Full-biomass-based environment-friendly underwater adhesive and preparation method thereof
Through the depolymerization and modification of lignin powder, combined with epoxy soybean oil and bisaldehyde starch, tanninized lignin oligomers with crosslinking and accelerator functions were prepared, solving the existing biomass-based underwater The lack of performance of adhesives has achieved efficient and environmentally friendly underwater adhesive preparation, which is suitable for underwater bonding applications.
Patent Information
- Application Number
- CN202411212828.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing biomass-based underwater adhesives have problems such as high toxicity of raw materials, redundant preparation processes, low performance of target products and poor water resistance. It is urgently necessary to seek new preparation paths to achieve functional applications.
After heating, lignin powder and isopropanol solution are filtered and distilled under reduced pressure to remove isopropanol to obtain lignin monomers and oligomers, and phenolamine-based curing agents are catalyzed by sulfuric acid solution and sodium hydroxide, combined with epoxy Soybean oil and bisaldehyde starch, tanninized lignin oligomers with dual functions of crosslinking and accelerators are prepared for the preparation of fully biomass-based epoxy resins and underwater adhesives.
It realizes the high added value utilization of lignin, improves the adhesive performance, water resistance and stability, simplifies the preparation process, reduces the dependence on petroleum resources, conforms to the concept of green chemistry, and is suitable for underwater environments. Bonding application.
Smart Images

Figure CN119039914A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-value utilization of biomass-based materials, and in particular to a fully biomass-based green and environmentally friendly underwater adhesive and a preparation method thereof. Background Art
[0002] Epoxy resin adhesives are widely used in chemical, home appliance, aerospace and other fields due to their low price and good bonding properties. The most commonly used epoxy adhesive is bisphenol A diglycidyl ether (DGEBA) type, but bisphenol A has certain impacts on people and the environment; at the same time, underwater adhesives have great prospects in daily life, biomedical fields and industrial engineering; however, compared with adhesives used in dry (air) environments, adhesives used for wet or submerged surfaces in water environments face specific challenges in development and performance. Therefore, it is of great significance to develop a green and environmentally friendly biomass-based underwater adhesive.
[0003] At present, there are some reports on the synthesis of biomass-based underwater adhesives. For example, in the publication number CN113493665B "A palm oil-based underwater adhesive and its preparation method", palm oil is used as a raw material to synthesize palm oil fatty acid acrylamide ethyl ester, and it is mixed with isobornyl acrylate, and the palm oil-based underwater adhesive is prepared by ultraviolet light curing technology under the action of a photoinitiator; in the publication number CN114369435A "Preparation method of biomass-based adhesive and adhesive", biomass is used as a raw material to synthesize palm oil fatty acid acrylamide ethyl ester, and it is mixed with isobornyl acrylate, and the palm oil-based underwater adhesive is prepared by ultraviolet light curing technology under the action of a photoinitiator; The biomass hydrolyzate rich in aldehydes obtained by hydrolysis of the raw material reacts with the activated lignin obtained by the biomass raw material rich in lignin to obtain a biomass-based adhesive; in the publication number CN118325576A "A gelatin-based dopamine and tung oil full biomass adhesive and its preparation method", dopamine and tung oil are used to prepare dopamine-tung oil polymer, and then gelatin-based dopamine and tung oil adhesive is prepared. The adhesive has excellent bonding properties and can replace adhesives derived from petroleum materials with biomass materials. However, underwater adhesives currently still have shortcomings such as high raw material toxicity, complicated preparation process, low target product performance and poor product water resistance. It is urgent to seek a new preparation path to realize the functional application of biomass-based underwater adhesives. Summary of the invention
