Glass substrate and method for producing same
The glass substrate with convexly curved surfaces and controlled radii of curvature addresses glare issues in in-vehicle display devices by minimizing light reflections, improving safety and visibility.
Patent Information
- Application Number
- JP2021530624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-10
- Filing Date
- 2020-06-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-30
AI Technical Summary
In-vehicle display devices experience rapid changes in light direction and intensity, leading to strong reflections at the chamfered portions of the cover glass, which can cause glare and interfere with driving.
A glass substrate design with convexly curved boundary surfaces and controlled radii of curvature and angles, along with a method of manufacturing using a rotating grindstone to shape the chamfered edges, reduces glare by minimizing light reflection.
The designed glass substrate effectively suppresses glare at chamfered portions, enhancing visibility and safety in vehicle-mounted display devices.
Smart Images

Figure 0007567790000002 
Figure 0007567790000003 
Figure 0007567790000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass substrate and a method for producing the same. [Background technology]
[0002] 2. Description of the Related Art Vehicles such as automobiles are equipped with on-board display devices such as car navigation devices. 2. Description of the Related Art In in-vehicle display devices, a glass cover member (cover glass) is used to protect the display panel (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2017 / 208995 Summary of the Invention [Problem to be solved by the invention]
[0004] Unlike stationary display devices that are installed in a fixed position, in-vehicle display devices installed in vehicles experience rapid changes in the direction and intensity of light hitting the cover glass, which can result in strong light hitting the chamfered edge of the cover glass.
[0005] According to the inventors' investigations, depending on the glass substrate used as the cover glass, the reflected light from the chamfered portion may be dazzling. If such reflected light enters the driver's eyes, it may cause problems while driving. Therefore, in a glass substrate used as a cover glass of an in-vehicle display device or the like, it is preferable that glare caused by reflected light from the chamfered portion is suppressed (hereinafter, also referred to as "having excellent anti-glare properties at the chamfered portion").
[0006] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a glass substrate having excellent antiglare properties at a chamfered portion and a method for producing the same. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above object can be achieved by employing the following configuration, and have completed the present invention.
[0008] That is, the present invention provides the following [1] to
[10] . [1] A glass base comprising: a first main surface; a second main surface which is a main surface opposite to the first main surface; an end surface sandwiched between the first main surface and the second main surface; a first boundary surface which is disposed between the first main surface and the end surface and connects to the end surface; and a second boundary surface which connects the first main surface and the first boundary surface, wherein the second boundary surface is a convexly curved surface, and the radius of curvature R2 of the second boundary surface is 0.1 mm or more and 2.0 mm or less. [2] The glass base according to [1] above, wherein an angle θ1 between the second boundary surface and the first main surface is 10° or more and 45° or less. [3] The glass substrate according to the above [1] or [2], wherein the first boundary surface is a convexly curved surface, and the radius of curvature R1 of the first boundary surface is 0.1 mm or more and 1.0 mm or less. [4] The glass substrate according to [3] above, wherein the radius of curvature R2 of the second boundary surface is larger than the radius of curvature R1 of the first boundary surface. [5] The glass base according to any one of the above [1] to [4], wherein the first main surface and the second main surface have bent portions. [6] The glass base according to any one of the above [1] to [5], wherein the size of the chipping on the second interface is 0.08 mm or less. [7] The glass base according to any one of [1] to [6] above, wherein a difference between a length L1 from the end face to the first main surface in a tangential direction to the first main surface and a length L2 from the end face to the second main surface in a tangential direction to the second main surface is 0.2 mm or less. [8] The glass base according to any one of the above [1] to [7], which is used as a cover glass for a display device. [9] The glass substrate according to the above [8], wherein the display device is an in-vehicle display device.
[10] A method for producing a glass base according to any one of the above [1] to [9], comprising the steps of: preparing a glass plate; and grinding the glass plate with a grinding wheel, the grinding surface of the grinding wheel having a shape corresponding to the shapes of the first boundary surface and the second boundary surface. Effect of the Invention
[0009] According to the present invention, it is possible to provide a glass substrate having excellent antiglare properties at a chamfered portion and a method for producing the same. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a cross-sectional view showing a glass substrate. [Diagram 2] FIG. 2 is a cross-sectional view showing the in-vehicle display device. [Diagram 3] FIG. 3 is a cross-sectional view showing a modified example of the glass substrate. [Figure 4] FIG. 4 is a cross-sectional view showing grinding of a glass plate using a rotary grindstone. [Diagram 5] FIG. 5 is a graph for explaining how to determine the radius of curvature. [Figure 6] FIG. 6 is an enlarged view of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the present invention will be described with reference to the drawings. However, the present invention is not limited to the following embodiments. Various modifications and substitutions can be made to the following embodiments without departing from the spirit of the present invention.
