Propenyl group-containing composition, curable resin composition, cured product, and electric / electronic parts

A propenyl group-containing composition addresses the heat resistance and reliability issues in semiconductor encapsulants by controlling curing temperature and isomer ratios, resulting in low viscosity and high heat resistance for high-power semiconductor applications.

JP7567503B2Active Publication Date: 2024-10-16MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021009672
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-29
Filing Date
2021-01-25
Publication Date
2024-10-16
Estimated Expiration
2041-01-25

AI Technical Summary

Technical Problem

Existing semiconductor encapsulants lack sufficient heat resistance, low viscosity, and long-term reliability for high-power applications, particularly in power semiconductors used for controlling motors and converting power.

Method used

A propenyl group-containing composition is developed, allowing for a curable resin composition that achieves low viscosity and high heat resistance by controlling the curing reaction temperature, with specific proportions of trans and cis isomers and blending with maleimide resins and epoxy resins.

Benefits of technology

The composition provides cured products with excellent heat resistance, long-term reliability, and low water absorption, enhancing the performance and reliability of electrical and electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567503000001
    Figure 0007567503000001
  • Figure 0007567503000002
    Figure 0007567503000002
  • Figure 0007567503000003
    Figure 0007567503000003
Patent Text Reader

Abstract

To provide: a propenyl group-containing composition which has low viscosity and can form a cured product excellent in heat resistance and long-term reliability; and a curable resin composition based on the same.SOLUTION: The propenyl group-containing composition comprises a compound represented by the formula (1) in the figure, where the content of the compound represented by the formula (1) is 80.0 to 99.9 mass%. The curable resin composition contains 0.01 to 1000 pts.mass of one or more selected from the group consisting of epoxy resins, maleimide resins and phenol resins, based on 100 pts.mass of the propenyl group-containing composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a propenyl group-containing composition, a curable resin composition, a cured product, and an electric / electronic device. [Background technology]

[0002] 2. Description of the Related Art Thermosetting resin compositions are used in various fields as thermosetting molding materials, etc., taking advantage of their curability. Examples of such materials include adhesives and sealing materials for electric and electronic parts.

[0003] As thermosetting resin compositions, resin compositions have been proposed in which allylphenol, alkenylphenol, alkenylphenol ether or the like is mixed with maleimide resin or epoxy resin.

[0004] For example, Patent Documents 1 and 2 disclose compositions comprising a mixture of bismaleimide, an amine, an alkenylphenol, an alkenylphenol ether, and the like, and disclose that the alkenylphenol is produced by rearrangement of an allyl ether of phenol.

[0005] Furthermore, Patent Document 3 discloses a resin composition that has excellent heat resistance, low water absorption, and can suppress voids in the cured product, and that contains a specific propenyl group-containing resin having a benzene ring or a naphthalene ring having a propenyl group, and a maleimide compound having two or more maleimide groups in one molecule. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 181335 / 1983 [Patent Document 2] Japanese Patent Application Publication No. 4-227931 [Patent Document 3] JP 2019-019149 A Summary of the Invention [Problem to be solved by the invention]

[0007] Traditionally, most semiconductors have been used with relatively small currents and power, such as LSIs, but in recent years, there has been rapid development of power semiconductors, which use semiconductors to control motors, lighting, and other devices and convert power. This has led to a demand for semiconductors and semiconductor encapsulation materials that can be used with higher power and current than before, and semiconductor encapsulation materials are required to have higher heat resistance, lower viscosity, and long-term reliability than before.

[0008] The cured product obtained by curing the resin composition containing a propenyl group-containing resin and a maleimide compound described in Patent Document 3 was not satisfactory in terms of heat resistance, low viscosity, and long-term reliability as a semiconductor encapsulant used in the above-mentioned applications.

[0009] The present invention aims to provide a propenyl group-containing composition capable of providing a curable resin composition which has a low viscosity and gives a cured product having excellent heat resistance and long-term reliability, a curable resin composition using the same, and a cured product and an electric / electronic device using the same. [Means for solving the problem]

[0010] As a result of intensive research to solve the above problems, the present inventors focused on the temperature range at which the maleimide resin hardening reaction begins, and, based on the assumption that controlling the hardening start temperature makes it possible to achieve low viscosity and long-term reliability while exhibiting high heat resistance even when the hardening reaction is carried out at a low temperature, found that the skeleton and purity of the propenyl group-containing compound blended together with the maleimide resin can be important control factors for controlling the hardening start temperature.The inventors then found that a specific propenyl group-containing composition can achieve low viscosity and long-term reliability while exhibiting high heat resistance even when the hardening temperature is low, and thus completed the present invention.

[0011] That is, the gist of the present invention lies in the following [1] to [8].

[0012] [1] A propenyl group-containing composition comprising a compound represented by the following formula (1), wherein the content of the compound represented by the formula (1) is 80.0 to 99.9 mass %:

[0013] [ka]

[0014] (In the above formula (1), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S-, and an aliphatic hydrocarbon group having 1 to 20 carbon atoms. R 1 and R 2 are hydrogen atoms, hydrocarbon groups having 1 to 10 carbon atoms, or halogen atoms, and may be the same or different.

[0015] [2] The propenyl group-containing composition according to [1], comprising 0.1 to 20.0 mass % of a compound represented by the following formula (2):

[0016] [ka]

[0017] (In the above formula (2), X and R 1 , R 2 has the same meaning as in the above formula (1).

[0018] [3] The propenyl group-containing composition according to [1] or [2], wherein the proportion of trans isomers in which all propenyl groups are of trans configuration among the compounds represented by formula (1) is 20 to 95%.

[0019] [4] The propenyl group-containing composition according to any one of [1] to [3], wherein, among the compounds represented by formula (1), a proportion of cis isomers in which all of the propenyl groups are of cis type is 30% or less.

[0020] [5] The propenyl group-containing composition according to any one of [1] to [4], having a melt viscosity at 150°C in the range of 0.01 to 10.0 P.

[0021] [6] A curable resin composition comprising, per 100 parts by mass of the propenyl group-containing composition according to any one of [1] to [5], 0.01 to 1,000 parts by mass of at least one resin selected from the group consisting of epoxy resins, maleimide resins, phenolic resins, benzoxazine resins, cyanate ester resins, active ester resins, resins having a radically polymerizable functional group, isocyanate resins, acid anhydride resins, and carbodiimide resins.

[0022] [7] A cured product obtained by curing the curable resin composition described in [6].

[0023] [8] An electric or electronic part comprising a cured product of the curable resin composition described in [6]. Effect of the Invention

[0024] The curable resin composition of the present invention obtained by mixing the propenyl group-containing composition of the present invention with a maleimide resin, an epoxy resin, or the like, has a low viscosity and can give a cured product having high heat resistance and excellent long-term reliability. Therefore, the propenyl group-containing composition and the curable resin composition of the present invention can provide highly reliable cured products and electrical / electronic components that have excellent electrical reliability, thermal decomposition resistance, adhesion, low moisture absorption, low elasticity, and little change in physical properties at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The following describes in detail an embodiment of the present invention, but the following description is merely an example of an embodiment of the present invention, and the present invention is not limited to the following description as long as it does not deviate from the gist of the present invention. Note that in this specification, when the expression "~" is used, it is used as an expression including the numerical values ​​or physical property values ​​before and after it.

[0026] [Propenyl group-containing composition] The propenyl group-containing composition of the present invention contains a compound represented by the following formula (1), and is characterized in that the content of the compound is 80.0 to 99.9 mass %.

[0027] [ka]

[0028] (In the above formula (1), X is a divalent linking group selected from a direct bond, -SO2-, -O-, -CO-, -C(CF3)2-, -S-, and an aliphatic hydrocarbon group having 1 to 20 carbon atoms. R 1 and R 2 are hydrogen atoms, hydrocarbon groups having 1 to 10 carbon atoms, or halogen atoms, and may be the same or different.