[0004] The purpose of the present invention is to provide a fully biomass-based green and environmentally friendly underwater adhesive and a preparation method thereof, so as to overcome the problems existing in the prior art. The present invention can solve the defects of the current underwater adhesives, such as the non-renewable traditional raw materials, the high toxicity of the preparation raw materials, the long curing time, and the complex preparation process, and provide a new idea and method for the preparation of green and environmentally friendly underwater adhesives via non-petroleum routes.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a fully biomass-based green and environmentally friendly underwater adhesive comprises the following steps: (1) Mixing lignin powder and isopropanol solution and placing them in a reactor to heat up to obtain a reaction product, filtering the reaction product to obtain a liquid product, subjecting the liquid product to reduced pressure distillation to remove the isopropanol solution to obtain bio-oil A, adding a mixed solvent of dichloromethane and petroleum ether to the bio-oil A, and then standing to obtain bio-oil B, and then separating the bio-oil B to obtain an upper layer mixed solution and a lower layer lignin oligomers, and subjecting the upper layer mixed solution to reduced pressure distillation at room temperature to obtain lignin monomers; (2) the lignin oligomers obtained in (1) and polyphenols are mixed in water and stirred to obtain a solution C, a sulfuric acid solution is added dropwise to the solution C to obtain a solution D, the solution D is heated for reaction, and then repeatedly washed with deionized water, and then vacuum dried to obtain a tannin lignin oligomer; (3) dissolving the lignin monomer obtained in (1) in a sodium hydroxide solution, heating to 60° C. and stirring, then adding aliphatic polyamine and glyoxal to obtain a solution E, heating the solution E to react to obtain a product, centrifuging the product to obtain a precipitate, repeatedly washing the precipitate with deionized water, and then drying to obtain a phenolamine lignin monomer curing agent; (4) adding 0.2 to 0.3 parts of the tannin oligomer obtained in (2) to the epoxidized soybean oil and uniformly stirring, then adding a nucleophilic reagent to react, then adding 0.3 to 0.4 parts of the tannin oligomer and uniformly stirring, then adding a nucleophilic reagent to react, and cooling to room temperature after the reaction is completed to obtain a biomass-based epoxy resin; (5) uniformly mixing the biomass-based epoxy resin obtained in (4) and the phenolamine lignin monomer curing agent obtained in (3), and then sequentially adding dialdehyde starch and 0.1 to 0.2 parts of tannin lignin oligomer obtained in (2) and uniformly stirring to obtain a biomass-based underwater adhesive; Furthermore, the lignin powder in (1) is any one of kraft lignin powder, cellulose ethanol residue enzymatic hydrolysis lignin powder or laboratory extracted ground wood lignin powder; the mass ratio of isopropanol to water in the isopropanol solution is (1-5):1; the mass ratio of the lignin powder to the isopropanol solution is 1:(15-18); Furthermore, the step of heating the reactor in (1) is specifically heating the reactor to 200-300°C at a power of 1200-1500 W and a heating rate of 50-200°C / min, and the reaction time is 0.5-2 min; the reduced pressure distillation is performed at 45-55°C; the mass ratio of the bio-oil A to dichloromethane and petroleum ether is 1:(0.1-0.2):(0.1-0.3); the standing time is 5-10 min; Furthermore, the mass ratio of lignin oligomers to polyphenols in (2) is 1:(1-3); the temperature of mixing in water is 60°C; the polyphenol is any one of catechol, gallic acid or pyrogallol; the mass ratio of water to lignin oligomers in solution C is 10:1; Furthermore, the mass fraction of the sulfuric acid solution in (2) is 78%; the mass ratio of the lignin oligomers in the solution D to the sulfuric acid solution is 1:(0.5-0.8); the heating reaction is carried out at 30-50°C for 1 h; the deionized water is repeatedly washed until the pH value is 5-6; the vacuum drying is carried out at 40°C for 24 h; Furthermore, the mass fraction of the sodium hydroxide solution in (3) is 40%; the stirring speed is 300 rpm; the aliphatic polyamine is any one of ethylenediamine, diethylenetriamine or triethylenetetramine; Furthermore, the mass ratio of lignin monomer, sodium hydroxide solution, aliphatic polyamine and glyoxal in the solution E in (3) is 1:10:(3-6):(1-2); the heating reaction is carried out at 70-90°C for 3-6 hours; the washing with deionized water is repeated until the pH value is 5-6; the drying is carried out at 60-80°C for 12 hours; Furthermore, the (4) is specifically as follows: according to the mass fraction, 0.2 to 0.3 parts of tannin oligomer obtained in (2) are added to 1 part of epoxidized soybean oil, and the mixture is stirred uniformly at a temperature of 70°C and a rotation speed of 400 rpm, and then 0.05 to 0.1 parts of a nucleophile are added to react for 30 min, and then 0.3 to 0.4 parts of tannin oligomer are added to stir uniformly, and then 0.15 to 0.2 parts of a nucleophile are added to react for 8 to 12 h, and after the reaction is completed, the mixture is cooled to room temperature to obtain a biomass-based epoxy resin; the nucleophile is any one of citric acid, malic acid or fumaric acid; Furthermore, in (5), the mass ratio of the biomass-based epoxy resin to the phenolamine lignin monomer curing agent is 1:(0.05-0.1); the mass ratio of the biomass-based epoxy resin, dialdehyde starch and tannin lignin oligomer is 1:(0.3-0.5):(0.1-0.2).
