Substrate with film for reflective mask blank, reflective mask blank, and method for manufacturing reflective mask

The reflective mask blank with a silicon-nitrogen-tantalum back conductive film addresses substrate deformation and pattern misalignment issues by maintaining film integrity and improving productivity in EUV lithography.

JP7567742B2Active Publication Date: 2024-10-16SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021162855
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-10-01
Publication Date
2024-10-16
Estimated Expiration
2041-10-01

AI Technical Summary

Technical Problem

Existing reflective mask blanks face challenges with back conductive films that deteriorate in properties like sheet resistance and film stress during heat treatment, leading to substrate deformation and pattern misalignment issues, especially when using EUV lithography with reflective masks.

Method used

A reflective mask blank with a back conductive film composed of silicon and nitrogen on one side and tantalum on the other, with a thickness of 50 nm or less, providing high film stress and transmittance for local heating, while maintaining low sheet resistance and surface roughness.

Benefits of technology

The solution enhances productivity by reducing defects and substrate deformation, improves pattern alignment accuracy through effective local heating, and maintains film integrity during heat treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567742000001
    Figure 0007567742000001
  • Figure 0007567742000002
    Figure 0007567742000002
  • Figure 0007567742000003
    Figure 0007567742000003
Patent Text Reader

Abstract

SOLUTION: A substrate with a film for a reflective mask blank includes a substrate, a multilayer reflective film formed on one main surface side of the substrate, and a rear surface conductive film formed in contact with the other main surface, wherein the composition of a substrate-contacting side of the rear surface conductive film differs from the composition of the side farthest away from the substrate; the composition of the substrate-contacting side is composed of Si and N, or contains Si, N, and at least one selected from Ta, Mo, Cr, Ti, Zr, Nb, Hf, and W, and / or at least one selected from O and C, the total content of Si and N being 70 atom% or more; and the composition of the side farthest away from the substrate contains Ta and at least one selected from Si, Ge, and Al, the content of Ta being 60 atomic% or more, and a total content of N and O being 15 atomic% or less.EFFECT: The backside conductive film according to the present invention has a high film stress yet being thin, and has a high transmittance at the wavelength of light used to locally heat the substrate.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask blank that is a material for a reflective mask used in the manufacture of semiconductor devices such as LSIs, and in particular to a film-coated substrate for a reflective mask blank that is suitable for an EUV mask blank that is a material for an EUV mask, a reflective mask blank in which an absorber film is formed on a film-coated substrate for a reflective mask blank, and a method for manufacturing a reflective mask using a reflective mask blank. [Background technology]

[0002] In the manufacturing process of semiconductor devices (semiconductor device), photolithography technology is repeatedly used, in which exposure light is irradiated onto a transfer mask, and the circuit pattern formed on the mask is transferred onto a semiconductor substrate (semiconductor wafer) via a reduced projection optical system. Conventionally, the wavelength of the exposure light has been mainly 193 nm using argon fluoride (ArF) excimer laser light, and a process called multi-patterning, which combines exposure processes and processing processes multiple times, has been used to ultimately form patterns with dimensions smaller than the exposure wavelength.

[0003] However, as the device patterns continue to become finer, the formation of even finer patterns is becoming necessary, and thus EUV lithography technology using EUV (Extreme Ultra Violet) light, which has a shorter wavelength than ArF excimer laser light, as exposure light has been developed. EUV light is light with a wavelength of, for example, about 10 to 20 nm, more specifically, light with a wavelength of about 13.5 nm. This EUV light has extremely low permeability to materials, and conventional transmission type projection optical systems and masks cannot be used, so reflective optical elements are used. For this reason, reflective masks have been proposed as masks for pattern transfer. In a reflective mask, a multilayer reflective film that reflects EUV light is formed on a substrate, and an absorber film that absorbs EUV light is formed in a pattern on the multilayer reflective film. On the other hand, a mask in a state before patterning the absorber film (including a state in which a resist film is formed) is called a reflective mask blank, and this is used as a material for a reflective mask.

[0004] The reflective mask blank has a basic structure including a low thermal expansion substrate, a multilayer reflective film formed on one of the two main surfaces of the substrate to reflect EUV light, and an absorber film formed thereon to absorb EUV light. As the multilayer reflective film, a multilayer reflective film is usually used in which molybdenum (Mo) layers and silicon (Si) layers are alternately stacked to obtain a necessary reflectance for EUV light. Furthermore, a ruthenium (Ru) film is formed on the multilayer reflective film as a protective film for protecting the multilayer reflective film. In addition, as the absorber film, tantalum (Ta) or the like, which has a relatively large extinction coefficient value for EUV light, is used (JP Patent Publication 2002-246299 (Patent Document 1) and the like). Meanwhile, a backside conductive film is formed on the other main surface of the substrate. As the backside conductive film, a metal nitride film has been proposed for electrostatic chucking, and mainly includes nitride films of chromium, tantalum, molybdenum, or silicon. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-246299 A [Patent Document 2] JP 2012-22323 A Summary of the Invention [Problem to be solved by the invention]

[0006] The back conductive film is required to have low sheet resistance and small surface roughness for electrostatic chucking, and also to have a role of alleviating the deformation of the substrate caused by the film stress caused by the formation of a multilayer reflective film and a protective film laminated on the main surface opposite to the side on which the back conductive film is formed, by the film stress of the back conductive film. In particular, the reflective mask blank may be heated to a temperature of 150 to 200°C during the processing step into a reflective mask, and in consideration of this, the reflective mask blank is usually subjected to a heat treatment in advance. However, when the heat treatment is performed, the characteristics of the back conductive film, such as the sheet resistance and the film stress, may be deteriorated after the heat treatment.

[0007] In addition, in the case of pattern transfer using a reflective mask, a technique has been proposed in which a pulsed laser with a wavelength of 400 to 800 nm is locally irradiated from the back side of the reflective mask to locally heat the substrate, thereby improving the positional deviation of the pattern during transfer (JP Patent Publication 2012-22323 A (Patent Document 2)). However, in order to obtain a reflective mask blank that can be used with this technique, the back conductive film needs to have a high transmittance for light with a wavelength of 400 to 800 nm. Furthermore, when the film stress of the back conductive film is increased in order to alleviate the deformation of the substrate caused by the film stress generated by the formation of a multilayer reflective film or a protective film, a thick film is advantageous, but a thin film is preferable from the viewpoint of productivity and suppression of defect occurrence, and it is generally advantageous for the film thickness of the back conductive film to be 50 nm or less.

[0008] The present invention has been made to solve the above-mentioned problems, and has an object to provide a film-coated substrate for a reflective mask blank and a reflective mask blank, which are provided with a thinner back surface conductive film which is advantageous in terms of productivity and suppressing the occurrence of defects, a back surface conductive film having high film stress which is advantageous for alleviating, with the film stress of the back surface conductive film, deformation of the substrate due to film stress caused by the formation of a multilayer reflective film and a protective film which are laminated on the main surface opposite to the side on which the back surface conductive film is formed, and a back surface conductive film having high transmittance at the wavelength of light used for heating which is advantageous when locally heating the substrate, and a method for manufacturing a reflective mask using the reflective mask blank. [Means for solving the problem]

[0009] As a result of extensive investigations to solve the above-mentioned problems, the inventors have found that in a reflective mask blank, when a multilayer reflective film or a multilayer reflective film and a protective film thereof are formed on one main surface side of a substrate, and a back surface conductive film is formed on the other main surface side of the substrate, the composition of the back surface conductive film on the side in contact with the substrate is made different from the composition of the side furthest from the substrate, and the composition of the side in contact with the substrate is made to be mainly composed of silicon and nitrogen, and the composition of the side furthest from the substrate is made to be mainly composed of tantalum.