[0029] The propenyl group-containing composition of the present invention is specified as a "propenyl group-containing composition" since it contains a compound represented by the above formula (1) (hereinafter, may be referred to as "propenyl group-containing compound (1)") and other optional components (for example, a compound represented by formula (2) described below). However, in the technical field of the compound, the "propenyl group-containing compound" may be obtained as a "composition" consisting of multiple components other than a single component. Therefore, the propenyl group-containing composition of the present invention may be expressed in the industry as a "propenyl group-containing compound" (sometimes referred to as a "propenyl group-containing resin") or sold as a "propenyl group-containing compound" (sometimes referred to as a "propenyl group-containing resin").

[0030] <Propenyl group-containing compound (1)> In the above formula (1) representing the propenyl group-containing compound (1), the aliphatic hydrocarbon group having 1 to 20 carbon atoms for X is preferably an aliphatic hydrocarbon group having 1 to 10 carbon atoms, particularly preferably an alkylene group having 1 to 10 carbon atoms which may be branched. X is preferably a direct bond or an aliphatic hydrocarbon group having 1 to 10 carbon atoms, more preferably a direct bond, a methylene group, or an isopropylidene group, and most preferably a direct bond.

[0031] R 1 ,R 2 Examples of the halogen atom in R include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. 1 ,R 2 Examples of the hydrocarbon group having 1 to 10 carbon atoms include an alkyl group having 1 to 10 carbon atoms. 1 ,R 2 are each independently a hydrogen atom or a methyl group, and most preferably R 1 and R 2 are both hydrogen atoms.

[0032] The propenyl group-containing compound (1) represented by formula (1) contains cis-trans isomers of the double bonds of the propenyl groups (1-propenyl groups) bonded to each of the two benzene rings, and includes a "trans isomer" in which both of the two propenyl groups in formula (1) are in the trans form, and a "cis isomer" in which both of the propenyl groups in formula (1) are in the cis form.

[0033] The proportion of trans isomers in the propenyl group-containing compound (1) is preferably 20 to 95%, more preferably 30 to 85%, and even more preferably 45 to 75%. The larger the proportion of trans isomers, the higher the crystallinity and the easier it is to handle the powder, whereas the smaller the proportion of trans isomers, the better the solubility in solvents.

[0034] In addition, the proportion of cis-isomer in the propenyl group-containing compound (1) is preferably 30% or less, more preferably 20% or less, and even more preferably 10% or less. The smaller the proportion of cis-isomer, the higher the crystallinity and the easier it is to handle in powder form. The lower limit of the proportion of cis-isomer is not particularly limited, but is preferably 1% or more from the viewpoint of melting property during heating.

[0035] The propenyl group-containing compound (1) also includes other propenyl group-containing compounds (1) that do not belong to either the trans form or the cis form. These are compounds in which one of the two propenyl groups in the formula (1) is a trans form and the other is a cis form, and are usually contained in the propenyl group-containing compound (1) in an amount of about 5 to 50%.

[0036] The ratio of trans- and cis-isomers of the propenyl group-containing compound (1) can be controlled, for example, by changing the type of solvent used in the propenylation reaction during the production of the propenyl group-containing compound (1).

[0037] The propenyl group-containing composition of the present invention contains 80.0 to 99.9% by mass of the propenyl group-containing compound (1). If the content of the propenyl group-containing compound (1) in the propenyl group-containing composition of the present invention is less than 80.0% by mass, the effects of high heat resistance, low viscosity, and long-term reliability due to the inclusion of the propenyl group-containing compound (1) cannot be fully obtained. Since it is practically difficult to produce a propenyl group-containing composition consisting of 100% by mass of the propenyl group-containing compound (1), the content of the propenyl group-containing compound (1) in the propenyl group-containing composition of the present invention is usually 99.9% by mass or less. In order to further enhance the effect of the propenyl group-containing compound (1) while also improving solubility in a solvent, the content of the propenyl group-containing compound (1) in the propenyl group-containing composition of the present invention is preferably 85.0 to 99.8% by mass, more preferably 90.0 to 99.5% by mass.

[0038] In the propenyl group-containing composition of the present invention, a propenyl group-containing compound (2) described below remains in the propenylation reaction for producing a propenyl group-containing compound (1). The contents of the propenyl group-containing compound (1) and the propenyl group-containing compound (2) described below can be controlled, for example, by changing the amount of the solvent in the propenylation reaction. That is, to decrease the amount of propenyl group-containing compound (1) and increase the amount of propenyl group-containing compound (2), for example, the amount of solvent can be increased. Conversely, to increase the amount of propenyl group-containing compound (1) and decrease the amount of propenyl group-containing compound (2), for example, the amount of solvent can be decreased.

[0039] The propenyl group-containing composition of the present invention essentially comprises the propenyl group-containing compound (1) and the propenyl group-containing compound (2) described below, and although a trace amount of impurities may be contained during the production of the propenyl group-containing compound (1), the total content of the propenyl group-containing compound (1) and the propenyl group-containing compound (2) in the propenyl group-containing composition is preferably 70 mass% or more, particularly 80 to 100 mass%. Inevitable impurities during the production of the propenyl group-containing compound (1) can be reduced by purifying the resulting propenyl group-containing composition by washing with water, chromatographic separation, crystallization, etc.

[0040] <Propenyl group-containing compound (2)> The propenyl group-containing composition of the present invention preferably contains 0.1 to 20.0 mass % of a compound having a 2-propenyl group (allyl group) represented by the following formula (2) (hereinafter, may be referred to as "propenyl group-containing compound (2)").

[0041] [ka]

[0042] (In the above formula (2), X and R 1 , R 2 has the same meaning as in the above formula (1).

[0043] The propenyl group-containing composition of the present invention tends to have a lower melt viscosity as the propenyl group-containing compound (2) is more abundant, and tends to have a longer curing time of a curable resin composition containing the propenyl group-containing composition as the propenyl group-containing compound (2) is less abundant. From this viewpoint, the content of the propenyl group-containing compound (2) in the propenyl group-containing composition of the present invention is preferably 0.2 to 10.0 mass%, more preferably 0.3 to 5.0 mass%.

[0044] <Melt viscosity> The propenyl group-containing composition of the present invention preferably has a melt viscosity at 150°C of 0.01 to 10.0 P, more preferably 0.05 to 5 P, and even more preferably 0.1 to 3 P. If the melt viscosity is equal to or less than the upper limit, the composition is easily mixed with a maleimide resin or epoxy resin, which will be described later, due to its low viscosity. If the melt viscosity is equal to or more than the lower limit, bleeding out is unlikely to occur when the composition is molded into a mold or the like. The melt viscosity of the propenyl group-containing composition is measured by the method described in the Examples section below.

[0045] <Softening point> The softening point of the propenyl group-containing composition of the present invention is preferably 30 to 100° C., more preferably 35 to 80° C., and even more preferably 40 to 70° C. If the softening point is equal to or higher than the above lower limit, blocking is unlikely to occur, and if the softening point is equal to or lower than the above upper limit, the composition will flow in a short time when heated. The softening point of the propenyl group-containing composition is measured by the method described in the Examples section below.

[0046] <Production of Propenyl Group-Containing Composition> The method for producing the propenyl group-containing composition of the present invention is not particularly limited, but examples thereof include a method in which a dihydric phenol compound represented by the following formula (3) (hereinafter may be abbreviated as "dihydric phenol compound (3)") is allylated to obtain an allyloxy group-containing compound represented by the following formula (4) (hereinafter may be abbreviated as "allyloxy group-containing compound (4)"), and then the allyl group of the allyloxy group-containing compound (4) is transferred to obtain the above-mentioned propenyl group-containing compound (2), and the allyl group of this propenyl group-containing compound (2) is converted to a 1-propenyl group to obtain the propenyl group-containing composition of the present invention.

