Manufacturing method of white paperboard

By incorporating calcium carbonate in specific amounts and particle sizes in the surface and lower layers, and applying a pigment coating, the method addresses the issues of low-quality pulp whiteness and layer voids, achieving high surface whiteness and preventing creases and blistering in white paperboard production.

JP7567637B2Active Publication Date: 2024-10-16OJI HLDG CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021070408
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-19
Publication Date
2024-10-16
Estimated Expiration
2041-04-19

AI Technical Summary

Technical Problem

The challenge of producing white paperboard with high surface whiteness and preventing creases and blistering, especially when using low-quality pulp with insufficient whiteness, is exacerbated by the saturation of pigment effects and void formation between layers during drying.

Method used

A method involving the use of calcium carbonate in specific amounts and particle sizes in the surface and lower surface layers of white paperboard, combined with a pigment coating, to enhance surface whiteness and prevent creases and blistering.

Benefits of technology

The method results in white paperboard with improved surface whiteness, reduced crease formation, and minimized blistering during drying, ensuring high-quality production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567637000001
    Figure 0007567637000001
Patent Text Reader

Abstract

To provide a method for producing a white paperboard which can give a white paperboard having a sufficiently high surface whiteness and resistance to ruled cracking, and also resistance to swelling during drying.SOLUTION: The present invention discloses a method for producing a white paperboard at least comprising a surface layer, a subsurface layer, a middle layer and a back layer. The surface layer is made using a paper stock therefor, the paper stock comprising a slurry of a surface-layer pulp material containing deinking pulp and / or bleached pulp with calcium carbonate of 5-12 pts.mass added relative to the surface-layer pulp material 100 pts.mass. The subsurface layer is made using a paper stock therefor, the paper stock comprising a slurry of a subsurface-layer pulp material containing old magazine-derived deinking pulp with calcium carbonate of 3-8 pts.mass added relative to the subsurface-layer pulp material 100 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing white paperboard. [Background technology]

[0002] White paperboards are known that have at least a surface layer, a subsurface layer, and a middle layer. The middle layer of the white paperboard uses recycled paper pulp with low whiteness from the viewpoints of low cost and resource conservation. In order to conceal the color of this middle layer, the surface layer of the white paperboard is required to have hiding properties. However, because there is a cost problem when trying to conceal the color of the middle layer with only the surface layer, pulp with a certain degree of whiteness is also used in the subsurface layer immediately below the surface layer (Patent Document 1). Patent Document 1 proposes blending a pigment such as talc in the surface layer or subsurface layer at 10% by weight or more relative to the pulp in order to improve the surface whiteness of white paperboard. Patent Document 1 also specifies that the Canadian Standard Freeness of the surface layer, etc., should be within a specific numerical range in order to prevent crease cracks on the surface even when 10% by weight or more of pigment is blended in the surface layer, etc. Here, "crease cracks" refers to the phenomenon in which the surface of the white paperboard cracks when a crease is made in the white paperboard and the white paperboard is folded. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 6-41896 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, it has become more difficult to obtain good quality pulp materials than before, and it is sometimes necessary to use pulp materials with insufficient brightness for use in white paperboard. Therefore, even when using pulp materials with low brightness, it is required to reliably conceal the color of the middle layer and further improve the surface brightness. However, according to the research of the present inventors, even if the amount of pigment used in the surface layer is increased in order to further improve the surface whiteness, the effect of improving the surface whiteness will soon reach a plateau. In addition, the more pigment used, the more likely the white paperboard is to have cracks along the lines.

