Multilayer ceramic electronic components
The multilayer ceramic electronic component addresses overcurrent and creeping discharge through a structured design with embedded fuses and resin-covered terminals, ensuring insulation and controlled disconnection.
Patent Information
- Application Number
- JP2021149712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Conventional laminated ceramic electronic components effectively suppress creeping discharge but lack adequate measures to prevent overcurrent occurrences.
A multilayer ceramic electronic component design featuring stacked ceramic and conductor layers with external electrodes, metal terminals, and a fuse embedded in an exterior material, where the fuse is partially exposed and covered by a thermoplastic resin to disconnect during overcurrent, while being surrounded by a thermosetting resin to prevent creeping discharge.
The design effectively suppresses creeping discharge and addresses overcurrent issues by ensuring insulation and providing a controlled disconnection mechanism for fuses, enhancing safety and reliability.
Smart Images

Figure 0007567728000001 
Figure 0007567728000002 
Figure 0007567728000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic electronic component. [Background technology]
[0002] Conventionally, there are known multilayer ceramic electronic components covered with a resin exterior material. In such multilayer ceramic electronic components, metal terminals extending to the outside of the exterior material and external electrodes disposed on the surfaces of the main body of the multilayer ceramic electronic component are joined inside the exterior material by a joining material containing a metal such as solder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-145767 A Summary of the Invention [Problem to be solved by the invention]
[0004] Such multilayer ceramic electronic components can ensure a sufficient distance between the metal terminals, thereby preventing creeping discharges from occurring. However, there is still room for improvement in terms of measures to be taken in the event of an overcurrent.
[0005] An object of the present invention is to provide a multilayer ceramic electronic component in which a measure is taken when an overcurrent occurs while suppressing creeping discharge. [Means for solving the problem]
[0006] The multilayer ceramic electronic component according to the present invention comprises a laminate including a plurality of laminated ceramic layers and a plurality of internal conductor layers laminated on the ceramic layers, the laminate including a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction, a first external electrode disposed on the first end surface side, and a second external electrode disposed on the second end surface side, a first metal terminal electrically connected to the first external electrode, a second metal terminal electrically connected to the second external electrode, and a terminal for connecting the multilayer ceramic electronic component to the first external electrode and the second external electrode. a multilayer ceramic electronic component comprising a multilayer ceramic electronic component body and an exterior material covering a portion of the first metal terminal and a portion of the second metal terminal, the multilayer ceramic electronic component further comprising a fuse electrically connecting the first external electrode and the first metal terminal, the exterior material having a first exterior material covering the multilayer ceramic electronic component body, a portion of the first metal terminal and a portion of the second metal terminal, and a second exterior material covering at least a portion of the first exterior material, the fuse being embedded in the exterior material, at least a portion of which protrudes and is exposed from the first exterior material, and the protruding and exposed portion being embedded so as to be surrounded by the second exterior material. Effect of the Invention
[0007] According to the present invention, it is possible to provide a multilayer ceramic electronic component in which a measure is taken when an overcurrent occurs while suppressing creeping discharge. [Brief description of the drawings]
[0008] [Figure 1] 1 is an external perspective view of a multilayer ceramic capacitor according to an embodiment of the present invention; [Diagram 2] 2 is a view of the multilayer ceramic capacitor of FIG. 1 as seen from the direction of arrow II. [Diagram 3] 3 is a view of the multilayer ceramic capacitor of FIG. 2 as seen in the direction of arrow III. [Figure 4]4 is a view of the multilayer ceramic capacitor of FIG. 2 as seen in the direction of arrow IV. [Diagram 5] 5 is a cross-sectional view taken along line VV of the multilayer ceramic capacitor 1 in FIG. [Figure 6] 1 is an external perspective view showing the external appearance of a multilayer ceramic capacitor body before it is covered with an exterior material and before metal terminals are attached; [Figure 7] 7 is a cross-sectional view taken along line VII-VII of the multilayer ceramic capacitor body of FIG. 6. [Figure 8] 8 is a cross-sectional view of the multilayer ceramic capacitor body taken along line XIII-XIII in FIG. 7. [Figure 9] 9 is a cross-sectional view taken along line IX-IX of the multilayer ceramic capacitor body of FIG. 7. [Figure 10] 6 is an enlarged view of a portion X of the multilayer ceramic capacitor shown in FIG. 5. [Figure 11] 1 is an external perspective view showing a mounting structure in which a multilayer ceramic capacitor according to an embodiment of the present invention is mounted on a mounting board. [Figure 12] 3 is a diagram showing a modified example of the multilayer ceramic capacitor of the present embodiment, and corresponds to FIG. 2. FIG. [Figure 13A] FIG. 1 is a diagram showing a multilayer ceramic capacitor having a double structure. [Figure 13B] FIG. 1 is a diagram showing a triple-structure multilayer ceramic capacitor. [Figure 13C] FIG. 1 is a diagram showing a multilayer ceramic capacitor having a four-row structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a multilayer ceramic capacitor 1 as a multilayer ceramic electronic component according to an embodiment of the present invention will be described. Fig. 1 is an external perspective view of the multilayer ceramic capacitor 1. Fig. 2 is a view of the multilayer ceramic capacitor 1 in Fig. 1 as viewed from the direction of arrow II. Fig. 3 is a view of the multilayer ceramic capacitor 1 in Fig. 2 as viewed from the direction of arrow III. Fig. 4 is a view of the multilayer ceramic capacitor 1 in Fig. 2 as viewed from the direction of arrow IV. Fig. 5 is a cross-sectional view of the multilayer ceramic capacitor 1 in Fig. 4 taken along line VV.
[0010] The multilayer ceramic capacitor 1 has a multilayer ceramic capacitor body 2 as a multilayer ceramic electronic component body, metal terminals 100, an exterior material 3, and a fuse 200. The multilayer ceramic capacitor body 2 and the fuse 200 are not shown in Figures 1 to 4 because they are covered by the exterior material 3. The multilayer ceramic capacitor body 2 and the fuse 200 are shown in Figure 5.
[0011] The multilayer ceramic capacitor body 2 will be described with reference to Fig. 5 as well as Fig. 6 to Fig. 9. Fig. 6 is an external perspective view showing the appearance of the multilayer ceramic capacitor body 2 before it is covered with the exterior material 3 and before the metal terminals 100 are attached. Fig. 7 is a cross-sectional view taken along line VII-VII of the multilayer ceramic capacitor body 2 in Fig. 6. Fig. 8 is a cross-sectional view taken along line VIII-VIII of the multilayer ceramic capacitor body 2 in Fig. 7. Fig. 9 is a cross-sectional view taken along line IX-IX of the multilayer ceramic capacitor body 2 in Fig. 7.
[0012] The multilayer ceramic capacitor body 2 includes a laminate 10 and external electrodes 40 .
[0013] 6 to 9 show an XYZ orthogonal coordinate system. As shown in FIG. 6, the length direction L of the multilayer ceramic capacitor body 2 and the laminate 10 corresponds to the X direction. The width direction W of the multilayer ceramic capacitor body 2 and the laminate 10 corresponds to the Y direction. The height direction T of the multilayer ceramic capacitor body 2 and the laminate 10 corresponds to the Z direction. Here, the cross section shown in FIG. 7 is also referred to as an LT cross section. The cross section shown in FIG. 8 is also referred to as a WT cross section. The cross section shown in FIG. 9 is also referred to as an LW cross section. Note that similar XYZ orthogonal coordinate systems are also shown in FIGS. 1 to 5, 11, and 12.
[0014] As shown in Figures 6 to 9, the laminate 10 includes a first main surface TS1 and a second main surface TS2 facing each other in a height direction T, a first side surface WS1 and a second side surface WS2 facing each other in a width direction W perpendicular to the height direction T, and a first end surface LS1 and a second end surface LS2 facing each other in a length direction L perpendicular to the height direction T and the width direction W.
[0015] The laminate 10 has a substantially rectangular parallelepiped shape. The dimension of the laminate 10 in the length direction L is not necessarily longer than the dimension in the width direction W. The corners and ridges of the laminate 10 are preferably rounded. The corners are the parts where three faces of the laminate intersect, and the ridges are the parts where two faces of the laminate intersect. Incidentally, unevenness may be formed on a part or all of the surfaces constituting the laminate 10.
[0016] The dimensions of the laminate 10 are not particularly limited, but if the dimension of the laminate 10 in the length direction L is the L dimension, then the L dimension is preferably 0.2 mm or more and 10 mm or less. If the dimension of the laminate 10 in the height direction T is the T dimension, then the T dimension is preferably 0.1 mm or more and 10 mm or less. If the dimension of the laminate 10 in the width direction W is the W dimension, then the W dimension is preferably 0.1 mm or more and 10 mm or less.
[0017] 7 and 8, the laminate 10 has an inner layer portion 11, and a first main surface side outer layer portion 12 and a second main surface side outer layer portion 13 arranged so as to sandwich the inner layer portion 11 in the height direction T. The inner layer portion 11 is also referred to as an effective layer portion.
[0018] The internal layer portion 11 includes a plurality of dielectric layers 20 as a plurality of ceramic layers, and a plurality of internal electrode layers 30 as a plurality of internal conductor layers. The internal layer portion 11 includes the internal electrode layer 30 located closest to the first main surface TS1 side to the internal electrode layer 30 located closest to the second main surface TS2 side in the height direction T. In the internal layer portion 11, the multiple internal electrode layers 30 are arranged opposite each other with the dielectric layer 20 interposed therebetween. The internal layer portion 11 is a portion that generates electrostatic capacitance and substantially functions as a capacitor.
[0019] The multiple dielectric layers 20 are made of a dielectric material. The dielectric material may be, for example, a dielectric ceramic containing components such as BaTiO3, CaTiO3, SrTiO3, or CaZrO3. The dielectric material may also be one in which a subcomponent such as a Mn compound, an Fe compound, a Cr compound, a Co compound, or a Ni compound is added to the main components.