[0012] [Glass base] FIG. 1 is a cross-sectional view showing a glass substrate 1. As shown in FIG. The glass base 1 is a plate-like glass and has a first main surface 2 and a second main surface 3 opposite to the first main surface 2. The first main surface 2 and the second main surface 3 are parallel to each other.
[0013] The glass substrate 1 has an end surface 4 sandwiched between a first main surface 2 and a second main surface 3 . 1, the end surface 4 is illustrated as a flat surface perpendicular to the first main surface 2 and the second main surface 3. However, the end surface 4 may be a convexly curved surface, similar to the first boundary surface 5 and the second boundary surface 6 described later.
[0014] The glass substrate 1 has a first interface 5 disposed between the first main surface 2 and the edge surface 4. The first interface 5 is connected to the edge surface 4.
[0015] Furthermore, the glass substrate 1 has a second boundary surface 6 disposed between the first main surface 2 and the first boundary surface 5. The second boundary surface 6 connects the first boundary surface 5 and the first main surface 2. The second boundary surface 6 is a convexly curved surface. The radius of curvature R2 of the second boundary surface 6 is not less than 0.1 mm and not more than 2.0 mm.
[0016] Hereinafter, in the glass base 1, the first boundary surface 5 and the second boundary surface 6 may be collectively referred to as a "chamfered portion."
[0017] When such a glass substrate 1 is used as a cover glass for an in-vehicle display device as described below, the chamfered portion has excellent antiglare properties.
[0018] FIG. 2 is a cross-sectional view showing the in-vehicle display device 21. As shown in FIG. The in-vehicle display device 21 shown in FIG. 2 is, for example, a car navigation device. The in-vehicle display device 21 has a housing 22 that houses each component. A backlight unit 23 is housed inside the housing 22, and a display panel 24, which is a liquid crystal panel, is disposed thereon. The display panel 24 may be, for example, an organic EL panel, an electronic ink type panel, or the like, and may have a touch panel or the like.
[0019] A glass substrate is attached to the display panel 24 via an adhesive layer 25 such that the second main surface 3 of the glass substrate 1 is in contact with the adhesive layer 25. The adhesive layer 25 is, for example, an OCA (Optical Clear Adhesive). The glass substrate 1 functions as a cover member (cover glass) that covers the display panel 24.
[0020] In the in-vehicle display device 21, the second main surface 3 of the glass base 1 is a surface facing the display panel 24. On the other hand, the first main surface 2 of the glass substrate 1 is a surface that does not face the display panel 24, and faces the user (for example, the driver) side of the in-vehicle display device 21.
[0021] Incidentally, since the in-vehicle display device 21 is mounted on a vehicle, the direction and intensity of the light that strikes the first main surface 2 of the glass base 1 changes rapidly. For this reason, strong light may strike the chamfered portions (first boundary surface 5 and second boundary surface 6) of the glass base 1, resulting in reflected light.
[0022] However, in this embodiment, the glare caused by the light reflected from the chamfered portion of the glass base 1 is suppressed. In other words, the chamfered portion has excellent anti-glare properties. This is presumably because the glass base 1 has the second boundary surface 6 described above, thereby reducing the amount of reflected light that enters the eye.
[0023] Let us return to the explanation of Figure 1.
[0024] <Radius of curvature of the second boundary surface R2> As described above, the second boundary surface 6 is a convexly curved surface, and the radius of curvature R2 of the second boundary surface 6 is not less than 0.1 mm and not more than 2.0 mm. For the reason that the antiglare property of the chamfered portion is superior, the radius of curvature R2 of the second boundary surface 6 is preferably 0.2 mm or more, more preferably 0.3 mm or more, further preferably 0.4 mm or more, and particularly preferably 0.6 mm or more. Similarly, in order to obtain better antiglare properties at the chamfered portion, the radius of curvature R2 of the second boundary surface 6 is preferably 1.5 mm or less, more preferably 1.2 mm or less, and even more preferably 1.0 mm or less.