[0005] Furthermore, in the white paperboard in which a pigment is added to the underside layer as described in Patent Document 1, there is a problem in that voids form between the underside layer and the middle layer during drying, causing the white paperboard to blister. White paperboard that has blistered may cause problems such as delamination during printing. To provide a method for producing white paperboard which has a sufficiently high surface whiteness and is less likely to crack at creases, and which is less likely to blister when dried. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] A method for producing white paperboard having at least a surface layer, a subsurface layer, a middle layer, and a back layer, comprising the steps of: making the surface layer using a surface layer paper material obtained by adding 5 to 12 parts by mass of calcium carbonate per 100 parts by mass of the surface layer pulp raw material to a slurry of the surface layer pulp raw material containing at least one of de-inked pulp and bleached pulp; and making the subsurface layer using a subsurface layer paper material obtained by adding 3 to 8 parts by mass of calcium carbonate per 100 parts by mass of the surface sublayer pulp raw material to a slurry of the subsurface layer pulp raw material containing de-inked pulp derived from recycled magazine paper. [2] The method for producing white paperboard according to [1], wherein the number of parts by mass of calcium carbonate added per 100 parts by mass of the pulp raw material for the surface layer is greater than the number of parts by mass of calcium carbonate added per 100 parts by mass of the pulp raw material for the undersurface layer. [3] The method for producing white paperboard according to [1] or [2], wherein the calcium carbonate added to the slurry of the pulp raw material for the undersurface layer is light calcium carbonate. [4] The method for producing white paperboard according to [3], wherein the particle size distribution of the precipitated calcium carbonate added to the slurry of the pulp raw material for the undersurface layer has peaks in the range of 0.1 μm to 1 μm and in the range of 1 μm to 10 μm. [5] The method for producing white paperboard according to any one of [1] to [4], wherein the calcium carbonate added to the slurry of the surface layer pulp raw material is light calcium carbonate. [6] The method for producing white paperboard according to [5], wherein the particle size distribution of the precipitated calcium carbonate added to the slurry of the surface layer pulp raw material has peaks in the range of 0.1 μm to 1 μm and in the range of 1 μm to 10 μm. [7] The method for producing white paperboard according to any one of [1] to [6], further comprising coating a surface of the surface layer with a pigment coating liquid containing a pigment and a binder. [8] The method for producing white paperboard according to any one of [1] to [7], further comprising adding a calcium carbonate dispersion in which calcium carbonate is dispersed in water to a slurry of a pulp raw material for a surface layer and a slurry of a pulp raw material for a subsurface layer, respectively. Effect of the Invention

[0007] According to the method for producing white paperboard of the present invention, it is possible to obtain white paperboard having a sufficiently high surface brightness and being less susceptible to cracking at the creases. Also, according to the method for producing white paperboard of the present invention, it is less likely to blister during drying. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] In the method for producing a white paperboard of the present invention, a white paperboard having at least a surface layer, a subsurface layer, a middle layer and a back layer is produced. The surface layer is the layer that is placed on the top side of a multi-layered whiteboard, and the back layer is the layer that is placed on the back side (opposite the surface layer). The underlayer is the layer immediately below the surface layer. The underlayer can also be said to be the layer that is in contact with the surface layer on the inside of the whiteboard. In the present invention, the intermediate layer is disposed between the lower surface layer and the back surface layer. The intermediate layer may be formed of one layer or multiple layers. However, in order to increase the amount of low-quality recycled paper pulp used, it is preferable to form the intermediate layer of multiple layers.

[0009] The manufacturing method of the white paperboard of the present invention is characterized in that the surface layer is made using a surface layer paper material obtained by adding 5 to 12 parts by mass of calcium carbonate per 100 parts by mass of the surface layer pulp raw material to a slurry of a specific surface layer pulp raw material, and the undersurface layer is made using a undersurface layer paper material obtained by adding 3 to 8 parts by mass of calcium carbonate per 100 parts by mass of the undersurface layer pulp raw material to a slurry of a specific undersurface layer pulp raw material. The pulp, fillers such as calcium carbonate, paper stock auxiliaries, and basis weight of each layer used in the manufacturing method of the white paperboard of the present invention will be described below, and the papermaking method will be described in detail in order.

[0010] <About pulp> (surface) The pulp raw material for the surface layer includes at least one of deinked pulp and bleached pulp having high brightness. Pulps other than these can also be used as the pulp for the surface layer as long as the effect of the invention is not impaired. Deinked pulp is waste paper pulp that has been deinked and has a high whiteness. It may be bleached to increase the whiteness. Examples of waste paper that can be used as a raw material for deinked pulp include paper that has been used once but has a small printed area, such as white, ruled white, extra white, medium white, and white manila; printed matter such as cards, imitation, colored paper, Kent, and white art, and colored paper that has been used once; used high-quality waste paper such as coated paper for printing, beverage cartons, and office paper; medium-quality waste paper for business use, such as tickets, medium-quality waste rolls, and Kent manila; general medium-quality waste paper, such as newspapers and magazines; and brown waste paper, such as cut brown, plain brown, miscellaneous bags, and cardboard. The waste paper may be shredded office paper or tickets that have confidentiality. These may be used alone or in combination of two or more. As the deinked pulp for the surface layer, deinked pulp derived from waste paper with high whiteness such as white paper, cards, extra white, medium white, white Manila, imitation, colored paper, etc.; deinked pulp derived from Kent paper is preferable, and deinked pulp derived from Kent paper is particularly preferable.