[0020] The thickness of the dielectric layer 20 is preferably 0.5 μm or more and 72 μm or less. The number of laminated dielectric layers 20 is preferably 10 to 700. The number of dielectric layers 20 is the total number of the dielectric layers in the inner layer portion 11 and the dielectric layers in the first main surface side outer layer portion 12 and the second main surface side outer layer portion 13.
[0021] The multiple internal electrode layers 30 (internal conductor layers 30) have multiple first internal electrode layers 31 (first internal conductor layers 31) and multiple second internal electrode layers 32 (second internal conductor layers 32). The multiple first internal electrode layers 31 are arranged on the multiple dielectric layers 20. The multiple second internal electrode layers 32 are arranged on the multiple dielectric layers 20. The multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 are arranged alternately in the height direction T of the laminate 10 with the dielectric layer 20 interposed therebetween. The first internal electrode layers 31 and the second internal electrode layers 32 are arranged so as to sandwich the dielectric layer 20 therebetween.
[0022] The first internal electrode layer 31 has a first opposing portion 31A opposing the second internal electrode layer 32, and a first lead portion 31B led from the first opposing portion 31A to the first end face LS1. The first lead portion 31B is exposed at the first end face LS1.
[0023] The second internal electrode layer 32 has a second opposing portion 32A opposing the first internal electrode layer 31, and a second lead portion 32B led from the second opposing portion 32A to the second end face LS2. The second lead portion 32B is exposed at the second end face LS2.
[0024] In this embodiment, the first opposing portion 31A and the second opposing portion 32A face each other via the dielectric layer 20, forming a capacitance and exhibiting the characteristics of a capacitor.
[0025] The shapes of the first opposing portion 31A and the second opposing portion 32A are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or the corners of the rectangular shape may be formed at an angle. The shapes of the first drawn-out portion 31B and the second drawn-out portion 32B are not particularly limited, but are preferably rectangular. However, the corners of the rectangular shape may be rounded or the corners of the rectangular shape may be formed at an angle.
[0026] The dimension in the width direction W of the first opposing portion 31A and the dimension in the width direction W of the first drawn-out portion 31B may be the same dimension, or one of the dimensions may be smaller. The dimension in the width direction W of the second opposing portion 32A and the dimension in the width direction W of the second drawn-out portion 32B may be the same dimension, or one of the dimensions may be smaller.
[0027] The first internal electrode layer 31 and the second internal electrode layer 32 are made of an appropriate conductive material such as a metal such as Ni, Cu, Ag, Pd, Au, or an alloy containing at least one of these metals. When an alloy is used, the first internal electrode layer 31 and the second internal electrode layer 32 may be made of, for example, an Ag-Pd alloy.
[0028] The thickness of each of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably, for example, about 0.2 μm or more and 3.0 μm or less. The total number of the first internal electrode layers 31 and the second internal electrode layers 32 is preferably 5 to 350.
[0029] The first main surface side outer layer portion 12 is located on the first main surface TS1 side of the laminate 10. The first main surface side outer layer portion 12 is an assembly of dielectric layers 20 as a plurality of ceramic layers located between the first main surface TS1 and the internal electrode layer 30 closest to the first main surface TS1. That is, the first main surface side outer layer portion 12 is formed of a plurality of dielectric layers 20 located between the first main surface TS1 and the internal electrode layer 30 located closest to the first main surface TS1 side among the plurality of internal electrode layers 30. The dielectric layer 20 used in the first main surface side outer layer portion 12 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0030] The second main surface side outer layer portion 13 is located on the second main surface TS2 side of the laminate 10. The second main surface side outer layer portion 13 is an assembly of dielectric layers 20 as a plurality of ceramic layers located between the second main surface TS2 and the internal electrode layer 30 closest to the second main surface TS2. That is, the second main surface side outer layer portion 13 is formed of a plurality of dielectric layers 20 located between the second main surface TS2 and the internal electrode layer 30 located closest to the second main surface TS2 side among the plurality of internal electrode layers 30. The dielectric layer 20 used in the second main surface side outer layer portion 13 may be the same as the dielectric layer 20 used in the internal layer portion 11.
[0031] As described above, the laminate 10 has a plurality of laminated dielectric layers 20 and a plurality of internal electrode layers 30 laminated on the dielectric layers 20. In other words, the multilayer ceramic capacitor 1 has the laminate 10 in which the dielectric layers 20 and the internal electrode layers 30 are alternately laminated.
[0032] The laminate 10 has a counter electrode portion 11E. The counter electrode portion 11E is a portion where the first counter portion 31A of the first internal electrode layer 31 and the second counter portion 32A of the second internal electrode layer 32 face each other. The counter electrode portion 11E is configured as a part of the inner layer portion 11. FIG. 7 shows the range in the length direction L of the counter electrode portion 11E. FIG. 8 shows the range in the width direction W of the counter electrode portion 11E. FIG. 9 shows the range in the width direction W and length direction L of the counter electrode portion 11E. The counter electrode portion 11E is also called a capacitor effective portion.
[0033] The laminate 10 has a side surface outer layer portion. The side surface outer layer portion has a first side surface outer layer portion WG1 and a second side surface outer layer portion WG2. The first side surface outer layer portion WG1 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the first side surface WS1. The second side surface outer layer portion WG2 is a portion including the dielectric layer 20 located between the counter electrode portion 11E and the second side surface WS2. In FIG. 8 and FIG. 9, the range of the width direction W of the first side surface outer layer portion WG1 and the second side surface outer layer portion WG2 are shown. The first side surface outer layer portion WG1 and the second side surface outer layer portion WG2 are also called W gaps or side gaps.
[0034] The laminate 10 has an end surface side outer layer portion. The end surface side outer layer portion has a first end surface side outer layer portion LG1 and a second end surface side outer layer portion LG2. The first end surface side outer layer portion LG1 is a portion including the dielectric layer 20 and the first lead portion 31B located between the counter electrode portion 11E and the first end surface LS1. The second end surface side outer layer portion LG2 is a portion including the dielectric layer 20 and the second lead portion 32B located between the counter electrode portion 11E and the second end surface LS2. FIG. 7 and FIG. 9 show the range of the length direction L of the first end surface side outer layer portion LG1 and the second end surface side outer layer portion LG2. The first end surface side outer layer portion LG1 and the second end surface side outer layer portion LG2 are also called L gaps or end gaps.
[0035] The external electrode 40 has a first external electrode 40A arranged on the first end face LS1 side, and a second external electrode 40B arranged on the second end face LS2 side.
[0036] The first external electrode 40A is preferably disposed at least on the first end face LS1. In this embodiment, the first external electrode 40A is disposed on the first end face LS1, a part of the first main surface TS1, a part of the second main surface TS2, a part of the first side surface WS1, and a part of the second side surface WS2. In this embodiment, the first external electrode 40A is connected to the first internal electrode layer 31 on the first end face LS1. The first external electrode 40A may be disposed, for example, extending from the first end face LS1 to a part of the first main surface TS1. In other words, the cross-sectional shape of the first external electrode 40A may be L-shaped (not shown). The part of the first external electrode 40A disposed on the first end face LS1 is connected to a lead terminal 500 (described later) via a first bonding material 5A (described later).
[0037] In addition, when the first external electrode 40A is also provided on the first main surface TS1, the second main surface TS2, the first side surface WS1, and the second side surface WS2, it is preferable that the length L1 in the longitudinal direction L of the first external electrode 40A provided on these surfaces is 10% or more and 40% or less of the L dimension of the laminate 10 (for example, 20 μm or more and 4000 μm or less).
[0038] Furthermore, when the first external electrode 40A is provided also on the first main surface TS1 and the second main surface TS2, it is preferable that the length W1 in the width direction W of the first external electrode 40A provided on these surfaces is substantially equal to the dimension W of the laminate 10 (for example, 0.1 mm or more and 10 mm or less). When the first external electrode 40A is provided also on the first side surface WS1 and the second side surface WS2, it is preferable that the length T1 in the height direction T of the first external electrode 40A provided on these portions is substantially equal to the dimension T of the laminate 10 (for example, 0.1 mm or more and 10 mm or less).
[0039] The second external electrode 40B is preferably disposed at least on the second end face LS2 and a part of the first main surface TS1. In this embodiment, the second external electrode 40B is disposed on the second end face LS2, a part of the first main surface TS1, a part of the second main surface TS2, a part of the first side surface WS1, and a part of the second side surface WS2. In this embodiment, the first external electrode 40A is connected to the second internal electrode layer 32 on the second end face LS2. The second external electrode 40B may be disposed, for example, extending from the second end face LS2 to a part of the first main surface TS1. In other words, the cross-sectional shape of the second external electrode 40B may be L-shaped (not shown). Of the second external electrode 40B, the portion disposed on the first main surface TS1 is connected to a second metal terminal 100B (described later) via a second bonding material 5B (described later).
[0040] In addition, when the second external electrode 40B is also provided on the first main surface TS1, the second main surface TS2, the first side surface WS1, and the second side surface WS2, the length L2 in the longitudinal direction L of the second external electrode 40B provided on these surfaces is preferably 10% or more and 40% or less of the L dimension of the laminate 10 (for example, 20 μm or more and 4000 μm or less).
[0041] Furthermore, when the second external electrode 40B is also provided on the first main surface TS1 and the second main surface TS2, it is preferable that the length W1 in the width direction W of the second external electrode 40B provided on these surfaces is substantially equal to the dimension W of the laminate 10 (for example, 0.1 mm or more and 10 mm or less). When the second external electrode 40B is also provided on the first side surface WS1 and the second side surface WS2, it is preferable that the length T1 in the height direction T of the second external electrode 40B provided on these portions is substantially equal to the dimension T of the laminate 10 (for example, 0.1 mm or more and 10 mm or less).
[0042] 6, in this embodiment, the length L3 of the portion of the surface of the laminate 10 that is exposed from the external electrode 40 in the longitudinal direction L is preferably 20% to 80% (e.g., 40 μm to 8000 μm) of the L dimension of the laminate. In other words, the separation distance L3 between the first external electrode 40A and the second external electrode 40B is preferably 20% to 80% (e.g., 40 μm to 8000 μm) of the L dimension of the laminate.
