this configuration, the circuit layer has a circuit pattern including a copper plate laminate in which two or more copper plates are laminated, so that the thickness of the circuit layer can be increased by increasing the number of copper plates. By increasing the thickness of the circuit layer, the heat transferred to the circuit layer spreads in the surface direction as well as the lamination direction of the insulating circuit board, and the heat is easily spread throughout the circuit layer, so that the thermal resistance of the circuit layer is reduced. In addition, in the copper plate laminate, the copper plate located on the surface opposite to the insulating layer, i.e., the copper plate on which the element is mounted, has a thickness in the range of 0.5 mm to 3.0 mm. As a result, the heat transferred to the circuit layer spreads more quickly throughout the circuit layer, so that the thermal resistance of the circuit layer is lowered. Therefore, the insulating circuit board of this configuration has excellent heat dissipation characteristics. Furthermore, since the thickness of each copper plate does not need to be increased, a fine circuit pattern can be formed. If the thickness of the copper plate on which the elements are mounted exceeds 3.0 mm, it becomes difficult to form the plate by punching, and if it is less than 0.5 mm, the heat transfer rate is somewhat poor, resulting in high thermal resistance as an insulating circuit board.
[0009] In the insulating circuit board according to one aspect of the present invention, the copper plate laminate preferably has a copper plate in contact with the insulating layer having a thickness in the range of 0.01 mm to 2.0 mm. In this case, since the thickness of the copper plate in contact with the insulating layer is thin, within the range of 0.01 mm to 2.0 mm, it is possible to form a fine circuit pattern.
[0010] In addition, in an insulating circuit board according to one embodiment of the present invention, the two or more copper plates may be bonded to each other via a bonding material, and the bonding material may be a metal having a thermal conductivity of 80 W / mK or more and a bonding temperature in the range of 200°C or more and 400°C or less. In this case, two or more copper plates are joined with a metal having a thermal conductivity of 80 W / mK or more and a joining temperature in the range of 200°C to 400°C, which increases the thermal conductivity between the copper plates and further reduces the thermal resistance of the circuit layer.
[0011] In addition, in the insulating circuit board according to one embodiment of the present invention, the two or more copper plates may be bonded to each other via a bonding material, and the bonding material may be aluminum having a purity of 99.99% by mass or more. In this case, two or more copper plates are bonded together with a bonding material that is aluminum with a purity of 99.99% by mass or more, which increases the thermal conductivity between the copper plates and further reduces the thermal resistance of the circuit layer.
[0012] In the insulating circuit board according to one aspect of the present invention, it is preferable that the circuit pattern includes an element mounting area on which an element is mounted, and the element mounting area is made of the copper plate laminate. In this case, since the element mounting area where the elements of the circuit pattern are mounted is made of a copper plate laminate, the thickness of the element mounting area can be increased, and the thermal resistance of the circuit layer can be further reduced. Therefore, the insulating circuit board of this configuration has even better heat dissipation characteristics. In addition, since the area where no elements are mounted can use a thinner copper plate instead of a copper plate laminate, it is possible to form a finer circuit pattern.
[0013] Furthermore, in the insulating circuit board according to one aspect of the present invention, it is preferable that the copper plate laminate has a thickest copper plate located on the surface opposite to the insulating layer. In this case, the copper plate located on the side opposite the insulating layer of the copper plate laminate, i.e., the copper plate in contact with the element, is the thickest and transmits heat easily, so that the heat transmitted to the copper plate laminate is easily transmitted to the insulating layer. Therefore, the insulating circuit board of this configuration has even better heat dissipation characteristics.
[0014] A method for manufacturing an insulated circuit board according to one embodiment of the present invention includes the steps of: joining a copper plate formed in a circuit pattern onto an insulating layer of a metal substrate with an insulating layer, the metal substrate including a metal substrate and an insulating layer provided on one surface of the metal substrate; and joining a separately prepared copper plate to the surface of the copper plate opposite the insulating layer to form a copper plate laminate. According to the method for producing an insulating circuit board having this configuration, a copper plate formed in a circuit pattern is bonded onto the insulating layer of a metal substrate with an insulating layer, and another copper plate is sequentially bonded onto the copper plate to form a copper plate laminate, so that an insulating circuit board having a thick copper plate laminate (circuit layer) can be industrially and stably produced without increasing the thickness of each copper plate. Since the copper plate does not need to be thick, a fine circuit pattern can be formed. Therefore, an insulating circuit board produced using the method for producing an insulating circuit board of this embodiment has a thick circuit layer with a fine circuit pattern and excellent heat dissipation characteristics.