[0011] Examples of bleached pulp include bleached hardwood kraft pulp (LBKP), semi-bleached hardwood kraft pulp (LSBKP), bleached softwood kraft pulp (NBKP), semi-bleached softwood kraft pulp (NSBKP), and bleached chemi-thermomechanical pulp (BCTMP). Of these, bleached hardwood kraft pulp and bleached softwood kraft pulp are particularly preferred. Examples of unbleached pulp include chemical pulps such as softwood unbleached kraft pulp (NUKP), hardwood unbleached kraft pulp (LUKP), hardwood sulfite pulp, and softwood sulfite pulp, and mechanical pulps such as thermomechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), chemi-ground pulp (CGP), refiner ground pulp (RGP), ground pulp (GP), pressed stone ground pulp (PGW), and stone ground pulp (SGP), and these can be used in combination as long as the effects of the invention are not impaired.

[0012] (lower surface layer) The pulp raw material for the underside layer includes deinked pulp derived from recycled magazine paper. Pulp other than deinked pulp derived from recycled magazine paper can also be used for the underside layer as long as it does not impair the effects of the invention. The pulp used for the underside layer is composed of pulp having a lower brightness than the pulp of the surface layer and a higher brightness than the pulp of the middle layer. As the pulp constituting the underside layer, deinked pulp derived from low-grade waste paper compared to the surface layer, i.e., deinked pulp derived from waste paper containing a large amount of medium-density fiber, is preferably used. For example, deinked pulp derived from newspapers, colored paper, balls, etc. is preferable.

[0013] (middle layer) The pulp used for the middle layer is generally the lowest grade pulp among the layers constituting the white paperboard, such as disintegrated pulp from newspapers, magazines, tickets, medium-quality waste paper, brown paper, corrugated cardboard, cardboard backing, ground paper, and balls. The middle layer may be formed of one layer or multiple layers. However, in order to increase the amount of low-quality recycled paper pulp used, it is preferable to form the middle layer with multiple layers. When the middle layer is composed of multiple layers, the pulps constituting each layer of the middle layer may all be the same or different.

[0014] (Lower back layer) In the manufacturing method of the white paperboard of the present invention, a back underlayer may be provided between the back layer and the middle layer. The back underlayer is disposed between the back layer and the middle layer. The back underlayer can also be said to be a layer that contacts the back layer on the inside of the white paperboard. The pulp constituting the lower back layer is pulp with a higher whiteness than the pulp of the middle layer, but with a lower whiteness than the pulp of the lower back layer. The pulp used for the upper and lower back layers may be used for the lower back layer, but generally, lower-grade waste paper, i.e., waste paper containing a large amount of medium-density fiber, is used for the lower back layer. For example, unbleached deinked waste paper pulp from newspapers, magazines, colored paper, cardboard, etc. is generally used.

[0015] (Back layer) The back layer does not require the same whiteness as the surface layer, but since it is visible to the human eye, pulp with a higher whiteness than the middle layer is usually used. The back layer may contain pulp derived from shredded office paper or the like. Pulp obtained by disintegrating shredded office paper or the like has a relatively high whiteness even without deinking or bleaching, so it is preferable to incorporate it in the back layer. When a whiteness similar to that of the surface layer is required, the back lower layer should be the same as the surface lower layer, and the back layer should be the same as the surface layer.

[0016] <About calcium carbonate and other fillers> The surface layer paper material is obtained by adding calcium carbonate to a slurry of the surface layer pulp raw material. The amount of calcium carbonate added to the slurry of the surface layer pulp raw material is 5 to 12 parts by mass, preferably 8 to 11 parts by mass, per 100 parts by mass of the surface layer pulp raw material. If the amount of calcium carbonate added is equal to or more than the lower limit, the blackness of the middle layer is easily concealed sufficiently. If the amount of calcium carbonate added is equal to or less than the upper limit, cracks in the lines of the white board are less likely to occur. The surface layer paper material is obtained by adding calcium carbonate to a slurry of the pulp raw material for the surface under layer. The amount of calcium carbonate added to the slurry of the pulp raw material for the surface under layer is 3 to 8 parts by mass, preferably 5 to 7 parts by mass, per 100 parts by mass of the pulp raw material for the surface under layer. If the amount of calcium carbonate added is equal to or more than the lower limit, the blackness of the middle layer can be sufficiently concealed. In addition, swelling during production can be suppressed. If the amount of calcium carbonate added is equal to or less than the upper limit, swelling during production can be suppressed. In particular, when the number of parts by mass of calcium carbonate added per 100 parts by mass of the pulp raw material for the surface layer is greater than the number of parts by mass of calcium carbonate added per 100 parts by mass of the pulp raw material for the undersurface layer, this is preferable because it provides excellent hiding power for the intermediate layer, excellent effect in preventing cracking of creases, and excellent control of swelling during production.