[0043] As described above, in the laminate 10, the first opposing portion 31A of the first internal electrode layer 31 and the second opposing portion 32A of the second internal electrode layer 32 face each other via the dielectric layer 20, thereby forming a capacitance. Therefore, the characteristics of a capacitor are exhibited between the first external electrode 40A to which the first internal electrode layer 31 is connected and the second external electrode 40B to which the second internal electrode layer 32 is connected.
[0044] The first external electrode 40A has a first base electrode layer 50A and a first plating layer 60A disposed on the first base electrode layer 50A.
[0045] The second external electrode 40B has a second base electrode layer 50B and a second plating layer 60B disposed on the second base electrode layer 50B.
[0046] The first base electrode layer 50A is disposed on the first end face LS1. The first base electrode layer 50A is connected to the first internal electrode layer 31. In this embodiment, the first base electrode layer 50A is formed to extend from the first end face LS1 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0047] The second base electrode layer 50B is disposed on the second end face LS2. The second base electrode layer 50B is connected to the second internal electrode layer 32. In this embodiment, the second base electrode layer 50B is formed to extend from the second end face LS2 to a part of the first main surface TS1 and a part of the second main surface TS2, as well as a part of the first side surface WS1 and a part of the second side surface WS2.
[0048] The first base electrode layer 50A and the second base electrode layer 50B of this embodiment are baked layers. The baked layer preferably contains a metal component and either a glass component or a ceramic component, or both. The metal component includes at least one selected from, for example, Cu, Ni, Ag, Pd, Ag-Pd alloy, Au, etc. The glass component includes at least one selected from, for example, B, Si, Ba, Mg, Al, Li, etc. The ceramic component may be the same type of ceramic material as the dielectric layer 20, or a different type of ceramic material. The ceramic component includes at least one selected from, for example, BaTiO3, CaTiO3, (Ba,Ca)TiO3, SrTiO3, CaZrO3, etc.
[0049] The baked layer is, for example, a conductive paste containing glass and metal applied to the laminate and baked. The baked layer may be a laminated chip having an internal electrode layer and a dielectric layer and a conductive paste applied to the laminated chip, which are simultaneously baked, or a laminated chip having an internal electrode layer and a dielectric layer is baked to obtain a laminate, and then a conductive paste is applied to the laminate and baked. In the case where a laminated chip having an internal electrode layer and a dielectric layer and a conductive paste applied to the laminated chip are simultaneously baked, it is preferable to form the baked layer by baking a material to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as the dielectric layer 20 as the ceramic material to be added. The baked layer may be a multi-layered layer.
[0050] The thickness in the longitudinal direction of the first base electrode layer 50A located on the first end face LS1 is preferably, for example, about 10 μm or more and 200 μm or less at the center in the height direction T and width direction W of the first base electrode layer 50A.
[0051] The thickness in the longitudinal direction of the second base electrode layer 50B located on the second end face LS2 is preferably, for example, about 10 μm or more and 200 μm or less at the center in the height direction T and width direction W of the second base electrode layer 50B.
[0052] When the first base electrode layer 50A is provided on a portion of at least one of the first main surface TS1 or the second main surface TS2, the height-wise thickness of the first base electrode layer 50A provided on this portion is preferably, for example, approximately 5 μm or more and 40 μm or less at the center in the length direction L and width direction W of the first base electrode layer 50A provided on this portion.
[0053] When the first base electrode layer 50A is provided on a portion of at least one of the first side surface WS1 or the second side surface WS2, the widthwise thickness of the first base electrode layer 50A provided on this portion is preferably, for example, approximately 5 μm or more and 40 μm or less at the center in the length direction L and height direction T of the first base electrode layer 50A provided on this portion.
[0054] When the second base electrode layer 50B is provided on a portion of at least one of the first main surface TS1 or the second main surface TS2, the height-wise thickness of the second base electrode layer 50B provided on this portion is preferably, for example, approximately 5 μm or more and 40 μm or less at the center in the length direction L and width direction W of the second base electrode layer 50B provided on this portion.
[0055] When the second base electrode layer 50B is provided on a portion of at least one of the first side surface WS1 or the second side surface WS2, the widthwise thickness of the second base electrode layer 50B provided on this portion is preferably, for example, approximately 5 μm or more and 40 μm or less at the center in the length direction L and height direction T of the second base electrode layer 50B provided on this portion.
[0056] The first base electrode layer 50A and the second base electrode layer 50B are not limited to baked layers, but may be thin film layers. The thin film layer is a layer in which metal particles are deposited, formed by a thin film formation method such as sputtering or vapor deposition. The thin film layer preferably contains at least one metal selected from the group consisting of Mg, Al, Ti, W, Cr, Cu, Ni, Ag, Co, Mo, and V. This can increase the adhesive strength of the external electrode 40 to the laminate 10. The thin film layer may be a single layer or may be formed of multiple layers. For example, it may be formed of a two-layer structure of a NiCr layer and a NiCu layer.
[0057] When the thin film layer as the base electrode is formed by a sputtering electrode by a sputtering method, the sputtered electrode is preferably formed on a part of the first main surface TS1 and a part of the second main surface TS2 of the laminate 10. The sputtered electrode preferably contains at least one metal selected from, for example, Ni, Cr, Cu, etc. The thickness of the sputtered electrode is preferably 50 nm or more and 400 nm or less, and more preferably 50 nm or more and 130 nm or less.
[0058] As the base electrode layer, a sputtered electrode may be formed on a part of the first main surface TS1 and a part of the second main surface TS2 of the laminate 10, while a baked layer may be formed on the first end face LS1 and the second end face LS2. Alternatively, a plating layer (described later) may be formed directly on the laminate 10 without forming a base electrode layer on the first end face LS1 and the second end face LS2. When a baked layer is formed on the first end face LS1 and the second end face LS2, the baked layer may be disposed so as to extend not only on the first end face LS1 and the second end face LS2 but also on a part of the first main surface TS1 and a part of the second main surface TS2. In this case, the sputtered electrode may be disposed so as to overlap the baked layer.
[0059] The first plating layer 60A is disposed so as to cover the first base electrode layer 50A.
[0060] The second plating layer 60B is disposed so as to cover the second base electrode layer 50B.
[0061] The first plating layer 60A and the second plating layer 60B may contain at least one selected from, for example, Cu, Ni, Sn, Ag, Pd, an Ag-Pd alloy, Au, etc. The first plating layer 60A and the second plating layer 60B may each be formed of a plurality of layers. The first plating layer 60A and the second plating layer 60B are preferably of a two-layer structure in which a Sn plating layer is formed on a Ni plating layer.
[0062] The first plating layer 60A is disposed so as to cover the first base electrode layer 50A. In this embodiment, the first plating layer 60A has a first Ni plating layer 61A and a first Sn plating layer 62A located on the first Ni plating layer 61A.
[0063] The second plating layer 60B is disposed so as to cover the second base electrode layer 50B. In the present embodiment, the second plating layer 60B has a second Ni plating layer 61B and a second Sn plating layer 62B located on the second Ni plating layer 61B.
[0064] The Ni plating layer prevents the first base electrode layer 50A and the second base electrode layer 50B from being eroded by solder serving as a bonding material 5 to be described later for bonding the multilayer ceramic capacitor body 2 and the metal terminal 100. The Sn plating layer improves the wettability of the solder serving as a bonding material 5 to be described later for bonding the multilayer ceramic capacitor body 2 and the metal terminal 100. This facilitates bonding between the multilayer ceramic capacitor body 2 and the metal terminal 100. When the first plating layer 60A and the second plating layer 60B each have a two-layer structure of a Ni plating layer and a Sn plating layer, the thickness of each of the Ni plating layer and the Sn plating layer is preferably 1 μm or more and 15 μm or less.
[0065] The first external electrode 40A and the second external electrode 40B of this embodiment may have a conductive resin layer containing, for example, conductive particles and a thermosetting resin. When a conductive resin layer is provided as the base electrode layer (first base electrode layer 50A, second base electrode layer 50B), the conductive resin layer may be disposed so as to cover the baked layer, or may be disposed directly on the laminate 10 without providing a baked layer. When the conductive resin layer is disposed so as to cover the baked layer, the conductive resin layer is disposed between the baked layer and the plating layer (first plating layer 60A, second plating layer 60B). The conductive resin layer may completely cover the baked layer, or may cover a part of the baked layer.
[0066] The conductive resin layer containing a thermosetting resin is more flexible than a conductive layer made of, for example, a plating film or a fired conductive paste. Therefore, even if the multilayer ceramic capacitor 1 is subjected to a physical shock or a shock caused by a thermal cycle, the conductive resin layer functions as a buffer layer. Therefore, the conductive resin layer suppresses the occurrence of cracks in the multilayer ceramic capacitor 1.
[0067] The metal constituting the conductive particles may be Ag, Cu, Ni, Sn, Bi, or an alloy containing them. The conductive particles preferably contain Ag. The conductive particles are, for example, Ag metal powder. Ag has the lowest resistivity among metals, so it is suitable as an electrode material. In addition, Ag is a precious metal, so it is resistant to oxidation and has high weather resistance. Therefore, Ag metal powder is suitable as a conductive particle.
[0068] The conductive particles may be metal powder with Ag coating on the surface. When using metal powder with Ag coating on the surface, the metal powder is preferably Cu, Ni, Sn, Bi or an alloy powder thereof. In order to make the base metal inexpensive while maintaining the characteristics of Ag, it is preferable to use Ag-coated metal powder.
[0069] Furthermore, the conductive particles may be Cu or Ni that has been subjected to an anti-oxidation treatment. The conductive particles may also be metal powders whose surfaces are coated with Sn, Ni, or Cu. When using metal powders whose surfaces are coated with Sn, Ni, or Cu, the metal powder is preferably Ag, Cu, Ni, Sn, Bi, or an alloy powder thereof.