[0025] <Angle θ1 between the second boundary surface and the first principal surface> The angle θ1 between the second boundary surface 6 and the first main surface 2 is preferably 10° or more and 45° or less, and more preferably 15° or more and 35° or less, because the chamfered portion has better antiglare properties.
[0026] <Chipping size> A chip is a defect formed on the surface of glass, and the portion where such a chip is formed may have particularly strong reflected light. For this reason, the size of the chipping at the second boundary surface 6 is preferably 0.08 mm or less, and more preferably 0.05 mm or less, because the chamfered portion has better antiglare properties. The size of the chipping is measured by observing the surface of the glass substrate 1 at a magnification of 100 times using a scanning confocal laser microscope (for example, OLS3000, manufactured by Olympus Corporation). Observation is performed in any five fields of view, and the chipping with the longest diameter is found, and the diameter is taken as the size of the chipping. The diameter is the longest distance between two points in the chipping area shown in the observation field of view image.
[0027] <Radius of curvature of the first boundary surface R1> The first boundary surface 5 is preferably a convexly curved surface. In this case, the radius of curvature R1 of the first boundary surface 5 is preferably 0.1 mm or more, and more preferably 0.3 mm or more, because the chamfered portion has better antiglare properties. Similarly, the radius of curvature R1 of the first boundary surface 5 is preferably 1.0 mm or less, and more preferably 0.8 mm or less, because the chamfered portion has better antiglare properties.
[0028] <Relationship between radius of curvature R1 and radius of curvature R2> It is preferable that the radius of curvature R2 of the second boundary surface 6 is larger than the radius of curvature R1 of the first boundary surface 5 because this provides better antiglare properties at the chamfered portion.
[0029] <The third and fourth boundaries> 1, the glass substrate 1 may have a third interface 7 disposed between the second main surface 3 and the end surface 4. The third interface 7 is connected to the end surface 4. Furthermore, the glass substrate 1 may have a fourth boundary surface 8 disposed between the second principal surface 3 and the third boundary surface 7. The fourth boundary surface 8 is connected to the second principal surface 3 and the third boundary surface 7. The third boundary surface 7 and the fourth boundary surface 8 are preferably each a convexly curved surface. The radius of curvature of the third boundary surface 7 may be the same as the radius of curvature R1 of the first boundary surface 5, or may be different. The radius of curvature of the fourth boundary surface 8 may be the same as the radius of curvature R2 of the second boundary surface 6, or may be different. The third boundary surface 7 and the fourth boundary surface 8 may be continuous surfaces having the same radius of curvature.
[0030] <Surface width> The difference between the length L1 from the end face 4 to the first main surface 2 in the tangential direction to the first main surface 2 and the length L2 from the end face 4 to the second main surface 3 in the tangential direction to the second main surface 3 (hereinafter, for convenience, also referred to as the "face width") is preferably 0.2 mm or less, and more preferably 0.1 mm or less.
[0031] The radii of curvature R1 and R2, the lengths L1 and L2, and the angle θ1 are measured using a contour measuring device (for example, Contour Record manufactured by Tokyo Seimitsu Co., Ltd.) at a magnification of, for example, 100 to 200 times.
[0032] A method for determining the radius of curvature R1 and the radius of curvature R2 will be described with reference to FIG. FIG. 5 is a graph for explaining how to determine the radius of curvature, and the contour shape of the glass base 1 is also shown in the upper part of FIG. First, a contour measuring device is used to measure the contour shape of the glass substrate 1, and the radius of curvature R of the chamfered portion (first boundary surface 5 and second boundary surface 6) is calculated, for example, at intervals of 10 μm from the end surface 4. In FIG. 5, a number of points representing the calculated radii of curvature R are plotted. First, the average value R of the calculated curvature radii R of the three points (the curvature radii R surrounded by the dashed line S1 in FIG. 5) in order from the end face 4 is calculated. A (Indicated by the dashed line in FIG. 5) is calculated. Next, the average value R A Range G with median A A plurality of radii of curvature R included in the above are selected, and their average value is set as the radius of curvature R1 (shown by the dashed line in FIG. 5). Similarly, the average value R of the radii of curvature R of three points (radii of curvature R surrounded by a dashed line S2 in FIG. 5) in order from the closest to the first main surface 2 is B (Indicated by the dashed line in FIG. 5) is calculated. Next, the average value R B Range G with median B A plurality of radii of curvature R included in the above are selected, and their average value is set as the radius of curvature R2 (shown by a dashed line in FIG. 5). Range G A and range G B are, for example, the average value R A and the average value R B The range is from ±50 μm. Here, 50 μm is appropriately set in consideration of processing accuracy and measurement accuracy, and may be, for example, ±100 μm, ±70 μm, ±30 μm, etc. In this way, regardless of the distance between the first boundary surface 5 and the second boundary surface 6, and even when there are multiple radii of curvature R, the radii of curvature R1 and the radii of curvature R2 can be efficiently calculated.
