Rosin phenolic resin composition, tackifier resin composition, pressure-sensitive adhesive composition, and method for producing rosin phenolic resin composition
Incorporating polycyclic aromatic compounds like xanthone, thioxanthone, or acridone in the rosin phenol resin composition addresses the issue of insufficient color tone, achieving a Gardner color number of 6 or less, thus improving the resin's appearance and suitability for various applications.
Patent Information
- Application Number
- JP2022031051
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-05
- Filing Date
- 2022-03-01
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-03-01
AI Technical Summary
Conventional rosin phenol resins exhibit insufficient color tone, often with Gardner color numbers of 7 or more, which is a significant drawback in applications where color clarity is important.
A rosin phenol resin composition is developed by incorporating specific polycyclic aromatic compounds such as xanthone, thioxanthone, acridone, or anthrone during the reaction with rosin and phenol, resulting in a composition with a Gardner color number of 6 or less.
The inclusion of these compounds significantly improves the color tone of the rosin phenol resin, enhancing its appearance and suppressing unwanted coloring, making it suitable for applications requiring better color clarity.
Smart Images

Figure 0007567834000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rosin phenolic resin composition, a tackifier resin composition, a pressure-sensitive adhesive composition, and a method for producing the rosin phenolic resin composition. [Background technology]
[0002] Rosin resins are used in various fields, such as tackifiers for hot melts, pressure-sensitive adhesives, and other adhesives, modifiers for rubber and plastics, emulsifiers for synthetic rubber, base materials for chewing gum, binder resins for road marking paints and inks, and sizing agents for papermaking. Examples of such rosin resins include natural rosin, purified rosin, hydrogenated rosin, disproportionated rosin, polymerized rosin, acid-modified rosin, rosin esters, rosin phenolic resins, rosin-modified phenolic resins, and metal salts thereof.
[0003] Among these, rosin phenolic resins are used as tackifiers in acrylic-based pressure-sensitive adhesives, chloroprene-based pressure-sensitive adhesives, and hot melt pressure-sensitive adhesives, and can impart excellent heat stability and adhesive strength to these pressure-sensitive adhesives (Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2007-504325 [Patent Document 2] Japanese Patent Application Publication No. 10-287855 Summary of the Invention [Problem to be solved by the invention]
[0005] However, many conventional rosin phenolic resins have insufficient color tones, and most of them have a Gardner color scale of at least 7. For example, Patent Document 1 also discloses that the color tone of the rosin phenolic resin actually obtained is at least 8 on the Gardner color scale, which is problematic in terms of color tone.
[0006] An object of the present invention is to provide a rosin phenolic resin composition having a good color tone. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by a rosin phenolic resin composition containing a specific polycyclic aromatic compound. That is, the present invention relates to the following rosin phenolic resin composition, tackifier resin composition, pressure-sensitive adhesive composition, and method for producing the rosin phenolic resin composition.
[0008] 1. Rosin phenolic resin, which is a reaction product of rosins (A) and phenols (B), and A rosin phenolic resin composition comprising at least one compound (C) selected from the group consisting of xanthone, thioxanthone, acridone and anthrone.
[0009] 2. The rosin phenolic resin composition according to item 1, wherein the color tone of the rosin phenolic resin composition is 6 or less in terms of the Gardner color scale.
[0010] 3. The rosin phenolic resin composition according to item 1 or 2, wherein the rosins (A) are derived from at least one pine species selected from the group consisting of swamp pine (slash pine), Merkus pine, Caribbean pine, Dao pine, Loblolly pine, Yunnan pine and Sibo pine.
[0011] 4. The rosin phenolic resin composition according to any one of items 1 to 3, wherein the rosin (A) is a purified rosin.
[0012] 5. In the presence of at least one compound (C) selected from the group consisting of xanthone, thioxanthone, acridone and anthrone, A method for producing a rosin phenolic resin composition, comprising the step of reacting a rosin (A) with a phenol (B).
[0013] 6. The method for producing the method according to item 5, The amount of the compound (C) used is 0.05 to 5% by mass based on 100% by mass of the rosins (A). A method for producing a rosin phenolic resin composition.
[0014] 7. The method according to item 5 or 6, A method for producing a rosin phenolic resin composition, comprising the step of reacting a rosin (A) with a phenol (B) in the presence of a compound (C) and a phenol sulfide.
[0015] 8. A tackifier resin composition comprising the rosin phenolic resin composition according to any one of items 1 to 4 above.
[0016] 9. A tackifier resin composition according to item 8, which is an aqueous dispersion of the rosin phenolic resin composition according to any one of items 1 to 4.
[0017] 10. A pressure-sensitive adhesive composition comprising the tackifier resin composition according to item 8 or 9 above and a base polymer. Effect of the Invention
[0018] The rosin phenolic resin composition of the present invention has a good color tone. Furthermore, since the tackifier resin composition and pressure-sensitive adhesive composition of the present invention contain the rosin phenolic resin composition, coloring is suppressed and the appearance is excellent. BEST MODE FOR CARRYING OUT THEINVENTION
[0019] [Rosin phenolic resin composition] The rosin phenolic resin composition of the present invention contains a rosin phenolic resin which is a reaction product of a rosin (A) (hereinafter referred to as component (A)) and a phenol (B) (hereinafter referred to as component (B)), and at least one compound (C) (hereinafter referred to as component (C)) selected from the group consisting of xanthone, thioxanthone, acridone, and anthrone.
[0020] (Rosins (A)) The component (A) is not particularly limited and various known compounds can be used. The component (A) may be used alone or in combination of two or more.
[0021] Examples of component (A) include natural rosins (gum rosin, tall oil rosin, wood rosin) derived from masson pine (Pinus massoniana), swamp pine (Pinus elliottii), Merkusii pine (Pinus caribaea), Pinus palustris, Loblolly pine (Pinus taeda), Yunnan pine (Pinus yunnanensis), Pinus kesiya, etc., refined rosin (hereinafter, natural rosin and refined rosin are collectively referred to as unmodified rosin), disproportionated rosin, hydrogenated rosin, etc.
[0022] The purified rosin can be obtained by using various known means. Specifically, the purified rosin can be obtained by using various known purification means such as distillation, extraction, recrystallization, and adsorption. The distillation method includes, for example, a method of distilling the natural rosin at a temperature of about 200 to 300° C. under a reduced pressure of about 0.01 to 3 kPa. The extraction method includes, for example, a method of making the natural rosin into an alkaline aqueous solution, extracting insoluble unsaponifiable matter with various organic solvents, and then neutralizing the aqueous layer. The recrystallization method includes, for example, a method of dissolving the natural rosin in an organic solvent as a good solvent, distilling off the solvent to obtain a concentrated solution, and further adding an organic solvent as a poor solvent. Examples of good solvents include aromatic hydrocarbon solvents such as benzene, toluene, and xylene, chlorinated hydrocarbon solvents such as chloroform, lower alcohols, ketones such as acetone, and acetates such as ethyl acetate. Examples of poor solvents include n-hexane, n-heptane, cyclohexane, and isooctane. The adsorption method may, for example, be a method in which unmodified rosin in a molten state or unmodified rosin in a solution state dissolved in an organic solvent is contacted with a porous adsorbent, for example, activated carbon, metal oxides such as alumina, zirconia, silica, molecular sieves, zeolite, and porous clay having fine holes.