[0047] [ka]

[0048] (In the above formulas (3) and (4), X and R 1 , R 2 has the same meaning as in the above formula (1).

[0049] An example of a method for allylation of the dihydric phenol compound (3) is a method in which the dihydric phenol compound (3) is reacted with an allyl halide to convert at least a portion of the hydroxyl groups into an allylic ether, i.e., -O-CH-CH=CH.

[0050] In this reaction, the allyl halide is preferably used in an amount of 2.0 to 8.0 times by mole, particularly 3.0 to 6.0 times by mole, based on the dihydric phenol compound (3), from the viewpoints of efficiently proceeding with the reaction and reducing production costs.

[0051] The allyl etherification reaction of the dihydric phenol compound (3) with an allyl halide is preferably carried out in the presence of a catalyst.

[0052] Examples of catalysts for the allyl etherification reaction include alkali metals such as sodium hydroxide, potassium hydroxide, and potassium carbonate, amines such as diazabicyclononene, diazabicycloundecene, and triethylamine, sodium tert-butoxide, potassium tert-butoxide, lithium diisopropylamide, silicon-basic amines, and lithium tetramethylpiperidine. Among these, alkali metals, diazabicyclononene, and diazabicycloundecene are preferred because they are relatively inexpensive and do not easily cause side reactions. The catalyst may be used alone or in combination of two or more.

[0053] The amount of the catalyst used in the allyl etherification reaction is preferably 0.7 to 2.0 times, more preferably 0.8 to 1.5 times, by mole relative to the amount of the allyl halide used. If the amount of the catalyst used is too small, the reaction rate is slow, whereas if the amount used is too large, the excess alkali must be removed, resulting in reduced productivity.

[0054] The allyl etherification reaction is preferably carried out in the presence of a solvent. Examples of the solvent for the allyl etherification reaction include the polar solvents used in the propenylation reaction described below.

[0055] The reaction temperature for the allyl etherification reaction is not particularly limited as long as the hydroxyl group of the dihydric phenol compound (3) reacts with the allyl halide, and is preferably 10 to 150°C, more preferably 40 to 130°C.

[0056] After the allyl etherification reaction, the reaction product may be subjected to treatments such as removal of unreacted raw materials by distillation or the like, concentration, purification (washing, column chromatography, etc.), etc., as necessary.

[0057] The transfer of the allyl group of the allyloxy group-containing compound (4) obtained by the allylation of the dihydric phenol compound (3) can be carried out, for example, by the Claisen rearrangement reaction by heating the allyloxy group-containing compound (4) after the allylation reaction. By the Claisen rearrangement reaction, the allyl group of the allyloxy group (-O-CH2-CH=CH2) bonded to the benzene ring of the allyloxy group-containing compound (4) is transferred to the ortho position of the position where the allyloxy group was previously located.

[0058] The Claisen rearrangement reaction may be carried out according to a conventional method, for example, the allyloxy group-containing compound (4) is heated in the presence of a high boiling point solvent such as carbitol, paraffin oil, N,N'-dimethylaniline, N,N'-diethylaniline, or the like, or in the absence of a solvent. The solvent is used as necessary in an amount of 10 to 200 parts by mass per 100 parts by mass of the allyloxy group-containing compound (4). After the reaction is completed, the solvent used can be removed as necessary to obtain the propenyl group-containing compound (2). After the reaction, the propenyl group-containing compound (2) can be recovered by dropping the reaction solution into an aqueous sodium hydroxide solution, dropping the separated aqueous layer into an acid solution, and stirring.

[0059] The heating temperature during the Claisen rearrangement reaction is preferably 150 to 220° C., more preferably 170 to 200° C., and further preferably a rearrangement reaction in the presence of an inert gas such as nitrogen. If the heating temperature is equal to or higher than the lower limit, the rearrangement reaction of the allyl group is likely to occur. If the heating temperature is equal to or lower than the upper limit, polymerization of the allyl group is unlikely to occur.

[0060] After the reaction, the reaction product may be subjected to a treatment such as washing with water, if necessary.

[0061] The dropwise addition time into the aqueous sodium hydroxide solution after the reaction is preferably 10 to 30 minutes. If the dropwise addition time is equal to or more than the above lower limit, heat generation due to mixing is suppressed and safe production can be achieved. If the dropwise addition time is equal to or less than the above upper limit, productivity is improved. The stirring time after dropwise addition into the acid solution is preferably 15 to 60 minutes. If the stirring time is equal to or more than the above lower limit, the neutralization reaction proceeds and the yield in the subsequent separation step is improved. If the stirring time is equal to or less than the above upper limit, productivity is improved.

[0062] As a method for converting the allyl group of the propenyl group-containing compound (2) into a 1-propenyl group, there may be mentioned a method in which the propenyl group-containing compound (2) is dissolved in a solvent and heated in the presence of a propenylation catalyst.

[0063] The solvent used in the propenylation reaction may be any solvent capable of dissolving the propenyl group-containing compound (2), and typically includes polar solvents. Examples of polar solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, methanol, ethanol, butanol, ethyl acetate, butyl acetate, methyl cellosolve, ethyl diglycol acetate, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and tetrahydrofuran. As the solvent, one type may be used alone, or two or more types may be used in combination.

[0064] The solvent is preferably used in an amount of 20 to 900 parts by mass, particularly 50 to 600 parts by mass, per 100 parts by mass of the propenyl group-containing compound (2).

[0065] Examples of catalysts for the propenylation reaction include alkali metals such as sodium hydroxide and potassium hydroxide, amines such as diazabicyclononene, diazabicycloundecene, triethylamine, sodium tert-butoxide, potassium tert-butoxide, lithium diisopropylamide, silicon-basic amines, and lithium tetramethylpiperidine. Among these, potassium hydroxide and sodium hydroxide are preferred because they are relatively inexpensive and do not easily cause side reactions. The catalyst may be used alone or in combination of two or more.

[0066] The amount of the catalyst used in the propenylation reaction is preferably 0.4 to 6.0 times, more preferably 1.0 to 4.0 times, by mole relative to the total molar amount of hydroxyl groups in the propenyl group-containing compound (2). If the amount of the catalyst used is too small, the propenylation reaction does not proceed easily, whereas if the amount used is too large, the excess alkali must be removed, resulting in reduced productivity.

[0067] The reaction temperature of the propenylation reaction is preferably 40 to 140° C., more preferably 70 to 120° C. If the reaction temperature is equal to or higher than the lower limit, the propenylation reaction is likely to proceed. If the reaction temperature is equal to or lower than the upper limit, polymerization of the propenyl group is unlikely to occur.

[0068] After the propenylation reaction, the reaction product may be subjected to treatments such as removal of unreacted raw materials by distillation or the like, concentration, purification (washing, column chromatography, etc.), and the like, if necessary.

[0069] In the present invention, the propenyl group-containing compound (1) after the propenylation reaction and the propenyl group-containing compound (2) may be blended to form the propenyl group-containing composition of the present invention.

[0070] [Curable resin composition] The curable resin composition of the present invention contains the propenyl group-containing composition of the present invention described above and one or more resins selected from the group consisting of epoxy resins, maleimide resins, phenolic resins, benzoxazine resins, cyanate ester resins, active ester resins, resins having a radically polymerizable functional group, isocyanate resins, acid anhydride resins, and carbodiimide resins (hereinafter, these may be referred to as "curing components"), and the curing component is preferably one or more resins selected from the group consisting of epoxy resins, maleimide resins, and phenolic resins.