[0015] A method for producing an insulating circuit board according to another embodiment of the present invention includes the steps of: bonding two or more copper plates, at least one of which is formed into a circuit pattern, in a stacking direction to produce a copper plate laminate; and bonding the copper plate laminate onto an insulating layer of a metal substrate with an insulating layer, the metal substrate comprising a metal substrate and an insulating layer provided on one surface of the metal substrate. According to this manufacturing method for an insulated circuit board, two or more copper plates formed into a circuit pattern are joined to produce a copper plate laminate, and then the copper plate laminate is joined onto the insulating layer of a metal substrate with an insulating layer. This makes it possible to industrially stably manufacture an insulated circuit board having a thick copper plate laminate (circuit layer) without increasing the thickness of each copper plate. Effect of the Invention
[0016] According to the present invention, it is possible to provide an insulating circuit board having a circuit layer that has excellent heat dissipation characteristics and on which a fine circuit pattern can be formed, and a method for manufacturing the insulating circuit board. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a plan view of a power module using an insulating circuit board according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 11 is a plan view of a power module using an insulating circuit board according to another embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. [Diagram 5] FIG. 11 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. [Figure 6] FIG. 11 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. [Figure 7] FIG. 11 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views illustrating a method for manufacturing an insulating circuit board according to an embodiment of the present invention. [Figure 9] 6A to 6C are cross-sectional views illustrating a method for manufacturing an insulating circuit board according to another embodiment of the present invention. [Figure 10] FIG. 2 is a cross-sectional view of the insulating circuit boards produced in Examples 1 to 4 and 11 of the present invention. [Figure 11] FIG. 1 is a cross-sectional view of the insulating circuit boards produced in Examples 5 to 10 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings. FIG. 1 is a plan view of a power module using an insulating circuit board according to one embodiment of the present invention, and FIG. 2 is a cross-sectional view taken along line II-II in FIG.
[0019] 1 and 2, power module 1a includes an insulating circuit board 10a and an element 3 mounted on insulating circuit board 10a via a solder layer 2. Insulating circuit board 10a includes a metal board 20, an insulating layer 30 provided on one surface of metal board 20, and a circuit layer 40 provided on the surface of insulating layer 30 opposite to metal board 20.
[0020] The metal substrate 20 is a base member of the insulating circuit substrate 10a. The metal substrate 20 is, for example, a copper substrate or an aluminum substrate. The copper substrate includes copper and a copper alloy. The aluminum substrate includes aluminum and an aluminum alloy.
[0021] The insulating layer 30 is a layer for insulating the metal substrate 20 and the circuit layer 40. The insulating layer 30 is formed, for example, from an insulating resin or an insulating resin composition containing an insulating resin and an inorganic filler. By forming the insulating layer 30 from an insulating resin composition containing an insulating resin and an inorganic filler having high thermal conductivity, it is possible to improve the thermal conductivity of the insulating layer 30 while maintaining the insulation properties.
[0022] The insulating resin may be, for example, an epoxy resin, a polyimide resin, or a polyamide-imide resin. One of these resins may be used alone, or two or more of them may be used in combination. The insulating resin is preferably a resin having high heat resistance. The insulating resin may have a thermal decomposition temperature of 400° C. or higher. The insulating resin may contain a polyimide resin.
[0023] Examples of inorganic fillers that can be used include alumina (Al2O3) particles, alumina hydrate particles, aluminum nitride (AlN) particles, silica (SiO2) particles, silicon carbide (SiC) particles, titanium oxide (TiO2) particles, and boron nitride (BN) particles. These inorganic fillers may be used alone or in combination of two or more. As the alumina (Al2O3) particles, α-alumina single crystal particles may be used. The inorganic filler may have an average particle size in the range of 0.1 μm to 20 μm. The content of the inorganic filler in the insulating layer 30 may be, for example, in the range of 50 volume % or more and 85 volume % or less, or in the range of 50 volume % or more and 80 volume % or less.
[0024] The circuit layer 40 has a circuit pattern. A part of the circuit layer 40 may be made into a circuit pattern, or the entire circuit layer 40 may be made into a circuit pattern. In this embodiment, the entire circuit layer 40 is made into a circuit pattern.
[0025] The circuit layer 40 (circuit pattern) is made of a copper plate laminate 45 in which a first copper plate 41 provided on the surface of the insulating layer 30 opposite to the metal substrate 20 and a second copper plate 42 provided on the surface of the first copper plate 41 opposite to the insulating layer 30 are laminated. The first copper plate 41 and the second copper plate 42 have element mounting areas 41a, 42a and wiring areas 41b, 42b, respectively. The element 3 is connected onto the element mounting area 42a of the second copper plate 42 via the solder layer 2. The element 3 is electrically connected to the wiring area 42b of the second copper plate 42 via the lead wire 4. The thickness of the second copper plate 42 is within a range of 0.5 mm to 3.0 mm. The thickness of the first copper plate 41 is, for example, within a range of 0.01 mm to 2.0 mm, preferably within a range of 0.01 mm to 1.5 mm, and may be thinner than the second copper plate 42.
[0026] The element mounting area 42a of the second copper plate 42 directly transmits heat generated by the element 3. Therefore, the surface size of the element mounting area 42a may be made the same as or larger than the size of the mounting surface of the element 3 on the side where the element mounting area 42a is mounted, thereby lowering the thermal resistance of the element mounting area 42a. Also, the surface size of the element mounting area 41a of the first copper plate 41 may be made the same as or larger than the size of the element mounting area 42a of the second copper plate 42, thereby lowering the thermal resistance of the element mounting area 41a. In this embodiment, the element mounting area 42a of the second copper plate 42 and the element mounting area 41a of the first copper plate 41 have the same size, and are configured to be larger than the size of the mounting surface of the element 3. Also, the thickness of the element mounting areas 41a, 42a (the total thickness of the element mounting area 41a of the first copper plate 41 and the element mounting area 42a of the second copper plate 42) may be within a range of 1 mm to 3 mm. By setting the thickness of the element mounting areas 41a, 42a within the above range, the heat transferred to the element mounting areas 41a, 42a spreads in the lamination direction of the insulating circuit board 10a as well as in the planar direction, and the heat transferred to the element mounting areas 41a, 42a spreads easily throughout the element mounting areas 41a, 42a. This reduces the thermal resistance of the circuit layer 40. The surface size of the element mounting areas 41a, 42a is preferably within a range of 200 to 5000, more preferably within a range of 300 to 4000, and particularly preferably within a range of 500 to 3000. The total thickness of the element mounting areas 41a, 42a is more preferably within a range of 1 mm to 8 mm, and particularly preferably within a range of 2 mm to 6 mm.