[0017] Although calcium carbonate may be added to the pulp slurry in the form of a powder or in the form of a calcium carbonate dispersion in which calcium carbonate is dispersed in water, it is preferable to add calcium carbonate to the pulp slurry as a calcium carbonate dispersion, which allows for a fixed amount to be added and makes it easier to prevent fluctuations in the amount added. It is preferable to add the calcium carbonate dispersion to each of the slurry of the pulp raw material for the surface layer and the slurry of the pulp raw material for the undersurface layer. In this case, the calcium carbonate dispersion prepared in the same batch is divided into two or more portions, and a predetermined amount of calcium carbonate is added to each of the slurry of the pulp raw material for the surface layer and the slurry of the pulp raw material for the undersurface layer using the same calcium carbonate dispersion. When calcium carbonate is added as a calcium carbonate dispersion, a dispersant may be added to the calcium carbonate dispersion in order to obtain good dispersibility. Examples of the dispersant include an anionic surfactant.

[0018] The calcium carbonate is not particularly limited. As the calcium carbonate, light calcium carbonate or heavy calcium carbonate may be used, and light calcium carbonate is preferred. Volume-based average primary particle size D of precipitated calcium carbonate 50 The thickness is preferably from 0.2 to 10 μm, more preferably from 1 to 5 μm, and even more preferably from 2 to 3 μm. Here, the primary particle size refers to the particle size measured by dropping an aqueous dispersion of precipitated calcium carbonate into the circulation system of a laser diffraction type particle size distribution analyzer, and then subjecting it to ultrasonic treatment. 50 is the 50% primary particle size based on volume.

[0019] Since light reflection occurs easily in the surface layer of the white paperboard and the surface whiteness of the white paperboard is further improved, it is preferable that the particle size distribution of the precipitated calcium carbonate has peaks in the range of 0.1 μm to 1 μm and in the range of 1 μm to 10 μm. The particle size distribution of the precipitated calcium carbonate can be obtained, for example, by a laser diffraction particle size distribution measuring device, but is not particularly limited thereto.

[0020] Other fillers may be blended into the surface layer and the undersurface layer as long as they do not impair the effects of the invention. Examples of other fillers include known fillers such as white clay, clay, calcined clay, talc, titanium oxide, and silica. Since the undersurface layer contains a filler derived from waste paper material, the amount of calcium carbonate added may be adjusted within the above-mentioned range, taking into account the content of the filler.

[0021] <About auxiliary agents> The stock used for making each layer may contain paper strength agents, aluminum sulfate, and other auxiliary agents, as required. The composition of the stock used in making each layer can be appropriately changed taking into consideration the quality required for the white board, convenience in manufacturing, etc. For example, the ratio of deinked pulp and the ratio of bleached pulp to the total pulp in the stock are not particularly limited. They are appropriately adjusted taking into consideration which layer the stock is used to form, etc.

[0022] Strengthening agents are papermaking chemicals that give strength to the paper product. There are two types of strength agents: wet and dry. Dry strength agents are preferable because they improve internal strength, surface strength, and interlaminar strength.

[0023] Among dry strength agents, polyacrylamide-based strength agents are preferred for their strength development effect and improved pulp yield. The proportion of polyacrylamide-based strength agents in the strength agents used in the paper stock is preferably 0.1% or more, more preferably 0.4% or more, and it is particularly preferred that the polyacrylamide-based strength agents are used alone.

[0024] The polyacrylamide-based paper strength agent is not particularly limited, and any of anionic, amphoteric, and cationic types can be used. Among these, amphoteric polyacrylamide-based paper strength agents are preferred because of their wide fixing range.

[0025] Examples of paper strength agents other than polyacrylamide-based paper strength agents include natural paper strength agents such as starch and vegetable gum, and synthetic paper strength agents such as polyvinyl alcohol resin, styrene butadiene latex, urea formaldehyde resin, melamine resin, polyamide resin, ketone resin, polyamide epichlorohydrin resin, polyamine epichlorohydrin resin, polyamide epoxy resin, glycerol polyglycidyl ether resin, and polyethyleneimine resin. These can be used alone or in combination. Among these, starches, polyvinyl alcohol resins, and styrene-butadiene latex are preferred, and starches are particularly preferred. Examples of starches include oxidized starch, esterified starch such as urea phosphate esterified starch, enzyme-modified starch, etherified starch such as hydroxyethyl etherified starch, and the like, and these can be used alone or in combination. Among these, it is preferred to use oxidized starch.

