How zinc oxide ore is produced
By adjusting the fluorine content ratio in raw materials and controlling dry heating temperatures, the method produces high-grade zinc oxide ore with reduced fluorine, addressing energy and equipment challenges in existing production processes.
Patent Information
- Application Number
- JP2020218540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-12-28
AI Technical Summary
Existing methods for producing zinc oxide ore from fluorine-containing raw materials, such as steel dust, face challenges in efficiently removing fluorine impurities while minimizing high-temperature operations that increase energy costs and equipment wear.
A method involving raw material ore preparation to adjust the fluorine content ratio, followed by reduction roasting, wet processing, and controlled dry heating at temperatures below 1100°C to produce high-grade zinc oxide ore with reduced fluorine concentration.
The method effectively reduces fluorine content to 0.03% or less in zinc oxide ore, suitable for electrolytic smelting, while minimizing heat load and energy consumption.
Smart Images

Figure 0007567468000003 
Figure 0007567468000001 
Figure 0007567468000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing zinc oxide ore. [Background technology]
[0002] Conventionally, zinc oxide ore obtained by separating and removing impurities from zinc-containing ores such as crude zinc oxide has been widely used as a raw material for zinc ingots in zinc smelters.
[0003] Crude zinc oxide can be obtained, for example, from steel dust generated in steelmaking furnaces such as blast furnaces and electric furnaces in the steel industry through reduction roasting treatment. From the viewpoint of promoting resource recycling, it is desirable to reuse steel dust as a zinc raw material. However, on the other hand, there is a problem in that steel dust contains halogens such as fluorine as impurities in addition to iron and zinc.
[0004] One example of a method for separating iron and zinc in steel dust is the reduction and calcination method using a rotary kiln. In this method, zinc is reduced in the kiln furnace and then volatilized as metallic zinc. The metallic zinc, once separated into the gas side as a gas, quickly reacts with the surrounding oxygen to become zinc oxide and solidify, and is then collected by a dust collector such as an electric dust collector as particulate crude zinc oxide (crude zinc oxide dust) mixed with halogens, steel dust carried over from the kiln, and valuable metals that behave in the same way as zinc.
[0005] Here, it is of course necessary that the concentration of impurities in the final zinc product be extremely low. For example, in order to use zinc oxide ore as a raw material for zinc smelting using the ISP smelting method or the electrolytic smelting method, the halogen concentration of zinc oxide ore must be reduced to the value permitted by each smelting method.
[0006] The process for separating and removing halogens from crude zinc oxide dust includes a method of washing with an alkali (wet process) and a method of decomposing the halogens in a dry heating furnace such as a rotary kiln (dry heat process).However, because the refining principles of chlorine and fluorine are essentially different, and crude zinc oxide dust contains unreacted iron and steel dust that has been carried over, these methods, i.e., a combination of wet process and dry heat process, are generally used industrially to separate and remove halogens.
[0007] Here, for example, among the above zinc refining methods, the zinc oxide ore used as a raw material in the electrolytic smelting method needs to have a fluorine concentration lower than that of the zinc oxide ore used as a raw material in the ISP smelting method in order to suppress the progress of corrosion of the aluminum permanent cathode used in the electrowinning process. In order to separate and remove fluorine with such high accuracy, it was necessary to set the heating temperature in the above-mentioned dry heat treatment to a high temperature of about 1100°C or higher (see Patent Document 1).
[0008] If the temperature inside a drying and heating furnace such as a rotary kiln is raised to this high temperature range of about 1100°C or more as described above, energy costs will increase, and in addition, the increased heat load on the equipment due to high-temperature operation will be a factor in shortening the life of the equipment such as the rotary kiln. However, in order to obtain high-quality zinc oxide ore that can be used as a raw material for electrolytic smelting, the current situation is that the above-mentioned disadvantages associated with high-temperature operation of the drying and heating furnace must be accepted to some extent, and further improvements in the method of removing halogens have been required in the zinc oxide ore production process. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP2014-62304A Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to produce high-quality zinc oxide ore in which the fluorine concentration is sufficiently reduced to an extent that it can be used as a raw material for electrolytic smelting, while suppressing the heat load on a drying and heating furnace due to high-temperature operation, in a process for producing zinc oxide ore from a raw material ore containing fluorine. [Means for solving the problem]
[0011] The present inventors have come up with the idea of producing high-quality zinc oxide ore with a sufficiently reduced fluorine concentration while suppressing the thermal load on a drying and heating furnace by making a raw ore preparation step of obtaining a raw ore for a reduction roasting step, the fluorine content ratio of which is optimized to a predetermined ratio, an essential step in a process for producing zinc oxide ore from a raw ore containing fluorine, and have completed the present invention. More specifically, the present invention provides the following.
