Method for manufacturing silicon-containing member having recess

By applying an active material and fluorine-based gas to silicon-containing members, the method addresses the slow processing speeds of conventional dry etching, enabling rapid and high-aspect-ratio recess formation.

JP7567547B2Active Publication Date: 2024-10-16AGC INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021025628
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-10-16
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Conventional dry etching techniques for forming recesses in silicon-containing members are limited by slow processing speeds, making it difficult to rapidly manufacture such components.

Method used

A method involving the installation of an active material on the surface of a silicon-containing member, followed by the application of a fluorine-based gas in a heated environment to form recesses, which significantly enhances the etching speed.

Benefits of technology

The method allows for the rapid formation of silicon-containing members with recesses at speeds ranging from 1 μm/min to 100 μm/min, enabling high-aspect-ratio microfabrication and large-area patterning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567547000003
    Figure 0007567547000003
  • Figure 0007567547000004
    Figure 0007567547000004
  • Figure 0007567547000005
    Figure 0007567547000005
Patent Text Reader

Abstract

To provide a method capable of rapidly manufacturing a silicon-containing member having a recess.SOLUTION: In a manufacturing method of a silicon-containing member having a recess, (i) an active material is disposed on a part of the surface of a silicon-containing member, (ii) a fluorine-based gas is supplied to the silicon-containing member under a heating environment, and a recess is formed in the surface of the underlying silicon-containing member after (ii).SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a silicon-containing component having a recess. [Background technology]

[0002] There is a need for silicon-containing members having recesses such as grooves and / or holes in various fields. For example, in the field of semiconductors, techniques for forming recesses in silicon substrates and various films formed thereon are widely used.

[0003] Such recesses can be formed, for example, by dry etching. For example, Patent Document 1 describes that a silicon dioxide film or a silicon nitride film can be microfabricated with a high aspect ratio by dry etching technology. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2012 / 008282 Summary of the Invention [Problem to be solved by the invention]

[0005] Dry etching technology can form recesses with high precision on the surface of a silicon-containing member (including a substrate, a film, etc.).

[0006] However, the dry etching technique has a problem in terms of processing speed. For example, in the dry etching technique described in the above-mentioned Patent Document 1, the etching speed of a silicon dioxide film or a silicon nitride film is at most on the order of 200 nm / min. Therefore, the dry etching technique has a problem in that it is difficult to rapidly manufacture a silicon-containing member having a recess.

[0007] The present invention has been made in view of the above background, and an object of the present invention is to provide a method that enables a silicon-containing member having a recess to be produced more quickly. [Means for solving the problem]

[0008] The present invention provides a method for producing a silicon-containing member having a recess, comprising the steps of: (i) placing an activator on a portion of a surface of a silicon-containing component; (ii) supplying a fluorine-based gas to the silicon-containing member in a heated environment; There is provided a manufacturing method in which, after (ii), a recess is formed in the surface of the silicon-containing component below the active material. Effect of the Invention

[0009] The present invention can provide a method that can more quickly manufacture a silicon-containing member having a recess. [Brief description of the drawings]