[0070] The shape of the conductive particles is not particularly limited. The conductive particles may be spherical, flat, or the like, but it is preferable to use a mixture of spherical metal powder and flat metal powder.
[0071] The conductive particles contained in the conductive resin layer mainly play a role in ensuring the electrical conductivity of the conductive resin layer. Specifically, a plurality of conductive particles come into contact with each other to form an electrical path inside the conductive resin layer.
[0072] The resin constituting the conductive resin layer may contain at least one selected from various known thermosetting resins such as epoxy resin, phenol resin, urethane resin, silicone resin, and polyimide resin. Among them, epoxy resin, which has excellent heat resistance, moisture resistance, and adhesion, is one of the most suitable resins. In addition, it is preferable that the resin of the conductive resin layer contains a curing agent together with the thermosetting resin. When an epoxy resin is used as the base resin, the curing agent of the epoxy resin may be various known compounds such as phenol-based, amine-based, acid anhydride-based, imidazole-based, active ester-based, and amide-imide-based compounds.
[0073] The conductive resin layer may be formed of a plurality of layers. The conductive resin layer preferably has a thickness of 10 μm or more and 150 μm or less at its thickest portion.
[0074] Alternatively, a configuration may be adopted in which a first plating layer 60A and a second plating layer 60B, which will be described later, are disposed directly on the laminate 10 without providing the first base electrode layer 50A and the second base electrode layer 50B. That is, the multilayer ceramic capacitor 1 may be configured to include plating layers that are directly and electrically connected to the first internal electrode layer 31 and the second internal electrode layer 32. In such a case, the plating layers may be formed after a catalyst is disposed on the surface of the laminate 10 as a pretreatment.
[0075] Even in this case, the plating layer is preferably a multi-layer. The lower plating layer and the upper plating layer each preferably contain at least one metal selected from, for example, Cu, Ni, Sn, Pb, Au, Ag, Pd, Bi, or Zn, or an alloy containing these metals. The lower plating layer is more preferably formed using Ni, which has solder barrier properties. The upper plating layer is more preferably formed using Sn or Au, which has good solder wettability. For example, when the first internal electrode layer 31 and the second internal electrode layer 32 are formed using Ni, the lower plating layer is preferably formed using Cu, which has good bonding properties with Ni. The upper plating layer may be formed as necessary, and the external electrode 40 may be composed of only the lower plating layer. In addition, the plating layer may be the upper plating layer as the outermost layer, or another plating layer may be formed on the surface of the upper plating layer.
[0076] The thickness of each plating layer disposed without providing a base electrode layer is preferably 2 μm to 10 μm. The plating layer preferably does not contain glass. The metal ratio per unit volume of the plating layer is preferably 99 volume % or more.
[0077] In addition, when the plating layer is formed directly on the laminate 10, the thickness of the base electrode layer can be reduced. Therefore, the dimension in the height direction T of the multilayer ceramic capacitor body 2 can be reduced by the amount of the reduction in the thickness of the base electrode layer, and the height of the multilayer ceramic capacitor body 2 can be reduced. Alternatively, the thickness of the dielectric layer 20 sandwiched between the first internal electrode layer 31 and the second internal electrode layer 32 can be increased by the amount of the reduction in the thickness of the base electrode layer, and the thickness of the element can be improved. In this way, by forming the plating layer directly on the laminate 10, the design freedom of the multilayer ceramic capacitor can be improved.
[0078] If the lengthwise dimension of the multilayer ceramic capacitor body 2 including the laminate 10 and the external electrodes 40 is taken as L dimension, then the L dimension is preferably 0.2 mm or more and 10 mm or less. If the heightwise dimension of the multilayer ceramic capacitor body 2 is taken as T dimension, then the T dimension is preferably 0.1 mm or more and 10 mm or less. If the widthwise dimension of the multilayer ceramic capacitor body 2 is taken as W dimension, then the W dimension is preferably 0.1 mm or more and 10 mm or less.
[0079] In this embodiment, the first surface S1 on the first end face LS1 side of the multilayer ceramic capacitor body 2 is formed by the surface of the first external electrode 40A arranged on the first end face LS1. The second surface S2 on the second end face LS2 side of the multilayer ceramic capacitor body 2 is formed by the surface of the second external electrode 40B arranged on the second end face LS2.
[0080] The exterior material 3 will be described with reference to Fig. 10 in addition to Figs. 1 to 5. Fig. 10 is an enlarged view of a portion X of the multilayer ceramic capacitor shown in Fig. 5.
[0081] The exterior packaging material 3 includes a first main surface MTS1 and a second main surface MTS2 facing in a height direction T, a first side surface MWS1 and a second side surface MWS2 facing in a width direction W perpendicular to the height direction T, and a first end surface MLS1 and a second end surface MLS2 facing in a length direction L perpendicular to the height direction T and the width direction W. The first end surface MLS1 of the exterior packaging material 3 is the surface of the exterior packaging material 3 facing the first end surface LS1 of the laminate 10. The second end surface MLS2 of the exterior packaging material 3 is the surface of the exterior packaging material 3 facing the second end surface LS2 of the laminate 10.
[0082] The first side surface MWS1, the second side surface MWS2, the first end surface MLS1, and the second end surface MLS2 of the exterior packaging material 3 have a parting line PL near the center in the height direction T. The parting line PL is a line that corresponds to the parting surface of a mold used when molding the exterior packaging material 3. The surface of the exterior packaging material 3 has a draft slope with the parting line PL as the boundary.
[0083] The first side surface MWS1 of the exterior cladding material 3 has a surface MWS1A on the first main surface side and a surface MWS1B on the second main surface side. The second side surface MWS2 of the exterior cladding material 3 has a surface MWS2A on the first main surface side and a surface MWS2B on the second main surface side. The first end surface MLS1 of the exterior cladding material 3 has a surface MLS1A on the first main surface side and a surface MLS1B on the second main surface side. The second end surface MLS2 of the exterior cladding material 3 has a surface MLS2A on the first main surface side and a surface MLS2B on the second main surface side. These first main surface side and second main surface side surfaces are arranged separated by a parting line PL as a boundary.
[0084] Each of the surfaces MWS1A, MWS2A, MLS1A, and MLS2A on the first principal surface side has a draft gradient such that the cross-sectional area of the LW cross section of the exterior material 3 decreases from the parting line PL toward the first principal surface TS1. Each of the surfaces MWS1B, MWS2B, MLS1B, and MLS2B on the second principal surface side has a draft gradient such that the cross-sectional area of the LW cross section of the exterior material 3 decreases from the parting line PL toward the second principal surface TS2.
[0085] The exterior material 3 covers the multilayer ceramic capacitor body 2, a portion of the metal terminal 100, and the fuse 200. Specifically, the exterior material 3 is arranged so as to cover the entire multilayer ceramic capacitor body 2, a portion of a first metal terminal 100A (to be described later) constituting the metal terminal 100, a portion of a second metal terminal 100B (to be described later) constituting the metal terminal, and the entire fuse 200.
[0086] The second main surface MTS2 of the packaging material 3 is preferably configured to be planar with a predetermined flatness. This makes it possible to prevent poor suction by a mounter of a mounting machine used when mounting the multilayer ceramic capacitor 1 on a mounting board. This makes it possible to reliably mount the multilayer ceramic capacitor 1 on the mounting board. As a result, it becomes possible to suppress the occurrence of mounting defects.
[0087] The exterior material 3 has a first exterior material 3A that covers the multilayer ceramic capacitor body 2, a portion of the first metal terminal 100A, and a portion of the second metal terminal 100B, and a second exterior material 3B that covers at least a portion of the first exterior material 3A.
[0088] The second packaging material 3B is preferably disposed on at least one of the surfaces of the first main surface TS1 side, the second main surface TS2 side, the first side surface WS1 side, and the second side surface WS2 side of the first packaging material 3A, corresponding to the position where the fuse 200 is disposed. However, the second packaging material 3B may be disposed on the surface of the first end surface LS1 side or the surface of the second end surface LS2 side of the first packaging material 3A, corresponding to the position where the fuse 200 is disposed. In this embodiment, the fuse 200 is disposed on the surface F of the second main surface TS2 side of the first packaging material 3A. Therefore, the second packaging material 3B is disposed so as to cover the surface F of the second main surface TS2 side of the first packaging material 3A.
[0089] In this embodiment, the first exterior material 3A is a thermosetting resin. The second exterior material 3B is a thermoplastic resin. The first exterior material 3A may be, for example, a thermosetting epoxy resin. The second exterior material 3B may be, for example, polyethylene, polypropylene, polyamide, or polystyrene. As a result, since the fuse 200 is covered by the exterior material 3 under normal circumstances, creeping discharge can be suppressed. Then, when an overcurrent occurs, the fuse 200 covered by the second exterior material 3B, which is a thermoplastic resin that melts by heat, can be appropriately disconnected.
[0090] The first exterior material 3A and the second exterior material 3B may be different types of thermosetting resin. In this case, the heat resistance temperature of the second exterior material 3B is lower than the heat resistance temperature of the first exterior material 3A. For example, the first exterior material 3A may be a thermosetting epoxy resin. The second exterior material 3B may be a thermosetting resin having a lower heat resistance temperature than the thermosetting epoxy resin. The second exterior material 3B may be, for example, polyurethane.
[0091] The first exterior material 3A and the second exterior material 3B may be different types of thermoplastic resins. In this case, the melting point of the second exterior material 3B is lower than the melting point of the first exterior material 3A. For example, the first exterior material 3A may be polyamide. The second exterior material 3B may be a thermoplastic resin having a melting point lower than that of polyamide. The second exterior material 3B may be, for example, polyethylene.
[0092] Thus, the heat resistance temperature of the second exterior material 3B is preferably lower than that of the first exterior material 3A. The heat resistance temperature of the first exterior material 3A is preferably 200°C or more and 400°C or less, and more preferably 250°C or more and 350°C or less. The heat resistance temperature of the second exterior material 3B is preferably 70°C or more and less than 200°C, and more preferably 70°C or more and 150°C or less. As a result, since the fuse 200 is covered by the exterior material 3 under normal conditions, creeping discharge can be suppressed. Then, when an overcurrent occurs, the fuse 200 covered by the second exterior material 3B, which is a resin with a low heat resistance temperature, can be appropriately disconnected. The heat resistance temperature of a thermosetting resin is defined by its glass transition temperature. The heat resistance of a thermoplastic resin is defined by its melting point.