[0012] (1) A method for producing zinc oxide ore from a raw ore containing fluorine, comprising: a raw ore preparation step for obtaining a raw ore for a reducing roasting step, the raw ore having a fluorine content ratio adjusted to a predetermined ratio by mixing a plurality of raw ores having different fluorine content ratios, which is the ratio of the fluorine content ratio to the zinc content ratio, or by selecting a raw ore having the fluorine content ratio adjusted to a predetermined ratio; a reducing roasting step for obtaining crude zinc oxide dust by subjecting the raw ore for the reducing roasting step to a reducing roasting treatment; and a reducing roasting step for adding water to the crude zinc oxide dust. 1. A method for producing zinc oxide ore, comprising: a wet process for obtaining a crude zinc oxide cake by performing a wet treatment to remove soluble impurities; and a dry heating process for obtaining the zinc oxide ore by performing a dry heating process on the crude zinc oxide cake, wherein in the dry heating process, the dry heating process is performed at a heating temperature of 1000°C or more and 1100°C or less, and the fluorine content of the zinc oxide ore is maintained at 0.03% or less by adjusting the dry heating process time in accordance with the fluorine content ratio of the raw material ore for the reduction roasting process.
[0013] (2) The method for producing zinc oxide ore described in (1), wherein in the raw ore preparation step, a plurality of types of raw ores having different fluorine content ratios are mixed to adjust the fluorine content ratio to the predetermined ratio, thereby obtaining a raw ore for the reduction roasting step.
[0014] (3) The method for producing zinc oxide ore according to (1) or (2), wherein the raw material ore is iron ore dust.
[0015] (4) A method for producing zinc oxide ore described in any one of (1) to (3), wherein the fluorine content ratio of the raw ore for the reduction roasting process is set to 0.015 or less in the raw ore preparation process, thereby setting the dry heat treatment time in the dry heat process to 130 minutes or more and 150 minutes or less.
[0016] (5) A method for producing zinc oxide ore described in any one of (1) to (3), wherein the fluorine content ratio of the raw ore for the reduction roasting process is set to 0.005 or less in the raw ore preparation process, thereby setting the dry heat treatment time in the dry heat process to 110 minutes or more and 130 minutes or less. Effect of the Invention
[0017] According to the present invention, in a process for producing zinc oxide ore from a raw material ore containing fluorine, it is possible to produce high-quality zinc oxide ore having a sufficiently reduced fluorine concentration while suppressing the heat load on a drying and heating furnace due to high-temperature operation. The zinc oxide ore obtained by the production method of the present invention can be used as a raw material for electrolytic smelting, and the industrial value of the production method of the present invention is extremely great. [Brief description of the drawings]
[0018] [Figure 1] 1 is a flowchart showing an example of an embodiment of a method for producing zinc oxide ore of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The present invention is a manufacturing method that can be widely applied to the production of zinc oxide ore using a raw material ore containing fluorine as an impurity in addition to at least zinc. The raw material ore containing fluorine as an impurity is not limited to a specific raw material ore, but a typical example is the above-mentioned iron and steel dust.
[0020] <Overall process> Fig. 1 shows the overall process of zinc oxide ore production to which the method for producing zinc oxide ore of the present invention can be applied. As shown in Fig. 1, this overall process includes a raw ore preparation step S10 for obtaining a "raw ore for reduction roasting step" in which a "fluorine content ratio" that is the ratio of the fluorine content to the zinc content in the raw ore is optimized, a reduction roasting step S20 for obtaining crude zinc oxide dust by reduction roasting the "raw ore for reduction roasting step", a wet process S30 for separating and removing halogen elements such as fluorine and chlorine from the crude zinc oxide dust obtained in the reduction roasting step S20 into a treatment liquid to obtain a crude zinc oxide cake, a dry heating step S40 for drying and heating the crude zinc oxide cake obtained in the wet process S30 to obtain zinc oxide ore, an exhaust gas dust cleaning step S50 for cleaning the exhaust gas dust generated in the dry heating step S40 to obtain a cleaned exhaust gas dust cake, and a wastewater treatment step S60 for detoxifying the discharged liquid discharged from the wet process S30.