[0033] The length L1 and the length L2 are defined as follows. Please refer to Figure 1. An arbitrary point on the intersection line X1 between the first main surface 2 and the second boundary surface 6 is defined as point Y1. A plane (cross section) that passes through point Y1 and perpendicularly intersects with the intersection line X1 is defined as cross section Z. Cross section Z is also a plane (cross section) perpendicular to the tangent to the intersection line X1 at point Y1. Among the distances on cross section Z from point Y1 to the end face 4 in the direction parallel to the first main surface 2, the longest distance is defined as length L1. Next, a point on the cross section Z that is on the intersection line X2 between the second main surface 3 and the fourth boundary surface 8 is defined as point Y2. Among the distances on the cross section Z from point Y2 to the end surface 4 in the direction parallel to the second main surface 3, the longest distance is defined as length L2. If the end face 4 is a convexly curved surface, the distance from the most protruding apex of the curved surface is measured. In this case, "end face" shall be read as "apex".
[0034] The angle θ1 will be described with reference to FIG. Fig. 6 is an enlarged view of Fig. 1. The same parts as those explained based on Fig. 1 are designated by the same reference numerals, and the explanation thereof will be omitted. Point P1 is a point on the first main surface 2, and the distance between point Y1 and point P1 (the distance in a direction parallel to the first main surface 2) is 50 μm. A straight line passing through point Y1 and point P1 is defined as a straight line Y1P1. Point P2 is a point on the second boundary surface 6, and the distance between point Y1 and point P2 (the distance in a direction parallel to the first main surface 2) is 50 μm. A straight line passing through point Y1 and point P2 is defined as a straight line Y1P2. The angle between the straight lines Y1P1 and Y1P2 is defined as angle θ1.
[0035] <Chemically strengthened glass> When the glass base 1 is used as a cover glass, it is preferably glass that has been subjected to a chemical strengthening treatment (chemically strengthened glass). A compressive stress layer is formed on the surface layer of the chemically strengthened glass. The depth of the compressive stress layer (DOL) is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 25 μm or more. The compressive stress value (CS) of the compressive stress layer is preferably 500 MPa or more, more preferably 650 MPa or more, and even more preferably 750 MPa or more, while it is preferably 1200 MPa or less. The compressive stress value (CS) of the compressive stress layer and the depth (DOL) of the compressive stress layer can be measured, for example, using a surface stress meter (FSM-6000, manufactured by Orihara Seisakusho Co., Ltd.) or a scattered light photoelastic stress meter (SLP-2000, manufactured by Orihara Seisakusho Co., Ltd.).
[0036] <Functional Layer> A functional layer may be formed on the first main surface 2 and / or the second main surface 3 of the glass base 1. Examples of the functional layer include an antireflection layer, an antiglare layer (AG layer), an antifouling layer, and a light-shielding layer. The functional layer may be formed by treating the surface layer of the glass base 1, or may be formed by laminating another layer on the surface of the glass base 1.
[0037] <Thickness, shape and size> The thickness of the glass substrate 1 is preferably 0.5 mm or more and 2.5 mm or less, and more preferably 0.7 mm or more and 2.0 mm or less. The shape and size of the main surfaces (the first main surface 2 and the second main surface 3) of the glass base 1 are appropriately determined according to, for example, the shape of the in-vehicle display device 21 to be used.
[0038] <Bend> FIG. 3 is a cross-sectional view showing a modified example of the glass base 1. As shown in FIG. In FIG. 1, the glass base 1 is illustrated as a flat glass plate, but the shape of the glass base 1 is not limited to this. For example, as shown in Fig. 3, the glass base 1 may have a bent portion 12. In the bent portion 12, the first main surface 2 is bent (curved) concavely, and the other second main surface 3 is bent (curved) convexly. When the glass base 1 has a bent portion 12, the radius of curvature of the bent portion 12 is, for example, not less than 10 mm and not more than 100 mm. Conversely, in the bent portion 12, the first main surface 2 may be bent in a convex shape, and the second main surface 3 may be bent in a concave shape.