[0093] The first and second exterior materials 3A and 3B constituting the exterior material 3 are preferably made of resin. For example, the first and second exterior materials 3A and 3B may be formed by molding engineering plastics by a transfer molding method, an injection molding method, or the like. In particular, the material of the first exterior material 3A is preferably made of a thermosetting epoxy resin. This ensures adhesion between the first exterior material 3A and the multilayer ceramic capacitor body 2 and the metal terminals 100, and can improve the withstand voltage and moisture resistance. The first and second exterior materials 3A and 3B may be formed by painting, for example, a liquid or powdered silicone or epoxy resin.
[0094] As described above, the insulating surface distance (creepage distance) between the conductors can be secured by the exterior material 3 covering a wide range of the conductor metal parts, such as the external electrode 40 and the metal terminal 100. In addition, by covering a wide range of the conductor metal parts with the exterior material 3, the risk of surface discharge can be avoided.
[0095] The shape of the exterior material 3 is not particularly limited. For example, it may be a truncated pyramid such as a pyramid. The shape of the corners of the exterior material 3 is not particularly limited and may be rounded.
[0096] The metal terminal 100 will be described with reference to FIG. 10 in addition to FIG. 1 to FIG.
[0097] The metal terminal 100 includes a first metal terminal 100A and a second metal terminal 100B. In this embodiment, the metal terminal 100 further includes a lead-out terminal 500 connected to the first metal terminal 100A via a fuse.
[0098] The first metal terminal 100A and the second metal terminal 100B are metal terminals mounted on a mounting surface of a mounting board (see mounting board 310 in FIG. 11) to be described later on, on which the multilayer ceramic capacitor 1 is to be mounted. The first metal terminal 100A and the second metal terminal 100B are, for example, plate-shaped lead frames. In this embodiment, the first main surface TS1 of the laminate 10 is a surface facing the mounting surface of the mounting board on which the multilayer ceramic capacitor 1 is to be mounted.
[0099] As shown in FIG. 10, the lead-out terminal 500 has a first joint 510 connected to the first external electrode 40A, and a first fuse connecting portion 520 connected to the first metal terminal 100A via the fuse 200, which is connected to the first joint 510 and extends away from the mounting surface of the mounting board. In this embodiment, the lead-out terminal 500 is made of a metal plate having a substantially linear cross section, and an end P1 of the first fuse connecting portion 520 is slightly bent. In this embodiment, the first joint 510 faces the first end face LS1 and is connected to the first surface S1 on the first end face LS1 side of the first external electrode 40A. However, the aspect of the lead-out terminal is not limited thereto. For example, the first joint 510 may face the first main surface TS1 and be connected to the surface on the first main surface TS1 side of the first external electrode 40A. In this case, the lead-out terminal 500 may be made of a metal plate having a substantially L-shaped cross section.
[0100] 5 and 10, the first metal terminal 100A has a second fuse connecting portion 120A connected to the lead-out terminal 500 via the fuse 200, a first extension portion 130A connected to the second fuse connecting portion 120A and extending in the length direction L away from the multilayer ceramic capacitor body 2, a first falling portion 140A connected to the first extension portion 130A and extending toward the mounting surface side of the mounting board, and a first mounting portion 150A connected to the first falling portion 140A and extending in a direction along the mounting surface of the mounting board. In this embodiment, the end P2 of the second fuse connecting portion 120A is slightly bent.
[0101] The distance between the end P1 of the first fuse connecting portion 520 of the draw-out terminal 500 and the end P2 of the second fuse connecting portion 120A of the first metal terminal 100A is preferably 500 μm or more and 2000 μm or less. This makes it possible to suppress the occurrence of dielectric breakdown after the fuse is blown. The end P1 of the first fuse connecting portion 520 of the draw-out terminal 500 and the end P2 of the second fuse connecting portion 120A of the first metal terminal 100A are preferably arranged to protrude from the surface F of the first exterior material 3A.
[0102] As shown in FIG. 5, the second metal terminal 100B has a second joint portion 110B facing the first main surface TS1 and connected to the second external electrode 40B, a second rising portion 120B connected to the second joint portion 110B, extending away from the mounting surface of the mounting board, and facing the second end face LS2, a second extension portion 130B connected to the second rising portion 120B and extending in the length direction L away from the multilayer ceramic capacitor body 2, a second falling portion 140B connected to the second extension portion 130B and extending toward the mounting surface of the mounting board, and a second mounting portion 150B connected to the second falling portion 140B and extending in a direction along the mounting surface of the mounting board.
[0103] It is preferable that the first falling portion 140A and the second falling portion 140B extend toward the mounting surface of the mounting board to an extent that enables a gap to be provided between the exterior material 3 of the multilayer ceramic capacitor 1 and the mounting surface of the mounting board.
[0104] As shown in Fig. 4, the first metal terminal 100A may have a first notch 180A. The second metal terminal 100B may have a second notch 180B.
[0105] As shown in FIG. 5, the separation distance L4 between the first mounting portion 150A of the first metal terminal 100A and the second mounting portion 150B of the second metal terminal 100B is longer than the separation distance L3 between the first external electrode 40A and the second external electrode 40B of the multilayer ceramic capacitor body 2.
[0106] The exterior material 3 is arranged so as to cover the entirety of the lead-out terminal 500. The exterior material 3 is also arranged so as to cover the entirety of the second fuse connecting portion 120A and at least a part of the first extension portion 130A of the first metal terminal 100A. The exterior material 3 is also arranged so as to cover the entirety of the second joint portion 110B, the entirety of the second rising portion 120B, and at least a part of the second extension portion 130B of the second metal terminal 100B.
[0107] In this embodiment, the first extension portion 130A of the first metal terminal 100A protrudes from the first end face MLS1 of the outer casing 3 and is partially exposed. The second extension portion 130B of the second metal terminal 100B protrudes from the second end face MLS2 of the outer casing 3 and is partially exposed. More specifically, the first extension portion 130A of the first metal terminal 100A protrudes from the parting line PL of the first end face MLS1 of the outer casing 3 and is partially exposed. The second extension portion 130B of the second metal terminal 100B protrudes from the parting line PL of the second end face MLS2 of the outer casing 3 and is partially exposed.
[0108] The first metal terminal 100A, the second metal terminal 100B, and the lead-out terminal 500 each have a terminal body and a plating film disposed on the surface of the terminal body.
[0109] The terminal body is preferably made of Ni, Fe, Cu, Ag, Cr, or an alloy containing at least one of these metals as a main component. For example, the base metal of the terminal body can be an Fe-42Ni alloy, an Fe-18Cr alloy, or a Cu-8Sn alloy. From the viewpoint of heat dissipation, the base metal of the terminal body can be oxygen-free copper or a Cu-based alloy with high thermal conductivity. In this way, by making the material of the terminal body a copper-based material with good thermal conductivity, it is possible to achieve low ESR and low thermal resistance. In this embodiment, the base metal of the terminal body can be stainless steel or aluminum with low solder wettability. At least the surface of the base metal of the terminal body has a surface with lower solder wettability than the plating film on the outermost surface. The thickness of the terminal body is preferably about 0.05 mm or more and 0.5 mm or less.
[0110] The plating film preferably has an upper layer plating film disposed on the outermost surface of the plating film and a lower layer plating film disposed below the upper layer plating film. For example, the plating film may have a two-layer structure in which an upper layer plating film is formed on a lower layer plating film. The lower layer plating film is preferably made of Ni, Fe, Cu, Ag, Cr, or an alloy containing one or more of these metals as a main component. More preferably, the lower layer plating film is made of Ni, Fe, Cr, or an alloy containing one or more of these metals as a main component. By forming the lower layer plating film from an alloy containing high melting point Ni, Fe, Cr, or one or more of these metals as a main component, the heat resistance of the metal terminal 100 can be improved. The thickness of the lower layer plating film is preferably about 0.2 μm or more and 5.0 μm or less. The upper layer plating film is preferably made of an alloy containing Sn, Ag, Au, or one or more of these metals as a main component. More preferably, the upper layer plating film is made of Sn or an alloy containing Sn as a main component. By forming the upper layer plating film from Sn or an alloy containing Sn as a main component, it is possible to improve the solderability between the external electrode 40 and the metal terminal 100. The thickness of the upper layer plating film is preferably about 1.0 μm or more and 5.0 μm or less.
[0111] The upper layer plating film disposed on the outermost surface of the plating film has a surface that is more wettable to solder than the surface of the base metal of the terminal body. The upper layer plating film disposed on the outermost surface of the plating film has a surface that is more wettable to solder than the surface of the lower layer plating film. For example, the lower layer plating film is preferably a Ni plating film. The upper layer plating film is preferably a Sn plating film.
[0112] The first metal terminal 100A, the second metal terminal 100B and the lead terminal 500 may have an exposed surface in which the material inside the plating film of the outermost surface of the plating film is exposed on the surface. By providing an exposed surface on a part of the surface, it becomes difficult for solder to flow to that part, and therefore it is possible to prevent problems such as solder splash.
[0113] Here, the exposed surface may be a surface where a lower layer plating film is exposed. The lower layer plating film has a lower wettability with solder than the upper layer plating film. The exposed surface may be a surface where a base material of the terminal body is exposed. The surface of the base material of the terminal body has a lower wettability with solder than the upper layer plating film.
[0114] The exposed surface may be formed by performing a removal process after forming a plating film on the terminal body. The removal process may be, for example, various removal processes such as mechanical removal processes by grinding or polishing, removal processes by laser trimming, removal processes using a plating stripper such as sodium hydroxide, etc. Also, before forming the plating film, the part to be the exposed surface may be covered with a resist. In this case, the exposed surface is formed by removing the resist after forming the plating film.