[0021] The method for producing zinc oxide ore of the present invention is a method in which the minimum essential steps in the overall process for producing zinc oxide ore are the raw ore preparation step S10, the reduction roasting step S20, the wet step S30, and the dry heating step S40. The exhaust gas dust cleaning step S50 and the wastewater treatment step S60 may be performed according to conventional methods in a required manner as necessary.
[0022] The method for producing zinc oxide ore of the present invention is characterized in that, in producing zinc oxide using a raw ore containing fluorine, it is possible to maintain the fluorine content of the zinc oxide ore at 0.03% by weight or less, while lowering the dry heat treatment temperature in the dry heat step S40 to a temperature range of 1100°C or less, which is lower than conventional temperatures.
[0023] In addition, the manufacturing method of the present invention is characterized in that the raw ore preparation step S10 is an essential step preceding the reduction roasting step S20 as the most upstream step in the overall process of zinc oxide ore production, in which complex chemical changes occur in stages over multiple stages, and therefore it is possible to control the quality of the final product, zinc oxide ore, with high precision simply by adjusting the operating conditions in the drying and heating step S40, which is the most downstream step.
[0024] The method for producing zinc oxide ore according to the present invention, which has the above-mentioned characteristics, is intended to be carried out in a zinc oxide ore production plant in which a plurality of types of iron and steel dust with different "fluorine content ratios" are sequentially carried in as raw materials. More specifically, the method for producing zinc oxide ore according to the present invention is a method that can be suitably carried out in a zinc oxide ore production plant in which a plurality of types of iron and steel dust to be actually used in each operation period are sequentially selected from the plurality of types of iron and steel dust sequentially carried in and used as raw materials. The above-mentioned condition of iron and steel dust carrying in is not a special condition in the production of zinc oxide ore using iron and steel dust as raw material, but is also a very common supply mode of raw materials. Therefore, the production method according to the present invention has sufficient practicality and versatility.
[0025] <Raw ore preparation process> The raw ore preparation step S10 is a step of obtaining raw ore for the reduction roasting step, in which the fluorine content ratio is adjusted to a predetermined ratio. In this specification, the "fluorine content ratio" refers to the ratio of the fluorine grade to the zinc grade in the raw ore.
[0026] In the raw ore preparation step S10, in order to obtain a raw ore for the reducing roasting step in which the "fluorine content ratio" has been adjusted to a predetermined ratio, for example, when multiple types of raw ores having different "fluorine content ratios" are used as described above, the above adjustment can be performed by mixing them in an optimal ratio. Alternatively, by selecting one type of raw ore whose "fluorine content ratio" is the same as or sufficiently close to the predetermined ratio, the selected raw ore can be used as the raw ore for the reducing roasting step.
[0027] The predetermined ratio of the "fluorine content ratio" is determined within a range in which the fluorine content of the zinc oxide ore can be maintained at 0.03% or less by performing the dry heating process in the dry heating step S40 at a heating temperature of 1100°C or less and adjusting the dry heating process time according to the heating temperature and the "fluorine content ratio" of the raw ore for the reduction roasting process. For example, as disclosed later as an example, even when the above heating temperature in the dry heating step S40 is set to 1100°C, the "fluorine content ratio" is adjusted to a predetermined ratio (e.g., about 0.005), unlike the conventional process, so that the fluorine content of the zinc oxide ore can be reliably maintained at 0.03% or less with the minimum dry heating process time.
[0028] When iron ore dust is used as the raw ore, the "fluorine content ratio" can be adjusted by, for example, investigating in advance the "fluorine content ratios" of multiple brands of steel dust supplied by an electric furnace manufacturer, and mixing these brands of steel dust in a desired ratio. The "fluorine content ratios" of steel dust supplied by an electric furnace manufacturer vary from brand to brand, and there are steel dusts with various fluorine grades, for example, from steel dusts with low fluorine grades having a "fluorine content ratio" of about 0.002 to steel dusts with high fluorine grades having a "fluorine content ratio" of about 0.07. In the production method of the present invention, a mixture of steel dusts with different fluorine grades is used, and therefore, only one specific brand of steel dust is not consumed, and these steel dusts can be consumed in a planned manner.