[0010] [Figure 1] FIG. 2 is a flow diagram illustrating an example of a flow of a method for producing a silicon-containing member having a recess according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram showing an example of a method for applying an active material to a first surface of a silicon-containing component by a photolithography method. [Diagram 3] FIG. 2 is a diagram showing an example of a method for applying an active material to a first surface of a silicon-containing component by a photolithography method. [Figure 4] FIG. 2 is a diagram showing an example of a method for applying an active material to a first surface of a silicon-containing component by a photolithography method. [Diagram 5] FIG. 2 is a diagram showing an example of a method for applying an active material to a first surface of a silicon-containing component by a photolithography method. [Figure 6] FIG. 2 is a schematic diagram illustrating a state in which a processing target object is supported by a holder and accommodated in a processing chamber. [Figure 7] FIG. 2 is a schematic diagram showing a cross section of a silicon-containing member having a recess. [Figure 8] 1 is a graph showing the rate of increase in the amount of etching when substrates coated with various activators are etched with hydrogen fluoride gas. [Figure 9] 1 is a photograph showing a part of a cross section of a substrate coated with manganese dioxide after etching. [Figure 10] FIG. 2 is a top view showing a schematic diagram of a portion of the shape of a pattern of an active material provided on the surface of a substrate. [Figure 11] 4 is a photograph showing an example of a shape of a groove formed according to an embodiment of the present invention. [Figure 12] 1 is a graph showing the relationship between the HF gas concentration during etching and the depth of a recess formed. [Figure 13] 1 is a graph showing the relationship between the etching process time and the depth of the recessed portion formed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, one embodiment of the present invention will be described.

[0012] As described above, there is a problem in that it is difficult to rapidly manufacture a silicon-containing member having a recess using conventional dry etching techniques.

[0013] In order to address such problems, the present inventors have been actively researching and developing a method for more rapidly microfabricating silicon-containing members, and have discovered that when a silicon-containing member is treated under specific conditions with a specific substance (hereinafter referred to as an "activator") placed on the surface of the silicon-containing member, the etching rate of the surface is significantly improved, leading to the present invention.

[0014] Thus, in one embodiment of the present invention, A method for producing a silicon-containing member having a recess, comprising the steps of: (i) placing an activator on a portion of a surface of a silicon-containing component; (ii) supplying a fluorine-based gas to the silicon-containing member in a heated environment; There is provided a manufacturing method in which, after (ii), a recess is formed in the surface of the silicon-containing component below the active material.

[0015] In the present application, the term "silicon-containing member" refers to any object to be processed that contains silicon, such as a silicon-containing substrate and a silicon-containing layer.

[0016] In the present application, the term "depression" refers to a form having a level lower than the level of the target surface of the silicon-containing member. Therefore, the term "depression" includes grooves, holes, and the like.

[0017] In one embodiment of the present invention, recesses can be formed on the surface of a silicon-containing member at a processing speed of the order of 1 μm / min to 100 μm / min, for example. This processing speed can be controlled by the concentration of the fluorine-based gas during processing, the processing time, the processing temperature, the type of activator, and the like.

[0018] Thus, one embodiment of the present invention can produce recessed silicon-containing features more quickly than conventional dry etching techniques.

[0019] At present, the reason why the above-mentioned "high speed" etching process is possible in one embodiment of the present invention is as follows.

[0020] It is known that fluorine (F) radicals dissociated from fluorine-based gases such as hydrogen fluoride gas are more reactive with silicon-containing materials such as glass than hydrogen fluoride gas. However, hydrogen fluoride gas usually has a large bond energy, making it difficult for it to dissociate into F radicals.

[0021] Transition metals, on the other hand, have electrons in their d orbitals and can assume multiple valence states. Transition metals can also easily change to multiple energy states, as is evident from their frequent use as catalysts.

[0022] Therefore, it is believed that when a fluorine-based gas comes into contact with a transition metal, the catalytic action of the transition metal promotes the dissociation of F radicals from the fluorine-based gas.

[0023] It is believed that the promotion of dissociation of such active F radicals allows for a significantly higher etching rate than conventional techniques to be achieved in an environment in which transition metals and fluorine-based gases coexist.

[0024] According to an embodiment of the present invention, a high aspect ratio recess can be formed on the surface of a silicon-containing member relatively easily, and therefore, the embodiment of the present invention can be applied to microfabrication techniques such as deep trenches and / or holes used in the semiconductor field.

[0025] A conventional high-speed recess formation technique is laser processing, which irradiates the surface of a silicon-containing member with laser light and scans the laser light to process high-precision grooves.

[0026] However, the laser processing technique is not suitable for forming a large number of grooves at once in a large-area workpiece.