[0010] The inventors then discovered that a film-coated substrate for a reflective mask blank and a reflective mask blank having such a back surface conductive film combine a thinness that is advantageous for productivity and suppressing the occurrence of defects with a high film stress that is effective in mitigating deformation of the substrate, and are a film-coated substrate for a reflective mask blank and a reflective mask blank having a back surface conductive film that has a high transmittance at the wavelength of light used to heat the substrate, thereby completing the present invention.

[0011] Therefore, the present invention provides the following film-coated substrate for a reflective mask blank, a reflective mask blank, and a method for producing a reflective mask. 1. A film-coated substrate for a reflective mask blank, comprising: a substrate; a multilayer reflective film that reflects EUV light and is formed on one of two main surfaces of the substrate; and a back surface conductive film that is formed in contact with the other of the two main surfaces, the rear surface conductive film has a composition different between a side in contact with the substrate and a side farthest from the substrate, The composition of the side in contact with the substrate is A composition consisting of silicon and nitrogen; The silicon-containing material contains at least one selected from the group consisting of silicon, nitrogen, oxygen, and carbon, and the total content of silicon and nitrogen is 92 A composition that is at least 1 atomic percent. The present invention relates to a method for manufacturing a semiconductor device comprising the steps of: (a) providing a semiconductor material which comprises: silicon; nitrogen; and at least one selected from the group consisting of tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten; and (b) providing a semiconductor material which comprises: 92 At. % or more, or The present invention relates to a method for manufacturing a semiconductor device comprising the steps of: (a) providing a semiconductor device which includes silicon, nitrogen, at least one selected from tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten, and at least one selected from oxygen and carbon, and wherein the total content of silicon and nitrogen is 92 Composition with atomic percent or more and The composition of the side farthest from the substrate is The present invention relates to a material containing tantalum and at least one selected from silicon, germanium, and aluminum, and the content of tantalum is 80 At% or more 90 atomic% or less The total content of nitrogen and oxygen is 15 atomic % or less. A film-attached substrate for a reflective mask blank, comprising: 2 The thickness of the back conductive film is 50 nm or less. 1 to A substrate with the above-described reflective mask blank film. 3 The back conductive film is made up of multiple layers, and the thickness of the layer furthest from the substrate is 5 nm to 20 nm. 2 The film-attached substrate for a reflective mask blank according to claim 1. 4 The back conductive film is characterized in that it is composed of multiple layers. or 2 The film-attached substrate for a reflective mask blank according to claim 1. 5 Further, the present invention is characterized in that a protective film is formed on the multilayer reflective film. 4 2. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 6 The size of the substrate is 152 mm square on the main surface and 6.35 mm thick. a warp of the one main surface before forming the multilayer reflective film or the multilayer reflective film and the protective film, and the rear surface conductive film on the substrate; a warp of the one main surface in a state in which the multilayer reflective film or the multilayer reflective film and the protective film, and the rear conductive film are formed on the substrate; The change in warpage (ΔTIR) between the two is within the range of −0.3 to +0.3 μm. 5 2. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 7 The size of the substrate is 152 mm square on the main surface and 6.35 mm thick. a warp of the one main surface before forming the multilayer reflective film or the multilayer reflective film and the protective film, and the rear surface conductive film on the substrate; The multilayer reflective film or the multilayer reflective film and the protective film, and the rear conductive film are formed on the substrate, and a heat treatment is performed at 150° C. for 10 minutes. In this state, The change in warpage (ΔTIR) between the two is within the range of −0.3 to +0.3 μm. 6 2. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 8 The back conductive film has a transmittance of 10% or more for light having a wavelength in the range of 400 to 800 nm. 7 2. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 9 The sheet resistance (RS) of the back conductive film is 250 Ω / □ or less. 82. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 10 The surface roughness (RMS) of the back conductive film is 0.3 nm or less. 9 2. A film-attached substrate for a reflective mask blank according to any one of claims 1 to 11. 11 .1 to 10 13. A reflective mask blank comprising a multilayer reflective film of a film-coated substrate for a reflective mask blank according to any one of claims 1 to 12, further comprising an absorber film that absorbs EUV light formed on the multilayer reflective film. 12 . 11 2. A method for producing a reflective mask, comprising the steps of: producing the reflective mask by using the reflective mask blank according to claim 1 ; Effect of the Invention

[0012] The back surface conductive film of the present invention, even if it is a thin film advantageous in terms of productivity and suppression of defect occurrence, has a high film stress advantageous for mitigating deformation of the substrate due to film stress caused by the formation of a multilayer reflective film or a protective film. In addition, since the back surface conductive film of the present invention has a high transmittance at the wavelength of light used for heating when locally heating the substrate with a pulsed laser or the like, after forming it into a reflective mask, a method of improving the positional deviation of a pattern during transfer using a reflective mask by heating with light can be effectively applied. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1(A) is a cross-sectional view showing an example of a film-attached substrate for a reflective mask blank of the present invention, and FIG. 1(B) is a cross-sectional view showing an example of a reflective mask blank in which an absorber film is formed on the film-attached substrate for a reflective mask blank of (A). [Diagram 2] FIG. 1(A) is a cross-sectional view showing another example of a film-attached substrate for a reflective mask blank of the present invention, and FIG. 1(B) is a cross-sectional view showing another example of a reflective mask blank in which an absorber film is formed on the film-attached substrate for a reflective mask blank of (A). [Diagram 3]FIG. 1(A) is a cross-sectional view showing another example of a film-attached substrate for a reflective mask blank of the present invention, and FIG. 1(B) is a cross-sectional view showing another example of a reflective mask blank in which an absorber film is formed on the film-attached substrate for a reflective mask blank of (A). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will now be described in further detail. The reflective mask blank (EUV mask blank) of the present invention is used as a material for a reflective mask (EUV mask) used in EUV lithography using EUV light as exposure light. The reflective mask blank can be obtained by forming an absorber film on a film-attached substrate for a reflective mask blank, and further forming other films as necessary. The wavelength of the EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, and is usually light having a wavelength of about 13.5 nm.

[0015] The film-attached substrate for a reflective mask blank of the present invention comprises a substrate, a multilayer reflective film that reflects EUV light formed on one of the two main surfaces of the substrate, preferably in contact with the substrate, and a back conductive film that is formed on the other of the two main surfaces, preferably in contact with the substrate. The reflective mask blank of the present invention comprises a substrate, a multilayer reflective film that reflects EUV light formed on one of the two main surfaces of the substrate, preferably in contact with the substrate, an absorber film formed on the multilayer reflective film, and a back conductive film that is formed on the other of the two main surfaces, preferably in contact with the substrate. A reflective mask blank can be obtained by forming an absorber film on the film-attached substrate for a reflective mask blank, and further forming other films as necessary. A reflective mask having an absorber pattern (pattern of the absorber film) can be manufactured from the reflective mask blank by patterning the absorber film using the reflective mask blank.