[0026] The amount of the paper strength agent added is preferably 0.1 to 1.5% by mass, and more preferably 0.4 to 1.0% by mass, relative to 100% by mass of the solid content of the pulp slurry. By setting the amount of the paper strength agent to be equal to or greater than the lower limit, the generation of precipitates can be more reliably suppressed, while by setting the amount of the paper strength agent to be equal to or less than the upper limit, the deterioration of drainage due to excessive aggregation can be suppressed.

[0027] Aluminum sulfate is the common name for aluminum sulfate. Aluminum sulfate is a typical inorganic flocculant. By adding aluminum sulfate, it is possible to prevent fine fibers from falling off in the wire part even when using recycled paper pulp, and improve the yield of the pulp slurry.

[0028] The amount of aluminum sulfate added is preferably 0.1 to 2.0 mass %, and more preferably 0.4 to 1.0 mass %, relative to 100 mass % of the solid content of the pulp slurry. By setting the amount of aluminum sulfate to be equal to or more than the lower limit, the effect of improving the retention of the pulp slurry can be easily obtained, while by setting the amount of aluminum sulfate to be equal to or less than the upper limit, the generation of precipitates can be more reliably suppressed.

[0029] Other auxiliaries include paper strength agents, water-resistant agents, water repellents, foamable microcapsules, sizing agents, dyes, fillers, pH adjusters, slime control agents, thickeners, preservatives, antifungal agents, antibacterial agents, flame retardants, rodenticides, insect repellents, moisturizers, freshness-retaining agents, oxygen absorbers, microcapsules, foaming agents, surfactants, electromagnetic shielding materials, antistatic agents, rust inhibitors, fragrances, deodorants, etc. These may be used alone or in combination of two or more.

[0030] <About Grammage> The surface layer has a basis weight of 15 to 90 g / m 2 is preferable, and 25 to 70 g / m 2 The basis weight of each layer can be measured in accordance with JIS P8124. If the basis weight of the surface layer is equal to or greater than the lower limit, the blackness of the middle layer can be sufficiently concealed. If the basis weight of the surface layer is equal to or less than the upper limit, swelling during papermaking can be suppressed.

[0031] The basis weight of the surface layer is 15 to 70 g / m 2 is preferable, and 20 to 60 g / m 2 More preferably, 25 to 55 g / m 2 When the basis weight of the undersurface layer is equal to or more than the lower limit, the blackness of the middle layer can be sufficiently concealed together with the surface layer. When the basis weight of the undersurface layer is equal to or less than the upper limit, swelling during papermaking can be suppressed. In the white paperboard of the present invention, the basis weight of the subsurface layer is preferably greater than that of the surface layer, since this can prevent cracks from occurring on the surface of the white paperboard.

[0032] The total basis weight of the middle layer is appropriately adjusted according to the thickness required for the application of the white paperboard. The basis weight per layer of the middle layer is, for example, 15 to 90 g / m 2 It is preferable to set the thickness to 25 to 75 g / m 2 It is more preferable to set the above.

[0033] When the backing layer is formed, its basis weight is 15 to 90 g / m 2 is preferable, and 25 to 75 g / m 2 When the basis weight of the lower back layer is equal to or more than the lower limit, the lower back layer can sufficiently conceal colored foreign matter in the middle layer together with the back layer.

[0034] The basis weight of the backing layer is 15 to 90 g / m 2 is preferable, and 25 to 70 g / m 2 When the basis weight of the back layer is equal to or more than the lower limit, the colored foreign matter in the middle layer can be sufficiently concealed, and when the basis weight of the back layer is equal to or less than the upper limit, sufficient strength of the paper layer can be obtained.

[0035] <Paper making method> The papermaking method for forming each layer is not particularly limited. It is preferable to use a papermaking machine equipped with at least a wire part, a press part, and a dryer part. A size press may be performed in the dryer part. A papermaking machine equipped with a calendar part (pre-calendar) after the dryer part may be used. When laminating each layer, an adhesive such as starch may be used between each layer. The adhesive may be applied by a spray method or the like.

[0036] As the wire part, a known multi-stage wire part can be appropriately used. The multi-stage wire part has at least two or more wire part portions. The types of wire parts generally used in papermaking include the cylinder type, the fourdrinier type, the short wire type, the inclined type, and the twin wire type. In multi-stage wire parts, these methods can be combined in multiple stages. For example, there are Fourdrinier combination, short net combination, short net cylinder combination, and Fourdrinier cylinder combination.

[0037] As the press part, a known press machine can be appropriately used, but it is preferable to include a shoe press. It is also preferable to combine a roll press and a shoe press. When a shoe press is used, water can be sufficiently squeezed out in the press part, so that the water content during size pressing in the dryer part can be easily controlled.