[0006] A fully biomass-based green and environmentally friendly underwater adhesive is obtained based on the above-mentioned preparation method of the fully biomass-based green and environmentally friendly underwater adhesive.
[0007] The above technical solution has the following advantages or beneficial effects: The present invention provides a method for preparing a fully biomass-based green and environmentally friendly underwater adhesive. Lignin oligomers and lignin monomers are obtained by depolymerizing lignin and fractionating and separating them in one step, and all of them are used to prepare the biomass-based underwater adhesive, thereby realizing high added value utilization of all components of lignin, and providing a new idea and method for preparing underwater adhesives via non-petroleum routes. The reaction system formed by alcohol solvent and water has a great influence on the depolymerization process of lignin, especially isopropanol, which can quickly act on the depolymerization of lignin. Lignin oligomers are modified by tannin and used as the cross-linking part of the underwater adhesive. , lignin monomers are used as curing agents for underwater adhesives through amination treatment, effectively realizing the high-value full-component utilization of lignin conversion products; lignin oligomers are treated with tannins by reacting with polyphenols (catechol, gallic acid and pyrogallol) to obtain tannin lignin oligomers, which can greatly increase the content of phenolic hydroxyl groups and reaction sites in lignin oligomers, thereby obtaining structural characteristics similar to tannic acid, further significantly improving the reaction activity of lignin oligomers, and providing reaction sites for subsequent reactions. At the same time, tannin lignin oligomers are used as promoters Adding it to biomass-based epoxy resin not only accelerates the reaction curing process and improves the bonding performance, but also increases the solid content, further improving the water resistance and stability. Therefore, the tannin lignin oligomer has the dual functions of crosslinking and accelerator. By aminating the lignin monomer to obtain the phenolamine lignin monomer curing agent, and using environmentally friendly glyoxal as a substitute for formaldehyde and glyoxylic acid imine, it not only helps to reduce dependence on petroleum-based raw materials, but also the addition of this type of curing agent can achieve curing under mild conditions, improve curing efficiency, improve bonding strength, and also make the reaction The process is easy to operate, safe, green and environmentally friendly; by adding tannin oligomers to the epoxidized soybean oil in batches, not only can the full reaction be ensured, the conversion rate of the reactants and the yield of the products be improved, but also the viscosity of the system will change significantly with the addition of tannin oligomers, and the batch addition is helpful to control the viscosity of the final product and improve the accuracy of the reaction endpoint control. At the same time, the batch addition of tannin oligomers can effectively prevent implosion, avoid the rapid and disordered increase of molecular weight, which makes the reaction endpoint difficult to control, and can effectively ensure the normal progress of the reaction;By learning from the adhesion principle of marine mussels, a fully biomass-based underwater adhesive is obtained. Compared with traditional underwater adhesives, the modified tannin lignin oligomers have a catechol-like structure, which can form various non-covalent and covalent interactions, which are conducive to interfacial adhesion and cohesion. The full utilization of lignin depolymerization products is the joint action of tannin lignin oligomers and phenolamine lignin monomer curing agents, thereby forming reversible ionic bonds, cation-π bonds and hydrogen bonds, enhancing the cohesive properties of the adhesive. The catechol-like groups in tannin lignin oligomers can also be oxidized to quinones, forming dynamic or permanent covalent bonds with phenolamine lignin monomer curing agents through Schiff base and Michael addition reactions, thereby further improving the covalent curing and mechanical reinforcement properties of the adhesive. ;
[0008] Furthermore, the preparation method of the present invention is completely based on biomass materials, such as sulfate lignin powder, cellulose ethanol residue enzymatic hydrolysis lignin powder or laboratory extracted ground wood lignin powder, and solvents such as isopropanol, dichloromethane and petroleum ether, all of which are renewable or recyclable materials, significantly reducing dependence on fossil resources, reducing environmental pollution, and complying with the concepts of green chemistry and sustainable development; by precisely controlling the reaction conditions, such as using a power of 1200-1500 W and a heating rate of 50-200 ° C / min, the required temperature of 200-300 ° C can be reached in a relatively short time of 0.5-2 min, thereby improving production efficiency; at the same time, the reduced pressure distillation is carried out at 45-55 ° C, which helps to effectively remove the solvent and further improves the preparation efficiency; the preparation method also specifies in detail the raw material ratio (such as the mass ratio of isopropanol to water, the mass ratio of lignin powder to isopropanol solution, the mass ratio of dichloromethane to petroleum ether) and reaction conditions (such as heating rate, reaction time and standing time), and the controllability of the parameters ensures the stability and consistency of product quality, which is conducive to industrial production.