[0023] The disproportionated rosin can be obtained by using various known means. Specifically, for example, the unmodified rosin can be obtained by a method (disproportionation) of heating the unmodified rosin in the presence of a disproportionation catalyst. As the disproportionation catalyst, various known catalysts such as supported catalysts on palladium-carbon, rhodium-carbon, platinum-carbon, etc.; metal powders such as nickel and platinum; and iodides such as iodine and iron iodide can be used. The amount of the catalyst used is usually about 0.01 to 5 parts by mass, preferably about 0.01 to 1 part by mass, based on 100 parts by mass of the unmodified rosin. The reaction temperature is about 100 to 300°C, preferably about 150 to 290°C.
[0024] Furthermore, the disproportionated rosin used may be one obtained by subjecting a disproportionated rosin to the above-mentioned purification.
[0025] The hydrogenated rosin can be obtained by using various known means. Specifically, for example, the hydrogenated rosin can be obtained by hydrogenating the unmodified rosin under known hydrogenation conditions. For example, the hydrogenation conditions include a method of heating the unmodified rosin to about 100 to 300° C. under a hydrogen pressure of about 2 to 20 MPa in the presence of a hydrogenation catalyst. In addition, the hydrogen pressure is preferably about 5 to 20 MPa, and the reaction temperature is preferably about 150 to 300° C. As the hydrogenation catalyst, various known catalysts such as supported catalysts and metal powders can be used. As the supported catalysts, palladium-carbon, rhodium-carbon, ruthenium-carbon, platinum-carbon, and the like can be used. As the metal powder, nickel, platinum, and the like can be used. Among these, palladium, rhodium, ruthenium, and platinum-based catalysts are preferred because they increase the hydrogenation rate of the unmodified rosin and shorten the hydrogenation time. The amount of the hydrogenation catalyst used is usually about 0.01 to 5 parts by mass, and preferably about 0.01 to 2 parts by mass, based on 100 parts by mass of the unmodified rosin.
[0026] The hydrogenation may be carried out, if necessary, in a state where the unmodified rosin is dissolved in a solvent. The solvent to be used is not particularly limited, but may be any solvent that is inert to the reaction and easily dissolves the raw materials and products. Specifically, for example, cyclohexane, n-hexane, n-heptane, decalin, tetrahydrofuran, dioxane, etc. may be used alone or in combination of two or more. The amount of the solvent used is not particularly limited, but it is usually sufficient to use the solvent so that the solid content is 10% by mass or more, preferably about 10 to 70% by mass, relative to the unmodified rosin.
[0027] The hydrogenated rosin may be one obtained by subjecting hydrogenated rosin to the above-mentioned purification.
[0028] The rosin phenolic resin composition of the present invention has the characteristic of excellent color tone even when rosins other than those derived from Masson pine (Pinus massoniana) are used as component (A).
[0029] Conventionally, rosin phenolic resin compositions obtained using rosins derived from pine species other than Masson pines, such as slash pine (Pinus elliottii), Merkusii, Caribaea, Palustris, Loblolly pine (Pinus taeda), Yunnanensis, and Pinus kesiya, tended to have insufficient color tone compared to those obtained using rosins derived from Masson pines. The rosin phenolic resin composition of the present invention, when reacted in the presence of component (C) described below, has excellent color tone even when rosins derived from pine species other than Masson pines are used as component (A).
[0030] The component (A) is preferably the above-mentioned purified rosin, since it provides an excellent color tone to the rosin phenolic resin composition.
[0031] (Phenols (B)) The component (B) is not particularly limited, and various known components can be used. The component (B) may be used alone or in combination of two or more.
[0032] Examples of the component (B) include phenol, naphthols, alkylphenols, and arylphenols.
[0033] Examples of the alkylphenols include o-cresol, o-normal butylphenol, o-isobutylphenol, o-tertiary butylphenol, o-pentylphenol, o-(cyclohexyl)phenol, o-octylphenol, o-nonylphenol, m-cresol, m-normal butylphenol, m-isobutylphenol, m-tertiary butylphenol, m-pentylphenol, m-(cyclohexyl)phenol, m-octylphenol, m-nonylphenol, p-cresol, p-normal butylphenol, p-isobutylphenol, p-tertiary butylphenol, p-pentylphenol, p-(cyclohexyl)phenol, p-octylphenol, and p-nonylphenol.
[0034] (Compound (C)) The component (C) is at least one compound selected from the group consisting of xanthone, thioxanthone, acridone, and anthrone. The component (C) may be used alone or in combination of two or more.
[0035] Component (C) may have various substituents on the aromatic ring contained therein, such as alkyl groups, aryl groups, arylalkyl groups, alkenyl groups, arylalkenyl groups, alkynyl groups, arylalkynyl groups, cycloalkyl groups, alkylene groups, cycloalkylalkylene groups, alkynylene groups, phenyl groups, halogens, hydroxyl groups, carboxyl groups, acyl groups, alkoxy groups, amino groups, and dialkylamino groups.
[0036] The content of component (C) in the rosin phenolic resin composition is not particularly limited, but in terms of excellent color tone of the rosin phenolic resin composition, it is preferably about 0.05 to 5 mass %, and more preferably about 0.1 to 0.5 mass %, relative to 100 mass % of the rosin phenolic resin composition.
[0037] The content of component (C) means the remaining amount of component (C) in the rosin phenolic resin composition obtained by the production method described below.
[0038] (Additives) The rosin phenolic resin composition may contain various additives as long as they do not impair the effects of the present invention. Examples of the additives include dehydrating agents, crystal nucleating agents, plasticizers, flow improvers, weather resistance agents, antioxidants, UV absorbers, heat stabilizers, light stabilizers, etc. The additives may be used alone or in combination of two or more.
[0039] (Antioxidants) Examples of the antioxidant include phenol sulfides, thiophosphites, phosphorus-based compounds, and hindered phenols.
[0040] Examples of the phenol sulfides include 4,4'-thiobis(6-t-butyl-3-methylphenol), 2,4-bis(dodecylthiomethyl)-6-methylphenol, 4,4'-bis(phenol) sulfide, 4,4'-bis(phenol) sulfoxide, 4,4'-bis(phenol) sulfone, 4,4'-bis(phenol) thiolsulfinate, 4,4'-bis(phenol) thiolsulfonate, 2,2'-bis(p-cresol) sulfide, 2,2'-bis(p-cresol) sulfoxide, 2,2'-bis(p-cresol) sulfone, 2,2'-bis(pt-butylphenol) sulfide, 2,2'-bis(pt-butylphenol) sulfoxide, 2,2'-bis(pt-butylphenol) sulfone, 4,4'-bis(6-t-butyl-m-cresol) sulfoxide, 4,4'-bis(6-t-butyl-m-cresol) sulfoxide, 4,4'-bis(6-t-butyl-o-cresol) sulfide, 4,4'-bis(6-t-butyl-o-cresol) sulfoxide, 4,4'-bis(6-t-butyl-o-cresol) sulfone, 4,4'-bis(6-t-butyl-o-cresol) sulfide, 4,4'-bis(resorcinol) sulfide, 4,4'-bis(resorcinol) sulfoxide, 4,4'-bis(resorcinol) sulfone, 1,1'-bis(β-naphthol ) sulfide, 1,1'-bis(β-naphthol) sulfoxide, 1,1'-bis(β-naphthol) sulfone, 4,4'-bis(α-naphthol) sulfide, 4,4'-bis(α-naphthol) sulfoxide, 4,4'-bis(α-naphthol) sulfone, t-amylphenol disulfide oligomer, nonylphenol disulfide oligomer, and t-butylphenol disulfide oligomer.