[0038] As the dryer part, a known dryer can be appropriately used. For example, a cylinder dryer that contacts and heats the wet white paperboard, an infrared dryer, a hot air dryer, or other non-contact dryer can be used alone or in combination.

[0039] <About the pigment coating layer> In the manufacturing method of the white paperboard of the present invention, a pigment coating layer containing a pigment and a binder may be provided on the surface of the surface layer. Examples of pigments include pigments used in the general coated paper manufacturing field, such as kaolin, calcium carbonate (heavy calcium carbonate, light calcium carbonate), titanium dioxide, aluminum hydroxide, silica, satin white, talc, etc. Among these, calcium carbonate is preferred because it exhibits excellent printability.

[0040] As the binder, a water-based adhesive is preferable. Examples of the water-based adhesive include starches such as oxidized starch, phosphated starch, hydroxyethyl etherified starch, dextrin, enzyme-modified starch, and water-soluble starch; latexes such as conjugated diene copolymer latexes such as styrene-butadiene copolymer latex, methyl methacrylate-butadiene copolymer latex, and styrene-methyl methacrylate-butadiene copolymer latex; acrylic copolymer latexes such as copolymer latexes of acrylic acid esters and / or methacrylic acid esters; proteins such as casein, gelatin, and soybean protein; synthetic resin adhesives such as various polyvinyl alcohols, various polyacrylamides, and melamine resins; and various cellulose derivatives such as carboxymethyl cellulose. The binder can be used by selecting one or more of these adhesives.

[0041] Among these, it is preferable to use a latex having a glass transition temperature of -50 to 30°C as measured by Vibron viscoelasticity, since this increases the flexibility of the coating surface and improves resistance to cracking. The glass transition temperature of the latex is more preferably -50 to 0°C. It is also preferable to mix starch together with latex, since the combined use of latex and starch makes it possible to achieve a good balance between the fixation of the fine fibers inside the backing layer and the surface strength of the backing layer. The mass ratio of latex to starch is preferably 100:0 to 5:50.

[0042] The pigment coating liquid may further contain, as necessary, one or more of a dispersant, a pH adjuster such as sodium hydroxide or aqueous ammonia, an antifoaming agent, a fluorescent dye, a release agent, a water-resistant agent, a flow improver, a slime control agent, a preservative, a dye, a coloring pigment, and the like. A pigment coating layer may also be provided on the surface of the back surface layer.

[0043] When providing a pigment coating layer on the surface of the surface layer of the white paperboard, a pigment coating liquid is applied to the surface of the surface layer to provide the coating layer, and then the coating layer is dried to provide the pigment coating layer on the surface of the surface layer. The pigment coating liquid preferably contains 2 to 50 parts by mass, and more preferably 5 to 25 parts by mass, of the binder per 100 parts by mass of the pigment. When the proportion of the binder is equal to or greater than the lower limit, the strength of the pigment coating layer tends to be sufficient, whereas when the proportion of the binder is equal to or less than the upper limit, the ink drying property and the suitability for box making are excellent. The coating amount of the pigment coating liquid is 5 to 50 g / m2 in terms of dry mass. 2 is preferable, and 8 to 40 g / m 2 is preferable, and 10 to 35 g / m 2 is more preferred.

[0044] The pigment coating liquid may be applied in multiple steps. When the pigment coating liquid is applied in multiple steps, for example, in two steps, the first (undercoat layer) and second (topcoat layer) coating liquids may be the same or different. The pigment coating liquid may be applied directly to the surface layer, or may be applied via a coating film of a size press liquid applied to the surface layer. Before applying the pigment coating liquid, the surface of the surface layer may be smoothed by pre-calendering. The pigment coating liquid may be applied only once or multiple times. In particular, it is preferable to apply a pigment coating liquid for the undercoat layer and a pigment coating liquid for the topcoat layer to successively form the undercoat layer and the topcoat layer. By applying a pigment coating liquid, it is possible to improve the printability of the surface layer side and to increase the whiteness.

[0045] The coater may be on-machine or off-machine, but is preferably an on-machine coater using a known coater part attached to a paper machine. Examples of the coating device of the coater part include a blade coater, an air knife coater, a roll coater, a reverse roll coater, a bar coater, a curtain coater, a slot die coater, a gravure coater, a champlex coater, a brush coater, a slide bead coater, a two-roll or metering blade type size press coater, a bill blade coater, a short dwell coater, a gate roll coater, and a nip coater using a calendar. Among these, rod metering coaters and curtain coaters are preferred because they can provide a coating layer with a constant coating amount and thus suppress coating unevenness. The applied coating layer is dried by a known drying device to form a pigment coating layer. The papermaking machine may have multiple coater parts. In this case, the coating layer can be applied in multiple steps.