[0039] <Application> The use of the glass substrate 1 is not particularly limited, and it is used, for example, as a cover glass for a display device, and is particularly suitable for use as a cover glass for an in-vehicle display device 21.
[0040] [Method of manufacturing glass substrate] Next, a method for producing the above-mentioned glass base 1 (hereinafter, for convenience, also referred to as "this production method") will be described.
[0041] <Preparing the glass plate> First, a glass plate 31 is prepared. The glass plate 31 has a first main surface 32 which is one of its main surfaces, a second main surface 33 which is the other of its main surfaces, and an end surface 34 which is connected to the first main surface 32 and the second main surface 33. A first main surface 32 of the glass plate 31 becomes the first main surface 2 of the glass base 1. A second main surface 33 of the glass plate 31 becomes the second main surface 3 of the glass base 1. The thickness of the glass plate 31 is the same as the thickness of the glass base 1 described above.
[0042] Examples of the glass type of the glass plate 31 include soda lime glass and aluminosilicate glass (SiO2-Al2O3-Na2O-based glass). Examples of the glass composition of the glass plate 31 include the glass compositions described in paragraph
[0019] of JP 2019-006650 A. When a chemical strengthening treatment described later is carried out, for example, aluminosilicate glass-based chemically strengthened glass (Dragontrail (registered trademark), manufactured by AGC) is suitably used.
[0043] <grinding> FIG. 4 is a cross-sectional view showing grinding of a glass plate 31 using a rotary grindstone 35. As shown in FIG. 4, the edge of the glass plate 31 is ground using a rotary grindstone 35. In this way, the glass plate 31 is subjected to so-called chamfering. An annular grinding groove extending in the circumferential direction is formed on the grinding surface 36, which is the outer circumferential surface of the rotary grindstone 35. The grinding surface 36 contains abrasive grains such as alumina, silicon carbide, diamond, etc. The grain size (JIS R 6001) of the abrasive grains is not particularly limited, but is selected from the range of #300 to #2000, for example. The rotary grindstone 35 moves relatively along the edge of the glass sheet 31 while rotating about the center line of the rotary grindstone 35, and grinds the edge of the glass sheet 31 with the grinding surface 36. A coolant such as water may be used during grinding.
[0044] In this manufacturing method, the grinding surface 36 of the grindstone 35 has a shape that corresponds at least to the shape of the desired chamfered portion (the first boundary surface 5 and the second boundary surface 6) of the glass base 1 (however, since FIG. 4 is a schematic diagram, it does not have such a shape). Such a grindstone 35 can be obtained, for example, as a custom-made product. By using such a grindstone 35 to grind and chamfer the edge of the glass plate 31, the above-mentioned glass base 1 is obtained.
[0045] In order to obtain the glass base 1 as shown in Fig. 3, the glass plate 31 must also be bent. In this case, the glass plate 31 has the same radius of curvature as the radius of curvature of the bent portion 12 of the glass base 1. When grinding a bent glass plate 31, if the diameter D1 of the grindstone 35 is too large, the corners of the grindstone 35 may come into contact with the glass plate 31 on the concave side of the bent glass plate 31, which may easily cause chipping. For this reason, when grinding a curved glass plate 31, it is preferable that the diameter D1 of the grindstone 35 is smaller than the radius of curvature of the glass plate 31. This suppresses the formation of chipping. Taking into account the peripheral speed of the grindstone, it is preferable that the diameter D1 of the grindstone is 5 to 30 mm.
[0046] As long as the above-mentioned glass base 1 can be finally obtained, rough processing may be performed first using a grindstone having a coarse grain size, and then finish processing may be performed using a grindstone having a fine grain size.
[0047] Furthermore, grinding may be performed using a grinding tool other than a grindstone, so long as the above-mentioned glass base 1 can be obtained. However, from the viewpoint of productivity, a grindstone is preferable.