[0029] Here, Table 1 shows an example of the results of measuring the fluorine content and iron content in the crude zinc oxide dust recovered in the reduction roasting step S20 and the fluorine content and iron content in the crude zinc oxide dust recovered by the electrostatic precipitator when zinc oxide ore is produced by a conventional production method that does not perform the raw ore preparation step S10. The fluorine content and iron content in the recovered crude zinc oxide dust are higher than the fluorine content and iron content in the recovered crude zinc oxide dust, and it can be seen that most of the fluorine and iron are distributed in the crude zinc oxide dust, which has a relatively large particle size. In other words, the results in Table 1 show that the iron in the steel dust that did not contribute to the reduction reaction and was carried over unreacted was introduced into the dust collection equipment together with the exhaust gas, and most of it was collected by the gravity settling type dust collector. Referring to Table 1, fluorine also behaves in the same way as iron, so it can be determined that a part of the fluorine in the steel dust was also collected by the gravity settling type dust collector together with the carried-over iron.
[0030] [Table 1]
[0031] In addition to the fluorine carried over with the iron, the crude zinc oxide dust contains fluorine in the form of volatile compounds such as lead trifluoride (PbFCl) etc. Thus, in the conventional manufacturing method, it was extremely difficult to eliminate the distribution of fluorine into the crude zinc oxide dust in the reduction roasting step S20, which was the most upstream step.
[0032] The manufacturing method of the present invention is the same as the conventional manufacturing method in that crude zinc oxide dust is collected using a gravity settling dust collector and an electric dust collector. Therefore, it is difficult to eliminate the distribution of fluorine in the crude zinc oxide dust, as in the conventional manufacturing method. However, in the manufacturing method of the present invention, when the iron and steel dust is charged into the reduction roasting rotary kiln (RRK), the "fluorine content ratio" of the iron and steel dust input into the RRK is adjusted to an optimal predetermined ratio in advance. Therefore, it is possible to maintain high quality of the zinc oxide ore, which is the final product, by only adjusting the operating conditions in the drying and heating process S40, which is the most downstream process that is relatively easy to adjust, without particularly adjusting the operating conditions in the wet process S30.
[0033] <Reduction roasting process> As a specific method for carrying out the reduction roasting step S20 for recovering crude zinc oxide from iron and steel dust, etc., a reduction roasting method using a reduction roasting rotary kiln (RRK) is widely adopted. The reduction roasting step S20 will be described in detail below for the case where iron and steel dust is used as the raw material for crude zinc oxide and is reduction roasted in a reduction roasting rotary kiln. In this case, the iron and steel dust is formed into pellets having a size of about 5 to 10 mm in advance as necessary, and is continuously charged into the reduction roasting rotary kiln together with a carbonaceous reducing agent such as coal or coke and limestone (CaO) and the like.
[0034] During the reduction roasting step S20, the maximum temperature of the material to be treated inside the reduction roasting rotary kiln is controlled to about 1000°C or higher and 1400°C or lower by the combustion of heavy oil and the charged carbonaceous reducing agent. In this furnace, the steel dust is reduction roasted, and the volatilized metallic zinc is reoxidized in the furnace to become particulate crude zinc oxide (crude zinc oxide dust).
[0035] Small amounts of lead contained in steel dust are also roasted under reduced conditions, and the evaporated metallic lead is reoxidized in the furnace to form powdered lead oxide. If a large amount of halogen is present in the steel dust, some of the metallic zinc and lead are evaporated as halogen compounds.
[0036] In this reduction roasting step S20, the reduction roasting residue that does not volatilize and remains in the furnace of the reduction roasting rotary kiln contains a large amount of reduced iron, so it is collected from the kiln discharge end as a product called reduced iron pellets and delivered to steel manufacturers as a raw iron material.