[0041] Examples of the thiophosphites include trilauryl trithiophosphite, tridecyl trithiophosphite, tribenzyl trithiophosphite, tricyclohexyl trithiophosphite, tri(2-ethylhexyl) trithiophosphite, trinaphthyl trithiophosphite, diphenyldecyl trithiophosphite, diphenyllauryl trithiophosphite, tetralauryl-4-oxaheptylene-1,7-tetrathiophosphite, tetrakis(mercaptolauryl)-1,6-dimercaptohexyl, and the like. dithiophosphite, pentakis(mercaptolauryl)bis(1,6-hexylene-dimercapto)trithiophosphite, tetrakis(mercaptolauryl)-2,9-dimercapto-p-methylene diphosphite, bis(mercaptolauryl)-1,6-dimercaptohexylene-bis(benzene phosphite), dioctyldithiopentaerythritol diphosphite, dilauryldithiopentaerythritol diphosphite, phenyllauryldithiopentaerythritol diphosphite, and the like.
[0042] Examples of the phosphorus-based compound include neutralized products such as phosphorous acid, hypophosphorous acid, and metal salts, amine salts, and ammonium salts thereof, triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2-ethylhexyl)phosphite, tridecyl phosphite, tris(tridecyl)phosphite, diphenyl mono(2-ethylhexyl)phosphite, diphenyl monodecyl phosphite, diphenyl mono(tridecyl)phosphite, 3,9-bis(2,6-di-t-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, dilauryl hydrogen phosphite, diphenyl hydrogen phosphite, tetraphenyl dipropylene glycol diphosphite, tetraphenyl Examples of such compounds include tetra(tridecyl)pentaerythritol tetraphosphite, tetra(tridecyl)-4,4'-isopropylidenediphenyl diphosphite, bis(t-butylphenyl)pentaerythritol diphosphite, bis(2,4-di-t-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(nonylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tris(2,4-di-t-butylphenyl)phosphite, hydrogenated bisphenol A·pentaerythritol phosphite polymer, and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0043] Examples of the hindered phenols include 2,5-di-tert-butylhydroquinone, anthraquinone, triethylene glycol bis{3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate}, 1,6-hexanediol bis{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate}, pentaerythrityl tetrakis{3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate}, octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, and the like. 3,9-bis[2-{3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionate}-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, N,N'-hexamethylenebis(3,5-di-t-butyl-4-hydroxy-hydrocinnamide), 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, Irganox (registered trademark) 565, and the like.
[0044] The antioxidant is preferably the phenol sulfide, because it provides an excellent color tone to the rosin phenol resin composition.
[0045] The content of the above additives in the rosin phenolic resin composition is not particularly limited, but in terms of excellent color tone of the rosin phenolic resin composition, it is preferably about 0.01 to 10 mass % relative to 100 mass % of the rosin phenolic resin composition, and more preferably about 0.01 to 1 mass %.
[0046] The content of the antioxidant in the rosin phenolic resin composition is not particularly limited, but in terms of excellent color tone of the rosin phenolic resin composition, it is preferably about 0.01 to 10 mass %, and more preferably about 0.01 to 1 mass %, relative to 100 mass % of the rosin phenolic resin composition.
[0047] (Method of producing rosin phenolic resin composition) The method for producing the rosin phenolic resin composition of the present invention is not particularly limited, but may be, for example, a method including a step of heating and reacting components (A) and (B) in the presence of component (C) and, if necessary, an acid catalyst, etc. The reaction may be carried out at a reaction temperature of 180 to 350°C for a reaction time of about 6 to 18 hours.
[0048] The method for producing the rosin phenolic resin composition of the present invention includes the following steps: (1) a step of reacting component (A) with component (B) at a temperature of about 100 to 200° C. for about 4 to 10 hours in the presence of an acid catalyst as necessary (addition step); and (2) a step of reacting the product (adduct) obtained in the step (1) at a temperature of about 250 to 350° C. for about 2 to 8 hours (condensation step), In the step (1) and / or the step (2), the reaction is preferably carried out in the presence of the component (C).
[0049] The above production method may include a step (neutralization step) of neutralizing the acid catalyst by adding a basic substance after the step (1). Examples of the basic substance include lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, etc.
[0050] In the above production method, the reaction in the step (2) may be carried out under reduced pressure. The reduced pressure conditions are not particularly limited, but are preferably about 0.1 to 10 kPa.
[0051] The acid catalyst is not particularly limited and various known ones can be used. Examples of the acid catalyst include inorganic acid catalysts such as sulfuric acid, hydrogen chloride, and boron trifluoride, and organic acid catalysts such as paratoluenesulfonic acid and methanesulfonic acid.
[0052] In the above production method, the amount of the component (B) used is not particularly limited, but it is preferably about 50 to 200 parts by mass per 100 parts by mass of the component (A).
[0053] In the above-mentioned production method, the amount of component (C) used is not particularly limited, but in terms of excellent color tone of the rosin phenolic resin composition, it is preferably about 0.05 to 5 mass % relative to 100 mass % of component (A), and more preferably about 0.1 to 0.5 mass %.
[0054] In the above production method, the amount of the acid catalyst used is not particularly limited, but it is preferably about 0.01 to 2.0 parts by mass per 100 parts by mass of the component (A).
[0055] In the above production method, the reaction may be carried out in the presence of the above antioxidant.
[0056] When the production method includes the steps (1) and (2), the antioxidant may be used in both steps (1) and (2), or in either one of the steps.
[0057] In the above-mentioned production method, the antioxidant is not particularly limited, but phenol sulfides are preferred in that they provide an excellent color tone to the rosin phenolic resin composition.
[0058] In the above production method, the amount of the antioxidant used is not particularly limited, but in terms of providing an excellent color tone to the rosin phenolic resin composition, it is preferably about 0.01 to 10 mass % relative to 100 mass % of component (A), and more preferably about 0.05 to 5 mass %.
[0059] (Physical Properties of Rosin Phenolic Resin Composition) The physical properties of the rosin phenolic resin composition are not particularly limited. The color tone of the rosin phenolic resin composition is preferably 6 or less in Gardner color scale, more preferably 5 or less in Gardner color scale. In the present invention, the color tone means the value of the Gardner unit color scale measured according to JIS K 0071-2.
[0060] In the present invention, the Gardner color number is as follows: A Gardner color number "between 5 and 6" means that the Gardner color number is 5, 5+, 5-6, 6-, or 6, where "5+" means that the color tone is darker than 5, "6-" means that the color tone is lighter than 6, and "5-6" means that the color tone is darker than 5+ but lighter than 6-. A Gardner color number "6 or less" means that the Gardner color number is a natural number of 6, 6-, 5-6, 5+, or 5 or less, and does not include 6+, 6-7, or natural numbers of 7 or more.