[0016] 1 is a cross-sectional view showing an example of a film-coated substrate for a reflective mask blank and a reflective mask blank of the present invention. In this case, a film-coated substrate for a reflective mask blank 101 shown in (A) comprises a multilayer reflective film 11 formed on one main surface of a substrate 10 in contact with the one main surface, and a back surface conductive film 21 formed on the other main surface of the substrate 10 in contact with the other main surface. Also, a reflective mask blank 201 shown in (B) has an absorber film 13 formed on the multilayer reflective film 11 of the film-coated substrate for a reflective mask blank 101 shown in (A) in contact with the multilayer reflective film 11.

[0017] The substrate preferably has low thermal expansion characteristics for EUV light exposure, and has a thermal expansion coefficient of, for example, ±2×10 -8 / °C, preferably within ±5×10 -9 It is preferable that the material is made of a material having a temperature within the range of 100°C / °F. Such a material is titania-doped quartz glass (SiO 2 -TiO 2 Glass-based glass). It is preferable to use a substrate having a sufficiently flat surface, and the surface roughness of the main surface of the substrate is preferably 0.5 nm or less, particularly 0.2 nm or less, in terms of RMS value. Such a surface roughness can be obtained by polishing the substrate. In the present invention, the size of the substrate is not particularly limited, but for example, a substrate called a 6025 substrate, which is 6 inches square and 0.25 inches thick as specified in the SEMI standard, is suitable, and when the SI unit system is used, it is usually expressed as a substrate having a 152 mm square and a thickness of 6.35 mm.

[0018] In the present invention, the back surface conductive film is configured such that the composition of the side in contact with the substrate is different from the composition of the side farthest from the substrate. In the back surface conductive film, the side in contact with the substrate preferably has high transmittance, particularly high transmittance for light with a wavelength of 400 to 800 nm, and also preferably has high film stress. On the other hand, in the back surface conductive film, the side farthest from the substrate is required to have low sheet resistance.

[0019] From the viewpoint of improving the characteristics of transmittance and film stress, particularly from the viewpoint of ensuring the necessary high film stress while reducing the thickness of the back conductive film, it is effective for the composition on the side in contact with the substrate to be a composition mainly composed of silicon (Si) and nitrogen (N). In this case, the total content of silicon and nitrogen is preferably 70 atomic % or more, and more preferably 80 atomic % or more. In addition, in the composition on the side in contact with the substrate, the content of nitrogen relative to the total of nitrogen and silicon is preferably 53 atomic % or more, and more preferably 55 atomic % or more.

[0020] The composition on the side in contact with the substrate may contain at least one selected from tantalum (Ta), molybdenum (Mo), chromium (Cr), titanium (Ti), zirconium (Zr), niobium (Nb), hafnium (Hf) and tungsten (W) from the viewpoint of further improving the characteristics of transmittance and film stress, and further improving the characteristics such as surface roughness, etc. Also, at least one selected from oxygen (O) and carbon (C) may be contained.

[0021] The specific composition of the side in contact with the substrate is as follows: (1) a composition consisting of silicon and nitrogen; (2) A composition containing silicon, nitrogen, and at least one selected from oxygen and carbon, the total content of silicon and nitrogen being 70 atomic % or more; (3) A composition containing silicon, nitrogen, and at least one selected from tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten, the total content of silicon and nitrogen being 70 atomic % or more; (4) A composition containing silicon, nitrogen, at least one selected from tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten, and at least one selected from oxygen and carbon, the total content of silicon and nitrogen being 70 atomic % or more. etc.

[0022] On the other hand, the composition on the side farthest from the substrate is preferably a composition mainly composed of tantalum (Ta) from the viewpoint of improving the characteristics of sheet resistance and hardness, in particular, since compositions mainly composed of silicon and nitrogen tend to have high sheet resistance (low electrical conductivity), in order to ensure a sufficiently low sheet resistance required on the side of the reflective mask farthest from the substrate, which is the side electrostatically chucked by the exposure device. In this case, the tantalum content is preferably 60 atomic % or more, and more preferably 80 atomic % or more.

[0023] In addition, the composition on the side farthest from the substrate preferably contains at least one selected from silicon (Si), germanium (Ge) and aluminum (Al). In the case of a composition with a high content of tantalum, tantalum has high crystallinity and may cause large surface roughness, so that defects are likely to occur when attaching and detaching the reflective mask to the exposure device when electrostatically chucking it. In order to reduce the surface roughness, the composition on the side farthest from the substrate preferably contains at least one element selected from silicon, germanium and aluminum. By containing these elements, the side farthest from the substrate mainly composed of tantalum becomes microcrystalline or amorphous, and the surface roughness can be reduced. When at least one element selected from silicon, germanium and aluminum is contained, the content is more than 0 atomic %, but is preferably 5 atomic % or more, and more preferably 10 atomic % or more.

[0024] On the other hand, when at least one element selected from silicon, germanium, and aluminum is included, the sheet resistance is higher than that of a composition containing only tantalum, and these elements are easily oxidized during heat treatment, and when oxidized, the sheet resistance after heat treatment may become even higher. Therefore, when at least one element selected from silicon, germanium, and aluminum is included, the content is preferably 40 atomic % or less, more preferably 30 atomic % or less, and even more preferably 20 atomic % or less.

[0025] Furthermore, the composition on the side farthest from the substrate may contain nitrogen (N) and oxygen (O), but the total content of nitrogen and oxygen is preferably 15 atomic % or less, more preferably 5 atomic % or less, and even more preferably substantially free of nitrogen and oxygen (free of nitrogen and oxygen in excess of the amount of impurities). In particular, since the inclusion of nitrogen tends to increase sheet resistance and reduce film stress, it is preferable that substantially no nitrogen is contained (free of nitrogen in excess of the amount of impurities).

[0026] In order to make the composition of the back conductive film different between the side in contact with the substrate and the side farthest from the substrate, the back conductive film can be a multi-layered film or a film having a gradient composition (a composition that changes in the thickness direction). When the back conductive film is multi-layered, each layer can be a layer of a single composition (a layer with a constant composition in the thickness direction) or a layer having a gradient composition. When the back conductive film is multi-layered, the back conductive film can be composed of two or three or more layers, but it is preferable to compose the back conductive film with two layers. When the back conductive film is composed of two layers, the composition of the layer in contact with the substrate may be the composition of the side in contact with the substrate, and the composition of the layer farthest from the substrate may be the composition of the side farthest from the substrate. The thickness of the layer farthest from the substrate is preferably 10% or more, more preferably 20% or more, of the total thickness of the back conductive film, and is preferably 70% or less, more preferably 60% or less, of the total thickness of the back conductive film. Specifically, the thickness of the layer farthest from the substrate is preferably 5 nm or more and 20 nm or less.

[0027] 2 is a cross-sectional view showing another example of the film-coated substrate for a reflective mask blank and the reflective mask blank of the present invention. In this case, the film-coated substrate for a reflective mask blank 102 shown in (A) comprises a multilayer reflective film 11 formed on one main surface of a substrate 10 in contact with the one main surface, and a back conductive film 21 formed on the other main surface of the substrate 10 in contact with the other main surface, and the back conductive film 21 is composed of two layers, a layer 21a on the side in contact with the substrate 10 and a layer 21b on the side furthest from the substrate 10. In addition, the reflective mask blank 202 shown in (B) has an absorber film 13 formed on the multilayer reflective film 11 of the film-coated substrate for a reflective mask blank 102 shown in (A) in contact with the multilayer reflective film 11.