[0037] The above-mentioned powdered zinc oxide and lead oxide are introduced into a dust collection facility consisting of a plurality of dust collectors connected together with the exhaust gas from the reduction roasting rotary kiln, and are recovered stepwise as crude zinc oxide dust. The dust collection facility is composed of a gravity settling dust collector arranged at the most upstream of the exhaust gas treatment path, an electric dust collector connected downstream of the gravity settling dust collector, and a bag filter connected further downstream of the electric dust collector. First, crude zinc oxide dust with a relatively large particle size is collected by the gravity settling dust collector, and crude zinc oxide dust with a relatively small particle size that has not been collected by the gravity settling dust collector is collected by the electric dust collector and the bag filter. The above-mentioned gravity settling dust collector is a dust collector that settles and collects crude zinc oxide dust contained in the exhaust gas by a sudden decrease in the flow rate of the exhaust gas and a collision effect with the inner wall, and the electric dust collector is a dust collector that introduces crude zinc oxide dust charged by corona discharge into an electric field and collects it on a dust collecting electrode. A bag filter is a dust collector that collects particles by filtering them using a filter cloth.
[0038] <Wet process> The wet process S30 is a wet process in which water-soluble impurities contained in the crude zinc oxide dust are separated and extracted into a treatment liquid, and then the impurities are removed from the crude zinc oxide by a water washing method through a solid-liquid separation process to obtain a crude zinc oxide cake. The wet process can be performed by a conventionally known method in which the treatment liquid in which the impurities are distributed is removed from the slurry by solid-liquid separation in a state in which impurities such as fluorine have been removed from the treatment liquid. As a result, the crude zinc oxide slurry becomes a crude zinc oxide cake with a high concentration. For the dehydration process for solid-liquid separation, a gravity settling type slurry concentrator such as a thickener or a forced moisture dehydrator such as a vacuum dehydrator can be used.
[0039] In the wet process S30, the crude zinc oxide dust obtained in the previous reduction roasting process is repulped with industrial water or the like. It is not essential to use an alkaline solution for this repulping. The crude zinc oxide slurry is subjected to pH adjustment and coagulation treatment, and then to primary dehydration. In this case, the pH is adjusted to a weak acid solution of about 6 to 7 to elute cadmium, and a coagulant or the like is used for coagulation to increase sedimentation. After this primary dehydration, the crude zinc oxide cake is diluted with industrial water and further subjected to secondary dehydration. It is preferable that the halogen concentration of the crude zinc oxide cake is reduced to less than 0.6% by weight for the fluorine concentration and less than 1.0% by weight for the chlorine concentration by these two washing and dehydration processes.
[0040] Alternatively, this wet treatment can be divided into a first wet treatment in which the crude zinc oxide slurry obtained by repulping using fresh water or appropriate circulating water in the production line and dissolving sodium carbonate or sodium hydroxide is adjusted to a low pH treatment solution of about pH 6.5 to remove mainly cadmium from the crude zinc oxide, and a second wet treatment in which a pH adjuster is added to the crude zinc oxide slurry obtained by the first wet treatment to adjust the pH to a high pH treatment solution of about pH 8.5 to remove mainly fluorine compounds from the crude zinc oxide. In this case, the pH adjuster used in the second wet treatment can be the neutralization treatment solution generated in the wastewater treatment process described below.
[0041] <Dry heating process> The dry heating step S40 is a step in which the crude zinc oxide cake obtained in the previous wet step S30 is charged into a heating furnace such as a dry heating rotary kiln (DRK) for calcination and granulation. By passing through this step, the fluorine concentration can be further reduced and high-quality zinc oxide ore can be granulated. In the production method of the present invention, the heating temperature of the dry heating treatment in the dry heating step S40 is maintained in a temperature range of 1000°C or more and 1100°C or less. Note that the heating temperature in the above-mentioned dry heating rotary kiln (DRK) can usually be adjusted in units of about 100°C, and is adjusted so that the fluctuation in the heating temperature in the furnace falls within a temperature range of about 100°C.
[0042] Here, the fluorine remaining in the crude zinc oxide cake can be in the form of volatile (e.g., lead trifluoride (PbFCl)) or non-volatile (e.g., calcium difluoride (CaF2)). Of these, the volatile substance (PbFCl) is almost entirely volatilized by maintaining the temperature of the ore calcination within the above-mentioned temperature range, and the volatile chlorine and fluorine are almost entirely discharged to the exhaust gas treatment equipment in the exhaust gas dust cleaning process S50. On the other hand, the non-volatile substance (CaF2) is an extremely stable compound, so it is fixed in the zinc oxide ore without decomposing and volatilizing in the dry heating rotary kiln.