[0115] The bonding material 5 includes a first bonding material 5A and a second bonding material 5B.
[0116] 5, the lead-out terminal 500 is connected to the first external electrode 40A via a first bonding material 5A. The second metal terminal 100B is connected to the second external electrode 40B via a second bonding material 5B.
[0117] The bonding material 5 is preferably a solder. For example, it may be a Pb-free solder. As the Pb-free solder, for example, a lead-free solder such as Sn-Sb, Sn-Ag-Cu, Sn-Cu, or Sn-Bi is preferable. For example, Sn-10Sb to Sn-15Sb solder can be used.
[0118] The fuse 200 electrically connects the first external electrode 40A and the first metal terminal 100A. In this embodiment, the fuse 200 electrically connects the first external electrode 40A and the first metal terminal 100A by connecting the first fuse connecting portion 520 of the lead-out terminal 500 and the second fuse connecting portion 120A of the first metal terminal 100A. The end P1 of the first fuse connecting portion 520 and the fuse 200 may be electrically connected by, for example, wire bonding. The end P2 of the second fuse connecting portion 120A and the fuse 200 may be electrically connected by, for example, wire bonding. However, the method of electrical connection is not limited thereto.
[0119] As shown in FIG. 10, the fuse 200 is embedded in the exterior material 3. At least a part of the fuse 200 is exposed from the first exterior material 3A and covered by the second exterior material 3B. More specifically, at least a part of the fuse 200 protrudes from the first exterior material 3A and is embedded so that the protruding and exposed part is surrounded by the second exterior material 3B. For example, it is preferable that the contact area of the part of the fuse 200 protruding from the first exterior material 3A and exposed to the second exterior material 3B is larger than the contact area of the part of the fuse 200 and exposed to the first exterior material 3A. In this embodiment, the fuse 200 is disposed on the surface F of the first exterior material 3A, and most of the surface of the fuse 200 is covered by the second exterior material 3B.
[0120] The length of the fuse 200 is preferably 500 μm or more and 2000 μm or less, which can prevent dielectric breakdown after the fuse is blown.
[0121] The thickness t of second exterior material 3B covering first exterior material 3A is preferably 10 μm or more and 1000 μm or less in the vicinity of fuse 200. The shortest distance d connecting the surface of fuse 200 embedded in exterior material 3 and the outer surface of second exterior material 3B is preferably 10 μm or more and 1000 μm or less.
[0122] The fuse 200 is made of a metal having a lower melting point than the metal constituting the terminal body of the first metal terminal 100A. The material of the fuse 200 may be, for example, Ag, Al, Sn, or an alloy of these metals. The heat resistance temperature of the second exterior material 3B is preferably lower than the melting temperature of the fuse 200. The heat resistance temperature of the first exterior material 3A is preferably higher than the melting temperature of the fuse 200.
[0123] As a result, under normal circumstances, creeping discharge can be suppressed because the fuse 200 is covered by the exterior material 3. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B having low heat resistance, can be properly disconnected.
[0124] Of the two external electrodes, the first external electrode 40A and the second external electrode 40B, the one electrically connected to the fuse 200 can be considered to be the first external electrode 40A. In addition to providing the fuse 200 between the first external electrode 40A and the first metal terminal 100A, the fuse 200 may also be provided between the second external electrode 40B and the second metal terminal 100B.
[0125] In the present embodiment, the fuse 200 is provided on the second main surface MTS2 side of the outer packaging material 3, but is not limited thereto. The fuse 200 may be disposed on any of the first main surface MTS1 side, the first side surface MWS1 side, the second side surface MWS2 side, the first end surface MLS1 side, and the second end surface MLS2 side of the outer packaging material 3. The second outer packaging material 3B is disposed on at least one of the surfaces of the first main surface TS1 side, the second main surface TS2 side, the first side surface WS1 side, the second side surface WS2 side, the first end surface LS1 side, and the second end surface LS2 side of the first outer packaging material 3A so as to cover the fuse 200. The second outer packaging material 3B may cover the entire surface of the first outer packaging material 3A together with the fuse 200. In this case, the second outer packaging material 3B may be formed by dipping.
[0126] If the lengthwise dimension of the multilayer ceramic capacitor 1 including the exterior material 3 and the metal terminals 100 is defined as L dimension, then the L dimension is preferably 3.2 mm or more and 20 mm or less. If the lengthwise dimension of the multilayer ceramic capacitor 1 in the stacking direction is defined as T dimension, then the T dimension is preferably 1.0 mm or more and 10 mm or less. If the widthwise dimension of the multilayer ceramic capacitor 1 is defined as W dimension, then the W dimension is preferably 1.5 mm or more and 20 mm or less.
[0127] Next, a method for manufacturing the multilayer ceramic capacitor 1 of this embodiment will be described. First, a method for manufacturing the multilayer ceramic capacitor body 2 will be described.
[0128] A dielectric sheet for the dielectric layer 20 and a conductive paste for the internal electrode layer 30 are prepared. The dielectric sheet and the conductive paste for the internal electrodes contain a binder and a solvent. The binder and the solvent may be known.
[0129] A conductive paste for the internal electrode layer 30 is printed in a predetermined pattern on the dielectric sheet by, for example, screen printing, gravure printing, etc. In this way, a dielectric sheet on which the pattern of the first internal electrode layer 31 is formed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is formed are prepared.
[0130] A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated to form a portion that will become the first main surface side outer layer portion 12 on the first main surface TS1 side. A dielectric sheet on which the pattern of the first internal electrode layer 31 is printed and a dielectric sheet on which the pattern of the second internal electrode layer 32 is printed are laminated in order thereon to form a portion that will become the internal layer portion 11. A predetermined number of dielectric sheets on which the pattern of the internal electrode layer is not printed are laminated on the portion that will become the internal layer portion 11 to form a portion that will become the second main surface side outer layer portion 13 on the second main surface TS2 side. In this way, a laminated sheet is produced.
[0131] The laminated sheets are pressed in the lamination direction by means of a hydrostatic press or the like to produce a laminated block.
[0132] The laminated block is cut to a predetermined size to obtain laminated chips. At this time, corners and edges of the laminated chips may be rounded by barrel polishing or the like.
[0133] The laminated chip is fired to produce the laminate 10. The firing temperature depends on the materials of the dielectric layers 20 and the internal electrode layers 30, but is preferably 900° C. or higher and 1400° C. or lower.
[0134] A conductive paste that will become the first base electrode layer 50A and the second base electrode layer 50B is applied to both end surfaces of the laminate 10. In this embodiment, the first base electrode layer 50A and the second base electrode layer 50B are baked layers. A conductive paste containing a glass component and a metal is applied to the laminate 10 by a method such as dipping. Then, a baking process is performed to form the first base electrode layer 50A and the second base electrode layer 50B. The temperature of the baking process at this time is preferably 700°C or higher and 900°C or lower.
[0135] In addition, when the laminated chip before firing and the conductive paste applied to the laminated chip are fired at the same time, it is preferable to form the fired layer by firing a material to which a ceramic material is added instead of a glass component. In this case, it is particularly preferable to use the same type of ceramic material as that of the dielectric layer 20 as the ceramic material to be added. In this case, the conductive paste is applied to the laminated chip before firing, and the laminated chip and the conductive paste applied to the laminated chip are fired at the same time to form the laminate 10 with the fired layer.
[0136] When forming thin film layers as the first base electrode layer 50A and the second base electrode layer 50B, the thin film layers may be formed on a part of the first main surface TS1 and a part of the second main surface TS2 of the laminate 10. The thin film layers may be sputtered electrodes formed by a sputtering method, for example. When forming sputtered electrodes as the first base electrode layer 50A and the second base electrode layer 50B on a part of the first main surface TS1 and a part of the second main surface TS2 of the laminate 10, baked layers may be formed on the first end surface LS1 and the second end surface LS2. Alternatively, a plating layer, which will be described later, may be formed directly on the laminate 10 without forming base electrode layers on the first end surface LS1 and the second end surface LS2.
[0137] Thereafter, a first plating layer 60A is formed on the surface of the first base electrode layer 50A. A second plating layer 60B is formed on the surface of the second base electrode layer 50B. In this embodiment, a Ni plating layer and a Sn plating layer are formed as the plating layers. The Ni plating layer and the Sn plating layer are formed in sequence, for example, by barrel plating.
[0138] Through these manufacturing steps, the multilayer ceramic capacitor body 2 is manufactured.
[0139] Next, a method for manufacturing the first metal terminal 100A, the second metal terminal 100B and the lead-out terminal 500 will be described.
[0140] A plating film is applied to the terminal body constituting the first metal terminal 100A, the second metal terminal 100B, and the lead-out terminal 500. Then, in the portion where solder is not desired to be attached, the film constituting at least the outermost surface of the plating film is peeled off. This forms an exposed surface that exposes a surface with low solder wettability. Alternatively, plating is applied to the terminal body in a state where the surface of the portion where solder is not desired to be attached is masked with a resist or the like. This may form an exposed surface that exposes a surface with low solder wettability.
[0141] Next, the process of joining the monolithic ceramic capacitor body 2 to the lead-out terminal 500 and the second metal terminal 100B will be described.
[0142] The first external electrode 40A and the lead-out terminal 500 are joined by a first bonding material 5A. The second external electrode 40B and the second metal terminal 100B are joined by a second bonding material 5B. In this embodiment, the first bonding material 5A and the second bonding material 5B are solder. For example, when bonding is performed by reflow soldering, the first bonding material 5A and the second bonding material 5B are heated at a temperature of, for example, 270° C. or higher and 290° C. or lower for 30 seconds or longer.
[0143] The heating during the reflow melts the first bonding material 5A and the second bonding material 5B. The first bonding material 5A then solidifies, bonding the multilayer ceramic capacitor body 2 to the lead-out terminal 500. The second bonding material 5B also solidifies, bonding the multilayer ceramic capacitor body 2 to the second metal terminal 100B.