[0061] [Tackifying resin composition] The tackifier resin composition of the present invention contains the rosin phenolic resin composition of the present invention. The rosin phenolic resin composition of the present invention can function as a tackifier when used in a pressure-sensitive adhesive (including the pressure-sensitive adhesive composition described below).
[0062] The tackifier resin composition may contain various additives as necessary, such as a plasticizer, the antioxidant, an ultraviolet absorber, a heat stabilizer, a light stabilizer, and a tackifier other than the rosin phenolic resin composition, as long as the additives do not impair the desired properties.
[0063] The content of the rosin phenolic resin composition in the tackifier resin composition is not particularly limited, but is preferably about 95 to 100 parts by mass, calculated as solid content, per 100 parts by mass of the tackifier resin composition. The content of the additive in the tackifier resin composition is not particularly limited, but is preferably about 0 to 5 parts by mass, calculated as solid content, per 100 parts by mass of the tackifier resin composition.
[0064] (Water Dispersion of Rosin Phenolic Resin Composition) The tackifier resin composition of the present invention may be an aqueous dispersion of the rosin phenolic resin composition of the present invention (hereinafter, also simply referred to as aqueous dispersion).
[0065] The above-mentioned aqueous dispersion is a composition (emulsion) containing the above-mentioned rosin phenolic resin composition and an emulsifier.
[0066] The emulsifier is not particularly limited and various known emulsifiers can be used.Specific examples include high molecular weight emulsifiers obtained by polymerizing monomers, low molecular weight anionic emulsifiers, low molecular weight nonionic emulsifiers, etc.The emulsifiers may be used alone or in combination of two or more.
[0067] Examples of monomers used in the production of the high molecular weight emulsifier include (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and polyoxyalkylene (meth)acrylate; monocarboxylic acid vinyl monomers such as (meth)acrylic acid and crotonic acid; dicarboxylic acid vinyl monomers such as maleic acid, maleic anhydride, fumaric acid, itaconic acid, and muconic acid; sulfonic acid vinyl monomers such as vinyl sulfonic acid, styrene sulfonic acid, and 2-acrylamido-2-methylpropanesulfonic acid; 2-(meth)acryloyloxyethyl ... Examples of suitable monomers include phosphoric acid vinyl monomers such as phosphoric acid ester vinyl monomers such as diphenyl-2(meth)acryloyloxyphosphate, diphenyl-2(meth)acryloyloxyphosphate, and alkali metal salts, alkaline earth metal salts, ammonium salts, and salts of organic bases of these various organic acids, (meth)acrylamide monomers such as (meth)acrylamide, N-methylol(meth)acrylamide, and other monomers, nitrile monomers such as (meth)acrylonitrile, vinyl ester monomers such as vinyl acetate, hydroxyl group-containing (meth)acrylic acid ester monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and other styrenes such as styrene, α-methylstyrene, and vinyl toluene, and other monomers such as methyl vinyl ether, glycidyl (meth)acrylate, urethane acrylate, α-olefins having 6 to 22 carbon atoms, and vinyl pyrrolidone. These monomers may be used alone or in combination of two or more.
[0068] The monomers used in the production of the above-mentioned high molecular weight emulsifier are preferably methyl (meth)acrylate, alkali metal salts of sulfonic acid vinyl monomers, and styrenes, from the viewpoints of polymerizability and emulsifying properties of the resulting polymer emulsifier.
[0069] The polymerization method of the high molecular weight emulsifier can be solution polymerization, suspension polymerization, emulsion polymerization using a reactive emulsifier other than the high molecular weight emulsifier described below, a non-reactive emulsifier other than the high molecular weight emulsifier, etc. Examples of the non-reactive emulsifier include a low molecular weight anionic emulsifier and a low molecular weight nonionic emulsifier described below.
[0070] The weight-average molecular weight of the high molecular weight emulsifier is not particularly limited, but is usually preferably about 1,000 to 500,000 in terms of the adhesive properties of the resulting aqueous dispersion. In this specification, the weight-average molecular weight refers to a polyethylene oxide-equivalent value measured by gel permeation chromatography (GPC).
[0071] Examples of reactive emulsifiers other than the high molecular weight emulsifiers include those having hydrophilic groups such as sulfonic acid groups and carboxyl groups, and hydrophobic groups such as alkyl groups and phenyl groups, and having a carbon-carbon double bond in the molecule. Examples of the carbon-carbon double bond include functional groups such as (meth)allyl groups, 1-propenyl groups, 2-methyl-1-propenyl groups, vinyl groups, isopropenyl groups, and (meth)acryloyl groups.
[0072] Examples of the reactive emulsifier include polyoxyethylene alkyl ethers having at least one of the functional groups in the molecule, polyoxyethylene phenyl ethers having at least one of the functional groups in the molecule, and their sulfosuccinates and sulfates, and further include polyoxyethylene alkyl phenyl ethers having at least one of the functional groups in the molecule, and their sulfosuccinates, sulfates, phosphates, and aliphatic or aromatic carboxylates. Other examples include acidic phosphoric acid (meth)acrylic acid ester emulsifiers, acid anhydride modified products of rosin glycidyl ester acrylate (see JP-A-4-256429), and emulsifiers described in JP-A-63-23725, JP-A-63-240931, and JP-A-62-104802. Further, the polyoxyethylene in the above reactive emulsifier may be replaced with polyoxypropylene or a block copolymer or random copolymer of polyoxyethylene and polyoxypropylene.
[0073] Representative examples of commercially available reactive emulsifiers include "KAYAMER PM-1", "KAYAMER PM-2", "KAYAMER PM-21" (all manufactured by Nippon Kayaku Co., Ltd.), "SE-10N", "NE-10", "NE-20", "NE-30", "ADEKA REASOAP SR-10", "ADEKA REASOAP SR-20", "ADEKA REASOAP ER-20" (all manufactured by ADEKA Corporation), "New Frontier A229E", "New Frontier N117E", "New Frontier N250Z", "Aqualon RN-10", "Aqualon RN-20", "Aqualon RN-50", "Aqualon HS-10", "Aqualon KH-05", "Aqualon KH-10" (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), "Eminol JS-2" (manufactured by Sanyo Chemical Industries, Ltd.), and "Latherm K-180" (manufactured by Kao Corporation).
[0074] The reactive emulsifier is preferably a polyoxyethylene alkyl ether or polyoxyethylene phenyl ether in terms of polymerizability and the emulsifying properties of the resulting polymer emulsifier.
[0075] Examples of the low molecular weight anionic emulsifier include dialkyl sulfosuccinate salts, alkanesulfonates, α-olefinsulfonates, polyoxyethylene alkyl sulfosuccinate salts, polyoxyethylene alkyl ether sulfosuccinate salts, polyoxyethylene styryl phenyl ether sulfosuccinate salts, naphthalenesulfonic acid formalin condensates, polyoxyethylene alkyl ether sulfate salts, polyoxyethylene dialkyl ether sulfate salts, polyoxyethylene trialkyl ether sulfate salts, polyoxyethylene alkyl phenyl ether sulfate salts, etc. These may be used alone or in combination of two or more.