[0043] As described above, the manufacturing method of the present invention requires that the heating temperature of the dry heat treatment be maintained in a temperature range of 1000° C. or more and 1100° C. or less. As described above, on the premise that the heating temperature is maintained in a range lower than the conventional range, the heating time for the dry heat treatment of the crude zinc oxide cake charged into the DRK is adjusted within a range that makes it possible to obtain, under such temperature conditions, zinc oxide ore of a quality equal to or higher than that obtained during conventional high-temperature operation, specifically, high-quality zinc oxide ore with a fluorine content of 0.03% by weight or less.
[0044] In the manufacturing method of the present invention, in the raw ore preparation step S10, which is the most upstream step, the "fluorine content ratio" (F / Zn ratio) of raw ore such as steel dust is adjusted to a predetermined ratio, thereby effectively suppressing non-volatile fluorine input into the DRK. Furthermore, the drying heat treatment time of the crude zinc oxide cake is optimally adjusted based on the above-mentioned "fluorine content ratio" (F / Zn ratio), thereby effectively volatilizing and removing volatile fluorine input into the DRK.
[0045] For example, when the "fluorine content ratio" (F / Zn ratio) of the steel dust charged into the RRK is adjusted to 0.015 in order to obtain high-quality zinc oxide ore, even if the heating temperature in the drying and heating step S40 is lowered to a temperature range of 1000°C or higher and 1100°C or lower, high-quality zinc oxide ore with a fluorine content of 0.03% by weight or less can be obtained by adjusting the drying and heating treatment time of the crude zinc oxide cake charged into the DRK to 130 minutes. It is preferable to determine in advance by testing or the like an appropriate combination of the "fluorine content ratio" (F / Zn ratio) of the steel dust and the drying and heating treatment time of the crude zinc oxide cake.
[0046] When a rotary kiln is used as the drying / heating furnace, the drying / heating treatment time is equal to the residence time in the furnace, and can be calculated by the known calculation formula shown below. Formula: Residence time [min]=0.19L / (NDtanθs) L: Furnace length [m] N: Rotation speed [rpm] D: Furnace inner diameter [m] θs: Inclination angle of furnace [deg]
[0047] Incidentally, the lower the fluorine content in the zinc oxide ore, the higher the quality. In other words, zinc oxide ore with a fluorine content of 0 is the highest quality. However, in order to obtain such high-quality zinc oxide ore, it is necessary to adjust the "fluorine content ratio" (F / Zn ratio) of the steel dust to be lower and the drying heat treatment time of the crude zinc oxide cake to be longer, and such adjustment is often difficult to make in actual operation. For this reason, in the production method of the present invention, it is preferable to adjust the "fluorine content ratio" (F / Zn ratio) of the steel dust to an optimal combination within a range that satisfies the conditions that the lower limit of the "fluorine content ratio" (F / Zn ratio) is 0.002 and the upper limit of the drying heat treatment time is 150 minutes or less, preferably 130 minutes or less, and more preferably 120 minutes or less. The above lower limit of the "fluorine content ratio" (F / Zn ratio) is the fluorine content of the brand of steel dust that has the lowest fluorine content among the brands of steel dust actually supplied. In addition, the shorter the drying heat treatment time is adjusted to within a range where the fluorine content of the zinc oxide ore can be maintained at 0.03% by weight or less, the more advantageous it is because the heat load on the DRK is reduced and the energy used in the drying heat treatment can be reduced. If the drying heat treatment time exceeds 150 minutes, there is a concern that the heat load on the heating furnace will increase, and operation will become inefficient.
[0048] More specifically, the above-mentioned optimum combination of the "fluorine content ratio" (F / Zn ratio) and the dry heat treatment time can be exemplified by, for example, adjusting the dry heat treatment time in the dry heat treatment step S40 to within a range of 130 minutes or more and 150 minutes or less by setting the "fluorine content ratio" (F / Zn ratio) of the raw ore for the reducing roasting step in the raw ore preparation step S10 to 0.015 or less. Alternatively, the "fluorine content ratio" (F / Zn ratio) of the raw ore for the reducing roasting step in the raw ore preparation step S10 can be further reduced to 0.0 05 By setting the above, it is also possible to adjust the dry heating treatment time in the dry heating step S40 to within the range of 110 minutes or more and 130 minutes or less.