[0027] The first copper plate 41 and the second copper plate 42 are bonded together via a bonding material 50. The bonding material 50 is preferably a metal (sintered bonding material) having a thermal conductivity of 80 W / mK or more and a bonding temperature (sintering temperature) in the range of 200° C. to 400° C. When the bonding temperature is in the above range, the types of resins that can be used as the insulating resin of the insulating layer 30 are increased. Examples of sintered bonding materials include metal particles with silver or copper as a base material, which have excellent thermal conductivity. This sintered bonding material is a material in which the reactivity of the metal particle surface is improved by finely reducing the size of the metal particles, and the thermal and electrical properties derived from the physical properties of the metal contained in the sintered bonding material can be expressed at a relatively low bonding temperature that does not melt the bonded material (copper plate). The bonding material 50 may also be an aluminum foil with a purity of 99.99% by mass or more. In this case, the bonding temperature is higher than that of the sintered bonding material, so the types of resins that can be used as the insulating resin of the insulating layer 30 are limited, but it exhibits even higher heat dissipation properties.
[0028] The element 3 may be a semiconductor element, an LED element, a thermoelectric resistor, a capacitor, a crystal oscillator, or the like. Examples of the semiconductor element include a metal-oxide-semiconductor field effect transistor (MOSFET), an insulated gate bipolar transistor (IGBT), and a large scale integration (LSI). Examples of the LED element (light emitting diode) include an LED chip and an LED-CSP (LED-Chip Size Package).
[0029] As the material of the solder layer 2, for example, a solder material such as Sn-Ag, Sn-Cu, Sn-In, or Sn-Ag-Cu (so-called lead-free solder material) can be used.
[0030] According to the insulating circuit board 10a of the present embodiment configured as described above, the circuit layer 40 has a circuit pattern including a copper plate laminate 45 in which the first copper plate 41 and the second copper plate 42 are laminated, so that the thickness of the circuit layer 40 can be increased. By increasing the thickness of the circuit layer 40, the heat transferred to the circuit layer 40 spreads in the lamination direction of the insulating circuit board 10a as well as in the planar direction, and the heat transferred to the circuit layer 40 spreads easily throughout the entire circuit layer 40, so that the thermal resistance of the circuit layer can be reduced. In addition, the copper plate laminate 45 has a second copper plate 42 located on the surface opposite to the insulating layer 30, that is, the second copper plate 42 to which the element 3 is connected via the solder layer 2, which has a thickness in the range of 0.5 mm to 3.0 mm. As a result, the heat transferred to the circuit layer 40 spreads more quickly throughout the entire circuit layer 40, so that the thermal resistance of the circuit layer 40 can be reduced. Therefore, the insulating circuit board 10a of the present embodiment has excellent heat dissipation characteristics. Furthermore, the first copper plate 41 and the second copper plate 42 do not need to be excessively thick, so that a fine circuit pattern can be formed.
[0031] Furthermore, in the insulating circuit board of this embodiment, when the thickness of the first copper plate 41 of the copper plate laminate 45 is small, within the range of 0.01 mm or more and 2.0 mm or less, it becomes possible to form a finer circuit pattern.
[0032] Furthermore, in the insulating circuit board 10a of this embodiment, if the bonding material 50 bonding the first copper plate 41 and the second copper plate 42 is a metal with a thermal conductivity of 80 W / mK or more and a bonding temperature in the range of 200°C to 400°C, or if it is aluminum with a purity of 99.99% by mass or more, the thermal conductivity between the first copper plate 41 and the second copper plate 42 will be high, and the thermal resistance of the circuit layer 40 can be further reduced.
[0033] Furthermore, in the insulated circuit board 10a of the present embodiment, when the element mounting area on which the element 3 of the circuit layer 40 is mounted is made of the copper plate laminate 45, the thickness of the element mounting area 42a can be increased, and the thermal resistance of the circuit layer 40 can be further reduced, resulting in further improved heat dissipation characteristics of the insulated circuit board.
[0034] Furthermore, in the insulating circuit board of this embodiment, when the second copper plate 42 located on the surface of the copper plate laminate 45 opposite the insulating layer 30 is the thickest, heat is easily transferred to the copper plate in contact with the element 3, and the heat transferred to the copper plate laminate 45 is easily transferred to the insulating layer 30. Therefore, the insulating circuit board 10a having this configuration has even better heat dissipation characteristics. Also, in the area where the element is not mounted, a thinner copper plate can be used instead of the copper plate laminate, making it possible to form a finer circuit pattern.
[0035] Although the insulating circuit board according to the embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate without departing from the technical concept of the invention. For example, in this embodiment, the first copper plate 41 and the second copper plate 42 of the circuit layer 40 are configured to have element mounting areas 41a, 42a and wiring areas 41b, 42b, respectively, but are not limited to this. For example, the second copper plate 42 may be configured to have only the element mounting area 42a, that is, the element mounting area may be formed of a copper plate laminate 45 including the first copper plate 41 and the second copper plate, and the wiring area may be formed of only the first copper plate 41.