[0071] In the curable resin composition of the present invention, the 1-propenyl group or allyl group of the propenyl group-containing composition of the present invention reacts with the maleimide group of the maleimide resin under certain conditions, whereby curing proceeds. Thus, in the present invention, the propenyl group-containing composition functions as a curing agent for the maleimide resin. In the case of epoxy resins, the curing reaction proceeds by reacting the hydroxyl groups of the propenyl group-containing composition of the present invention with the epoxy groups of the epoxy resin. In this case too, the propenyl group-containing composition functions as a curing agent for the epoxy resin. The phenolic resin can also be used in combination with an epoxy resin. The curable resin composition of the present invention preferably contains an epoxy resin as a curing component, particularly when used as a semiconductor encapsulant, because the cured product has excellent adhesion and the curing reaction is easily promoted to increase the molecular weight of the cured product.

[0072] In the curable resin composition of the present invention, the content of the curing component is 0.01 to 1000 parts by mass, preferably 0.1 to 500 parts by mass, and more preferably 1.0 to 300 parts by mass, based on 100 parts by mass of the propenyl group-containing composition of the present invention. If the content of the curing component is equal to or higher than the lower limit, a cured product having excellent heat resistance and good adhesiveness can be obtained. If the content of the curing component is equal to or lower than the upper limit, a uniform cured product having excellent curability can be produced.

[0073] <Curing component> Each curing component contained in the curable resin composition of the present invention will be described below.

[0074] <Maleimide resin> The maleimide resin is a maleimide compound having an average of one or more maleimide groups per molecule. Examples of the maleimide resin include bismaleimides having two maleimide groups per molecule, polyphenylmethanemaleimide, and the like.

[0075] Examples of bismaleimides include alkyl bismaleimide, diphenylmethane bismaleimide, phenylene bismaleimide, bisphenol A diphenyl ether bismaleimide, 4,4'-diphenylmethane bismaleimide such as 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6'-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenylsulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, and 1,3-bis(4-maleimidophenoxy)benzene. Polyphenylmethanemaleimide is a polymer in which three or more benzene rings substituted with maleimide groups are linked via methylene groups.

[0076] Of the above-mentioned maleimide resins, 4,4'-diphenylmethane bismaleimide and polyphenylmethane maleimide are preferred as the maleimide resin, because they have excellent compatibility with the propenyl group-containing composition of the present invention and are relatively inexpensive.

[0077] The maleimide resin may be a commercially available product. Examples of commercially available maleimide resins include "BMI-1100" (4,4'-diphenylmethane bismaleimide) and "BMI-2300" (polyphenylmethane maleimide), both manufactured by Daiwa Kasei Kogyo Co., Ltd.

[0078] The maleimide resin may be used alone or in combination of two or more kinds.

[0079] <Epoxy resin> The epoxy resin is not particularly limited, and examples thereof include phenol novolac type epoxy resins, orthocresol novolac type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenol type epoxy resins, naphthalene type epoxy resins, anthracene type epoxy resins, naphthol type epoxy resins, xylylene type epoxy resins, biphenyl type epoxy resins, triphenylmethane type epoxy resins, dicyclopentadiene type epoxy resins, stilbene type epoxy resins, sulfur atom-containing epoxy resins, phosphorus atom-containing epoxy resins, and the like.

[0080] As the epoxy resin, an epoxy resin in which at least a part of the hydroxyl groups of the propenyl group-containing composition is epoxidized may be used. The hydroxyl groups can be epoxidized by a known method. For example, by reacting the propenyl group-containing composition with epichlorohydrin, an epoxy resin having a structure in which some or all of the hydroxyl groups of the propenyl group-containing composition are -OZ (wherein Z is a glycidyl group) can be obtained.

[0081] The epoxy resin may be used alone or in combination of two or more kinds.

[0082] <Phenol resin> Examples of phenolic resins include novolak-type phenolic resins obtained by condensing or co-condensing phenols such as phenol, cresol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, and aminophenol, and / or naphthols such as α-naphthol, β-naphthol, and dihydroxynaphthalene with compounds having an aldehyde group such as formaldehyde, benzaldehyde, and salicylaldehyde under an acidic catalyst; phenol-aralkyl resins synthesized from phenols and / or naphthols and dimethoxy-paraxylene or bis(methoxymethyl)biphenyl; and biphenylene-type phenolic resins. These include aralkyl-type phenolic resins such as phenol aralkyl resins and naphthol aralkyl resins; dicyclopentadiene-type phenolic resins such as dicyclopentadiene-type phenolic novolac resins and dicyclopentadiene-type naphthol novolac resins, which are synthesized by copolymerizing phenols and / or naphthols with dicyclopentadiene; triphenylmethane-type phenolic resins; terpene-modified phenolic resins; paraxylylene and / or metaxylylene-modified phenolic resins; melamine-modified phenolic resins; cyclopentadiene-modified phenolic resins; and phenolic resins obtained by copolymerizing two or more of these.

[0083] The phenol resin may be used alone or in combination of two or more kinds.

[0084] <Benzoxazine resin> Examples of benzoxazine resins include 6,6-(1-methylethylidene)bis(3,4-dihydro-3-phenyl-2H-1,3-benzoxazine), 6,6-(1-methylethylidene)bis(3,4-dihydro-3-methyl-2H-1,3-benzoxazine), etc. The benzoxazine resin may contain a structure in which the oxazine ring is ring-opened and polymerized. The benzoxazine resin may be used alone or in combination of two or more kinds.

[0085] <Cyanate ester resin> Examples of cyanate ester resins include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate (oligo(3-methylene-1,5-phenylene cyanate)), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine.

[0086] The cyanate ester resin may be used alone or in combination of two or more kinds.

[0087] <Active ester resin> The active ester resin is not particularly limited, but generally, compounds having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, are preferably used. The active ester resin is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester resin obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of the phenol compound or naphthol compound include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compound, phenol novolak, etc. Here, the term "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0088] Specifically, active ester resins containing a dicyclopentadiene-type diphenol structure, active ester resins containing a naphthalene structure, active ester resins containing an acetylated product of phenol novolac, and active ester resins containing a benzoylated product of phenol novolac are preferred, and among these, active ester resins containing a naphthalene structure and active ester resins containing a dicyclopentadiene-type diphenol structure are more preferred. Here, the "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.

[0089] The active ester resin may be used alone or in combination of two or more kinds.

[0090] <Resin having radically polymerizable functional groups> The resin having a radical polymerizable functional group includes a resin having one or more ethylenically unsaturated groups having a carbon-carbon double bond in the molecule. The ethylenically unsaturated group is preferably one or more groups selected from the group consisting of an acrylic group, a methacrylic group, a styryl group, an olefin group, and a maleimide group. Preferred examples of the olefin group include an allyl group, a vinyl group, and a propenyl group. Thus, in a preferred embodiment, the radical polymerizable functional group is one or more selected from the group consisting of an acrylic group, a methacrylic group, a styryl group, an allyl group, a vinyl group, a propenyl group, and a maleimide group. The resin having a radically polymerizable functional group may have one or more types of radically polymerizable functional groups.

[0091] The resin having a radically polymerizable functional group may be used alone or in combination of two or more kinds.

[0092] <Isocyanate resin> The isocyanate resin may be a resin having one or more isocyanate groups in the molecule. The isocyanate resin may preferably have two or more isocyanate groups in the molecule. Examples of the isocyanate resin include 4,4'-diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, tolylene diisocyanate, and hexamethylene diisocyanate.

[0093] The isocyanate resin may be used alone or in combination of two or more kinds.

[0094] <Acid anhydride resin> Examples of the acid anhydride resin include resins having one or more acid anhydride groups in the molecule. Examples of the acid anhydride resin include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic dianhydride, and the like. Examples of such anhydrides include water, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid.

[0095] The acid anhydride resin may be used alone or in combination of two or more kinds.

[0096] <Carbodiimide resin> The carbodiimide resin may be a resin having one or more carbodiimide groups (-N=C=N-) in the molecule. The carbodiimide resin preferably has two or more carbodiimide groups in the molecule. Specific examples of the carbodiimide resin include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0097] The carbodiimide resin may be used alone or in combination of two or more kinds.