[0028] By making the composition of the back conductive film different between the side in contact with the substrate and the side farthest from the substrate, and by making each of the compositions of the side in contact with the substrate and the side farthest from the substrate a predetermined composition, the back conductive film can have a thickness advantageous for productivity and suppression of defect occurrence, and can have a high film stress effective for mitigating deformation of the substrate. In addition, the back conductive film can have a high transmittance for the wavelength of light used for heating the substrate, particularly light with a wavelength of 400 to 800 nm. Furthermore, by making the composition of the back conductive film different between the side in contact with the substrate and the side farthest from the substrate, and by making each of the compositions of the side in contact with the substrate and the side farthest from the substrate a predetermined composition, the back conductive film can have a low sheet resistance and a small surface roughness.

[0029] The thickness of the back surface conductive film is preferably as thin as possible from the viewpoints of film formation productivity and suppression of particle generation, and is also preferably as thin as possible from the viewpoint of increasing transmittance. Specifically, the thickness of the back surface conductive film is preferably 70 nm or less, and more preferably 50 nm or less. On the other hand, the lower limit of the thickness of the back surface conductive film is preferably 20 nm or more, and more preferably 30 nm or more.

[0030] The warpage of the substrate after a film has been formed on it varies depending on the composition and physical properties of the film, but for example, when the size of the substrate is such that the main surface is 152 mm square and the thickness is 6.35 mm (when the substrate is a 6025 substrate), it is preferable that the change in warpage (ΔTIR) between the warpage of one main surface (the main surface on the side on which the multilayer reflective film or the multilayer reflective film and the protective film are to be formed) before the multilayer reflective film or the multilayer reflective film and the protective film, and the back surface conductive film are formed on the substrate, and the warpage of one main surface (the main surface on the side on which the multilayer reflective film or the multilayer reflective film and the protective film are to be formed) after the multilayer reflective film or the multilayer reflective film and the protective film, and the back surface conductive film are formed on the substrate, is within a range of −0.3 to +0.3 μm. Therefore, it is preferable that the absolute value of the change in warpage (ΔTIR) of the substrate before and after forming only the multilayer reflective film or the multilayer reflective film and the protective film on the substrate is approximately the same as the absolute value of the change in warpage (ΔTIR) of the substrate before and after forming only the backside conductive film on the substrate. Here, the warpage can be within a range of 142 mm square on one side centered on the center of the main surface of the substrate. Note that, in the warpage change (ΔTIR) of the present invention, the main surface on which the multilayer reflective film or the multilayer reflective film and the protective film are formed is used as a reference, and the change in warpage after the film is formed is expressed as a positive (+) if it is a concave change, and as a negative (-) if it is a convex change, with respect to the warpage before the film is formed.

[0031] In addition, in consideration of the thermal history in the processing step into a reflective mask, the reflective mask blank is usually subjected to a heat treatment in advance, but since the reflectance of the multilayer reflective film generally decreases as the heat treatment temperature increases, the heat treatment temperature is preferably 150° C. or less. Therefore, it is preferable that the film-coated substrate for a reflective mask blank has a warpage change (ΔTIR) between the warpage of one main surface (the main surface on which the multilayer reflective film or the multilayer reflective film and the protective film are formed) before the multilayer reflective film or the multilayer reflective film and the protective film, and the back surface conductive film are formed on the substrate and the warpage of one main surface (the main surface on which the multilayer reflective film or the multilayer reflective film and the protective film are formed) in a state in which the multilayer reflective film or the multilayer reflective film and the protective film, and the back surface conductive film are formed on the substrate and heat treatment is performed at 150° C. for 10 minutes, within a range of −0.3 to +0.3 μm.

[0032] When applying a method for improving the positional deviation of a pattern during transfer using a reflective mask after making a reflective mask from a reflective mask blank, it is preferable that the back conductive film of the present invention has a high transmittance at the wavelength of light used for heating when locally heating a substrate with a pulsed laser or the like. Therefore, the back conductive film of the present invention preferably has a transmittance of 10% or more, more preferably 20% or more, and even more preferably 30% or more for light having a wavelength of 400 to 800 nm. The transmittance may be a predetermined transmittance or more for light of a specific wavelength (particularly 532 nm) within the wavelength range of 400 to 800 nm, but it is more preferable that the transmittance is a predetermined transmittance or more over the entire wavelength range of 400 to 800 nm.

[0033] Since the rear conductive film is a film used for electrostatically chucking the reflective mask to the exposure device, the sheet resistance (RS) is preferably 250 Ω / □ or less, and more preferably 100 Ω / □ or less.

[0034] From the viewpoint of suppressing particle generation during attachment and detachment of the electrostatic chuck, the surface roughness (RMS) of the back surface conductive film is preferably as small as possible, and is preferably 0.5 nm or less, and more preferably 0.3 nm or less.

[0035] The back surface conductive film may be formed before forming the multilayer reflective film, or after forming all of the films on the multilayer reflective film side of the substrate. Alternatively, the back surface conductive film may be formed after forming a portion of the films on the multilayer reflective film side of the substrate, and then the remaining films on the multilayer reflective film side of the substrate may be formed.

[0036] Methods for forming a backside conductive film include a sputtering method in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and sputtering is performed, and an ion beam sputtering method in which an ion beam is irradiated onto a target. Sputtering methods include a DC sputtering method in which a direct current voltage is applied to a target, and an RF sputtering method in which a high frequency voltage is applied to a target. The sputtering method is a film formation method in which a voltage is applied to a target with a sputtering gas introduced into a chamber, the gas is ionized, and the sputtering phenomenon caused by the gas ions is utilized. In particular, the magnetron sputtering method is advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering in which the negative bias applied to the target is reversed for a short period of time to prevent the target from charging up.

[0037] The back conductive film can be formed by a sputtering method using, for example, a sputtering device capable of mounting one or more targets. Specifically, the side in contact with the substrate uses, as targets, a silicon (Si) target, a silicon nitride (SiN) target, and, as necessary, a tantalum (Ta) target, a molybdenum (Mo) target, a chromium (Cr) target, a titanium (Ti) target, a zirconium (Zr) target, a niobium (Nb) target, a hafnium (Hf) target, a tungsten (W) target, or the like, and, as sputtering gas, a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas, and, as necessary, a nitrogen gas (N 2 Gas containing nitrogen, and oxygen gas (O 2 gas), carbon dioxide gas (CO gas, CO 2 Oxygen-containing gases such as carbon dioxide gas (CO gas, CO 2 gas), methane (CH 4 When a nitrogen-containing gas, an oxygen-containing gas, or a carbon-containing gas is used, reactive sputtering using a reactive gas is performed.

[0038] The side furthest from the substrate can be formed by using at least one target selected from a tantalum (Ta) target, a silicon (Si) target, a germanium (Ge) target, and an aluminum (Al) target as the target, and using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as the sputtering gas. In this case, nitrogen gas (N 2 Gas containing nitrogen and oxygen gas (O 2 gas), carbon dioxide gas (CO gas, CO 2 Oxygen-containing gases such as carbon dioxide gas (CO gas, CO 2 gas), methane (CH 4 Carbon-containing gases such as hydrocarbon gases such as toluene, hexane, etc. may also be used.

[0039] In the back surface conductive film, the composition of the side in contact with the substrate, the composition of the side furthest from the substrate, and the composition of other parts can all be made to be the desired composition by appropriately adjusting the power applied to the target (and the ratio between targets when multiple types of targets are used), the flow rate of the reactive gas (and the ratio between reactive gases when multiple types of reactive gases are used), etc.