[0027] In contrast, the manufacturing method according to an embodiment of the present invention can be applied to large-area patterning techniques such as conventional lithography, and therefore can be applied to silicon-containing members having large surfaces.

[0028] (Method for manufacturing a silicon-containing member having a recess according to one embodiment of the present invention) Next, an embodiment of the present invention will be described more specifically with reference to the drawings.

[0029] 1 shows an example of a method for producing a silicon-containing member having a recess according to one embodiment of the present invention (hereinafter referred to as a "first production method"). In the first production method, a silicon-containing member having a groove is produced.

[0030] As shown in FIG. 1, the first manufacturing method includes: (a) placing an active material on a portion of a surface of a silicon-containing component (S110); (b) supplying a fluorine-based gas to the silicon-containing member in a heated environment (S120); has.

[0031] Each step will be described below.

[0032] (Step S110) First, a silicon-containing member is prepared.

[0033] The silicon-containing member may be, for example, in the form of a substrate containing silicon or a layer containing silicon. The silicon contained in the silicon-containing member may be in a metallic state or an oxide state. For example, the silicon-containing member may be a silicon substrate or a glass substrate (e.g., quartz glass).

[0034] In the following description, each step will be described using, as an example, a case in which the silicon-containing member is a glass substrate.

[0035] Next, the active material is prepared.

[0036] The material of the active material is not particularly limited, so long as the portion of the silicon-containing component that comes into contact with the active material is etched in the subsequent step S120.

[0037] For example, the active material may comprise at least one selected from the group consisting of metal halides, transition metals, and transition metal oxides.

[0038] Among these, examples of metal halides include fluorides such as manganese fluoride, iron fluoride, sodium fluoride, and calcium fluoride.

[0039] Examples of the transition metal include niobium, silver, titanium nickel, copper, gold, cobalt, zinc, iron, and manganese. The transition metal is preferably metallic manganese or metallic iron, because these metals exhibit significantly higher activity in the treatment in step S120.

[0040] Examples of the oxides of transition metals include manganese dioxide, iron oxide, zinc oxide, copper oxide, nickel oxide, and chromium oxide.

[0041] Next, an activator is placed on the surface of the silicon-containing component to be treated (hereinafter referred to as the "first surface").

[0042] The method for applying the active material to the first surface of the silicon-containing member is not particularly limited. For example, the active material may be applied to the first surface by a spreading method, a coating method, a printing method, a photolithography method, or the like.

[0043] 2 to 5 show an example of a method for applying an active material to a first surface of a silicon-containing member by photolithography.

[0044] As shown in FIG. 2, the method begins by applying a photoresist layer 120 to a first surface 112 of a silicon-containing component 110 .

[0045] Next, the photoresist layer 120 is patterned into a predetermined shape. As a result, a patterned photoresist 121 is formed as shown in Fig. 3. For example, in the example shown in Fig. 3, a pattern is formed that is made up of a plurality of linear photoresists 121 that extend parallel to each other.

[0046] 4, an active material 130 is applied to the first surface 112 of the silicon-containing member 110. The method for applying the active material 130 is not particularly limited, and a film forming method such as a sputtering method may be used.

[0047] An active material 130 is disposed over the photoresist 121 and the exposed first surface 112 .

[0048] The patterned photoresist 121 is then removed, leaving a linear pattern of active material 130 on the first surface 112, as shown in FIG.

[0049] Hereinafter, the silicon-containing member 110 having the pattern of the active material 130 will be specifically referred to as the “processing target” 140 .

[0050] The thickness of the active material 130 is preferably in the range of, for example, 5 nm to 100 nm.

[0051] By making the thickness of the active material 130 100 nm or less, it is possible to suppress a decrease in the processing speed of the workpiece 140 in the subsequent step S120. Moreover, by making the thickness of the active material 130 5 nm or more, it is possible to process the silicon-containing member 110 at a realistic speed.