[0036] In the present embodiment, the surface sizes of the element mounting areas 41a, 42a of the circuit layer 40 are the same, but this is not limited to this. For example, the surface size of the element mounting area 41a of the copper plate (first copper plate 41) in contact with the insulating layer 30 may be larger than the surface size of the element mounting area 42a of the copper plate (second copper plate 42) located on the surface opposite to the insulating layer 30.
[0037] Furthermore, in this embodiment, the copper plate laminate 45 of the circuit layer 40 is configured by laminating two copper plates, the first copper plate 41 and the second copper plate 42, but there is no limit to the number of copper plates as long as it is two or more. For example, the number of copper plates may be three or more. The number of copper plates may be six or less. Even when the number of copper plates is three or more, the thickness of the copper plate bonded to the element is within the range of 0.5 mm to 3.0 mm. An insulating circuit board according to another embodiment of the present invention will be described below with reference to Figures 3 to 7. In the following description, the same components as those in the power module 1a shown in Figures 1 and 2 are denoted by the same reference numerals, and detailed description thereof may be omitted.
[0038] FIG. 3 is a plan view of a power module using an insulating circuit board according to another embodiment of the present invention, and FIG. 4 is a cross-sectional view taken along line IV-IV in FIG. 3 and 4 differs from the power module 1a shown in Figures 1 and 2 in that the second copper plate 42 of the insulating circuit board 10b has only an element mounting area 42a, that is, the element mounting area is formed of a copper plate laminate 45 including the first copper plate 41 and the second copper plate, and the wiring area is formed only by the first copper plate 41. For this reason, by reducing the thickness of the first copper plate 41, sufficient heat dissipation characteristics are obtained and the wiring area 41b can be made finer and thinner.
[0039] Furthermore, the power module 1b differs from the power module 1a in that the surface size of the element mounting area 41a of the first copper plate 41 of the insulating circuit board 10b is configured to be larger than the element mounting area 42a of the second copper plate 42. Since the surface size of the element mounting area 41a is configured to be larger than the element mounting area 42a, heat transferred from the element 3 to the element mounting area 42a is more easily transferred to the element mounting area 41a. Therefore, insulating circuit board 10b has the effect of enabling wiring area 41b to be made finer and thinner, in addition to the effect of insulating circuit board 10a, and thus has the effect of further improving heat dissipation characteristics.
[0040] FIG. 5 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. The power module 1c shown in FIG. 5 differs from the power module 1a shown in FIGS. 1 and 2 in that the element mounting area of the insulating circuit board 10c is formed of a copper plate laminate 45 including a first copper plate 41 and a second copper plate, and the wiring area is formed only by the first copper plate 41. Therefore, insulating circuit board 10c has the effect of enabling wiring region 41b to be made finer and thinner, in addition to the effect of insulating circuit board 10a.
[0041] FIG. 6 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. The power module 1d shown in FIG. 6 is different from the power module 1a shown in FIG. 1 and FIG. 2 in that the element mounting area of the insulating circuit board 10d is a copper plate laminate 45 including a first copper plate 41, a second copper plate 42, and a third copper plate 43. The first copper plate 41 and the second copper plate 42, and the second copper plate 42 and the third copper plate 43 are bonded to each other via a bonding material 50. The second copper plate 42 and the third copper plate 43 have a thickness in the range of 0.5 mm to 3.0 mm. In the insulating circuit board 10d, the copper plate laminate 45 constituting the element mounting area is formed from three copper plates, so that the thickness of each copper plate constituting the copper plate laminate 45 can be made thin. Therefore, the insulating circuit board 10d has sufficient heat dissipation characteristics and can have finer and thinner element mounting areas 41a, 42a, and 43a. The number of copper plate laminates 45 constituting the element mounting area may be four or more depending on the amount of heat transfer required, but ten or less is preferable when considering the balance between heat dissipation characteristics and fineness.
[0042] 1 and 2 in that the wiring region of the insulating circuit board 10d is formed only by the first copper plate 41. Therefore, by reducing the thickness of the first copper plate 41, it is possible to make the wiring region 41b finer and thinner. Therefore, insulating circuit board 10d has the effect of enabling element mounting areas 41a, 42a, 43a and wiring area 41b to be made finer and thinner, in addition to the effect of insulating circuit board 10a, and has the effect of further improving heat dissipation characteristics.
[0043] FIG. 7 is a cross-sectional view of a power module using an insulating circuit board according to still another embodiment of the present invention. The power module 1e shown in Fig. 7 differs from the power module 1d shown in Fig. 6 in that the surface size of the element mounting area 41a of the first copper plate 41 and the element mounting area 42a of the second copper plate 42 of the insulating circuit board 10e is configured to be larger than the element mounting area 43a of the third copper plate 43. Since the surface size of the element mounting area 41a is configured to be larger than the element mounting area 42a, heat transferred from the element 3 to the element mounting area 43a is more easily transferred to the element mounting area 42a. Therefore, insulating circuit board 10e has the effect of further improving heat dissipation characteristics in addition to the effect of insulating circuit board 10d.
[0044] Next, a method for manufacturing the insulating circuit board according to this embodiment will be described with reference to FIGS.