[0009] Furthermore, the mass ratio of lignin oligomers to polyphenols was precisely controlled within the range of 1: (1-3). The optimization of this ratio helps to form a more stable underwater adhesive with superior performance. The use of catechol, gallic acid or pyrogallol as polyphenols can enhance the adhesion, water resistance and antioxidant properties of the adhesive, making it more adaptable to underwater environments. The mixing temperature in water was set at 60 ℃, which helps to reduce the occurrence of side reactions and ensure the smooth progress of the reaction; the heating reaction is carried out at 30~50℃, which further ensures the mildness of the reaction conditions and is conducive to maintaining the activity and stability of the product; by dropping a sulfuric acid solution with a mass fraction of 78%, and by accurately controlling the mass ratio of sulfuric acid solution to lignin oligomers to 1: (0.5~0.8), the pH value of the reaction system can be effectively adjusted to promote the formation of the target product; repeated washing with deionized water to pH=5~6 ensures that the pH value of the final product is moderate and its performance will not be affected by overacidity or overalkalinity; by repeatedly washing with deionized water and vacuum drying at 40℃ for 24h, impurities and residual solvents in the product can be completely removed, thereby improving the purity and quality of the product. Vacuum drying also helps to maintain the morphology and performance of the product and avoid oxidation or decomposition at high temperatures.
[0010] Furthermore, a sodium hydroxide solution with a mass fraction of 40% was used as a catalyst, combined with a stirring speed of 300 rpm. This combination ensured the uniformity of the reaction system and the appropriateness of the reaction rate. The addition of aliphatic polyamines (such as ethylenediamine, diethylenetriamine or triethylenetetramine) enhanced the strength and stability of the adhesive. The mass ratio of lignin monomer, sodium hydroxide solution, aliphatic polyamine and glyoxal in solution E was precisely controlled in the range of 1:10:(3-6):(1-2), which was helpful in forming an underwater adhesive with uniform structure and excellent performance. The addition of glyoxal further improved the water resistance and durability of the adhesive. The reaction is heated at ℃ for 3 to 6 hours to allow the reaction to proceed fully and avoid side reactions caused by excessively high temperatures. After the reaction is completed, it is repeatedly washed with deionized water to pH = 5 to 6 to ensure that the product has a moderate pH value, remove excess salt and unreacted raw materials, and improve the purity and quality of the product. The drying process is carried out at 60 to 80℃ for 12 hours, which helps to remove moisture from the product and avoid thermal degradation or oxidation caused by high temperature. The dried adhesive has good stability and storage properties.
[0011] Furthermore, by precisely controlling the mass ratio of biomass-based epoxy resin to phenolamine lignin monomer curing agent to 1:(0.05~0.1), and the mass ratio of biomass-based epoxy resin, dialdehyde starch and tannin lignin oligomer to 1:(0.3~0.5):(0.1~0.2), not only the cross-linking density and strength of the adhesive are enhanced, but also its water resistance and environmental adaptability are improved.
[0012] Furthermore, the all-biomass-based green and environmentally friendly underwater adhesive obtained based on this preparation method can be used for the bonding of underwater wood, plastic, metal and other substrates. It has high bonding strength and can withstand multiple cycles of stretching. After being soaked underwater for one month, the bonding strength remains high. It not only has excellent adhesion and durability, but also has good water resistance, corrosion resistance and environmental adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 The present invention is a process flow chart of a method for preparing a fully biomass-based green and environmentally friendly underwater adhesive. DETAILED DESCRIPTION