[0076] Examples of the low molecular weight nonionic emulsifier include polyoxyethylene alkyl ether, polyoxyethylene styryl phenyl ether, polyoxyethylene sorbitan fatty acid ester, etc. These may be used alone or in combination of two or more kinds.
[0077] The content of the emulsifier in the above-mentioned aqueous dispersion is not particularly limited, but from the viewpoint of excellent emulsification properties, it is preferably about 1 to 20 parts by mass, and more preferably about 2 to 10 parts by mass, calculated as solid content, per 100 parts by mass of the rosin phenolic resin composition.
[0078] The above-mentioned aqueous dispersion may contain, as necessary, a crosslinking agent, an antifoaming agent, a thickener, a filler, an ultraviolet absorber, a light stabilizer, an antioxidant, a water-resistant agent, a film-forming assistant, a preservative, a pH adjuster such as aqueous ammonia or sodium bicarbonate, and the like, as long as the desired properties are not impaired.
[0079] Examples of the preservative include thiazoline-based preservatives and benzoisothiazole-based preservatives.
[0080] The aqueous dispersion can be obtained by emulsifying the rosin phenolic resin composition in the presence of the emulsifier. The emulsification method is not particularly limited, and known emulsification methods such as high-pressure emulsification and phase inversion emulsification can be used.
[0081] The high-pressure emulsification method is a method in which the rosin phenolic resin composition is put into a molten state, an emulsifier and water are premixed, finely emulsified using a high-pressure emulsifier, and the solvent is removed as necessary. The material to be emulsified may be put into a molten state by heating alone, by dissolving it in a solvent and then heating, or by mixing it with a non-volatile substance such as a plasticizer and then heating, but it is preferable to use heating alone. Examples of the solvent include organic solvents that can dissolve the material to be emulsified, such as toluene, xylene, methylcyclohexane, and ethyl acetate.
[0082] The phase inversion emulsification method is a method in which a rosin phenolic resin composition is heated and melted, and then an emulsifier and water are added with stirring to form a W / O emulsion, and then the phase is inverted to an O / W emulsion by adding water or changing the temperature.
[0083] The concentration of the aqueous dispersion thus obtained is not particularly limited, but is usually adjusted appropriately so that the solid content is about 20 to 70 mass%. From the viewpoint of storage stability, the volume average particle size of the aqueous dispersion obtained is preferably less than about 0.7 μm. The aqueous dispersion obtained has a white to milky white appearance and a viscosity of usually about 10 to 1,000 mPa·s (temperature 25°C, concentration 50 mass%).
[0084] The pH of the aqueous dispersion obtained above is usually about 2 to 10. If necessary, the pH of the aqueous dispersion may be adjusted by appropriately adding an inorganic acid such as hydrochloric acid, sulfuric acid, or phosphoric acid; an alkanolamine such as monomethylamine, monoethanolamine, diethanolamine, or diisopropanolamine; an aliphatic amine such as ethylamine, n-butylamine, or triethylamine; an alkali metal hydroxide such as potassium hydroxide or sodium hydroxide; or an alkaline earth metal hydroxide such as calcium hydroxide.
[0085] [Adhesive / adhesive composition] The pressure-sensitive adhesive composition of the present invention comprises the rosin phenolic resin composition of the present invention (or the tackifier resin composition of the present invention) and a base polymer. The pressure-sensitive adhesive composition of the present invention can be used as a pressure-sensitive adhesive. In this specification, it is clear that the term "pressure-sensitive adhesive" includes either or both of a pressure-sensitive adhesive and an adhesive.
[0086] Examples of the base polymer include acrylic polymers, synthetic rubber elastomers, olefin polymers, acrylic polymer emulsions, rubber latexes, and synthetic resin emulsions. The base polymers may be used alone or in combination of two or more. The base polymer may further contain crosslinking agents, defoamers, viscosity modifiers, fillers, antioxidants, water-resistant agents, film-forming assistants, preservatives, pH adjusters such as ammonia water and sodium bicarbonate, leveling agents, release adjusters, plasticizers, softeners, colorants (pigments, dyes, etc.), surfactants, antistatic agents, antioxidants, UV absorbers, light stabilizers, etc., as necessary.
[0087] In the pressure-sensitive adhesive composition of the present invention, when the above-mentioned aqueous dispersion is used as the tackifier resin composition, it is preferable to use an aqueous composition such as an acrylic polymer emulsion, a rubber latex, or a synthetic resin emulsion as the base polymer.
[0088] In the pressure-sensitive adhesive composition of the present invention, when the pressure-sensitive adhesive composition contains the above-mentioned aqueous dispersion as a tackifier resin composition and the above-mentioned aqueous composition as a base polymer, the concentration of the pressure-sensitive adhesive composition is usually about 40 to 70 mass %, preferably 55 to 70 mass %, in terms of solid content.
[0089] (Acrylic polymer) The acrylic polymer may be one generally used in various acrylic pressure-sensitive adhesives, such as a polymer of a monomer component containing alkyl (meth)acrylate. The acrylic polymer may be produced by various known polymerization methods, such as a method of radically polymerizing the monomer component in the presence of a polymerization initiator. Examples of the polymerization method include solution polymerization, emulsion polymerization, suspension polymerization, and bulk polymerization. The acrylic polymer may be used alone or in combination of two or more.
[0090] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, and isooctyl (meth)acrylate. Examples of the alkyl (meth)acrylate include acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. These alkyl (meth)acrylates can be used alone or in combination of two or more.
[0091] The monomer component in the acrylic polymer may further contain other monomers copolymerizable with the alkyl (meth)acrylate, such as carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, amino group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, keto group-containing monomers, monomers having a nitrogen atom-containing ring, alkoxysilyl group-containing monomers, and polyfunctional monomers.
[0092] Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids such as acrylic acid (AA), methacrylic acid (MAA), and crotonic acid; and ethylenically unsaturated dicarboxylic acids such as maleic acid, itaconic acid, and citraconic acid, as well as their anhydrides (maleic anhydride, itaconic anhydride, etc.).
[0093] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate; and unsaturated alcohols such as vinyl alcohol and allyl alcohol.
[0094] Examples of the amide group-containing monomer include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide, N-methoxymethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide.
[0095] Examples of the amino group-containing monomer include aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate.
[0096] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether. Examples of the cyano group-containing monomer include acrylonitrile and methacrylonitrile. Examples of the keto group-containing monomer include diacetone (meth)acrylamide, diacetone (meth)acrylate, vinyl methyl ketone, vinyl ethyl ketone, allyl acetoacetate, and vinyl acetoacetate.
[0097] Examples of the monomer having a nitrogen atom-containing ring include N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-vinylmorpholine, N-vinylcaprolactam, and N-(meth)acryloylmorpholine.
[0098] Examples of the alkoxysilyl group-containing monomer include 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, and 3-(meth)acryloxypropylmethyldiethoxysilane.
[0099] Examples of the polyfunctional monomer include 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, glycerin di(meth)acrylate, epoxy acrylate, polyester acrylate, urethane acrylate, divinylbenzene, butyl di(meth)acrylate, and hexyl di(meth)acrylate.