[0045] FIG. 8 is a cross-sectional view illustrating a method for manufacturing an insulating circuit board according to one embodiment of the present invention. The method for producing an insulating circuit board according to this embodiment includes a first copper plate joining step and a second copper plate joining step.
[0046] 8(a), the first copper plate bonding step is a step of bonding a first copper plate 41 onto the insulating layer 30 of a metal substrate 60 with an insulating layer. The metal substrate 60 with an insulating layer includes a metal substrate 20 and an insulating layer 30 provided on one surface of the metal substrate 20. The first copper plate 41 is formed in a circuit pattern having an element mounting region 41a and a wiring region 41b.
[0047] The method for manufacturing the metal substrate 60 with an insulating layer is not particularly limited. For example, a method of laminating a resin sheet on one side of the metal substrate 20 can be used as the method for manufacturing the metal substrate 60 with an insulating layer. The resin sheet may contain an inorganic filler. In addition, a method for manufacturing the metal substrate 60 with an insulating layer can be used in which a coating liquid containing a resin is applied to one side of the metal substrate 20, the resulting coating film is dried, and the coating film is baked by heating. The coating liquid may contain an inorganic filler. In addition, a method for manufacturing the metal substrate 60 with an insulating layer can be used in which resin particles are electrodeposited on one side of the metal substrate 20 using an electrodeposition liquid containing charged resin particles, the resulting electrodeposition film is dried, and the coating film is baked by heating. The electrodeposition liquid may contain an inorganic filler.
[0048] There is no particular limitation on the method for manufacturing the first copper plate 41 formed into a circuit pattern. For example, various methods used as copper plate processing methods, such as etching and punching, can be used.
[0049] The insulating layer 30 of the metal substrate 60 with an insulating layer and the first copper plate 41 can be bonded by, for example, a pressure bonding method. The insulating layer 30 of the metal substrate 60 with an insulating layer and the first copper plate 41 can be bonded by placing the first copper plate 41 on the insulating layer 30 of the metal substrate 60 with an insulating layer and heating the insulating layer 30 and the first copper plate 41 using a pressure bonding device. When bonding the insulating layer 30 and the first copper plate 41 by the pressure bonding method, the bonding may be performed under a reduced pressure atmosphere or an inert gas atmosphere in order to suppress oxidation of the first copper plate 41.
[0050] 8(b), the second copper plate bonding step is a step of bonding a separately prepared second copper plate 42 to the surface of the first copper plate 41 opposite the insulating layer 30. The second copper plate 42 is formed in a circuit pattern having an element mounting area 42a and a wiring area 42b.
[0051] The second copper plate 42 formed into a circuit pattern can be manufactured in the same manner as the first copper plate 41, using various methods that are used for processing copper plates, such as etching and punching.
[0052] The first copper plate 41 and the second copper plate 42 can be bonded using a bonding material 50. For example, silver, copper, and aluminum with a purity of 99.99% by mass or more can be used as the material of the bonding material 50. The bonding material 50 may be a thin film or particles of these metals. The first copper plate 41 and the second copper plate 42 can be bonded by placing the bonding material 50 on the first copper plate 41, placing the second copper plate 42 on the bonding material 50, and heating the first copper plate 41 and the second copper plate 42 while applying pressure using a pressure bonding device. When metal particles are used as the bonding material 50, a metal particle layer may be formed on the first copper plate 41 by preparing a dispersion of metal particles, applying the metal particle dispersion on the first copper plate 41, and drying the resulting coating film. When the first copper plate 41 and the second copper plate 42 are joined by the pressure bonding method, the joining may be performed in a reduced pressure atmosphere or an inert gas atmosphere in order to suppress oxidation of the first copper plate 41 and the second copper plate 42 .
[0053] According to the method for producing an insulating circuit board of this embodiment configured as described above, the first copper plate 41 formed in a circuit pattern is bonded onto the insulating layer 30 of the metal substrate 60 with an insulating layer, and then the second copper plate 42 formed in a circuit pattern is sequentially bonded to form the copper plate laminate 45. Therefore, even if the first copper plate 41 and the second copper plate 42 are not excessively thick, an insulating circuit board having a thick circuit layer 40 can be industrially and stably produced. Since the first copper plate 41 and the second copper plate 42 do not need to be thick, a fine circuit pattern can be formed. Therefore, the insulating circuit board produced by the method for producing an insulating circuit board of this embodiment has a thick circuit layer 40 with a fine circuit pattern and excellent heat dissipation characteristics.
[0054] FIG. 9 is a cross-sectional view illustrating a method for manufacturing an insulating circuit board according to another embodiment of the present invention. The method for producing an insulating circuit board according to this embodiment includes a copper plate laminate producing step and a copper plate laminate joining step.
[0055] 9(a), the copper plate laminate fabrication process is a process of bonding a first copper plate 41 and a second copper plate 42 to fabricate a copper plate laminate 45. The first copper plate 41 and the second copper plate 42 are formed into a circuit pattern having element mounting areas 41a, 42a and wiring areas 41b, 42b, respectively.
[0056] The first copper plate 41 and the second copper plate 42 can be bonded together using a bonding material 50. The method for bonding the first copper plate 41 and the second copper plate 42 using the bonding material 50 is the same as in the second copper plate bonding step described above.