[0052] (Process S120) Next, the object to be processed 140 prepared in step S110 is etched.

[0053] Prior to this, the workpiece 140 may be placed in a processing chamber.

[0054] FIG. 6 shows a schematic diagram of a state in which a processing object 140 is supported by a holder 152 and accommodated in a processing chamber 150. As shown in FIG.

[0055] The etching process of the workpiece 140 is performed by supplying a fluorine-based gas to the workpiece 140. For example, in the example shown in FIG.

[0056] The fluorine-based gas is, for example, hydrogen fluoride gas and / or fluorine gas.

[0057] The fluorine-based gas may be supplied alone or in a mixture with other gases into the process chamber 150. For example, the fluorine-based gas may be supplied in a mixture with a carrier gas. The carrier gas may be an inert gas, such as, for example, nitrogen and / or argon gas.

[0058] A fluorine-based gas is supplied into the processing chamber 150, whereby the object to be processed 140 is etched.

[0059] The etching conditions vary depending on the shape of the recesses to be formed, but the processing time is, for example, in the range of 5 seconds to 30 minutes. The concentration of the fluorine-based gas is, for example, in the range of 0.1 vol % to 50 vol %.

[0060] The etching process is preferably performed in a state where the object to be processed 140 or the inside of the processing chamber 150 is heated. The processing temperature is, for example, in the range of 50° C. to 1000° C. However, depending on the type of activator, the processing may be performed at room temperature.

[0061] In the first manufacturing method, the processing speed of the object to be processed 140 can be adjusted by controlling the concentration of the supplied fluorine-based gas, the processing temperature, and the processing time.

[0062] The processing speed may be, for example, in the range of 1 μm / min to 100 μm / min.

[0063] FIG. 7 shows a schematic cross section of the processed object 140, that is, a silicon-containing member 145 having a recessed portion.

[0064] After the processing, groove-shaped recesses 160 are formed on the surface of the workpiece 140 according to the pattern of the active material 130. That is, the recesses 160 are formed below the active material 130 from the first surface 112 of the silicon-containing member 110 toward the opposite surface (second surface) 114.

[0065] Strictly speaking, it should be noted that the surface 142 of the workpiece 140 at this stage is different from the first surface 112 of the silicon-containing member 110 before step S120 is performed. This is because the first surface 112 of the silicon-containing member 110 is also etched, albeit slightly, during the etching process.

[0066] However, typically, the etching rate of first surface 112 in step S120 is on the order of 20 nm / min. Thus, the etching rate of first surface 112 is negligibly small compared to the etching rate underneath active material 130.

[0067] The aspect ratio of the recess 160 can be adjusted to a desired range by controlling the processing conditions. For example, the aspect ratio of the recess 160 can be adjusted to a range of 0.1 to 100. The aspect ratio of the recess 160 is, for example, 1 or more, 10 or more, or 20 or more.

[0068] Here, the aspect ratio is calculated as the depth of the recess to the "smallest dimension" of the opening in the surface, which corresponds to the smallest width of the recess if it is a groove, or the diameter of the circle if it is a circular hole.

[0069] Through the above steps, silicon-containing member 145 having groove-shaped recesses 160 can be manufactured.

[0070] In the first manufacturing method, in step S120, the object to be processed 140 can be processed at a processing speed of, for example, 10 μm / min or more. Therefore, in the first manufacturing method, the silicon-containing member 145 having the recess 160 can be manufactured more quickly than the conventional dry etching method.

[0071] The manufacturing method of the silicon-containing member having a recess according to one embodiment of the present invention has been described above using the first manufacturing method as an example. However, the above description is merely an example, and the manufacturing method according to one embodiment of the present invention may include other steps.

[0072] For example, in the above description, the recesses 160 are configured as a plurality of linear grooves. However, the recesses formed may be non-linear grooves, holes, and / or the like.