[0100] The content of other monomers copolymerizable with alkyl (meth)acrylate in the monomer component is not particularly limited, but is preferably about 40% by mass or less relative to 100% by mass of the monomer component.
[0101] The monomer components further include vinyl ester monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrene (α-methylstyrene, etc.) and vinyl toluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate and isobornyl (meth)acrylate; aryl (meth)acrylates (e.g., phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (e.g., phenoxyethyl (meth)acrylate), arylalkyl ... The monomers may include aromatic ring-containing (meth)acrylates such as acrylates (e.g., benzyl (meth)acrylate); olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; isocyanate group-containing monomers such as 2-(meth)acryloyloxyethyl isocyanate; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether. The content of these monomers is not particularly limited, but is preferably about 10% by mass or less relative to 100% by mass of the above monomer components.
[0102] The polymerization initiator is not particularly limited, and examples thereof include azo-based initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride; and 1,1-bis(t-hexylperoxy)-3,3,5-trimethylaminopropane. Examples of the polymerization initiator include peroxide initiators such as ethylcyclohexane, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, benzoyl peroxide, t-butyl hydroperoxide, and hydrogen peroxide; and persulfate initiators such as potassium persulfate and ammonium persulfate. The polymerization initiator may be used alone or in combination of two or more.
[0103] The weight average molecular weight (Mw) of the acrylic polymer is not particularly limited, but is usually in the range of about 100,000 to 5,000,000. From the viewpoint of improving adhesive properties, the weight average molecular weight (Mw) of the acrylic polymer is preferably 1,500,000 or less, more preferably 1,000,000 or less, and from the viewpoint of cohesiveness, etc., it is preferably 200,000 or more, more preferably 300,000 or more. In this specification, the weight average molecular weight refers to a polystyrene-equivalent value in a gel permeation chromatography (GPC) method.
[0104] The content ratio of the acrylic polymer to the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of the modification by the rosin phenolic resin composition can be fully exerted and which does not cause a decrease in heat resistance retention, tackiness, etc. due to excessive use is usually about 2 to 40 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the acrylic polymer, calculated as solid content.
[0105] (Synthetic rubber elastomer) As the synthetic rubber elastomer, various known synthetic rubber elastomers used in pressure-sensitive adhesive compositions can be used. The synthetic rubber elastomers may be used alone or in combination of two or more.
[0106] Examples of the synthetic rubber elastomer include polyisoprene, styrene-butadiene rubber (SBR), styrene-isoprene (SI) rubber, styrene-isoprene-styrene block copolymer (SIS) rubber, styrene-butadiene-styrene block copolymer (SBS) rubber, styrene-ethylene-butylene-styrene block copolymer (SEBS) rubber, styrene-ethylene-propylene-styrene block copolymer (SEPS) rubber, styrene-ethylene-propylene block copolymer (SEP) rubber, reclaimed rubber, butyl rubber, polyisobutylene, styrene-butadiene-vinylpyridine rubber, polybutadiene, methyl methacrylate-butadiene rubber, acrylonitrile-butadiene rubber (NBR), polychloroprene (CR), and the like.
[0107] The content ratio of the synthetic rubber elastomer to the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of the modification by the rosin phenolic resin composition can be fully exerted and which does not cause a decrease in adhesive strength, tack, etc. due to excessive use is usually about 15 to 210 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the synthetic rubber elastomer, calculated as solid content.
[0108] (Olefin Polymer) The olefin-based polymer is not particularly limited as long as it is a polymer of a monomer component containing various olefins, and various known polymers can be used. Examples of the olefin-based polymer include an olefin-based homopolymer, which is a homopolymer of various olefins, and an olefin-based copolymer, which is a copolymer of various olefins and a copolymerizable monomer. The olefin-based polymer may be used alone or in combination of two or more kinds.
[0109] Examples of the olefins include ethylene, propylene, butene, butylene, isoprene, pentene, pentadiene, octene, isooctene, various isomers of hexene and hexadiene, various isomers of heptene and heptadiene, various α-olefins, and cyclic olefins such as cyclopentene, cyclohexene, norbornene, and dicyclopentadienyl. The olefins may be used alone or in combination of two or more.
[0110] Examples of the monomer copolymerizable with the olefins include vinyl acetate and the (meth)acrylic acid esters. The copolymerizable monomer is preferably vinyl acetate. The copolymerizable monomers may be used alone or in combination of two or more.
[0111] The amount of the copolymerizable monomer used in the olefin copolymer is not particularly limited, but is preferably in the range of about 20 to 45% by mass relative to 100% by mass of the olefin copolymer.
[0112] Examples of the olefin homopolymer include polyethylene, polypropylene, ethylene-α-olefin copolymer, amorphous atactic polypropylene, etc. Examples of the olefin copolymer include ethylene acrylic acid copolymer (EAA), ethylene methacrylic acid copolymer (EMAA), ethylene vinyl acetate copolymer (EVA), ethylene ethyl acrylate copolymer (EEA), ethylene methyl acrylate copolymer (EMA), ethylene methyl methacrylate copolymer (EMMA), etc. The olefin copolymer is preferably ethylene vinyl acetate copolymer (EVA).
[0113] The content ratio of the olefin polymer to the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of the modification by the rosin phenolic resin composition can be fully exerted and which does not cause a decrease in adhesive strength, tackiness, etc. due to excessive use is usually about 50 to 150 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the olefin polymer, calculated as solid content.
[0114] (Acrylic polymer emulsion) As the acrylic polymer emulsion, various known ones used for water-based pressure-sensitive adhesives can be used, for example, an emulsion of an acrylic polymer from a monomer component containing alkyl (meth)acrylate. The acrylic polymer emulsion can be produced by various known emulsion polymerization methods, for example, in the presence of a polymerization initiator, by known emulsion polymerization methods such as a batch-feed polymerization method, a monomer successive addition polymerization method, an emulsion monomer successive addition polymerization method, and a seed polymerization method. The acrylic polymer emulsion can be used alone or in combination of two or more kinds.
[0115] The alkyl (meth)acrylate may be, for example, the alkyl (meth)acrylate used in the acrylic polymer.
[0116] The monomer components in the acrylic polymer emulsion may further contain other monomers copolymerizable with the alkyl (meth)acrylate. Examples of such monomers include carboxyl group-containing monomers, hydroxyl group-containing monomers, amide group-containing monomers, amino group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, keto group-containing monomers, monomers having a nitrogen atom-containing ring, alkoxysilyl group-containing monomers, and polyfunctional monomers, which are used in the acrylic polymer.
[0117] The content of other monomers copolymerizable with alkyl (meth)acrylate in the monomer component is not particularly limited, but is preferably about 40% by mass or less relative to 100% by mass of the monomer component.