[0057] The copper plate laminate joining step is a step of joining the first copper plate 41 of the copper plate laminate 45 onto the insulating layer 30 of the metal substrate 60 with an insulating layer, as shown in FIG. 9(b). A pressure bonding method can be used as a method for bonding the first copper plate 41 of the copper plate laminate 45 and the insulating layer 30 of the metal substrate 60 with an insulating layer. The method for bonding the first copper plate 41 and the insulating layer 30 using the pressure bonding method is the same as in the first copper plate bonding step described above.
[0058] According to the manufacturing method for an insulated circuit board of this embodiment configured as described above, the first copper plate 41 formed in a circuit pattern and the second copper plate 42 formed in a circuit pattern are joined to form the copper plate laminate 45, and then the copper plate laminate 45 is joined onto the insulating layer 30 of the metal substrate 60 with an insulating layer. Therefore, even if the first copper plate 41 and the second copper plate 42 are not made excessively thick, an insulated circuit board having a thick copper plate laminate 45 (circuit layer 40) can be manufactured industrially in a stable manner.
[0059] Although the method for manufacturing an insulating circuit board according to an embodiment of the present invention has been described above, the present invention is not limited to this and can be modified as appropriate without departing from the technical concept of the invention. For example, in this embodiment, the copper plate laminate 45 is formed using two copper plates, the first copper plate 41 and the second copper plate 42, but there is no limit to the number of copper plates as long as it is two or more. For example, the number of copper plates may be three or more. EXAMPLES
[0060] [Example 1] (1) Manufacturing process of copper substrate with insulating layer A copper substrate with an insulating layer was fabricated by stacking an epoxy resin sheet (insulating layer A, length: 100 mm, width: 100 mm, thickness: 120 μm, thermal conductivity: 10 W / mK) containing alumina and aluminum nitride as fillers on one surface of a copper substrate (length: 100 mm, width: 100 mm, thickness: 1.0 mm). Thermal conductivity is a physical property after thermocompression bonding, and was measured by the laser flash method.
[0061] (2) First copper plate joining process (Preparation of the first copper plate) A copper plate (length: 100 mm, width: 100 mm, thickness: 1.0 mm) was punched to produce a first copper plate having an element mounting area and a wiring area. The size of the element mounting area was 30 mm x 30 mm.
[0062] (Joining of the first copper plate) The first copper plate was placed on the insulating layer of the copper substrate with an insulating layer prepared in (1) above, and placed in a pressure bonding device. The pressure bonding device was then evacuated to create a reduced pressure atmosphere, and the device was heated at 180°C for 60 minutes while being pressurized at 10 MPa, thereby bonding the first copper plate to the insulating layer.
[0063] (3) Joining the second copper plate (Preparation of copper particle paste) While stirring ion-exchanged water at room temperature, copper citrate 2.5 hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the ion-exchanged water to prepare a copper citrate aqueous dispersion with a concentration of 30% by mass. The obtained copper citrate aqueous dispersion was adjusted to a pH of 3 or more and less than 7 by adding an aqueous ammonium citrate solution. Next, while the pH-adjusted copper citrate aqueous dispersion was kept at 50°C, an aqueous hydrazine monohydrate solution was added to the copper citrate aqueous dispersion while stirring under a nitrogen gas atmosphere to obtain a mixed solution. The aqueous hydrazine monohydrate solution was prepared by diluting hydrazine monohydrate two-fold with water. The amount of the aqueous hydrazine monohydrate solution added was 1.2 times the equivalent amount required to elute copper in the copper citrate aqueous dispersion as copper ions. Next, the obtained mixture was heated to 70°C under a nitrogen gas atmosphere, and was held at 70°C (maximum temperature) for 2 hours, and then cooled to 20°C to obtain a copper particle slurry. The obtained copper particle slurry was placed in a centrifuge and processed at a rotation speed of 1000 rpm for 10 minutes to recover copper particles. The recovered copper particles were dried for 10 hours by a reduced pressure drying method to obtain copper particles for a bonding material. 8.5 g of the obtained copper particles for a bonding material, 1.4 g of ethylene glycol (manufactured by Kanto Chemical Co., Ltd.), and 0.1 g of glycerin (manufactured by Kanto Chemical Co., Ltd.) were mixed to prepare a copper particle paste.
[0064] (Preparation of the second copper plate) A second copper plate having an element mounting area and a wiring area was fabricated by punching a copper plate (length: 100 mm, width: 100 mm, thickness: 1 mm). The size of the element mounting area was 30 mm × 30 mm, the same as the first copper plate.
[0065] (Joining the second copper plate) The above copper particle paste was applied to the first copper plate bonded in (2) above to a thickness of 50 μm. Then, the above second copper plate was placed on the applied copper particle paste. Then, in a nitrogen atmosphere, the plate was heated at a temperature of 300° C. for 5 minutes while being pressurized at a pressure of 10 MPa to sinter the copper particles, thereby bonding the first copper plate and the second copper plate. In this manner, an insulating circuit board according to Example 1 of the present invention was produced.
[0066] [Example 2] An insulating circuit board of Example 2 of the present invention was produced in the same manner as in Example 1 of the present invention, except that in step (3) of joining the second copper plate of Example 1 of the present invention, a silver particle paste prepared by the following method was used instead of the copper particle paste.