[0040] The multilayer reflective film is a film that reflects EUV light, which is exposure light, in a reflective mask. The multilayer reflective film is a multilayer film in which layers of low refractive index material and layers of high refractive index material are alternately laminated, and for EUV light with an exposure wavelength of 13 to 14 nm, for example, a Mo / Si periodic laminate film in which molybdenum (Mo) layers and silicon (Si) layers are alternately laminated for about 40 periods (40 layers of each) to 60 periods (60 layers of each) is used. The film thickness of the multilayer reflective film is usually about 280 to 350 nm. A SiN layer may be formed between the Mo layer and the Si layer.

[0041] Methods for forming a multilayer reflective film include a sputtering method in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and sputtering is performed, and an ion beam sputtering method in which an ion beam is irradiated onto a target. As a sputtering method, magnetron sputtering is particularly advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering in which a negative bias applied to the target is reversed for a short period of time to prevent the target from charging up.

[0042] The multilayer reflective film can be formed by a sputtering method using, for example, a sputtering device capable of mounting multiple targets. Specifically, the multilayer reflective film can be formed by using, as the target, a molybdenum (Mo) target for forming a layer containing molybdenum (Mo) and a silicon (Si) target for forming a layer containing silicon (Si), and by using, as the sputtering gas, a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas. The sputtering may also be reactive sputtering using a reactive gas. In this case, for example, when forming a film containing nitrogen (N), nitrogen gas (N 2 A nitrogen-containing gas such as a nitrogen-containing gas (e.g., 1,2-dinitrogen fluoride gas) may be used in combination with a rare gas.

[0043] When forming a layer containing multiple elements, the power applied to the target (and the ratio between targets when multiple types of targets are used), the flow rate of the reactive gas (and the ratio between reactive gases when multiple types of reactive gases are used), etc. can be appropriately adjusted to obtain the desired composition, crystallinity, and other physical properties.

[0044] An absorber film is formed on the multilayer reflective film. The absorber film is a film that absorbs the EUV light, which is the exposure light, and reduces the reflectance of the exposure light. In a reflective mask, a transfer pattern is formed by the difference in reflectance between a portion where the absorber film is formed and a portion where the absorber film is not formed. The absorber film may be formed on the multilayer reflective film in contact with the multilayer reflective film, but is usually provided on the multilayer reflective film via a protective film, which will be described later.

[0045] The material of the absorber film is not limited as long as it absorbs EUV light and can be patterned. Examples of the material of the absorber film include materials containing tantalum (Ta) or chromium (Cr). In addition, materials containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), etc. Examples of materials containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0046] The absorber film can be formed by sputtering, and magnetron sputtering is preferable. Specifically, it can be formed by sputtering using a metal target such as a chromium (Cr) target or a tantalum (Ta) target, or a metal compound target such as a chromium compound target or a tantalum compound target (a target containing a metal such as Cr or Ta and oxygen (O), nitrogen (N), carbon (C), boron (B), or the like) as a sputtering gas, using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas, or by reactive sputtering using a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas together with a rare gas. The thickness of the absorber film is not particularly limited, but is usually about 50 to 90 nm.

[0047] It is preferable to form a protective film between the multilayer reflective film and the absorber film, preferably in contact with the multilayer reflective film, more preferably in contact with both the multilayer reflective film and the absorber film. The protective film is also called a capping layer, and is provided to protect the multilayer reflective film when forming a pattern on the absorber film thereon or when correcting the pattern of the absorber film.

[0048] 3 is a cross-sectional view showing another example of the film-attached substrate for a reflective mask blank and the reflective mask blank of the present invention. In this case, the film-attached substrate for a reflective mask blank 103 shown in (A) comprises a multilayer reflective film 11 formed on one main surface of a substrate 10 in contact with the one main surface, a protective film 12 formed on the multilayer reflective film 11 in contact with the one main surface, and a back surface conductive film 21 formed on the other main surface of the substrate 10 in contact with the other main surface, and the back surface conductive film 21 is composed of two layers, a layer 21a on the side in contact with the substrate 10 and a layer 21b on the side farthest from the substrate 10. In addition, the reflective mask blank 203 shown in (B) has an absorber film 13 formed on the protective film 12 of the film-attached substrate for a reflective mask blank 103 shown in (A) in contact with the protective film 12.

[0049] The material of the protective film is preferably a material containing ruthenium (Ru). As the material containing ruthenium (Ru), ruthenium (Ru) alone, or a compound in which niobium (Nb) or zirconium (Zr) is added to ruthenium (Ru) is preferably used. The thickness of the protective film is usually 5 nm or less, and particularly preferably 4 nm or less. The lower limit of the thickness of the protective film is usually 2 nm or more.

[0050] The protective film can be formed by a sputtering method such as ion beam sputtering or magnetron sputtering, as with the multilayer reflective film. The protective film can be formed by a sputtering method using a sputtering device capable of mounting one or more targets, specifically, by sputtering using a ruthenium (Ru) target, or a ruthenium (Ru) target to which niobium (Nb), zirconium (Zr), or the like is added, and a target of one or more elements selected from niobium (Nb) and zirconium (Zr) as necessary, and a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas.

[0051] When the protective film is formed of a compound containing an element other than a metal, it can be formed by reactive sputtering using a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas together with a rare gas as a sputtering gas. The target may also be a compound.

[0052] A hard mask film (an etching mask film of the absorber film that functions as an etching mask when the absorber film is dry-etched) having etching characteristics different from those of the absorber film may be provided on the side of the absorber film that is preferably in contact with the absorber film. This hard mask film functions as an etching mask when the absorber film is dry-etched. After the absorber pattern is formed, the hard mask film may be left as a part of the absorber film as a reflectance reduction layer for reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection, or may be removed so as not to remain on the reflective mask. Materials for the hard mask film include materials containing chromium (Cr). A hard mask film formed of a material containing Cr is particularly suitable when the absorber film is formed of a material containing Ta and not containing Cr. When a layer (reflectance reduction layer) that mainly plays a role of reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection is formed on the absorber film, the hard mask film can be formed on the reflectance reduction layer of the absorber film. The hard mask film can be formed by, for example, magnetron sputtering. The thickness of the hard mask film is not particularly limited, but is usually about 5 to 20 nm.

[0053] Furthermore, the reflective mask blank may have a resist film formed on the side farthest from the substrate. The resist film is preferably an electron beam (EB) resist. EXAMPLES

[0054] The present invention will be specifically described below with reference to Experimental Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0055] [Experimental Example 1] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A mask having a thickness of 100 nm and a thickness of 100 nm was prepared. ...

[0056] Next, a molybdenum (Mo) target and a silicon (Si) target were used on one of the main surfaces of the low thermal expansion glass substrate where the warpage had been measured, and these targets were placed opposite the main surface of the substrate, and a multilayer reflective film was formed by DC pulse magnetron sputtering while rotating the substrate. Each target was attached to a sputtering device capable of mounting a molybdenum (Mo) target and a silicon (Si) target, and discharging the targets individually or simultaneously, and the substrate was then placed.

[0057] First, while argon (Ar) gas (flow rate: 12 sccm) was flowing into the chamber, power was applied to the silicon (Si) target to form a silicon (Si) layer with a thickness of 4.2 nm at a sputtering pressure of 0.025 Pa. Next, while argon (Ar) gas (flow rate: 13 sccm) was flowing into the chamber, power was applied to the molybdenum (Mo) target to form a molybdenum (Mo) layer with a thickness of 2.8 nm at a sputtering pressure of 0.026 Pa.