[0118] The monomer components further include vinyl ester monomers such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene, substituted styrene (α-methylstyrene, etc.) and vinyl toluene; cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate and isobornyl (meth)acrylate; aryl (meth)acrylates (e.g., phenyl (meth)acrylate), aryloxyalkyl (meth)acrylates (e.g., phenoxyethyl (meth)acrylate), arylalkyl ... The monomers may include aromatic ring-containing (meth)acrylates such as acrylates (e.g., benzyl (meth)acrylate); olefin monomers such as ethylene, propylene, isoprene, butadiene, and isobutylene; chlorine-containing monomers such as vinyl chloride and vinylidene chloride; isocyanate group-containing monomers such as 2-(meth)acryloyloxyethyl isocyanate; alkoxy group-containing monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; vinyl ether monomers such as methyl vinyl ether and ethyl vinyl ether. The content of these monomers is not particularly limited, but is preferably about 10% by mass or less relative to 100% by mass of the above monomer components.
[0119] The polymerization initiator is not particularly limited, and examples thereof include the polymerization initiators used in the acrylic polymer.
[0120] The weight average molecular weight (Mw) of the acrylic polymer in the acrylic polymer emulsion is not particularly limited, but is usually in the range of about 100,000 to 5,000,000. The weight average molecular weight (Mw) of the acrylic polymer is preferably 1,500,000 or less, more preferably 1,000,000 or less from the viewpoint of improving adhesive properties, and is preferably 200,000 or more, more preferably 300,000 or more from the viewpoint of cohesiveness, etc. In this specification, the weight average molecular weight refers to a polystyrene equivalent value in a gel permeation chromatography (GPC) method.
[0121] The content ratio of the acrylic polymer emulsion to the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of the modification by the rosin phenolic resin composition can be fully exerted and which does not cause a decrease in heat resistance retention, tackiness, etc. due to excessive use is usually about 2 to 40 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the acrylic polymer emulsion, calculated as solid content.
[0122] (rubber latex) As the rubber latex, various known latexes used in aqueous pressure-sensitive adhesive compositions can be used. Examples of the rubber latex include natural rubber latex and synthetic rubber latex. The natural rubber latex may be modified natural rubber obtained by grafting natural rubber with an alkyl (meth)acrylate ester or the like. The rubber latex may be used alone or in combination of two or more.
[0123] The synthetic rubber latex is an aqueous dispersion of a synthetic polymer, such as the synthetic rubber elastomer.
[0124] The content ratio of the rubber latex and the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of the modification by the rosin phenolic resin composition can be fully exhibited and the adhesive strength, tackiness, etc. are not reduced due to excessive use is usually about 10 to 150 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the rubber latex in terms of solid content.
[0125] (Synthetic resin emulsion) As the synthetic resin emulsion, various known emulsions used in aqueous pressure-sensitive adhesive compositions can be used, such as vinyl acetate emulsions, ethylene-vinyl acetate copolymer emulsions, urethane emulsions, etc. The synthetic resin emulsions may be used alone or in combination of two or more.
[0126] The content ratio of the synthetic resin emulsion to the rosin phenolic resin composition is not particularly limited, but an appropriate range in which the effect of modifying the rosin phenolic resin composition can be fully exerted and which does not cause a decrease in adhesive strength, tack, etc. due to excessive use is usually about 2 to 40 parts by mass of the rosin phenolic resin composition per 100 parts by mass of the synthetic resin emulsion, calculated as solid content.
[0127] In the above pressure-sensitive adhesive composition, when an acrylic polymer, a synthetic rubber elastomer, or an olefin polymer is used as the base polymer, the pressure-sensitive adhesive composition can be used in either a varnish type or a hot melt type.
[0128] When the pressure-sensitive adhesive composition is used as the varnish type, various organic solvents can be used. The organic solvent is not particularly limited, but specific examples include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, acetone, ethyl acetate, cyclohexane, methylcyclohexane, methanol, ethanol, propanol, isopropanol, and hexylene glycol. The amount of the organic solvent used is not particularly limited, but is usually about 100 to 500 parts by mass relative to 100 parts by mass of the base polymer.
[0129] When the pressure-sensitive adhesive composition is used as the hot melt type, the organic solvent that can be used in the varnish type is not particularly required.
[0130] The pressure-sensitive adhesive composition of the present invention may contain various additives, such as a crosslinking agent, an oil, a wax, an antifoaming agent, a viscosity modifier, a filler, an antioxidant, a water-resistant agent, a film-forming aid, a preservative, a pH adjuster such as ammonia water or sodium bicarbonate, a leveling agent, a release adjuster, a plasticizer, a softener, a colorant (pigment, dye, etc.), a surfactant, an antistatic agent, an antiaging agent, an ultraviolet absorbing agent, and a light stabilizer, as necessary, so long as the desired properties are not impaired.
[0131] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, etc. The content of the crosslinking agent is not particularly limited, but is usually 10 parts by mass or less, preferably about 0.01 to 1.0 part by mass, per 100 parts by mass of the base polymer.
[0132] Examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as 1,2-ethylene diisocyanate, 1,4-butylene diisocyanate, and 1,6-hexamethylene diisocyanate; alicyclic polyisocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, isophorone diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated xylene diisocyanate; aromatic polyisocyanates such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate; and biuret, isocyanurate, allophanate, and adduct thereof, as well as complexes obtained by reacting two or more selected from the group consisting of biuret, isocyanurate, allophanate, and adduct.
[0133] Examples of the epoxy crosslinking agent include compounds having two or more epoxy groups in the molecule, such as bisphenol A epichlorohydrin type epoxy resins, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N'-diamineglycidylaminomethyl)cyclohexane.
[0134] Examples of the oil include plasticizing oils such as naphthenic oils, paraffinic oils, and aromatic oils. Preferred oils are naphthenic process oils, paraffinic process oils, and liquid polybutene.
[0135] The content of the oil is not particularly limited, but is usually preferably about 4 to 200 parts by mass per 100 parts by mass of the base polymer.
[0136] Examples of the wax include animal-derived waxes such as beeswax, spermaceti, and shellac wax; vegetable waxes such as carnauba wax, Japan wax, rice bran wax, and candelilla wax; petroleum-derived waxes such as paraffin wax and microcrystalline wax; synthetic waxes such as Fischer-Tropsch wax and low molecular weight polyethylene wax; and mineral-derived waxes such as montan wax and ozokerite. The waxes may be used alone or in combination of two or more.
[0137] The content of the wax is not particularly limited, but is usually preferably about 10 to 100 parts by mass per 100 parts by mass of the base polymer.
[0138] The pressure-sensitive adhesive composition of the present invention can be obtained by mixing the rosin phenolic resin composition (or the tackifier resin composition) and the base polymer, and optionally various organic solvents and additives. The mixing method is not particularly limited, and various known methods can be used.
[0139] [Adhesive / bonding sheets] The adhesive sheet of the present invention comprises an adhesive layer made of the adhesive composition and a substrate. The adhesive sheet of the present invention may be an adhesive sheet with a substrate in which the adhesive layer is provided on one or both sides of the substrate, or may be an adhesive sheet without a substrate in which the adhesive layer is supported by a release liner (which may also be understood as a substrate having a release surface). The concept of the adhesive sheet here may include those referred to as adhesive tapes, adhesive labels, adhesive films, etc.