[0067] (Preparation of silver particle paste) While 1200g of ion-exchanged water was kept at 50°C, 900g of silver nitrate aqueous solution kept at 50°C and 600g of sodium citrate aqueous solution kept at 50°C were simultaneously dropped into the ion-exchanged water over 5 minutes while stirring to prepare a silver citrate slurry. The silver nitrate concentration in the silver nitrate aqueous solution was 66% by mass, and the citric acid concentration in the sodium citrate aqueous solution was 56% by mass. Next, while the obtained silver citrate slurry was kept at 50°C, 300g of sodium formate aqueous solution kept at 50°C was dropped into the silver citrate slurry over 30 minutes while stirring to obtain a mixed slurry. The formic acid concentration in the sodium formate aqueous solution was 58% by mass. Next, the obtained mixed slurry was heated to a temperature of 60°C at a heating rate of 10°C / hour, held at 60°C (maximum temperature) for 30 minutes, and then cooled to 20°C over 60 minutes to obtain a silver particle slurry. The obtained silver particle slurry was put into a centrifuge and processed at a rotation speed of 1000 rpm for 10 minutes to recover the silver particles. The recovered silver particles were dried for 30 hours by freeze-drying to obtain a silver powder for a bonding material. 8.5 g of the obtained silver powder for a bonding material was mixed with 2.5 g of ethylene glycol (manufactured by Kanto Chemical Co., Ltd.) to prepare a paste.
[0068] [Example 3] An insulating circuit board of Example 3 of the present invention was prepared in the same manner as in Example 1 of the present invention, except that in the (1) step of preparing a copper substrate with an insulating layer of Example 1 of the present invention, the insulating layer (insulating layer B) was formed by the coating method described below. (Preparation of Coating Solution) A polyimide solution with a polyimide concentration of 10 mass% was prepared by mixing polyamic acid (Ube Industries, Upia ST) and NMP (N-methyl-2-pyrrolidone) and dissolving the polyimide. Also, an α-alumina particle dispersion with an α-alumina particle concentration of 10 mass% was prepared by mixing α-alumina powder (crystal structure: single crystal, average particle size: 1.6 μm) and NMP and subjecting the mixture to ultrasonic treatment for 30 minutes.
[0069] The polyimide solution and the α-alumina particle dispersion were mixed in such a ratio that the α-alumina concentration in the resin film was 60% by volume. The mixture obtained was dispersed by repeating a high-pressure injection process at a pressure of 50 MPa 10 times using a Starburst manufactured by Sugino Machine Co., Ltd., to prepare a coating liquid. The α-alumina concentration is the content of α-alumina particles in the solid material generated when the coating liquid is heated and dried.
[0070] (Preparation of copper substrate with insulating layer) The above coating solution was applied to one surface of a copper substrate (length: 100 mm, width: 100 mm, thickness: 1 mm) by a bar coating method to form a coating film. Next, the copper substrate on which the coating film was formed was placed on a hot plate, and the temperature was increased from room temperature to 60°C at a temperature increase rate of 3°C / min, and heated at 60°C for 100 minutes, and then the temperature was increased to 120°C at a temperature increase rate of 1°C / min, and heated at 120°C for 100 minutes to dry the coating film. Next, the copper substrate was heated at 250°C for 5 minutes, and then heated at 400°C for 60 minutes in a nitrogen atmosphere. In this way, a copper substrate with an insulating layer was prepared in which an insulating layer made of a polyimide resin in which α-alumina single crystal particles were dispersed was formed on the surface of the copper substrate. The obtained insulating layer had a film thickness of 50 μm and a thermal conductivity of 2 W / mK.
[0071] [Example 4] In (1) the step of preparing a copper substrate with an insulating layer of Inventive Example 1, an insulating layer was formed in the same manner as Inventive Example 3. In (3) the step of joining a second copper plate of Inventive Example 1, a 4N aluminum thin film (thickness: 400 μm) was used instead of the copper particle paste, and the second copper plate was joined as follows. Except for the above, an insulating circuit board of Inventive Example 4 was prepared in the same manner as Inventive Example 1.
[0072] (Joining the second copper plate) This 4N aluminum thin film and the second copper plate were placed on top of the first copper plate and placed in a pressure bonding device. After vacuuming to create a reduced pressure atmosphere, the first copper plate and the second copper plate were joined by heating at 540°C for 60 minutes while applying a pressure of 1 MPa.
[0073] [Example 5] In the (3) joining step of the second copper plate in the present invention example 1, the size of the element mounting area of the second copper plate was set to 15 mm × 15 mm. The first copper plate and the second copper plate were joined so that the center of the element mounting area of the first copper plate and the center of the element mounting area of the second copper plate were overlapped. Except for this, the insulating circuit board of the present invention example 5 was produced in the same manner as the present invention example 1.
[0074] [Examples 6 to 10 of the present invention] Insulated circuit boards of Inventive Examples 6 to 10 were produced in the same manner as Inventive Example 5, except that the thickness of the first copper plate or the second copper plate was changed to the thickness shown in Table 1 below.
[0075] [Example 11] An insulating circuit board of Example 11 of the present invention was produced in the same manner as Example 1 of the present invention, except that an epoxy paste with a thermal conductivity of 7 W / mK was used as the bonding material, and the epoxy paste was applied to a thickness of 50 μm on the first copper plate to bond the first copper plate and the second copper plate.
[0076] [Comparative Examples 1 to 3] Insulated circuit boards of Comparative Examples 1 to 3 were produced in the same manner as in Invention Example 1, except that the second copper plate was not joined and the thickness of the first copper plate was changed to the thickness shown in Table 1 below.