[0058] The operation of forming these Si layers and Mo layers constituted one cycle, and this was repeated 40 times to form 40 Si layers and 40 Mo layers. Finally, power was applied to the silicon (Si) target while flowing argon (Ar) gas (flow rate: 12 sccm) into the chamber, and a silicon (Si) layer with a thickness of 4.2 nm was formed at a sputtering pressure of 0.025 Pa, forming a multilayer reflective film with a thickness of 284.2 nm.

[0059] Next, a ruthenium (Ru) target was used on the multilayer reflective film, and the target was placed opposite the main surface of the substrate, and a protective film in contact with the multilayer reflective film was formed by DC pulse magnetron sputtering while rotating the substrate. The ruthenium (Ru) target was attached to a sputtering device other than the sputtering device that formed the multilayer reflective film, and the substrate on which the multilayer reflective film was formed was moved from the sputtering device that formed the multilayer reflective film to the sputtering device on which the ruthenium (Ru) target was attached via a transport path that maintained a vacuum state, without being taken out into the atmosphere, and then installed.

[0060] While flowing argon (Ar) gas (flow rate: 10 sccm) into the chamber, power was applied to the ruthenium (Ru) target to form a ruthenium (Ru) film with a thickness of 2.0 nm at a sputtering pressure of 0.023 Pa. The application of power to the ruthenium (Ru) target was then stopped to form a single-layer protective film.

[0061] The warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective coating and the protective coating were formed was measured, and ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective coating and the protective coating were formed, was calculated to be -1.10 μm.

[0062] Next, the substrate on which the multilayer reflective film and the protective film were formed was subjected to heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed was measured again. ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side previously measured before the multilayer reflective film and the protective film were formed, was calculated to be -0.80 μm.

[0063] [Experimental Example 2] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A glass substrate (based on the PTFE-based glass) was prepared, and the warpage (TIR) ​​of one of the main surfaces of the substrate was measured.

[0064] Next, a molybdenum (Mo) target and a silicon (Si) target were used on one of the main surfaces of the low thermal expansion glass substrate where the warpage had been measured, and these targets were placed opposite the main surface of the substrate, and a multilayer reflective film was formed by DC pulse magnetron sputtering while rotating the substrate. Each target was attached to a sputtering device capable of mounting a molybdenum (Mo) target and a silicon (Si) target, and discharging the targets individually or simultaneously, and the substrate was then placed.

[0065] First, power was applied to the silicon (Si) target while argon (Ar) gas (flow rate: 12 sccm) was flowing into the chamber, and a silicon (Si) layer with a thickness of 3.7 nm was formed at a sputtering pressure of 0.025 Pa. Next, argon (Ar) gas (flow rate: 12 sccm) and nitrogen (N 2 While flowing silicon (Si) gas (flow rate: 50 sccm), power was applied to the silicon (Si) target to form a silicon nitride (SiN) layer with a thickness of 0.5 nm at a sputtering pressure of 0.15 Pa. Next, while flowing argon (Ar) gas (flow rate: 13 sccm) into the chamber, power was applied to the molybdenum (Mo) target to form a molybdenum (Mo) layer with a thickness of 2.8 nm at a sputtering pressure of 0.026 Pa.

[0066] The operation of forming these Si layers, SiN layers, and Mo layers constituted one cycle, and this cycle was repeated 40 times to form 40 Si layers, 40 SiN layers, and 40 Mo layers. Finally, power was applied to the silicon (Si) target while flowing argon (Ar) gas (flow rate: 12 sccm) into the chamber, and a silicon (Si) layer with a thickness of 4.2 nm was formed at a sputtering pressure of 0.025 Pa, forming a multilayer reflective film with a thickness of 284.2 nm.

[0067] Next, a ruthenium (Ru) target was used on the multilayer reflective film, and the target was placed opposite the main surface of the substrate, and a protective film in contact with the multilayer reflective film was formed by DC pulse magnetron sputtering while rotating the substrate. The ruthenium (Ru) target was attached to a sputtering device other than the sputtering device that formed the multilayer reflective film, and the substrate on which the multilayer reflective film was formed was moved from the sputtering device that formed the multilayer reflective film to the sputtering device on which the ruthenium (Ru) target was attached via a transport path that maintained a vacuum state, without being taken out into the atmosphere, and then installed.

[0068] While flowing argon (Ar) gas (flow rate: 10 sccm) into the chamber, power was applied to the ruthenium (Ru) target to form a ruthenium (Ru) film with a thickness of 2.0 nm at a sputtering pressure of 0.023 Pa. The application of power to the ruthenium (Ru) target was then stopped to form a single-layer protective film.

[0069] The warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective coating and the protective coating were formed was measured, and ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective coating and the protective coating were formed, was calculated to be -0.70 μm.

[0070] Next, the substrate on which the multilayer reflective film and the protective film were formed was subjected to heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed was measured again. ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film and the protective film were formed that was initially measured, was calculated to be -0.40 μm.

[0071] [Example 1] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 1.

[0072] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others A tantalum (Ta) target and a silicon (Si) target were used on one of the main surfaces, and these targets were placed opposite the main surface of the substrate, and a back surface conductive film was formed by DC pulse magnetron sputtering while the substrate was rotated. Each target was attached to a sputtering device capable of mounting a tantalum (Ta) target and a silicon (Si) target, and discharging the targets individually or simultaneously, and the substrate was then placed thereon.

[0073] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 While flowing argon (Ar) gas (flow rate: 40 sccm), a power of 300 W was applied to the tantalum (Ta) target and a power of 1500 W was applied to the silicon (Si) target to form a 30 nm thick SiNTa layer. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 600 W was applied to the tantalum (Ta) target and a power of 60 W was applied to the silicon (Si) target to form a 20 nm thick TaSi layer, forming a 50 nm thick backside conductive film consisting of two layers: a SiNTa layer on the side in contact with the substrate and a TaSi layer on the side furthest from the substrate.

[0074] The composition of the backside conductive film was measured by X-ray photoelectron spectroscopy (XPS). The layer in contact with the substrate had a silicon content of 41 atomic %, a nitrogen content of 51 atomic %, and a tantalum content of 8 atomic %. The layer furthest from the substrate had a tantalum content of 90 atomic % and a silicon content of 10 atomic %.

[0075] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.82 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.28 μm. The sheet resistance (RS) of the back conductive film was 97 Ω / □.

[0076] The transmittance of the back conductive film was measured using a UV spectrometer Solidspec-3700 (Shimadzu Corporation) and was 10% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light with a wavelength of 532 nm was 11.2%. In addition, the surface roughness (RMS) of the back conductive film was measured using an atomic force microscope (AFM) and was 0.28 nm.

[0077] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film, and back conductive film were initially measured was calculated to be +0.02μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 100Ω / □.

[0078] [Example 2] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0079] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0080] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 A tantalum (Ta) target was powered at 300 W and a silicon (Si) target was powered at 1500 W while flowing nitrogen (N) gas (flow rate: 40 sccm) to form a 30 nm thick SiNTa layer. Next, argon (Ar) gas (flow rate: 18 sccm) and nitrogen (N 2 While flowing SiO2 gas (flow rate: 5 sccm), 600 W of power was applied to the tantalum (Ta) target and 60 W of power was applied to the silicon (Si) target to form a 20 nm thick TaSiN layer, and a 50 nm thick back surface conductive film consisting of two layers: a SiNTa layer on the side in contact with the substrate and a TaSiN layer on the side furthest from the substrate.