[0144] Next, the process of covering the multilayer ceramic capacitor body 2, the first bonding material 5A and the second bonding material 5B, a portion of the first metal terminal 100A, a portion of the second metal terminal 100B, the lead-out terminal 500, and the fuse 200 with the exterior material 3 will be described.
[0145] The exterior material 3 is formed by, for example, a transfer molding method. Specifically, the multilayer ceramic capacitor body 2 is placed in a mold. After that, the mold is filled with resin, and the resin is cured to form the exterior material 3.
[0146] In this step, a first mold and a second mold are used. First, the multilayer ceramic capacitor body 2 to which the lead-out terminal 500 and the second metal terminal 100B are connected, and the first metal terminal 100A are set in the first mold. At this time, the end P1 of the first fuse connecting portion 520 of the lead-out terminal 500 and the end P2 of the second fuse connecting portion 120A of the first metal terminal 100A are placed in a groove provided in the first mold.
[0147] Next, a resin that will form the first exterior material 3A is injected into the first mold, and the first exterior material 3A is molded.
[0148] The molded product molded with the first exterior material 3A is removed from the first mold. A part of the metal terminal 100 is exposed from the removed molded product. Specifically, a part of the first extension portion 130A, the first falling portion 140A, the first mounting portion 150A, a part of the second extension portion 130B, the second falling portion 140B, and the second mounting portion 150B are exposed from the first exterior material 3A. Furthermore, the end P1 of the first fuse connecting portion 520 and the end P2 of the second fuse connecting portion 120A, which are portions that were disposed in the grooves provided in the first mold during molding, protrude and are exposed from the surface F of the first exterior material 3A.
[0149] Thereafter, the fuse 200 is disposed to connect between the end P1 of the first fuse connection portion 520 and the end P2 of the second fuse connection portion 120A. The fuse 200 may be disposed on the surface F of the first exterior material 3A.
[0150] The fuse 200 and the end P1 of the first fuse connecting portion 520, and the fuse 200 and the end P2 of the second fuse connecting portion 120A are respectively bonded by, for example, wire bonding. As a result, the end P1 of the first fuse connecting portion 520 and the end P2 of the second fuse connecting portion 120A are connected by the fuse 200.
[0151] The semi-finished product with the fuse joined is then set in a second mold.
[0152] Next, the resin constituting the second external packaging material 3B is injected into the second mold to mold the second external packaging material 3B. As a result, the fuse 200 protruding and exposed from the surface F of the first external packaging material 3A is covered with the second external packaging material 3B.
[0153] Second exterior material 3B may be formed by dipping or painting with resin without using a second mold. Even in this case, second exterior material 3B is formed so as to cover at least fuse 200.
[0154] Finally, if there is an unnecessary portion of the metal terminal 100, the unnecessary portion is cut off using a punching die or the like. Then, the metal terminal 100 is bent into a desired shape using a bending die or the like. In this manner, the metal terminal 100 may be formed by bending. That is, each connection portion of the metal terminal 100 that is bent may be formed by bending. Note that some bending is performed before the exterior material 3 is molded.
[0155] By the above-described manufacturing method, the multilayer ceramic capacitor 1 of the present embodiment is manufactured.
[0156] 11 shows a mounting structure 300 of the multilayer ceramic capacitor 1. FIG 11 is an external perspective view showing a mounting structure 300 in which the multilayer ceramic capacitor 1 of this embodiment is mounted on a mounting substrate 310.
[0157] The multilayer ceramic capacitor 1, which has been covered with the exterior material 3 and turned into a finished product, is then reflow-mounted as a component on a mounting board 310 via a bonding material 320 for mounting on a board.
[0158] Specifically, the first metal terminal 100A and the second metal terminal 100B are joined to the wiring member 312 arranged on the mounting surface 311 of the mounting substrate 310 via the bonding material 320 for mounting on the substrate. The second metal terminal 100B is joined to the wiring member 312 arranged on the mounting surface 311 of the mounting substrate 310 via the bonding material 320 for mounting on the substrate.
[0159] 11, in the mounted state, the fuse 200 is not exposed on the surface of the exterior material 3. Therefore, while creeping discharge is suppressed, the fuse 200 can function as described above when an overcurrent occurs.
[0160] A modified example of the multilayer ceramic capacitor 1 of this embodiment will be described below. In the following description, the same components as those in the above embodiment will be denoted by the same reference numerals, and detailed description will be omitted. Fig. 12 is a diagram showing a modified example of the multilayer ceramic capacitor 1 of this embodiment, and corresponds to Fig. 2.
[0161] In this modification, the configuration of the metal terminal is different from that of the above embodiment. The metal terminal of this modification has a first metal terminal 100C and a second metal terminal 100D.
[0162] Of the first metal terminal 100C, the configuration of the portion disposed inside the exterior material 3 is the same as the configuration of the first metal terminal 100A of the above embodiment. Of the second metal terminal 100D, the configuration of the portion disposed inside the exterior material 3 is the same as the configuration of the second metal terminal 100B of the above embodiment.
[0163] The first metal terminal 100C has a first extension 130C, a first falling portion 140C, and a first mounting portion 150C. The first extension 130C is connected to the first falling portion 140C immediately after protruding from the surface MLS1 on the first end face LS1 side of the exterior material 3. The connection portion between the first extension 130C and the first falling portion 140C is formed by bending at a substantially right angle. The first falling portion 140C extends toward the mounting surface in a direction substantially perpendicular to the mounting surface. The first mounting portion 150C extends along the mounting surface toward the center of the length direction L of the multilayer ceramic capacitor 1.
[0164] The second metal terminal 100D has a second extension 130D, a second falling portion 140D, and a second mounting portion 150D. The second extension 130D is connected to the second falling portion 140D immediately after protruding from the surface MLS2 on the second end face LS2 side of the exterior material 3. The connection portion between the second extension 130D and the second falling portion 140D is formed by bending at a substantially right angle. The second falling portion 140D extends toward the mounting surface in a direction substantially perpendicular to the mounting surface. The second mounting portion 150D extends along the mounting surface toward the center of the length direction L of the multilayer ceramic capacitor 1.
[0165] This makes it possible to shorten the dimension L8 in the longitudinal direction of the multilayer ceramic capacitor 1 including the first metal terminals 100C and the second metal terminals 100D, thereby making it possible to reduce the mounting area required when mounting the multilayer ceramic capacitor 1 on a mounting board.
[0166] Even in this case, it is preferable that the separation distance L7 between the end of the first mounting portion 150C of the first metal terminal 100C and the end of the second mounting portion 150D of the second metal terminal 100D is longer than the separation distance L3 between the first external electrode 40A and the second external electrode 40B of the multilayer ceramic capacitor body 2 shown in Figure 5.
[0167] In the multilayer ceramic capacitor body 2 of the present embodiment, the multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 are alternately arranged in the height direction T of the laminate 10, but the configuration of the multilayer ceramic capacitor body 2 is not limited to this. The multiple first internal electrode layers 31 and the multiple second internal electrode layers 32 may be alternately arranged in the width direction W of the laminate 10.
[0168] In this case, the first lead portion of the first internal electrode layer 31 may be led to the first main surface TS1 on the first end face LS1 side, and the first external electrode 40A may be disposed only on the first end face LS1 side on the first main surface TS1. That is, the first external electrode 40A may not be provided on the first end face LS1. In this case, the first surface S1 on the first end face LS1 side of the multilayer ceramic capacitor body 2 is formed by the first end face LS1 of the laminate 10. Also, the second lead portion of the second internal electrode layer 32 may be led to the first main surface TS1 on the second end face LS2 side, and the second external electrode 40B may be disposed only on the second end face LS2 side on the first main surface TS1. That is, the second external electrode 40B may not be provided on the second end face LS2. In this case, the first surface S1 on the second end face LS2 side of the multilayer ceramic capacitor body 2 is formed by the second end face LS2 of the laminate 10.
[0169] In the present embodiment, an example has been described in which one multilayer ceramic capacitor body 2 is covered with an exterior material 3 to form the multilayer ceramic capacitor 1, but this is not limiting. A plurality of multilayer ceramic capacitor bodies 2 as multilayer ceramic electronic component bodies may be covered with an exterior material 3 to form the multilayer ceramic capacitor 1 as the multilayer ceramic electronic component. For example, a plurality of multilayer ceramic capacitor bodies 2 arranged in parallel may be covered with an exterior material 3 to form the multilayer ceramic capacitor 1. For example, two or more stacked multilayer ceramic capacitor bodies 2 may be covered with an exterior material 3 to form the multilayer ceramic capacitor 1.
[0170] The configuration of the multilayer ceramic capacitor body is not limited to the configurations shown in Figures 6 to 9. For example, the multilayer ceramic capacitor body may be a multilayer ceramic capacitor having a double structure, a triple structure, or a quadruple structure as shown in Figures 13A, 13B, and 13C.
[0171] The multilayer ceramic capacitor body 2 shown in FIG. 13A is a multilayer ceramic capacitor body 2 having a double structure, and includes, as the internal electrode layer 30, a first internal electrode layer 33 and a second internal electrode layer 34, as well as a floating internal electrode layer 35 that is not drawn out to either the first end face LS1 or the second end face LS2. The multilayer ceramic capacitor body 2 shown in FIG. 13B is a multilayer ceramic capacitor body 2 having a triple structure, including a first floating internal electrode layer 35A and a second floating internal electrode layer 35B as the floating internal electrode layer 35. The multilayer ceramic capacitor body 2 shown in FIG. 13C is a multilayer ceramic capacitor body 2 having a quadruple structure, including a first floating internal electrode layer 35A, a second floating internal electrode layer 35B, and a third floating internal electrode layer 35C as the floating internal electrode layer 35. In this way, by providing the floating internal electrode layer 35 as the internal electrode layer 30, the multilayer ceramic capacitor body 2 has a structure in which the opposing electrode portion is divided into multiple parts. As a result, a plurality of capacitor components are formed between the opposing internal electrode layers 30, and these capacitor components are connected in series. This reduces the voltage applied to each capacitor component, thereby enabling the multilayer ceramic capacitor body 2 to withstand high voltage. It goes without saying that the multilayer ceramic capacitor body 2 of this embodiment may have a multi-row structure of four or more rows.