[0077] [Comparative Examples 4 to 6] Insulated circuit boards of Comparative Examples 4 to 6 were produced in the same manner as in Invention Example 3, except that the second copper plate was not joined and the thickness of the first copper plate was changed to the thickness shown in Table 1 below.
[0078] [Comparative Example 7] An insulating circuit board of Comparative Example 7 was produced in the same manner as in Invention Example 5, except that the thickness of the second copper plate was 0.3 mm.
[0079] [evaluation] Sn-Ag-Cu solder was applied to the surface of the element mounting area to form a solder layer with a thickness of 100 μm. Next, an element with a mounting surface size of 6 mm×6 mm was mounted on the solder layer to obtain the power module shown in FIG. 10 or FIG. 11. The insulating circuit board on which the element 3 was mounted was pressed in the stacking direction from above the element 3 by a screw with a torque of 40 Ncm. A transient heat measurement device (T3Ster, manufactured by Mentor Graphics) 100 was connected to the element 3 and the element mounting area 42a of the second copper plate. Then, the thermal resistance from the element 3 to the copper board 10 was measured using the transient heat measurement device 100. The heat generation conditions of the element were 10 A and 180 seconds, and the measurement conditions of the thermal resistance were 0.1 A and the measurement time was 300 seconds. The same measurement was performed on a single copper board without an insulating layer, and the thermal resistance was subtracted from the measured value of the insulating circuit board to obtain the thermal resistance. The results are shown in Table 1 below.
[0080] [Table 1]
[0081] It is seen that the insulated circuit boards of the present invention in which the circuit pattern of the circuit layer is a copper plate laminate formed by laminating a first copper plate and a second copper plate whose thickness is within the range of the present invention have reduced thermal resistance compared to the insulated circuit boards of the comparative examples 1 to 6 in which the circuit pattern of the circuit layer is composed only of a first copper plate. In particular, it is seen that the insulated circuit boards of the present invention in which copper particles, silver particles, and an aluminum thin film are used as the bonding material have significantly reduced thermal resistance. Moreover, by comparing the inventive examples 8 to 10 with the comparative example 7, it is seen that the thickness of the second copper plate needs to be 0.5 mm or more. [Explanation of symbols]
[0082] 1a, 1b, 1c, 1d, 1e Power Modules 2 Solder Layer 3 Elements 4 Lead Wire 10a, 10b, 10c, 10d, 10e Insulating circuit board 20 Metal Substrate 30 Insulating layer 40 circuit layers 41 1st Copper Plate 42 Second copper plate 43 Third Copper Plate 41a, 42a, 43a Element mounting area 41b, 42b wiring area 45 Copper plate laminate 50 Bonding material 60 Metal substrate with insulating layer 100 Transient heat measurement device
Claims
1. An insulating circuit board comprising a metal substrate, an insulating layer provided on one surface of the metal substrate, and a circuit layer provided on a surface of the insulating layer opposite to the metal substrate, the insulating layer is formed of an insulating resin or an insulating resin composition containing an insulating resin and an inorganic filler, the circuit layer has a circuit pattern; The circuit pattern includes a copper plate laminate in which two or more copper plates are laminated, The copper plate laminate is an insulating circuit board, characterized in that the thickness of the copper plate located on the surface opposite to the insulating layer is within the range of 0.5 mm to 3.0 mm.
2. 2. The insulating circuit board according to claim 1, wherein the thickness of the copper plate in contact with the insulating layer of the copper plate laminate is within a range of 0.01 mm to 2.0 mm.
3. 3. The insulating circuit board according to claim 1, wherein the two or more copper plates are bonded to each other via a bonding material, the bonding material being a metal having a thermal conductivity of 80 W / mK or more and a bonding temperature in the range of 200° C. or more and 400° C. or less.
4. 3. The insulating circuit board according to claim 1, wherein the two or more copper plates are bonded to each other via a bonding material, the bonding material being aluminum with a purity of 99.99% by mass or more.
5. 5. The insulating circuit board according to claim 1, wherein the circuit pattern includes an element mounting area on which an element is mounted, and the element mounting area is formed as the copper plate laminate.
6. 6. The insulating circuit board according to claim 1, wherein the copper plate laminate has a thickest copper plate located on a surface opposite to the insulating layer.
7. A step of bonding a copper plate formed in a circuit pattern onto an insulating layer of a metal substrate having an insulating layer, the metal substrate including a metal substrate and an insulating layer provided on one surface of the metal substrate; 7. The method for producing an insulating circuit board according to claim 1, further comprising the step of joining a separately prepared copper plate to a surface of the copper plate opposite to the insulating layer to form a copper plate laminate.
8. A step of manufacturing a copper plate laminate by bonding two or more copper plates, at least one of which is formed into a circuit pattern, in a lamination direction; 7. The method for producing an insulating circuit board according to claim 1, further comprising: joining the copper plate laminate onto an insulating layer of a metal substrate having a metal substrate and an insulating layer provided on one surface of the metal substrate.
Citation Information
Patent Citations
Substrate for power module with heat sink, power module with heat sink and manufacturing method of substrate for power module with heat sink
JP2014060216A
Insulation circuit board and manufacturing method thereof
JP2019149460A
Insulation circuit board and manufacturing method of the insulation circuit board
JP2019169540A