[0081] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 41 atomic %, a nitrogen content of 51 atomic %, and a tantalum content of 8 atomic %. The layer farthest from the substrate had a tantalum content of 84 atomic %, a silicon content of 4 atomic %, and a nitrogen content of 12 atomic %.

[0082] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.69 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.01 μm. The sheet resistance (RS) of the back conductive film was 130 Ω / □.

[0083] The transmittance of the back conductive film was measured in the same manner as in Example 1 and was 12% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light with a wavelength of 532 nm was 13.0%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1 and was 0.21 nm.

[0084] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film and back conductive film were formed, which was initially measured, was calculated to be +0.28μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 130Ω / □.

[0085] [Example 3] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0086] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0087] First, xenon (Xe) gas (flow rate: 1.4 sccm) and nitrogen (N 2 While flowing argon (Ar) gas (flow rate: 18 sccm), a power of 150 W was applied to the tantalum (Ta) target and a power of 1650 W was applied to the silicon (Si) target to form a SiNTa layer with a thickness of 22 nm. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 600 W was applied to the tantalum (Ta) target and a power of 60 W was applied to the silicon (Si) target to form a TaSi layer with a thickness of 12 nm, forming a backside conductive film with a thickness of 34 nm consisting of two layers: a SiNTa layer on the side in contact with the substrate and a TaSi layer on the side furthest from the substrate.

[0088] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 44 atomic %, a nitrogen content of 52 atomic %, and a tantalum content of 4 atomic %. The layer farthest from the substrate had a tantalum content of 90 atomic % and a silicon content of 10 atomic %.

[0089] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.54 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.16 μm. The sheet resistance (RS) of the back conductive film was 185 Ω / □.

[0090] The transmittance of the back conductive film was measured in the same manner as in Example 1 and was 21% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light with a wavelength of 532 nm was 21.7%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1 and was 0.20 nm.

[0091] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film and back conductive film were formed, which was initially measured, was calculated to be +0.14μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 197Ω / □.

[0092] [Example 4] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0093] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0094] First, xenon (Xe) gas (flow rate: 1.4 sccm) and nitrogen (N 2While flowing argon (Ar) gas (flow rate: 18 sccm), a power of 1800 W was applied only to the silicon (Si) target to form a 20 nm thick SiN layer. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 600 W was applied to the tantalum (Ta) target and a power of 60 W was applied to the silicon (Si) target to form a 20 nm thick TaSi layer, forming a 40 nm thick backside conductive film consisting of two layers: a SiN layer on the side in contact with the substrate and a TaSi layer on the side furthest from the substrate.

[0095] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 47 atomic % and a nitrogen content of 53 atomic %. The layer farthest from the substrate had a tantalum content of 90 atomic % and a silicon content of 10 atomic %.

[0096] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.51 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.19 μm. The sheet resistance (RS) of the back conductive film was 100 Ω / □.

[0097] The transmittance of the back conductive film was measured in the same manner as in Example 1 and was 11% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light with a wavelength of 532 nm was 11.0%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1 and was 0.24 nm.

[0098] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film and back conductive film were formed, which was initially measured, was calculated to be +0.13μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 111Ω / □.

[0099] [Example 5] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0100] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0101] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 While flowing argon (Ar) gas (flow rate: 18 sccm), a power of 300 W was applied to the tantalum (Ta) target and a power of 1500 W was applied to the silicon (Si) target to form a SiNTa layer with a thickness of 16 nm. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 480 W was applied to the tantalum (Ta) target and a power of 180 W was applied to the silicon (Si) target to form a TaSi layer with a thickness of 20 nm, forming a backside conductive film with a thickness of 36 nm consisting of two layers: a SiNTa layer on the side in contact with the substrate and a TaSi layer on the side furthest from the substrate.

[0102] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 41 atomic %, a nitrogen content of 51 atomic %, and a tantalum content of 8 atomic %. The layer farthest from the substrate had a tantalum content of 80 atomic % and a silicon content of 20 atomic %.

[0103] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.41 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.29 μm. The sheet resistance (RS) of the back conductive film was 123 Ω / □.

[0104] The transmittance of the back conductive film was measured in the same manner as in Example 1 and was 13% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light at a wavelength of 532 nm was 13.4%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1 and was 0.22 nm.

[0105] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side measured initially before the multilayer reflective film, protective film, and back conductive film were formed, was calculated to be 0μm. In addition, the sheet resistance (RS) of the back conductive film after the heat treatment was 129Ω / □.

[0106] [Comparative Example 1] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0107] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0108] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 While flowing argon (Ar) gas (flow rate: 18 sccm), a power of 15,000 W was applied to the tantalum (Ta) target and a power of 300 W was applied to the silicon (Si) target to form a SiNTa layer with a thickness of 17 nm. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 600 W was applied to the tantalum (Ta) target and a power of 60 W was applied to the silicon (Si) target to form a TaSi layer with a thickness of 20 nm, forming a backside conductive film with a thickness of 37 nm consisting of two layers: a SiNTa layer on the side in contact with the substrate and a TaSi layer on the side furthest from the substrate.

[0109] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 10 atomic %, a nitrogen content of 43 atomic %, and a tantalum content of 47 atomic %. The layer farthest from the substrate had a tantalum content of 90 atomic % and a silicon content of 10 atomic %.

[0110] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.49 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.21 μm. The sheet resistance (RS) of the back conductive film was 85 Ω / □.

[0111] The transmittance of the back conductive film was measured in the same manner as in Example 1, and was less than 10% at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light at a wavelength of 532 nm was 8.8%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1, and was 0.22 nm.

[0112] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film and back conductive film were formed, which was initially measured, was calculated to be +0.11μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 96Ω / □.

[0113] [Comparative Example 2] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0114] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0115] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 While flowing argon (Ar) gas (flow rate: 18 sccm), a power of 300 W was applied to the tantalum (Ta) target and a power of 1500 W was applied to the silicon (Si) target to form a 20 nm thick SiNTa layer. Next, while flowing only argon (Ar) gas (flow rate: 18 sccm) in the same chamber, a power of 660 W was applied only to the tantalum (Ta) target to form a 20 nm thick Ta layer, forming a 40 nm thick backside conductive film consisting of two layers: a SiNTa layer on the side in contact with the substrate and a Ta layer on the side furthest from the substrate.

[0116] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 41 atomic %, a nitrogen content of 51 atomic %, and a tantalum content of 8 atomic %. The layer furthest from the substrate contained only tantalum, and contained substantially no elements other than tantalum.

[0117] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.67 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.03 μm. The sheet resistance (RS) of the back conductive film was 82 Ω / □.

[0118] The transmittance of the back conductive film was measured in the same manner as in Example 1, and was less than 10% at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light at a wavelength of 532 nm was 8.4%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1, and was 0.35 nm.

[0119] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and the difference ΔTIR from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side before the multilayer reflective film, protective film and back conductive film were formed, which was initially measured, was calculated to be +0.27μm. The sheet resistance (RS) of the back conductive film after the heat treatment was 84Ω / □.

[0120] [Comparative Example 3] A 152 mm square, 6.35 mm thick low thermal expansion glass substrate (SiO 2 -TiO 2 A low-thermal expansion glass substrate (a reflective glass substrate) was prepared, the warpage (TIR) ​​of one of the main surfaces of the substrate was measured, and a multilayer reflective film and a protective film were formed on the main surface of the low-thermal expansion glass substrate whose warpage (TIR) ​​had been measured, as in Experimental Example 2.