[0048] Chemical strengthening treatment The ground glass plate 31 may be subjected to a chemical strengthening treatment. In this case, the glass plate 31 that has been subjected to the chemical strengthening treatment becomes the glass base 1. When chemical strengthening treatment is performed, glass for chemical strengthening is used as the glass plate 31 . In the chemical strengthening treatment, a conventionally known method can be used, and typically, the glass sheet 31 is immersed in a molten salt. As a result, in the surface layer of the glass sheet 31, alkali ions (Li ions and / or Na ions) are ion-exchanged (substituted) with other alkali ions (Na ions and / or K ions) having a larger ionic radius in the molten salt. This ion exchange forms a layer (compressive stress layer) in which compressive stress is generated due to densification in the surface layer of the glass sheet 31. In this way, the glass sheet 31 can be strengthened. When the alkali ions contained in the glass sheet 31 are Na ions, the molten salt (inorganic salt composition) preferably contains potassium nitrate (KNO3). The treatment conditions, such as the temperature of the molten salt and the immersion time, may be set so that the compressive stress value (CS) and the thickness (DOL) of the compressive stress layer are desired.
[0049] In this manufacturing method, a functional layer may be formed on the first main surface 2 and / or the second main surface 3 of the glass base 1 as appropriate. EXAMPLES
[0050] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples. However, the present invention is not limited to the following examples. Below, Examples 1 to 4 and Example 7 are Examples, and Examples 5 to 6 are Comparative Examples.
[0051] Example 1: "Dragon Trail" manufactured by AGC was prepared as the glass plate 31. The size of the main surfaces (first main surface 32 and second main surface 33) of the glass plate 31 was 1200 mm x 300 mm. The thickness of the glass plate 31 was 2.0 mm. The glass plate 31 was bent so that the first main surface 32 was concave, and the radius of curvature of the glass plate 31 was 50 mm.
[0052] Next, the edge of the prepared glass plate 31 was ground using a custom-made grinding wheel 35 having a specific grinding surface 36, thereby obtaining the glass substrate 1 of Example 1. The diameter D1 of the grindstone 35 was 20 mm. The abrasive grains on the grinding surface 36 of the grindstone 35 were diamond grains with a grain size of #800. The grinding was performed in a wet manner, that is, water was used as cooling water during grinding.
[0053] The glass plate 31 was chamfered by grinding with a rotary grindstone 35, and an end surface 4, a first boundary surface 5, a second boundary surface 6, a third boundary surface 7 and a fourth boundary surface 8 were formed. The radius of curvature R1 of the first boundary surface 5, the radius of curvature R2 of the second boundary surface 6, the angle θ1 between the second boundary surface 6 and the first main surface 2, the size of the chipping of the second boundary surface 6, and the surface width (|L1-L2|) are shown in Table 1 below (the same applies to Examples 2 to 7 described below).
[0054] <Example 2 to Example 7> In each of Examples 2 to 7, a glass plate 31 was ground using a grindstone 35 having a grinding surface 36 with a different shape from that of Example 1, to obtain a glass base 1. In Examples 5 to 6, a flat surface, not a curved surface, was formed as the second boundary surface 6. For this reason, "-" is entered in the column for the radius of curvature R2 of the second boundary surface 6 in Table 1 below. Moreover, in Example 6, unlike Examples 1 to 5, the diameter D1 of the grindstone 35 was set to 50 mm.
[0055] <evaluation> Using each of the glass substrates 1 of Examples 1 to 7, 11 subjects aged from 30 to 60 were asked to carry out the following evaluations. First, the subjects were asked to hold the glass base 1, on which light was being irradiated, at a distance of 60 cm facing the first main surface 2, and to look at the chamfered portion (the first boundary surface 5 and the second boundary surface 6) of the glass base 1 from various angles. They were then asked to determine the angle A at which they felt the reflected light from the chamfer was strongest. At this time, the illuminance of the light shining on the glass base 1 was changed in sequence from 1000 lux (corresponding to the light of a fluorescent lamp) to 15000 lux (corresponding to the illuminance slightly higher than that in the shade on a sunny day). The subjects were asked to record the illuminance at which they felt that the reflected light from the chamfer of the glass base 1 was too dazzling at angle A. The average illuminance at which each of the 11 subjects felt it was dazzling (hereinafter referred to simply as "illuminance" in this paragraph) was determined. In Table 1 below, "C" is entered when the illuminance is less than 4000 lux, "B" is entered when the illuminance is between 4000 lux and 8000 lux, and "A" is entered when the illuminance is 8000 lux or more. The higher the illuminance, the more the glare caused by the light reflected from the chamfered portion of the glass base 1 is suppressed, and the better the chamfered portion anti-glare property can be evaluated.