[0046] A calendar part may be provided after the coater part, if necessary. By providing a calendar part after the coater part, the pigment coating layer is smoothed. A known calendaring device can be appropriately used for the calendaring part after the coater part, such as a super calendar, a gloss calendar, a soft nip calendar, a heat calendar, a shoe calendar, etc. These may be used in combination. Among them, a soft nip calendar equipped with a metal roll and an elastic roll is preferable because it can smooth the coating layer while maintaining the paper thickness. The calendaring part after the coater part may be on-machine or off-machine.

[0047] (Mechanism of action) In the manufacturing method of the white paperboard of the present invention described above, calcium carbonate with high concealing effect is blended in both the surface layer paper material and the undersurface layer paper material, so that the amount of calcium carbonate in the two layers, the surface layer and the undersurface layer, can be made sufficient to conceal the color of the middle layer. Therefore, the surface whiteness of the obtained white paperboard is improved. In addition, since it is not necessary to blend an excessive amount of pigment only in the surface layer paper material, it is possible to suppress cracking of the resulting white paperboard. In addition, by adjusting the amount of calcium carbonate added to the underlayer paper stock, steam can easily pass through the underlayer during drying during multi-layer papermaking, which makes it difficult for air to accumulate between the underlayer and the middle layer, suppressing the occurrence of blistering. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following description.

[0049] <Example 1> A multi-layer paper machine was used to obtain a white board having a surface layer, a subsurface layer, a middle layer, and a back layer. The basis weight of the surface layer was 45 g / m 2 , the surface layer has a basis weight of 50g / m 2 , the middle layer has a basis weight of 135g / m 2 , the backing layer has a basis weight of 45g / m 2 The paper was multi-layered so that the result was as follows. The surface layer paper material was a slurry of surface layer pulp raw material with a whiteness of 85%, which was a mixture of 80% by mass of deinked pulp made from Kent waste paper and 20% by mass of bleached hardwood kraft pulp, to which 9 parts by mass of light calcium carbonate (product name "Tama Pearl TP121-6S", manufactured by Okutama Kogyo Co., Ltd., with particle diameter peaks between 0.1 to 1 μm and 1 μm to 10 μm, and a volume-based average primary particle diameter of 2 to 3 μm) was added per 100 parts by mass of the surface layer pulp raw material. The paper material for the underside layer was prepared by adding 7 parts by mass of light calcium carbonate (product name "Tama Pearl TP121-6S", manufactured by Okutama Kogyo Co., Ltd., with particle diameter peaks between 0.1 to 1 μm and 1 to 10 μm, and a volume-based average primary particle diameter of 2 to 3 μm) to a slurry of the underside layer pulp raw material consisting of deinked pulp derived from waste magazine paper with a brightness of 70% per 100 parts by mass of the underside layer pulp raw material. A slurry of recycled magazine pulp with a brightness of 40% was used as the middle layer paper material. The backing layer paper material used was a slurry of pulp with a brightness of 51%, which was a mixture of 50% by mass of recycled newspaper, 40% by mass of recycled magazine paper, and 10% by mass of pulp derived from shredded office waste paper.

[0050] <Examples 2 and 3, Comparative Examples 1 to 3> A white paperboard was obtained in the same manner as in Example 1, except that the amount of calcium carbonate was changed as shown in Table 1.

[0051] <Evaluation> "Cracked lines" The obtained white paperboard was evaluated for crease cracking according to T495om-82 "Paperboard folding index", which was standardized as a Tappi standard test method, under the condition that the groove width of the recess was approximately 3.5 times the paper thickness. : No cracks were observed. ○: A small amount of cracking occurred, but no problem at all. △: Cracks occurred. ×: Severe cracking occurred.

[0052] "Surface strength" The surface of the obtained white paperboard was printed with Ink Tac 6 (manufactured by Toyo Ink Mfg. Co., Ltd.) using an RI tester (manufactured by Mei Seisakusho Co., Ltd.). 2 The state of peeled fibers around the area was visually observed and evaluated according to the following criteria. : Almost no fiber peeling. ○: There is a small amount of fiber peeling. △: Some fiber peeling. ×: Fibers peeled off.

[0053] "Swelling" The obtained white paperboard was measured in accordance with JAPAN TAPPI Paper and Pulp Test Method No. 18-1 Paper and Paperboard-Internal Bond Strength Test Method-Part 1: Z-Axis Tensile Test. ◎: Interlaminar strength exceeds 400 kPa, and no blistering occurs. ◯: Interlaminar strength is between 350 kPa and 400 kPa, and no blistering occurs. △: Interlaminar strength is less than 350 kPa, and blistering occurs. ×: Obvious swelling occurred during production, and production was discontinued.