[0073] Various other modifications are also possible. EXAMPLES

[0074] Examples of the present invention will now be described.

[0075] (Preliminary Examination) Various active materials (powdered) were uniformly applied onto a quartz glass substrate, which was then placed in a processing chamber. Hydrogen fluoride (HF) gas was then supplied into the processing chamber to etch the substrate.

[0076] The HF gas was mixed with nitrogen gas and supplied. The concentration of the HF gas was 20 vol% (the remainder was nitrogen gas). The temperature of the substrate was 800°C.

[0077] After 60 seconds of treatment, the substrate was taken out and the active material was washed off, after which the weight change (referred to as "W") of the substrate was measured.

[0078] Figure 8 shows the results obtained for each activator. In Figure 8, the vertical axis indicates the increase rate P of the etching amount. This increase rate P is calculated by the following formula (1), where Wr is the weight change obtained when the substrate alone is subjected to HF treatment without applying an activator: Increase rate of etching amount P=W / Wr (1) It can be seen from Figure 8 that the weight change after treatment increases in all cases with the activators selected in this study. In particular, in experiments using manganese dioxide, metallic manganese, metallic iron, manganese fluoride, and iron fluoride as activators, it was found that an extremely large weight change occurred compared to the substrate not coated with an activator.

[0079] FIG. 9 shows a part of a cross section of a substrate after etching when manganese dioxide is used as the activator.

[0080] From Figure 9, it can be seen that semicircular holes corresponding to the particle shape of the applied activator are formed on the surface of the substrate. Similar cross sections were also observed in tests using other activators.

[0081] From these observation results, it was confirmed that the weight loss was caused by the disappearance of the portion of the substrate directly below the active material.

[0082] (Pattern formation test) (Example 1) A quartz glass substrate was etched in the following manner to form a pattern of a plurality of linear grooves extending in parallel on a first surface of the substrate.

[0083] First, a linear pattern of an active material was formed on the first surface of the substrate. Manganese dioxide was used as the active material. The pattern of the active material was provided by the lithography method described above. The active material was deposited on the photoresist by sputtering.

[0084] FIG. 10 shows a schematic representation of a portion of the morphology of the pattern of the active material applied to the first surface of the substrate.

[0085] As shown in FIG. 10, the active material 530 formed on the first surface 512 has the form of a plurality of lines extending parallel to one another.

[0086] The width of the active material 530, ie, the width of each line, was about 10 μm, and the spacing T between the lines was 50 μm. The thickness of the active material 530 was about 10 nm.

[0087] The substrate having the pattern of active material was then etched using HF gas.

[0088] The concentration of HF gas was 20 vol% (the remainder being nitrogen gas), and the treatment temperature was 800° C. The treatment time was 5 seconds.

[0089] After treatment, the substrate was removed and washed.

[0090] As a result, a substrate having a pattern of linear grooves (hereinafter referred to as "Sample 1") was obtained.

[0091] (Example 2 to Example 19) A linear groove pattern was formed on the first surface of the substrate by the same method as in Example 1. However, in Examples 2 to 19, the activator, processing gas, processing time, and / or processing temperature were changed from those in Example 1.

[0092] As a result, Samples 2 to 19 were obtained.

[0093] (Example 20) A linear groove pattern was formed on the first surface of the substrate in the same manner as in Example 1. However, in this Example 20, a silicon substrate was used as the substrate, and the treatment time was 60 seconds.

[0094] This resulted in sample 20.

[0095] (Example 21) A pattern of linear grooves was formed on a first surface of a substrate in the same manner as in Example 20. However, in Example 21, the treatment time was changed from that in Example 20.

[0096] This resulted in sample 21.

[0097] Table 1 below shows the preparation conditions for Samples 1 to 21.

[0098] [Table 1] (evaluation) The cross-sections of each sample were observed using a scanning electron microscope (SEM). The depth and aspect ratio of the grooves formed in each sample were also measured. Furthermore, the etching rate of the HF treatment was calculated from the groove depth.