[0098] <Other ingredients> The curable resin composition of the present invention may contain one or more other components in addition to the propenyl group-containing composition of the present invention and the above-mentioned curing component, such as a curing accelerator, an inorganic filler, a solvent, a release agent, a surface treatment agent, a colorant, a thermoplastic polymer, an organic filler, and a flame retardant.

[0099] Examples of the curing accelerator include a curing accelerator that accelerates the curing reaction between the propenyl group-containing composition of the present invention and a maleimide resin (hereinafter also referred to as "curing accelerator (P)"), and a curing accelerator that accelerates the curing reaction between the propenyl group-containing composition of the present invention and an epoxy resin other than the curing accelerator (P) (hereinafter also referred to as "curing accelerator (Q)").

[0100] Examples of the curing accelerator (P) include imidazoles and organic peroxides. When the curable resin composition contains an epoxy resin, the curing reaction between the propenyl group-containing composition of the present invention and the epoxy resin is also accelerated by using an imidazole as the curing accelerator (P).

[0101] Examples of imidazoles include 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2,4-dimethylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-vinyl-2-methylimidazole, 1-propyl-2-methylimidazole, 2-isopropylimidazole, 1-cyanomethyl-2-methyl-imidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, and 1-cyanoethyl-2-phenylimidazole.

[0102] Examples of organic peroxides include ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, and peroxyesters.

[0103] The curing accelerator (P) is preferably one which is relatively stable at high temperatures, has good solvent solubility, and is easy to handle. Among imidazoles, 2-ethyl-4-methylimidazole is preferred, and among organic peroxides, dicumyl peroxide, a dialkyl peroxide, is preferred.

[0104] These curing accelerators (P) may be used alone or in combination of two or more.

[0105] When the curable resin composition of the present invention contains the curing accelerator (P), the content thereof is preferably 0.1 to 5.0% by mass relative to the maleimide resin.

[0106] The curing accelerator (Q) is not particularly limited, and examples thereof include phosphorus compounds, tertiary amines, organic acid metal salts, Lewis acids, and amine complex salts.

[0107] Examples of the phosphorus-based compounds include triphenylphosphine, tris-2,6-dimethoxyphenylphosphine, tri-p-tolylphosphine, and triphenyl phosphite. Examples of the tertiary amine include 2-dimethylaminomethylphenol, benzyldimethylamine, α-methylbenzyldimethylamine, and 1,8-diazabicyclo[5.4.0]undecene-7.

[0108] As the curing accelerator (Q), a phosphorus-based compound, particularly triphenylphosphine, is preferred, since it has superior curability, heat resistance, and electrical properties, and is less susceptible to deterioration in moisture resistance reliability.

[0109] These curing accelerators (Q) may be used alone or in combination of two or more.

[0110] When the curable resin composition of the present invention contains the curing accelerator (Q), the content thereof is preferably 0.1 to 5% by mass based on the epoxy resin.

[0111] Examples of inorganic fillers include crystalline silica powder, fused silica powder, quartz glass powder, talc, calcium silicate powder, zirconium silicate powder, alumina powder, calcium carbonate powder, etc. Among these, crystalline silica powder and fused silica powder are preferred. The inorganic fillers may be used alone or in combination of two or more.

[0112] When the curable resin composition of the present invention contains an inorganic filler, the content thereof is preferably 30 to 90% by mass based on the entire curable resin composition.

[0113] When the curable resin composition of the present invention is used as a thermosetting molding material for forming an encapsulant, the curable resin composition of the present invention preferably contains a curing accelerator and an inorganic filler.

[0114] The curable resin composition of the present invention can be made into a resin varnish by blending a solvent and dissolving the curing component such as maleimide resin or epoxy resin in the solvent. The solvent is not particularly limited as long as it dissolves the propenyl group-containing composition, the curing component, etc., and typically, a polar solvent is used. Examples of the polar solvent include the same ones as those mentioned in the explanation of the propenylation reaction. The solvent may be used alone or in combination of two or more kinds.

[0115] The resin varnish contains as essential components the propenyl group-containing composition of the present invention, a curing component such as a maleimide resin or an epoxy resin, and a solvent. This resin varnish can be used to produce a laminate, such as a copper-clad laminate, as described below.

[0116] The content of the solvent in the resin varnish is appropriately set according to the solid content of the resin varnish, which, although differing depending on the application, is preferably 30 to 80 mass %, more preferably 40 to 70 mass %. The solid content concentration of the resin varnish is the ratio of the mass of the resin varnish excluding the solvent to the total mass of the resin varnish.

[0117] The resin varnish can be produced by mixing a curing component such as a maleimide resin or an epoxy resin, the propenyl group-containing composition of the present invention, and other components and a solvent that are blended as necessary. The mixing of each component can be carried out by a conventional method.

[0118] In producing the resin varnish, a curing component such as a maleimide resin, the propenyl group-containing composition of the present invention, and a solvent may be mixed, and then the maleimide resin etc. may be pre-reacted with the propenyl group-containing composition of the present invention. By carrying out the pre-reaction in the varnish state, it is possible to prevent the maleimide resin etc., which has high crystallinity, from precipitating from the resin varnish.

[0119] The reaction temperature during the pre-reaction is preferably 50 to 150° C., more preferably 70 to 130° C., and even more preferably 80 to 120° C. If the reaction temperature is too low, the reaction does not proceed smoothly. If the reaction temperature is too high, it becomes difficult to control the reaction, and it becomes difficult to stably obtain a resin varnish.

[0120] Examples of the release agent include various waxes such as carnauba wax. The surface treatment agent may be a known silane coupling agent. The colorant may be carbon black or the like.

[0121] Examples of thermoplastic polymers include polyethylene, polypropylene, polystyrene, polyphenylene ether resin, phenoxy resin, polycarbonate resin, polyester resin, polyamide resin, polyamideimide resin, polyimide resin, xylene resin, polyphenylene sulfide resin, polyetherimide resin, polyether ether ketone resin, polyetherimide resin, silicone resin, and tetrafluoroethylene resin.

[0122] Examples of organic fillers include resin fillers having a uniform structure made of polyethylene, polypropylene, polystyrene, polyphenylene ether resin, silicone resin, tetrafluoroethylene resin, etc., and resin fillers having a core-shell structure having a rubber-like core layer made of an acrylate resin, a methacrylate resin, a conjugated diene resin, etc., and a glassy shell layer made of an acrylate resin, a methacrylate resin, an aromatic vinyl resin, a vinyl cyanide resin, etc.

[0123] Examples of the flame retardant include halogen-containing flame retardants containing bromine or chlorine; phosphorus-based flame retardants such as triphenyl phosphate, tricresyl phosphate, tris-dichloropropyl phosphate, phosphate ester compounds, and red phosphorus; nitrogen-based flame retardants such as guanidine sulfamate, melamine sulfate, melamine polyphosphate, and melamine cyanurate; phosphazene-based flame retardants such as cyclophosphazene and polyphosphazene; and inorganic flame retardants such as antimony trioxide.

[0124] The curable resin composition of the present invention is preferably cured by controlling the curing temperature to 150 to 250° C. One example of the curing operation is a method in which curing is first performed at the suitable curing temperature for 30 seconds to 3 hours, and then post-curing is performed at the suitable curing temperature for 1 to 20 hours.

[0125] The propenyl group contained in the curable resin composition of the present invention, i.e., the propenyl group possessed by the propenyl group-containing compound (1) in the propenyl group-containing composition of the present invention, is more likely to react with the maleimide group contained in the maleimide resin than the allyl group. Therefore, the curable resin composition of the present invention has a high curing rate and excellent curability. In addition, since the curable resin composition of the present invention has a high curing rate, it is not necessary to use a curing accelerator such as an organic peroxide, which requires careful handling. By not blending a curing accelerator into the curable resin composition of the present invention, the handling property is improved.