[0121] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and the protective film were formed was measured. , others On one of the main surfaces, a back surface conductive film was formed using the same apparatus and method as in Example 1.

[0122] First, argon (Ar) gas (flow rate: 10 sccm) and nitrogen (N 2 ) gas (flow rate: 40 sccm) and oxygen (O 2A tantalum (Ta) target was powered at 300 W and a silicon (Si) target was powered at 1500 W while flowing nitrogen (N) gas (flow rate: 10 sccm) to form a SiNTaO layer with a thickness of 21 nm. Next, argon (Ar) gas (flow rate: 18 sccm) and nitrogen (N 2 While flowing SiO2 gas (flow rate: 5 sccm), 600 W of power was applied to the tantalum (Ta) target and 60 W to the silicon (Si) target to form a 20 nm thick TaSiN layer, and a 41 nm thick backside conductive film was formed consisting of two layers: a SiNTaO layer on the side in contact with the substrate and a TaSiN layer on the side furthest from the substrate.

[0123] The composition of the back surface conductive film was measured in the same manner as in Example 1. The layer in contact with the substrate had a silicon content of 33 atomic %, a nitrogen content of 16 atomic %, a tantalum content of 7 atomic %, and an oxygen content of 44 atomic %. The layer farthest from the substrate had a tantalum content of 87 atomic %, a silicon content of 5 atomic %, and a nitrogen content of 8 atomic %.

[0124] Next, the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed was measured, and the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side immediately before the back conductive film was formed was calculated to be +0.35 μm. Meanwhile, the difference ΔTIR between the warpage (TIR) ​​of the main surface (one of the main surfaces) on the side on which the multilayer reflective film and the protective film were formed after the back conductive film was formed and the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side initially measured before the multilayer reflective film, the protective film, and the back conductive film was calculated to be -0.35 μm. The sheet resistance (RS) of the back conductive film was 99 Ω / □.

[0125] The transmittance of the back conductive film was measured in the same manner as in Example 1 and was 12% or more at any wavelength within the range of 400 to 800 nm, and in particular, the transmittance of light with a wavelength of 532 nm was 12.8%. In addition, the surface roughness (RMS) of the back conductive film was measured in the same manner as in Example 1 and was 0.23 nm.

[0126] Next, the substrate on which the back conductive film was formed was subjected to a heat treatment at 150°C for 10 minutes in a hot plate type heat treatment device, and then a back conductive film was formed again. The warpage (TIR) ​​of the main surface (one of the main surfaces) on which the multilayer reflective film and protective film were formed after the heat treatment was measured, and ΔTIR, which is the difference from the warpage (TIR) ​​of the main surface (one of the main surfaces) on the same side measured initially before the multilayer reflective film, protective film and back conductive film were formed, was calculated to be -0.41μm. In addition, the sheet resistance (RS) of the back conductive film after the heat treatment was 100Ω / □. [Explanation of symbols]

[0127] 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Absorber membrane 21 Back conductive film 21a Layer in contact with the substrate 21b Layer furthest from the substrate 101, 102, 103 Film-coated substrate for reflective mask blank 201, 202, 203 Reflective mask blanks

Claims

1. A film-coated substrate for a reflective mask blank, comprising: a substrate; a multilayer reflective film that reflects EUV light and is formed on one of two main surfaces of the substrate; and a back surface conductive film that is formed in contact with the other of the two main surfaces, the rear surface conductive film has a composition different between a side in contact with the substrate and a side farthest from the substrate, The composition of the side in contact with the substrate is A composition consisting of silicon and nitrogen; A composition containing silicon, nitrogen, and at least one selected from oxygen and carbon, the total content of silicon and nitrogen being 92 atomic % or more; A composition containing silicon, nitrogen, and at least one selected from tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten, the total content of silicon and nitrogen being 92 atomic % or more; or A composition comprising silicon, nitrogen, at least one selected from tantalum, molybdenum, chromium, titanium, zirconium, niobium, hafnium, and tungsten, and at least one selected from oxygen and carbon, the total content of silicon and nitrogen being 92 atomic % or more. and The composition of the side farthest from the substrate is A composition comprising tantalum and at least one selected from silicon, germanium, and aluminum, the tantalum content being 80 atomic % or more and 90 atomic % or less, and the total content of nitrogen and oxygen being 15 atomic % or less. A film-attached substrate for a reflective mask blank, comprising:

2. 2. The film-coated substrate for a reflective mask blank according to claim 1, wherein the rear surface conductive film has a thickness of 50 nm or less.

3. 3. The film-coated substrate for a reflective mask blank according to claim 2, wherein the rear conductive film is composed of multiple layers, and the thickness of the layer furthest from the substrate is 5 nm or more and 20 nm or less.

4. 3. The film-coated substrate for a reflective mask blank according to claim 1, wherein the rear surface conductive film is configured in a multi-layer structure.

5. The film-coated substrate for a reflective mask blank according to claim 1 , further comprising a protective film formed on the multilayer reflective film.

6. The size of the substrate is 152 mm square on the main surface and 6.35 mm thick, a warp of the one main surface before forming the multilayer reflective film or the multilayer reflective film and the protective film, and the rear surface conductive film on the substrate; a warp of the one main surface in a state in which the multilayer reflective film or the multilayer reflective film and the protective film, and the rear conductive film are formed on the substrate; 6. The film-attached substrate for a reflective mask blank according to claim 1, wherein a change in warpage (ΔTIR) between the above is within a range of −0.3 to +0.3 μm.

7. The size of the substrate is 152 mm square on the main surface and 6.35 mm thick, a warp of the one main surface before forming the multilayer reflective film or the multilayer reflective film and the protective film, and the rear surface conductive film on the substrate; The multilayer reflective film or the multilayer reflective film and the protective film, and the rear conductive film are formed on the substrate, and a heat treatment is performed at 150° C. for 10 minutes. In this state, 7. The film-attached substrate for a reflective mask blank according to claim 1, wherein a change in warpage (ΔTIR) between the above is within a range of −0.3 to +0.3 μm.

8. 8. The film-attached substrate for a reflective mask blank according to claim 1, wherein the rear conductive film has a transmittance of 10% or more for light having a wavelength in the range of 400 to 800 nm.

9. 9. The film-attached substrate for a reflective mask blank according to claim 1, wherein the sheet resistance (RS) of the rear conductive film is 250 Ω / □ or less.

10. 10. The film-coated substrate for a reflective mask blank according to claim 1, wherein the surface roughness (RMS) of the rear conductive film is 0.3 nm or less.

11. A reflective mask blank, comprising: a multilayer reflective film of a film-coated substrate for a reflective mask blank according to claim 1 ; and an absorber film that absorbs EUV light formed on the multilayer reflective film of the film-coated substrate for a reflective mask blank according to claim 1 .

12. A method for producing a reflective mask, comprising the step of producing the reflective mask by using the reflective mask blank according to claim 11.

Citation Information

Patent Citations

  • Reflecting type exposure mask, its manufacturing method and semiconductor element

    JP2002246299A

  • Method and apparatus for correcting error of photolithographic mask

    JP2012022323A

  • Reflective mask blank for EUV lithography, substrate with functional film for mask blank

    JP2012049498A

  • Substrate with multilayer reflection film for EUV lithography, reflective mask blank for EUV lithography, reflective mask for EUV lithography, and method of manufacturing semiconductor device

    JP2013225662A

  • Reflective mask blank for EUV lithography, and reflective mask for EUV lithography

    JP2015015420A