[0049] <Exhaust gas dust cleaning process> The exhaust gas dust cleaning step S50 is a step in which the exhaust gas dust generated in the drying and heating step S40 is cleaned to obtain a cleaned exhaust gas dust cake. The cleaning equipment for carrying out the exhaust gas dust cleaning step S50 generally comprises a combination of a cleaning tower and a wet-type electric dust collector. The cleaned exhaust gas dust cake recovered in these facilities is repeatedly recycled and fed into an upstream process such as a drying and heating rotary kiln in the drying and heating step S40, thereby making effective use of metal resources.
[0050] <Wastewater treatment process> The wastewater treatment process S60 is a process in which fluorine and cadmium are removed from the wastewater separated from the crude zinc oxide in the wet process S30 and containing high concentrations of these metals, and further, heavy metals contained in trace amounts in the wastewater are extracted by neutralization treatment, and finally, the pH is adjusted to make the wastewater harmless.
[0051] The waste liquid separated in the wet process S30 also contains trace amounts of zinc and / or lead components eluted from the crude zinc oxide. To recover these heavy metal components, a neutralization process is carried out as described above. This neutralization process is generally carried out by adding slaked lime. The slaked lime can be added by directly adding solid slaked lime to the wet processing liquid, or by adding a solution of slaked lime dissolved in a liquid form to the wet processing liquid. The amount of slaked lime added can also be adjusted by measuring the pH of the neutralization process liquid after the addition.
[0052] In addition, the neutralization residue containing zinc compounds or lead compounds recovered by this neutralization treatment is repeatedly used in the wet treatment step, where it is wet treated together with the zinc oxide slurry obtained from the reduction roasting step, and is generally calcined and granulated in a dry heating rotary kiln to fix it into zinc oxide ore.
[0053] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments. Furthermore, the effects described in the embodiments of the present invention are merely a list of the most preferable effects resulting from the present invention, and the effects of the present invention are not limited to those described in the examples of the present invention. EXAMPLES
[0054] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0055] [Example 1] A trial production of zinc oxide ore was carried out using the production method of the present invention. Specifically, the following steps were carried out in order under the conditions shown below, and the fluorine content of the obtained zinc oxide ore was measured. The results are shown in Table 2. (Raw ore preparation process) As the raw material ore for crude zinc oxide, steel dust of several brands with different fluorine contents was mixed and adjusted to have a "fluorine content ratio" (F / Zn ratio) of 0.005. This steel dust was used as the "raw material ore for the reduction roasting process," with the fluorine content ratio adjusted to a specified ratio. (Reduction roasting process) This "raw ore for the reduction roasting process" was charged into a reduction roasting rotary kiln (RRK) together with coal, coke and other carbonaceous reducing agents, limestone, etc., and reduction roasting was carried out while controlling the temperature of the reduction roasting rotary kiln so that the maximum temperature of the treated material was 1000°C to 1400°C. The crude zinc oxide dust generated during this process was collected using a gravity settling type dust collector and an electric dust collector and a bag filter connected downstream of the gravity settling type dust collector, to obtain crude zinc oxide dust. (Wet process) The entire amount of crude zinc oxide dust collected by the gravity settling dust collector was removed from the system, and the remaining crude zinc oxide dust was repulped with repulping water in which sodium carbonate was dissolved, to obtain a low pH treatment liquid adjusted to pH 6.5. Then, about 5 to 10 mass ppm of a polymeric flocculant was added to the low pH treatment liquid, and solid-liquid separation was performed in a thickener to obtain a crude zinc oxide slurry with reduced chlorine and fluorine. The crude zinc oxide slurry obtained by the above treatment was subjected to vacuum dehydration and dehydration using a press roll, to obtain a crude zinc oxide cake with a moisture content of about 20 to 30% by weight. (Dry heating process) This crude zinc oxide cake was loaded into a dry heat rotary kiln (DRK) and subjected to dry heat treatment while controlling the temperature and residence time of the dry heat rotary kiln (DRK) so that the maximum temperature of the treated material was 1000°C or higher and 1100°C or lower, and the dry heat treatment time was 130 minutes.