[0126] The hydroxyl group contained in the curable resin composition of the present invention, i.e., the hydroxyl group of the propenyl group-containing compound (1) in the propenyl group-containing composition of the present invention, reacts with the epoxy group of the epoxy resin. The reaction rate of the reaction between the hydroxyl group and the epoxy group can be accelerated by the presence of a curing accelerator such as triphenylphosphine. When cured with the epoxy resin, the propenyl group of the propenyl group-containing compound (1) undergoes a self-polymerization reaction, and the crosslinked structure formed by the self-polymerization has hydrophobicity and flexibility, so that the water absorption of the cured product is reduced and the adhesive strength is improved.

[0127] Since the curing of the curable resin composition containing the maleimide resin is usually performed by heating at a high temperature of 80 to 250°C, in the conventional curable resin composition, a part of the resin component may volatilize during curing, resulting in voids in the cured product. However, in the curable resin composition of the present invention, since the propenyl group-containing composition of the present invention is used, the curing reaction is fast, so that volatilization is unlikely to occur during curing. Therefore, voids are unlikely to occur in the cured product, and the defective rate in the production of electronic components and the like is reduced, resulting in high productivity. In addition, by using the propenyl group-containing composition of the present invention, a highly hydrophobic crosslinked structure is formed, the water absorption of the cured product is reduced, and cracks are unlikely to occur even when electronic components and the like using the cured product are subjected to high temperature.

[0128] The curable resin composition of the present invention containing the propenyl group-containing composition of the present invention has a high density per unit weight of the propenyl groups in the propenyl group-containing compound (1) and a high density of the crosslinked structure upon curing, and therefore the cured product has excellent heat resistance. In this way, by using the curable resin composition of the present invention, a cured product having excellent heat resistance and low water absorption can be formed in a short time while suppressing the occurrence of voids, and laminates, sealing materials, etc. can be produced with high productivity.

[0129] Applications of the curable resin composition of the present invention will be described further below, but examples thereof include sealing materials for electronic components such as semiconductors, electrical insulating materials, resins for copper-clad laminates, resists, resins for color filters of liquid crystals, various coating agents, adhesives, build-up laminate materials, fiber-reinforced plastics (FRP), and the like.

[0130] The curable resin composition of the present invention may be used after curing for these applications, or may be cured during the manufacturing process applied to these applications.

[0131] [Cured product] The cured product of the present invention can be obtained by curing the curable resin composition of the present invention. The cured product of the present invention obtained by curing the curable resin composition of the present invention has excellent properties in curability, crack resistance, heat resistance, low water absorption, adhesion, low linear expansion, moldability, and strength.

[0132] The method for curing the curable resin composition of the present invention is not particularly limited, but a cured product can usually be obtained by a thermosetting reaction by heating. During the thermosetting reaction, it is preferable to appropriately select the curing temperature depending on the type of curing component used. For example, when a maleimide resin is used, the curing temperature is usually 80 to 250°C, and when an epoxy resin is used, the curing temperature is usually 100 to 200°C. It is also possible to lower the curing temperature by adding a curing accelerator to these curing components. The curing reaction time is preferably 1 to 20 hours, more preferably 2 to 18 hours, and even more preferably 3 to 15 hours. If the reaction time is equal to or more than the lower limit, the curing reaction tends to proceed sufficiently, which is preferable. On the other hand, if the reaction time is equal to or less than the upper limit, it is preferable because deterioration due to heating and energy loss during heating are easily reduced.

[0133] [Application] The curable resin composition of the present invention has excellent curability, and a cured product using the curable resin composition of the present invention has excellent crack resistance, heat resistance, low water absorbency, adhesion, toughness, low linear expansion and moldability.

[0134] Therefore, the propenyl group-containing composition, the curable resin composition and the cured product thereof of the present invention can be effectively used in any application where these physical properties are required. For example, the propenyl group-containing composition, the curable resin composition and the cured product thereof can be suitably used in any application where these physical properties are required. For example, the propenyl group-containing composition, the curable resin composition and the cured product thereof can be suitably used in any application where these physical properties are required, such as optical materials, automotive paints such as electrocoating paints for automobiles, heavy-duty anticorrosive paints for ships and bridges, paints for the inner surface of beverage cans, etc.; composite materials, laminates, semiconductor sealants, liquid insulating sealants, insulating powder paints, coil impregnation, etc. in the electrical and electronic fields; earthquake-resistant reinforcement of bridges, concrete reinforcement, building flooring materials, linings for water facilities, drainage and permeable pavements, adhesives for structures, vehicles and aircraft, etc. in the civil engineering, construction and adhesive fields. Among these, the propenyl group-containing composition, the curable resin composition and the cured product thereof can be effectively used in any application where these physical properties are required, such as optical materials, automotive paints and the like, heavy-duty anticorrosive paints for ships and bridges, heavy-duty anticorrosive paints for ...

[0135] [Laminate] An example of a method for producing a laminate using the curable resin composition of the present invention is a method in which a laminate including a prepreg having a fibrous substrate impregnated with the resin varnish comprising the curable resin composition of the present invention is heated and pressurized to produce a laminate.

[0136] More specifically, a fibrous substrate is impregnated with a resin varnish, dried, and the solvent is removed to obtain a prepreg. This prepreg is laminated with other substrates as required to form a laminate, which is then cured by heating and pressurizing to obtain a laminate.

[0137] The number of layers of the prepreg in the laminate may be one or more. In the laminate, a base material other than the prepreg may be laminated. Examples of the base material include a metal foil such as a copper foil.

[0138] Examples of fibers constituting the fibrous substrate include inorganic fibers such as glass fibers, carbon fibers, ceramic fibers, and stainless steel fibers; natural fibers such as cotton, hemp, and paper; and synthetic organic fibers such as polyester resins and polyamide resins. Any one of these fibers may be used alone, or two or more of them may be used in combination.

[0139] The shape of the fibrous base material is not particularly limited, and examples thereof include staple fibers, yarns, mats, sheets, and the like.

[0140] The amount of resin varnish to be impregnated into the fibrous base material is not particularly limited, and for example, the solid content of the resin varnish to be impregnated is set to about 30 to 50 mass % with respect to the fibrous base material (100 mass %). The heating temperature when the laminate is heated and pressed is preferably the above-mentioned curing temperature. 2 is preferred.

[0141] The laminate thus manufactured includes a fiber-reinforced resin layer including a fibrous base material and a cured product of a resin varnish. The number of fiber-reinforced resin layers included in the laminate may be one layer or two or more layers. As described above, the laminate may include a metal foil layer such as a copper foil.

[0142] [Sealing material] When the curable resin composition of the present invention is used as an encapsulant, the shape of the encapsulant to which the curable resin composition of the present invention is applied is not particularly limited, and for example, a shape similar to that used in known semiconductors, etc. can be adopted. Examples of a method for forming an encapsulant using the curable resin composition of the present invention include methods for encapsulating a semiconductor using transfer molding, compression molding, or the like. EXAMPLES

[0143] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values ​​of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0144] [Materials used] The compounds and resins used in the following examples and comparative examples are as follows.

[0145] Other propenyl resins: Propylene derivatives of phenol biphenylene resins represented by the following structural formula (Gun-ei Chemical Industry Co., Ltd. "BPN-01S")

[0146] [ka]

[0147] Maleimide resin: Polyphenylmethanemaleimide represented by the following structural formula ("BMI-2300" manufactured by Daiwa Kasei Kogyo Co., Ltd.)