[0172] The multilayer ceramic capacitor body 2 may be a two-terminal type having two external electrodes, or a multi-terminal type having many external electrodes.
[0173] In the above-described embodiment, a multilayer ceramic capacitor using a dielectric ceramic is exemplified as a multilayer ceramic electronic component, but the multilayer ceramic electronic component of the present invention is not limited thereto, and can be applied to various multilayer ceramic electronic components such as a piezoelectric component using a piezoelectric ceramic, a thermistor using a semiconductor ceramic, an inductor using a magnetic ceramic, etc. Examples of piezoelectric ceramics include PZT (lead zirconate titanate) ceramics, examples of semiconductor ceramics include spinel ceramics, and examples of magnetic ceramics include ferrite.
[0174] The multilayer ceramic capacitor 1 serving as the multilayer ceramic electronic component of this embodiment provides the following advantages.
[0175] (1) The multilayer ceramic electronic component 1 of the present embodiment includes a laminate 10 including a plurality of laminated ceramic layers 20 and a plurality of internal conductor layers 30 laminated on the ceramic layers 20, the laminate 10 including a first main surface TS1 and a second main surface TS2 opposing each other in a height direction, a first side surface WS1 and a second side surface WS2 opposing each other in a width direction perpendicular to the height direction, and a first end face LS1 and a second end face LS2 opposing each other in a length direction perpendicular to the height direction and the width direction, a multilayer ceramic electronic component body 2 having a first external electrode 40A arranged on the first end face LS1 side and a second external electrode 40B arranged on the second end face LS2 side, a first metal terminal 100A electrically connected to the first external electrode 40A, and a second metal terminal 100B electrically connected to the second external electrode 40B. The laminated ceramic electronic component 1 includes a metal terminal 100B, a laminated ceramic electronic component body 2, and an exterior material 3 that covers a part of the first metal terminal 100A and a part of the second metal terminal 100B, and further includes a fuse 200 that electrically connects the first external electrode 40A and the first metal terminal 100A, and the exterior material 3 includes a first exterior material 3A that covers the laminated ceramic electronic component body 2, a part of the first metal terminal 100A, and a part of the second metal terminal 100B, and a second exterior material 3B that covers at least a part of the first exterior material 3A, and the fuse 200 is embedded in the exterior material 3, at least a part of which protrudes and is exposed from the first exterior material 3A, and the protruding and exposed part is embedded so as to be surrounded by the second exterior material 3B. This makes it possible to provide a laminated ceramic electronic component 1 that suppresses creeping discharge and takes measures against the occurrence of an overcurrent.
[0176] For example, in the case where a part of the fuse 200 is exposed from the exterior material 3, the fuse 200 can be broken in the event of an overcurrent. However, in the case of such a configuration, since a part of the fuse 200 is exposed from the exterior material 3, this is not a preferable configuration from the viewpoint of creeping discharge. On the other hand, in this embodiment, the second exterior material 3B is covered with a resin that deteriorates due to the heat of the fuse 200. Therefore, creeping discharge is suppressed, and the fuse effect is exerted in the event of an overcurrent. Note that, due to its structure, a multilayer ceramic capacitor generally suffers from a short circuit failure when an overvoltage exceeding the rated voltage is applied. Therefore, molding a multilayer ceramic capacitor with the exterior material 3 and providing a fuse is very useful from the viewpoint of creeping discharge and overcurrent countermeasures.
[0177] (2) In this embodiment, the first exterior material 3A is a thermosetting resin, and the second exterior material 3B is a thermoplastic resin. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, and creeping discharge can be suppressed. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B, which is a thermoplastic resin, can be appropriately disconnected.
[0178] (3) In (2), the first exterior material of this embodiment is a thermosetting epoxy resin, which ensures adhesion between the first exterior material 3A and the multilayer ceramic capacitor body 2 and the metal terminals 100, and improves the withstand voltage and moisture resistance.
[0179] (4) In this embodiment, the first exterior material 3A and the second exterior material 3B are different types of thermosetting resins, and the heat resistance temperature of the second exterior material 3B is lower than the heat resistance temperature of the first exterior material 3A. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, so that creeping discharge can be suppressed. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B, which is a resin with a low heat resistance temperature, can be appropriately disconnected.
[0180] In (5)(4), the first packaging material 3A in this embodiment is a thermosetting epoxy resin, which ensures adhesion between the first packaging material 3A and the multilayer ceramic capacitor body 2 and the metal terminals 100, and improves the withstand voltage and moisture resistance.
[0181] (6) In this embodiment, the first exterior material 3A and the second exterior material 3B are different types of thermoplastic resin, and the melting point of the second exterior material 3B is lower than the melting point of the first exterior material 3A. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, so that creeping discharge can be suppressed. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B, which is a thermoplastic resin with a low melting point, can be appropriately disconnected.
[0182] (7) In the multilayer ceramic electronic component 1 of this embodiment, the shortest distance between the outer surface of the second exterior material 3B and the surface of the fuse 200 embedded in the exterior material 3 is 10 μm or more and 1000 μm or less. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, and therefore creeping discharge can be suppressed. Furthermore, when an overcurrent occurs, the fuse 200 covered by the second exterior material 3B can be appropriately disconnected.
[0183] (8) The fuse 200 of the present embodiment is made of a metal having a lower melting point than the metal constituting the terminal body of the first metal terminal 100A. This allows the fuse 200 embedded in the exterior material 3 to be properly disconnected when an overcurrent occurs.
[0184] (9) The second exterior material 3B of the present embodiment is disposed on at least one of the surfaces of the first exterior material 3A facing the first principal surface TS1, the second principal surface TS2, the first side surface WS1, or the second side surface WS2. This allows the fuse 200 to be disposed in an appropriate position and covered by the second exterior material.
[0185] (10) The heat resistance temperature of the second exterior material 3B of the present embodiment is lower than the melting temperature of the fuse 200. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, and thus creeping discharge can be suppressed. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B, which has low heat resistance, can be appropriately disconnected.
[0186] (11) In this embodiment, the heat resistance temperature of the second exterior material 3B is lower than the melting temperature of the fuse 200, and the heat resistance temperature of the first exterior material 3A is higher than the melting temperature of the fuse 200. As a result, under normal circumstances, the fuse 200 is covered by the exterior material 3, and thus creeping discharge can be suppressed. When an overcurrent occurs, the fuse 200, which is covered by the second exterior material 3B, which has low heat resistance, can be appropriately disconnected.
[0187] The present invention is not limited to the configurations of the above-mentioned embodiments, and can be appropriately modified and applied within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual desirable configurations described in the above-mentioned embodiments. [Explanation of symbols]
[0188] 1. Multilayer ceramic capacitors (multilayer ceramic electronic components) 2. Multilayer ceramic capacitor body (multilayer ceramic electronic component body) 3 Exterior materials 3A First exterior material 3B Second exterior material 10 Laminate LS1 First end face LS2 Second end face WS1 First Aspect WS2 The Second Side TS1 First main surface TS2 Second main surface 20 Dielectric layer (ceramic layer) 30 Internal electrode layer (internal conductor layer) 31 First internal electrode layer 32 Second internal electrode layer 40 External electrode 40A First outer electrode 40B Second external electrode 100 metal terminals 100A, 100C First metal terminal 100B, 100D Second metal terminal 200 Fuse
Claims
1. a laminate including a plurality of laminated ceramic layers and a plurality of internal conductor layers laminated on the ceramic layers, the laminate including a first main surface and a second main surface opposing each other in a height direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the height direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the height direction and the width direction; a first external electrode disposed on the first end surface side, and a second external electrode disposed on the second end surface side; a first metal terminal electrically connected to the first external electrode; a second metal terminal electrically connected to the second external electrode; a laminated ceramic electronic component comprising: a laminated ceramic electronic component body; and an exterior material covering a portion of the first metal terminal and a portion of the second metal terminal, a fuse electrically connecting the first external electrode and the first metal terminal; the exterior material includes a first exterior material covering the multilayer ceramic electronic component body, a portion of the first metal terminal, and a portion of the second metal terminal, and a second exterior material covering at least a portion of the first exterior material, the fuse is embedded in the exterior material, at least a portion of the fuse is protruding and exposed from the first exterior material, and the protruding and exposed portion is embedded so as to be surrounded by the second exterior material; a contact area of a portion of the fuse protruding from the first exterior material and exposed therefrom with the second exterior material is larger than a contact area of the portion with the first exterior material; The heat resistance temperature of the second exterior material is lower than the melting temperature of the fuse, a laminated ceramic electronic component, wherein the first and second exterior materials are different types of thermosetting resins, and the heat resistance temperature of the second exterior material is lower than the heat resistance temperature of the first exterior material;
2. 2. The laminated ceramic electronic component according to claim 1, wherein the first exterior material is a thermosetting epoxy resin.
3. 3. The multilayer ceramic electronic component according to claim 1, wherein the shortest distance between an outer surface of said second exterior material and a surface of said fuse embedded in said exterior material is 10 μm or more and 1000 μm or less.
4. 4. The laminated ceramic electronic component according to claim 1, wherein the fuse is made of a metal having a melting point lower than that of a metal constituting the terminal body of the first metal terminal.
5. The multilayer ceramic electronic component according to any one of claims 1 to 4, wherein the second exterior material is disposed on at least one of a surface of the first main surface side, a surface of the second main surface side, a surface of the first side surface side, or a surface of the second side surface side of the first exterior material.
6. 6. The monolithic ceramic electronic component according to claim 1, wherein the heat-resistant temperature of the first exterior material is higher than a meltdown temperature of the fuse.
Citation Information
Patent Citations
JP1987149836U
JP1988016432U
JP1988197324U
Laminated ceramic capacitor
JP1989268011A
Molded chip tantalum solid electrolytic capacitor
JP1990106024A