[0054] "Surface quality of the surface" The surface quality of the surface layer of the obtained white paperboard was visually observed and evaluated according to the following criteria. : Excellent smoothness and surface whiteness. ◯: Either the smoothness or the surface whiteness is slightly inferior, but there is no problem in practical use. Δ: One of the smoothness and surface whiteness is poor, and there is a problem in practical use. ×: The surface is rough and problematic for practical use.

[0055] [Table 1]

[0056] In Examples 1 to 3, the evaluation results of all of the crease cracking, surface strength, interlaminar strength, and surface quality of the outer layer surface were good, and the surface whiteness was also sufficiently high. In addition, no crease cracking occurred, and no swelling occurred during drying. In Comparative Example 1, the amount of calcium carbonate added to the slurry of the surface layer pulp raw material was large, causing severe cracking of the creases, and the surface strength and interlaminar strength were reduced, and swelling occurred during drying. In Comparative Example 2, the amount of calcium carbonate added to the slurry of the pulp raw material for the subsurface layer was small, and the surface brightness was insufficient, and the surface quality of the surface layer was also insufficient. In Comparative Example 3, the amount of calcium carbonate added to the slurry of the pulp raw material for the surface layer was small, and the surface quality of the surface layer was insufficient. In Comparative Example 4, the amount of calcium carbonate added to the slurry of the pulp raw material for the surface layer was large, and cracks occurred in the creases, the surface strength was reduced, the surface of the surface layer was rough, and the smoothness was insufficient. Also, swelling occurred during drying.

Claims

1. A method for producing white paperboard in which at least a surface layer, a subsurface layer, a middle layer, and a back layer are made by a multi-layer papermaking machine, The surface layer is made from a surface layer paper material obtained by adding 5 to 12 parts by mass of calcium carbonate to 100 parts by mass of the surface layer pulp raw material to a slurry of the surface layer pulp raw material containing at least one of deinked pulp and bleached pulp, The underside layer is made from a paper stock obtained by adding 3 to 8 parts by mass of calcium carbonate to 100 parts by mass of the pulp raw material for the underside layer to a slurry of the pulp raw material for the underside layer, the slurry including deinked pulp derived from waste magazine paper; The pulp raw material for the surface underlayer is a pulp raw material having a lower brightness than the pulp raw material for the surface layer and a higher brightness than the pulp raw material for the middle layer, A method for producing white paperboard, characterized in that the surface layer has a basis weight of 25 g / m2 or more, the undersurface layer has a basis weight of 70 g / m2 or less and is greater than the basis weight of the surface layer, the middle layer has a basis weight of 25 to 75 g / m2 per layer, and the back layer has a basis weight of 25 to 70 g / m2.

2. The method for producing white paperboard according to claim 1 , wherein the number of parts of calcium carbonate added per 100 parts by mass of the pulp raw material for the surface layer is greater than the number of parts of calcium carbonate added per 100 parts by mass of the pulp raw material for the undersurface layer.

3. 3. The method for producing white paperboard according to claim 1, wherein the calcium carbonate added to the slurry of the pulp raw material for the undersurface layer is light calcium carbonate.

4. 4. The method for producing white paperboard according to claim 3, wherein the particle size distribution of the precipitated calcium carbonate added to the slurry of the pulp raw material for the lower surface layer has peaks in the range of 0.1 μm to 1 μm and in the range of 1 μm to 10 μm.

5. The method for producing white paperboard according to any one of claims 1 to 4, wherein the calcium carbonate added to the slurry of the surface layer pulp raw material is light calcium carbonate.

6. 6. The method for producing white paperboard according to claim 5, wherein the particle size distribution of the precipitated calcium carbonate added to the slurry of the surface layer pulp raw material has peaks in the range of 0.1 μm to 1 μm and in the range of 1 μm to 10 μm.

7. The method for producing white paperboard according to any one of claims 1 to 6, further comprising coating a pigment coating liquid containing a pigment and a binder on the surface of the surface layer.

8. The method for producing white paperboard according to any one of claims 1 to 7, wherein a calcium carbonate dispersion in which calcium carbonate is dispersed in water is added to each of a slurry of the pulp raw material for the surface layer and a slurry of the pulp raw material for the undersurface layer.

Citation Information

Patent Citations

  • Patent-coated board

    JP1994041896A

  • White liner

    JP2006176921A

  • Coated white lined chipboard

    JP2014019996A

  • Coated white cardboard

    JP2015030930A

  • Production method of coated white cardboard

    JP2019044326A