[0140] Examples of the substrate include polyolefin (polyethylene, polypropylene, ethylene-propylene copolymer, etc.) films, polyester (polyethylene terephthalate, etc.) films, vinyl chloride resin films, vinyl acetate resin films, polyimide resin films, polyamide resin films, fluorine resin films, and other plastic films such as cellophane; Japanese paper, craft paper, glassine paper, wood-free paper, synthetic paper, top-coated paper, and other papers; cotton fiber, staple fiber, Manila hemp, pulp, rayon, acetate fiber, polyester fiber, polyvinyl alcohol fiber, polyamide fiber, polyolefin fiber, and other natural fibers, semi-synthetic fibers, and synthetic fibers, woven fabrics and nonwoven fabrics made by blending or the like; rubber sheets made of natural rubber, butyl rubber, and the like; foam sheets made of foams such as polyurethane foam and polychloroprene rubber foam; metal foils such as aluminum foil and copper foil; and composites thereof. The film may be either a non-stretched type or a stretched type (uniaxially stretched type or biaxially stretched type). The substrate may have a single layer form or a laminate form.
[0141] In addition, the base material may contain various additives such as fillers (inorganic fillers, organic fillers, etc.), antiaging agents, antioxidants, UV absorbers, lubricants, plasticizers, colorants (pigments, dyes, etc.), etc., as necessary.
[0142] The surface of the substrate (particularly the surface on the polymer layer side) may be subjected to an appropriate known or conventional surface treatment, for example, a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as an undercoat treatment or a back surface treatment.
[0143] The pressure-sensitive adhesive sheet of the present invention can be produced by a known method. First, the pressure-sensitive adhesive composition is applied to one or both sides of a substrate to form a coating layer made of the pressure-sensitive adhesive composition. A known method can be applied as the coating method, and examples of the coating method include a roll coater method, a comma coater method, a die coater method, a reverse coater method, a silk screen method, and a gravure coater method. Next, the coating layer is heated or dried to form a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition. The heating or drying conditions can be appropriately set depending on the thickness of the pressure-sensitive adhesive layer, and the temperature is, for example, 10 to 120°C, and the time is, for example, 0.1 to 10 hours. The thickness of the pressure-sensitive adhesive layer (thickness after drying) varies depending on the application, but is preferably 5 to 200 μm. EXAMPLES
[0144] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0145] [Production of rosin phenolic resin composition] Example 1 A reaction vessel equipped with a stirrer, condenser, thermometer, and nitrogen and steam inlets was charged with 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol, then heated to 100°C, charged with 2.1 parts of 96% sulfuric acid, and reacted for 4 hours under a nitrogen gas stream. After adding 3.0 parts of slaked lime, 0.5 parts of xanthone (Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant), the mixture was heated to 280°C under reduced pressure of 10 kPa and reacted at the same temperature for 4 hours to obtain a rosin phenolic resin composition.
[0146] Example 2 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.2 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0147] Example 3 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.1 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0148] Example 4 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 2.0 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0149] Example 5 In a reaction vessel similar to that of Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 4.5 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0150] Example 6 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of thioxanthen-9-one (thioxanthone) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant Co., Ltd.) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0151] Example 7 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of Anthrone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0152] Example 8 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of 9(10H)-acridone (acridone) (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0153] Example 9 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese marsh pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0154] Example 10 In a reaction vessel similar to that of Example 1, 100.0 parts of gum rosin derived from Chinese Yunnan pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0155] Example 11 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0156] Example 12 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Brazilian Caribbean pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of xanthone (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0157] Comparative Example 1 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0158] Comparative Example 2 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of anthraquinone (manufactured by Kawasaki Chemical Industries, Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", manufactured by Addivant) were added, and the temperature was raised to 280°C under reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0159] Comparative Example 3 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese masson pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime, 0.5 parts of 9-fluorenone (Tokyo Chemical Industry Co., Ltd.), and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant Co., Ltd.) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0160] Comparative Example 4 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese marsh pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0161] Comparative Example 5 In a reaction vessel similar to that of Example 1, 100.0 parts of gum rosin derived from Chinese Yunnan pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0162] Comparative Example 6 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Chinese pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0163] Comparative Example 7 In a reaction vessel similar to that in Example 1, 100.0 parts of gum rosin derived from Brazilian Caribbean pine and 150.0 parts of phenol were charged, and the temperature was raised to 100°C. 2.1 parts of 96% sulfuric acid were charged and reacted for 4 hours under a nitrogen gas flow. 3.0 parts of slaked lime and 0.1 parts of 4,4'-thiobis(6-t-butyl-3-methylphenol) (trade name "Lowinox TBM-6", Addivant) were added, and the temperature was raised to 280°C under a reduced pressure of 10 kPa and the reaction was continued for 4 hours at the same temperature to obtain a rosin phenolic resin composition.
[0164] (Color Tone Measurement) The color tone (Gardner color scale) of the rosin phenolic resin compositions and the raw material natural rosin in Examples 1 to 12 and Comparative Examples 1 to 7 was measured in accordance with JIS K0071-2. The results are shown in Table 1.
[0165] [Table 1] The notes in Table 1 are as follows: *The amount (mass%) of compound (C) used relative to 100 mass% of rosin (A) in each Example and Comparative Example.
Claims
1. A rosin phenolic resin which is a reaction product of a rosin (A) and a phenol (B), and At least one compound (C) selected from the group consisting of xanthone, thioxanthone, acridone, and anthrone, The rosins (A) are derived from at least one pine species selected from the group consisting of marsh pine, Merkus pine, Caribbean pine, Dao pine, Loblolly pine, Yunnan pine, and Sibo pine. Rosin phenolic resin composition.
2. 2. The rosin phenolic resin composition according to claim 1, wherein the color tone of the rosin phenolic resin composition is 6 or less on the Gardner color scale.
3. 3. The rosin phenolic resin composition according to claim 1, wherein the rosin (A) is a purified rosin.
4. In the presence of at least one compound (C) selected from the group consisting of xanthone, thioxanthone, acridone, and anthrone, The method includes a step of reacting a rosin (A) with a phenol (B), The rosins (A) are derived from at least one pine species selected from the group consisting of marsh pine, Merkus pine, Caribbean pine, Dao pine, Loblolly pine, Yunnan pine, and Sibo pine. A method for producing a rosin phenolic resin composition.
5. The method according to claim 4, further comprising the steps of: The amount of the compound (C) used is 0.05 to 5% by mass based on 100% by mass of the rosins (A). A method for producing a rosin phenolic resin composition.
6. The method according to claim 4 or 5, A method for producing a rosin phenolic resin composition, comprising the step of reacting a rosin (A) with a phenol (B) in the presence of a compound (C) and a phenol sulfide.
7. A tackifier resin composition comprising the rosin phenolic resin composition according to any one of claims 1 to 3.
8. The tackifier resin composition according to claim 7, which is an aqueous dispersion of the rosin phenolic resin composition according to any one of claims 1 to 3.
9. A pressure-sensitive adhesive composition comprising the tackifier resin composition according to claim 7 or 8 and a base polymer.
Citation Information
Patent Citations
Curable resin composition, varnish and printing ink using the same
JP1997249811A
Hot-melt adhesive composition
JP1998287855A
Resins and adhesives containing them
JP2007504325A
Stickiness-imparting resin emulsion, its manufacturing method, and aqueous sticky and adhesive composition
JP2012007027A
Tackifier resin emulsion, aqueous tacky / adhesive composition and tacky / adhesive sheet
JP2020015904A