[0056] [Table 1]
[0057] <Summary of evaluation results> As is clear from the results shown in Table 1 above, Examples 1 to 4 and 7 were superior in chamfered portion antiglare property as compared with Examples 5 to 6 in which the second boundary surface 6 was a flat surface.
[0058] Comparing Example 1 and Example 2, Example 1 in which the radius of curvature R2 is larger than the radius of curvature R1 had better antiglare properties at the chamfered portion than Example 2 in which the radius of curvature R1 is larger than the radius of curvature R2. Comparing Example 1 and Example 7, which differ only in the radius of curvature R2, Example 1, in which the radius of curvature R2 is 0.6 mm, had better antiglare properties at the chamfered portion than Example 7, in which the radius of curvature R2 is 0.5 mm.
[0059] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2019-128071) filed on July 10, 2019, the contents of which are incorporated herein by reference. [Explanation of symbols]
[0060] 1: Glass substrate 2: First main surface 3: Second main surface 4: End face 5: First boundary surface 6:Second boundary surface 7: Third boundary surface 8: 4th boundary surface 12: Bend 21: Vehicle display device 22: Cabinet 23: Backlight unit 24: Display panel 25:Adhesive layer 31: Glass plate 32: First main surface of glass plate 33: Second main surface of glass plate 34: Edge of glass plate 35: Rotating grindstone 36: Grinding surface D1: diameter of grinding wheel R1: Radius of curvature of the first boundary surface R2: Radius of curvature of the second boundary surface θ1: Angle between the second boundary surface and the first principal surface L1: Length from the end face to the first main surface, in the tangential direction from the end face to the first main surface L2: Length from the end face to the second main surface, in the tangential direction from the end face to the second main surface
Claims
1. A first major surface; a second main surface that is a main surface opposite to the first main surface; an end surface sandwiched between the first main surface and the second main surface; a first boundary surface disposed between the first main surface and the end surface and connecting to the end surface; a second boundary surface connected to the first main surface and the first boundary surface, the second boundary surface is a convexly curved surface, The radius of curvature R of the second boundary surface 2 is 0.3 mm or more and 2.0 mm or less, A glass substrate, wherein the size of chipping at the second interface is 0.08 mm or less.
2. In a plane that passes through an arbitrary point Y1 on an intersection line X1 between said first principal surface and said second boundary surface and perpendicularly intersects said intersection line X1, a point on said first principal surface that is 50 μm away from said point Y1 is defined as point P1, and a point on said second boundary surface that is 50 μm away from said point Y1 in a direction parallel to said first principal surface is defined as point P2. Then, an angle θ between a straight line Y1P1 passing through said point Y1 and said point P1 and a straight line Y1P2 passing through said point Y1 and said point P2 is 1 The glass substrate according to claim 1 , wherein the angle is 10° or more and 45° or less.
3. the first boundary surface is a convexly curved surface, The radius of curvature R of the first boundary surface 1 The glass substrate according to claim 1 or 2, wherein the thickness is 0.1 mm or more and 1.0 mm or less.
4. The radius of curvature of the first boundary surface R 1 than the radius of curvature R of the second boundary surface 2 The glass substrate according to claim 3 , wherein 5. The glass substrate according to claim 4, wherein a difference between a radius of curvature R 1 of the first boundary surface and a radius of curvature R 2 of the second boundary surface is 0.2 mm or more.
6. 6. The glass substrate according to claim 1, wherein the first main surface and the second main surface have a bent portion.
7. A length L from the end surface to the first main surface in a tangential direction to the first main surface. 1 and a length L from the end surface to the second main surface in a tangential direction to the second main surface. 2 The glass substrate according to any one of claims 1 to 6, wherein the difference between the thickness and the thickness of the glass substrate is 0.2 mm or less.
8. The glass substrate according to any one of claims 1 to 7, which is used as a cover glass for a display device.
9. The glass substrate according to claim 8 , wherein the display device is an in-vehicle display device.
10. A method for producing a glass substrate according to any one of claims 1 to 9, comprising the steps of: Prepare the glass plate The glass plate is ground using a grindstone; The method for manufacturing a glass substrate, wherein the grinding surface of the rotary grindstone has a shape corresponding to the shapes of the first boundary surface and the second boundary surface.
Citation Information
Patent Citations
Photomask substrate, photomask blank, photomask, method for manufacturing photomask substrate, method for manufacturing photomask, and method for manufacturing display device
JP2017120416A
Glass plate
WO2013031548A1
Cover glass and display device
WO2017208995A1