[0056] [Other Examples and Comparative Examples] In Examples 2 to 5 and Comparative Examples 1 to 5, in the raw ore preparation step, either the "fluorine content ratio" (F / Zn ratio) of the "raw ore for the reduction roasting step" or the dry heat treatment time in the dry heat step, or both of these conditions were controlled under different conditions for each Example and Comparative Example as shown in Table 2 below. All zinc oxide ores were produced under the same conditions as in Example 1, and the fluorine grade of the obtained zinc oxide ore was measured in the same manner. The results are shown in Table 2.
[0057] [evaluation] Table 2 shows the embodiment of each test operation of the Examples and Comparative Examples, and the fluorine grade (F grade) of the zinc oxide ore obtained under each condition. Each Example and Comparative Example was evaluated from the viewpoints of Evaluation 1 and Evaluation 2 below, and if an evaluation of "○ (good)" was obtained in both evaluations, the overall evaluation was determined to be "○ (good)".
[0058] (Rating 1) In the drying and heating process, we evaluated whether the heat load on the drying and heating furnace due to high temperature operation was suppressed. The evaluation criteria are as follows. Heating temperature below 1100℃: ○ (good) Heating temperature exceeds 1100℃: × (bad)
[0059] (Rating 2) In the drying and heating process, an evaluation was performed to see whether the fluorine content of zinc oxide ore required for high-quality zinc oxide ore could be maintained. The evaluation criteria were as follows: F content [wt%] in zinc oxide ore is 0.030 wt% or less: ○ (good) F content [wt%] in zinc oxide ore is 0.030 wt% or less: × (bad) It's big. [Table 2]
[0060] As shown in Table 2, under the conditions of Example 1, the fluorine content of the zinc oxide ore was the lowest, and an extremely high-quality zinc oxide ore was obtained. Under the conditions of Examples 2 to 5, the fluorine content of the zinc oxide ore was slightly higher than that of Example 1, but zinc oxide ore of the second highest quality after Example 1 was obtained. On the other hand, under the conditions of Comparative Examples 1 to 3, the fluorine content of the zinc oxide ore further increased and exceeded 0.030% by weight. Moreover, under the conditions of Comparative Examples 4 and 5, the fluorine content of the zinc oxide ore was 0.030% by weight or less, but the heat load on the dry heating rotary kiln (DRK) increased.
[0061] From the above test and evaluation results, it has been confirmed that the zinc oxide ore manufacturing method of the present invention makes it possible to produce high-quality zinc oxide ore with a sufficiently reduced fluorine concentration while suppressing the heat load on the drying and heating furnace due to high-temperature operation in the process of manufacturing zinc oxide ore from raw ore containing fluorine. [Explanation of symbols]
[0062] S10 Raw ore preparation process S20 Reduction roasting process S30 Wet process S40 Drying heating process S50 Exhaust gas dust cleaning process S60 Wastewater treatment process
Claims
1. A method for producing zinc oxide ore, comprising the steps of: producing zinc oxide ore from a raw material ore containing fluorine, the method comprising the steps of: a raw ore preparation step of mixing a plurality of types of raw ores having different fluorine content ratios, which are the ratios of the fluorine content to the zinc content, to obtain a raw ore for a reduction roasting step, the fluorine content ratio of which is adjusted to a predetermined ratio; a reduction roasting step for obtaining crude zinc oxide dust by subjecting the raw material ore for the reduction roasting step to a reduction roasting treatment; a wet process for removing water-soluble impurities from the crude zinc oxide dust to obtain a crude zinc oxide cake; a drying and heating step of subjecting the crude zinc oxide cake to a dry and heat treatment to obtain the zinc oxide ore; Including, In the raw ore preparation step, the fluorine content ratio of the raw ore for the reduction roasting step is set to 0.005 or less, In the dry heating step, the temperature of the dry heating treatment is set to 1000° C. or more and 1100° C. or less, and the dry heating treatment time is set to 110 minutes or more and 130 minutes or less according to the fluorine content ratio of the raw material ore for the reduction roasting step. How zinc oxide ore is produced.
2. The raw material ore is iron and steel dust. A method for producing the zinc oxide ore according to claim 1.
Citation Information
Patent Citations
Method for producing zinc oxide ore
JP2014062304A
Zinc oxide ore production method
JP2014162960A
Method for manufacturing zinc oxide ore
JP2015120948A
Manufacturing method of zinc oxide ore