[0148] [ka]

[0149] Phenolic resin: Phenol novolac represented by the following structural formula (Gun-ei Chemical Industry Co., Ltd. "PSM4261")

[0150] [ka]

[0151] Epoxy resin: Tetramethylbiphenyl type epoxy resin represented by the following structural formula ("YX4000" manufactured by Mitsubishi Chemical Corporation)

[0152] [ka]

[0153] Curing accelerator: Triphenylphosphine

[0154] [Example 1: Preparation of propenyl group-containing composition] <Allylation> In a 10L autoclave, 840mL of N,N-dimethylformamide, 575g (7.51mol) of allyl chloride, 1245g (9.01mol) of potassium carbonate, and 280g (1.50mol) of biphenol were added and sealed, and the mixture was heated to 40°C, and then heated to 65°C over 1 hour. After aging at 65°C for 5 hours, the mixture was cooled to room temperature and the autoclave was opened. 1678g of water and 1600g of methyl isobutyl ketone were added to dissolve inorganic salts and crystals, and the water layer was removed by a separation operation. The remaining methyl isobutyl ketone layer was added with 1678g of water and washed with water at 60°C three times, and then methyl isobutyl ketone was distilled off to obtain a compound represented by the following formula (A) (hereinafter referred to as "compound (A)").

[0155] [ka]

[0156] <Claisen rearrangement reaction> Compound (A) 165g (620mmol) and N,N-diethylaniline 825mL were placed in a 2L four-neck flask, heated at 200℃ for 6 hours, and then cooled to room temperature. Next, 495mL of water and 149mL (1.86mol) of 50% by mass sodium hydroxide aqueous solution were placed in a 2L separable flask and cooled to 10℃, and the N,N-diethylaniline solution was added dropwise, stirred for 30 minutes, and then allowed to stand, and the upper and lower layers were extracted. Next, 495mL of water and 93.1g (1.86mol) of concentrated sulfuric acid were placed in a 2L separable flask and cooled to 10℃, and the lower layer extracted in the previous operation was added dropwise and stirred for 1 hour. The precipitated solid was collected by filtration, washed with water, and then dried under reduced pressure to obtain 148 g (1.19 mol, two-stage yield 80.4%) of a propenyl group-containing compound (2) represented by the following formula (2-1) (hereinafter referred to as "compound (2-1)") as a gray solid.

[0157] [ka]

[0158] <Propenylation> 100 parts by mass of compound (2-1) and 100 parts by mass of methanol were charged into a reaction vessel, stirred and dissolved, and then 79 parts by mass of granular potassium hydroxide (purity 85%) was added. After the addition, the methanol was distilled off while heating, and the reaction was carried out for 4 hours while maintaining the internal temperature at 100°C. Then, 203 parts by mass of methyl isobutyl ketone was added, neutralized with sulfuric acid, and repeatedly washed with water. Then, 95 parts by mass of a propenyl group-containing composition containing a compound having a structure represented by the following formula (1-1), which is a propenyl group-containing compound (1) (hereinafter referred to as "compound (1-1)"), was obtained.

[0159] As is apparent from the composition analysis below, this propenyl group-containing composition contains compound (1-1) and a compound represented by the following formula (2-1) (hereinafter referred to as "compound (2-1)").

[0160] [ka]

[0161] The resulting propenyl group-containing composition was subjected to compositional analysis by the following method. In addition, the melt viscosity and softening point were measured by the following methods. The results are shown in Table 1.

[0162] <Compositional Analysis of Propenyl Group-Containing Composition> The propenyl group-containing composition was dissolved in acetone to a concentration of 1% by mass, and analyzed by liquid chromatography under the following conditions. Equipment: Agilent 1100 series Column: Imtakt Unison UK-C18 (4.6mm ID×25cmL×3μm) Column tank temperature: 40℃ UV detection wavelength: 280 nm Mobile phase conditions: pure water / methanol = 25 / 75

[0163] <Measurement of Melt Viscosity of Propenyl Group-Containing Composition> The propenyl group-containing composition was melted on the hot plate of a cone-plate viscometer (manufactured by Tokai Yagami Co., Ltd.) adjusted to 150° C., and the melt viscosity was measured at a rotation speed of 750 rpm.

[0164] <Measurement of Softening Point of Propenyl Group-Containing Composition> The softening point of the propenyl group-containing composition was measured in accordance with JIS K7234.

[0165] [Example 2: Preparation of propenyl group-containing composition] The same procedure was carried out as in Example 1, except that the sulfuric acid used for neutralization in <propenylation> was changed to hydrochloric acid. The results are shown in Table 1.

[0166] [Example 3: Preparation of propenyl group-containing composition] The same procedure was carried out as in Example 1, except that the 100 parts by mass of methanol used in <Propenylation> was replaced by 900 parts by mass of dimethyl sulfoxide, and the 79 parts by mass of potassium hydroxide was replaced by 337 parts by mass of potassium t-butoxide. The results are shown in Table 1.

[0167] Comparative Example 1: Production of propenyl group-containing composition The same procedure as in Example 1 was carried out, except that the temperature during heating and decompression in the <propenylation> was 150° C. The results are shown in Table 1.

[0168] [Example 4: Preparation of propenyl group-containing composition] The same procedure was carried out as in Example 1, except that in the <propenylation>, 100 parts by mass of compound (2-1) was replaced with 100 parts by mass of compound (2-2) (DABPA, manufactured by Daiwa Chemical Industry Co., Ltd.). The results are shown in Table 2. As is clear from the composition analysis below, the propenyl group-containing composition obtained in Example 4 contains a compound represented by the following formula (1-2) (hereinafter referred to as "compound (1-2)") and a compound represented by the following formula (2-2) (hereinafter referred to as "compound (2-2)").

[0169] [ka]

[0170] [Table 1]

[0171] [Table 2]

[0172] [Example 5] The propenyl group-containing composition produced in Example 1 and a maleimide resin were mixed in the ratio shown in Table 3 to obtain a curable resin composition, and then a curing reaction was carried out at 120°C for 2 hours and then at 200°C for 6 hours to produce a cured product. The obtained cured product was measured for Tg (tan δ) and storage modulus E' (250°C) and E' (40°C) by the method described below. In addition, the shear adhesive strength to metal (Cu) was measured using the produced curable resin composition. The results are shown in Table 3.

[0173] [Example 6] The propenyl group-containing composition produced in Example 4 was mixed with a maleimide resin in the ratio shown in Table 3 to obtain a curable resin composition, and then a curing reaction was carried out at 120°C for 2 hours and then at 200°C for 6 hours to produce a cured product. The obtained cured product was measured for Tg (tan δ) and storage modulus E' (250°C) and E' (40°C) by the method described below. In addition, the shear adhesive strength to metal (Cu) was measured using the produced curable resin composition. The results are shown in Table 3.

[0174] [Comparative Example 2] Other propenyl resins and maleimide resins were mixed in the ratios shown in Table 3 to obtain curable resin compositions, which were then cured at 120°C for 2 hours and then at 200°C for 6 hours to produce cured products. The obtained cured product was measured for Tg (tan δ) and storage modulus E' (250°C) and E' (40°C) by the method described below. In addition, the shear adhesive strength to metal (Cu) was measured using the produced curable resin composition. The results are shown in Table 3.

[0175] <Cured product: Tg (tan δ) and storage modulus E' (250°C), E' (40°C)> The cured product was cut into a test piece 5 cm long, 1 cm wide, and 4 mm thick, and dynamic viscoelasticity measurements (DMA) were performed under the following conditions. The Tg (tan δ) and the storage modulus (E') at 250°C and 40°C were measured. Analytical equipment: Seiko Instruments EXSTAR6100 Measurement mode: 3-point bending mode Measurement temperature range: 30℃ to 280℃ Heating rate: 5℃ / min Cooling rate: 5℃ / min *The temperature at the peak top of tan δ was defined as Tg(tan δ).