[0099] The results obtained for Samples 1 to 21 are summarized in Table 2 below.

[0100] [Table 2] It can be seen from Table 2 that all samples had significantly high etching rates. Among samples 1 to 21, sample 15 had the lowest etching rate (0.3 μm / min). However, as described below, the etching rate can be controlled within a desired range by adjusting the HF concentration, processing time, processing temperature, and the like.

[0101] FIG. 11 shows an example of the shape of the grooves formed in Sample 2.

[0102] As is clear from FIG. 11, a groove with an extremely high aspect ratio is formed in Sample 2. The depth of the groove reaches approximately 20 μm. In particular, the treatment time with HF gas in Sample 2 is only 20 seconds. Therefore, in Sample 2, the groove is formed at a significantly high etching rate of 58.5 μm / min.

[0103] Thus, it was confirmed that, in one embodiment of the present invention, trenches with high aspect ratios can be formed more quickly than with conventional dry etching methods.

[0104] Fig. 12 shows the effect of the HF gas concentration during processing on the etching rate, and Fig. 13 shows the effect of processing time on the etching rate.

[0105] Fig. 12 shows the relationship between HF gas concentration and etching rate when the treatment temperature is 800°C, the treatment time is 60 seconds, and a 10 nm thick manganese dioxide is used as the activator. Fig. 13 shows the relationship between HF gas concentration and etching rate when the HF gas concentration is 20 vol%, the treatment temperature is 800°C, and a 10 nm thick manganese dioxide is used as the activator.

[0106] From these figures, it can be seen that the etching rate changes linearly with respect to the HF gas concentration and the treatment time.

[0107] In this way, it was confirmed that the etching rate of the substrate can be controlled by adjusting the conditions during the etching process. [Explanation of symbols]

[0108] 110 Silicon-containing materials 112 First Surface 120 Photoresist layer 121 Patterned Photoresist 130 Activated materials 140 Object to be treated 142 Surface of the object to be treated 145 Silicon-containing member having a recess 150 Processing chamber 152 Holder 160 Recess 512 First Surface 530 Activated material

Claims

1. A method for producing a member including silicon in an oxidized state having a recess, comprising: (i) placing an activator on a portion of a surface of a component containing silicon in an oxide state; (ii) supplying a fluorine-based gas to the member containing silicon in an oxide state in a heated environment; The manufacturing method, wherein after (ii), a recess is formed in the surface of the member containing silicon in an oxide state below the active material.

2. The method of claim 1 , wherein the active material comprises at least one selected from the group consisting of metal halides, transition metals, and transition metal oxides.

3. The method of claim 2 , wherein the active material comprises at least one of manganese dioxide, manganese fluoride, manganese metal, iron metal, and iron fluoride.

4. The method according to claim 1 , wherein the fluorine-based gas includes fluorine gas and / or hydrogen fluoride gas.

5. The method according to claim 1 , wherein the member containing silicon in an oxide state is a glass substrate.

6. The method according to claim 1 , wherein the recess is a groove or a hole.

7. When the depth of the recess is d and the minimum dimension of the opening of the recess on the surface is A, The method according to claim 6, wherein the aspect ratio of the recess, expressed as d / A, is in the range of 0.1 to 100.

8. The method of any one of claims 1 to 7, wherein step (ii) is carried out at a temperature of from 50°C to 1000°C.

Citation Information

Patent Citations

  • Apparatus for forming oxide film

    JP1988032930A

  • Method and device for surface processing

    JP2001345302A

  • Method for manufacturing substrate with single particle film etching mask and for formation of fine uneven surface structure

    JP2013030805A

  • Method for forming pore in crystal substrate, and functional device having wiring and piping in crystal substrate

    JP2014045030A

  • System and method for forming a thermoelectric device