[0176] <Shear adhesive strength to metal> The test was carried out in accordance with JIS-K6850. That is, the curable resin composition was applied between two metal pieces (copper plates (double-sided sandblasted plates manufactured by Yutaka Panel Service Co., Ltd.)) with a width of 25 mm, a length of 100 mm, and a thickness of 1.6 mm, so that the composition had a width of 25 mm and a length of 12.5 mm. After application, the composition was placed in a thermostatic chamber and cured at 120°C for 2 hours and at 175°C for 6 hours to prepare a peel test piece. The prepared peel test pieces were subjected to a tensile shear test at a speed of 5 mm / min (n=3) using a tensile tester "Instron5582" (manufactured by Instron Corporation), and the tensile shear strength was measured and the average value was calculated.

[0177] [Table 3]

[0178] [Example 7, Comparative Examples 3 and 4] The propenyl group-containing composition produced in Example 1, other propenyl resins, or phenolic resins were mixed with epoxy resins and curing accelerators in the formulations shown in Table 4 to obtain a curable resin composition, and then a curing reaction was carried out at 120°C for 2 hours and then at 200°C for 6 hours to produce a cured product. The storage modulus E' (250°C) of the obtained cured product was measured by the method shown above. In addition, the shear adhesive strength to metal (aluminum) was measured in the same manner as above using the obtained curable resin composition, using an aluminum plate (double-sided sandblasted plate manufactured by Yutaka Panel Service Co., Ltd.) instead of a copper plate (double-sided sandblasted plate manufactured by Yutaka Panel Service Co., Ltd.). Furthermore, a water absorption test was carried out on the obtained cured product by the method shown below. The results are shown in Table 4. In Comparative Example 3, the cured product was brittle in the tests for E' (250°C) and water absorption, and the viscosity was too high to prepare test pieces for the test of shear adhesive strength, so evaluation was not possible.

[0179] <Water absorption test> The cured product was cut into a size of 2 cm length, 2 cm width and 4 mm thickness to prepare a test piece, which was then left in a thermo-hygrostat (Nagano Science Co., Ltd. "LH21-11P") under an atmosphere of 85°C / 85% RH for 168 hours. The water absorption rate of the cured product was then calculated from the mass of the test piece before and after water absorption using the following formula. Water absorption rate (%) = {(mass of test piece after water supply - mass of test piece before water supply) / (mass of test piece before water supply)} x 100

[0180] [Table 4]

[0181] [Example 8, Comparative Example 5] According to the formulation shown in Table 5, the propenyl group-containing composition produced in Example 1 or the compound (2-1), a maleimide resin, an epoxy resin, and a curing accelerator were mixed to obtain a curable resin composition, and then a curing reaction was carried out at 200°C for 6 hours to produce a cured product. The storage modulus E' (40°C), storage modulus E' (250°C) and Tg (tan δ) of the obtained cured product were measured by the methods described above. The linear expansion coefficient and weight loss at 200°C were also evaluated by the methods described below. In addition, the obtained curable resin composition was used to measure the shear adhesive strength to metals (copper and aluminum) in the same manner as described above using a copper plate (double-sided sandblasted plate manufactured by Yutaka Panel Service Co., Ltd.) and an aluminum plate (double-sided sandblasted plate manufactured by Yutaka Panel Service Co., Ltd.), and the shear adhesive strength was evaluated according to the following criteria. ○: Shear adhesive strength is 8.0 MPa or more ×: Shear adhesive strength is less than 8.0 MPa Furthermore, the gel time was evaluated by the method described below. These results are shown in Table 5. In Comparative Example 5, the cured product was brittle in the tests for storage modulus E' (40° C.), storage modulus E' (250° C.), and Tg (tan δ), and test pieces could not be prepared and evaluation could not be performed.

[0182] <Evaluation of linear expansion coefficient> The cured product was cut into a cylindrical test piece with a diameter of about 7 mm and a thickness of 4 mm, and a thermomechanical analysis was performed in compression mode using a thermomechanical analyzer (TMA: EXSTAR6000 manufactured by Seiko Instruments Inc.) (measurement load: 30 mN, heating rate: 5°C / min twice, measurement temperature range: 30°C to 3000°C). From the results of the second measurement, the linear expansion coefficient in the temperature range shown in Table 5 was calculated.

[0183] <Evaluation of weight loss at 200℃> The cured product was cut into a rectangular parallelepiped test piece measuring 4 cm in length, 2 cm in width, and 4 mm in thickness, and placed in a heating furnace (Perfect Oven: SPHH-202, manufactured by ESPEC Corp.) and stored isothermally at 200° C. The weight change rate was calculated from the weight of the cured product before heating and the weight of the cured product at the test time shown in Table 5. Weight change rate (%) = -{(mass of test piece after weight change - mass of test piece before weight change) / (mass of test piece before weight change)} x 100

[0184] <Gel time evaluation> 0.1 g of the curable resin composition was placed on a gel time tester (BIG HEART, manufactured by Imoto Manufacturing Co., Ltd.) heated to 175°C, and the time until gelation proceeded (gel time) was measured. The time until gelation proceeded was defined as the time until the curable resin composition lost its fluidity as a liquid at 175°C.

[0185] [Table 5]

[0186] [Evaluation of results] From Table 3, it can be seen that the cured products of Examples 5 and 6, which used the propenyl group-containing composition of Example 1, have superior heat resistance, show smaller changes in elastic modulus, and exhibit high adhesion to metals compared to the cured product of Comparative Example 2, which used another propenyl resin. From Table 4, it can be seen that the cured product of Example 7, which used the propenyl group-containing composition of Example 1, exhibits a lower elastic modulus at high temperatures, lower moisture absorption, and higher adhesion compared to the cured products of Comparative Examples 3 and 4, which used other propenyl resins or phenol resins. From Table 5, it can be seen that the cured product of Example 8, which used the propenyl group-containing composition of Example 1, has a smaller linear expansion coefficient, higher strength, adhesive strength, and thermal decomposition resistance, and also has a shorter gel time and excellent moldability, compared to the cured product of Comparative Example 5, which used compound (2-1).

Claims

1. A propenyl group-containing composition comprising a compound represented by the following formula (1), wherein the content of the compound represented by the formula (1) is 80.0 to 99.9 mass %: [Formula 1] (In the above formula (1), X is a direct bond. R 1 and R 2 are hydrogen atoms, hydrocarbon groups having 1 to 10 carbon atoms, or halogen atoms, and may be the same or different.

2. The propenyl group-containing composition according to claim 1, comprising 0.1 to 20.0 mass% of a compound represented by the following formula (2): [chemical 2] (In the above formula (2), X, R 1 , R 2 has the same meaning as in the above formula (1).

3. 3. The propenyl group-containing composition according to claim 1, wherein the proportion of trans isomers in which both of the two propenyl groups are in the trans form among the compounds represented by formula (1) is 20 to 95%.

4. 4. The propenyl group-containing composition according to claim 1, wherein, among the compounds represented by formula (1), a proportion of cis isomers in which both of the two propenyl groups are cis-type is 30% or less.

5. 5. The propenyl group-containing composition according to claim 1, having a melt viscosity at 150° C. in the range of 0.01 to 10.0 P.

6. A curable resin composition comprising 0.01 to 1000 parts by mass of at least one selected from the group consisting of epoxy resins, maleimide resins, phenolic resins, benzoxazine resins, cyanate ester resins, active ester resins, resins having a radically polymerizable functional group, isocyanate resins, acid anhydride resins, and carbodiimide resins, relative to 100 parts by mass of the propenyl group-containing composition according to any one of claims 1 to 5.

7. A cured product obtained by curing the curable resin composition according to claim 6.

8. An electric / electronic part comprising a cured product of the curable resin composition according to claim 6.

Citation Information

Patent Citations

  • Thermosetting composition

    JP1987181335A

  • Fluorine-containing aromatic compound having alkenyl group and production thereof

    JP1991066639A

  • Curable composition

    JP1992227931A

  • Production of 1-propenyl group-substituted phenols

    JP1993017382A

  • Propenyl group-containing bisphenol derivative

    JP1999140007A