[0014] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it. In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention. It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0015] A method for preparing a fully biomass-based green and environmentally friendly underwater adhesive comprises the following steps: (1) Mix lignin powder and isopropanol solution in a mass ratio of 1:(15-18) and place them in a microwave reactor. Heat the mixture to 200-300 °C at a power of 1200-1500 W and a heating rate of 50-200 °C / min for a reaction time of 0.5-2 min to obtain a reaction product. Filter the reaction product to obtain a liquid product. Distill the liquid product under reduced pressure at 45-55 °C to remove the isopropanol solution to obtain bio-oil A. Slowly add a mixed solvent of dichloromethane and petroleum ether to the bio-oil A, wherein the mass ratio of bio-oil A to dichloromethane and petroleum ether is 1:(0.1-0.2):(0.1-0.3). Let stand for 5-10 min to obtain bio-oil B. Separate the bio-oil B to obtain an upper mixed solution and a lower lignin oligomer. Distill the upper mixed solution under reduced pressure at room temperature to obtain lignin monomer. Preferably, the lignin powder is any one of kraft lignin powder, cellulosic ethanol residue enzymatic hydrolysis lignin powder or laboratory extracted groundwood lignin powder; Preferably, the mass ratio of isopropanol to water in the isopropanol solution is (1-5):1; Preferably, by means of microwave chemical reaction, lignin is rapidly converted into the desired lignin oligomers and lignin monomers in an isopropanol aqueous solution within 0.5 to 2 minutes; microwave technology can be used to efficiently convert lignin into lignin oligomers and lignin monomers with a molecular weight of 800 to 1100 Da in a very short time, such as phenol, syringaldehyde, vanillin, etc. (2) The lignin oligomers obtained in (1) and polyphenols were mixed in a mass ratio of 1:(1-3) in water at 60°C and stirred to obtain a solution C. A 78% by mass sulfuric acid solution was added dropwise to the solution C to obtain a solution D. The solution D was reacted at 30-50°C for 1 h, and then repeatedly washed with deionized water until the pH value was 5-6, and then vacuum dried at 40°C for 24 h to obtain a tannin lignin oligomer. Preferably, the polyphenol is any one of catechol, gallic acid or pyrogallol; Preferably, the mass ratio of water to lignin oligomers in solution C is 10:1; Preferably, the mass ratio of lignin oligomers to sulfuric acid solution in solution D is 1:(0.5-0.8); (3) dissolving the lignin monomer obtained in (1) in a sodium hydroxide solution having a mass fraction of 40%, heating the solution to 60°C and stirring the solution at a speed of 300 rpm, then adding aliphatic polyamine and glyoxal to obtain a solution E, reacting the solution E at 70-90°C for 3-6 h to obtain a product, centrifuging the product to obtain a precipitate, repeatedly washing the precipitate with deionized water until the pH value is 5-6, and then drying the precipitate at 60-80°C for 12 h to obtain a phenolamine lignin monomer curing agent; Preferably, the aliphatic polyamine is any one of ethylenediamine, diethylenetriamine or triethylenetetramine; Preferably, the mass ratio of lignin monomer, sodium hydroxide solution, aliphatic polyamine and glyoxal in solution E is 1:10:(3-6):(1-2); (4) Add 0.2 to 0.3 parts of tannin oligomer obtained in (2) to 1 part of epoxidized soybean oil according to the mass ratio, stir evenly at a temperature of 70 ° C and a speed of 400 rpm, then add 0.05 to 0.1 parts of nucleophilic reagent to react for 30 min, then add 0.3 to 0.4 parts of tannin oligomer to stir evenly, then add 0.15 to 0.2 parts of nucleophilic reagent to react for 8 to 12 h, and after the reaction is completed, cool to room temperature to obtain a biomass-based epoxy resin; Preferably, the nucleophile is any one of citric acid, malic acid or fumaric acid; (5) The biomass-based epoxy resin obtained in (4) and the phenolamine lignin monomer curing agent obtained in (3) are uniformly mixed in a mass ratio of 1:(0.05-0.1), and then dialdehyde starch and 0.1-0.2 parts of tannin oligomers obtained in (2) are added in sequence and uniformly stirred to obtain a biomass-based underwater adhesive; wherein the dialdehyde starch acts as a stabilizer and the tannin oligomers act as a promoter; Preferably, when dialdehyde starch and tannin oligomers are added, the mass ratio of biomass-based epoxy resin, dialdehyde starch and tannin oligomers is 1: (0.3-0.5): (0.1-0.2).
[0016] A fully biomass-based green and environmentally friendly underwater adhesive is obtained based on the above-mentioned preparation method of the fully biomass-based green and environmentally friendly underwater adhesive.
[0017] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0018] Embodiment 1: The method for preparing the all-biomass-based green and environmentally friendly underwater adhesive in this embodiment comprises the following steps: (1) 3 g of kraft lignin powder was mixed with 45 g of isopropanol solution (including 22.5 g of isopropanol and 22.5 g of water) and placed in a microwave reactor. The temperature was raised to 200 °C at a power of 1200 W and a heating rate of 50 °C / min for a reaction time of 2 min to obtain a reaction product. The reaction product was filtered to obtain a liquid product. The isopropanol solution was removed from the liquid product under reduced pressure at 45 °C to obtain bio-oil A. A mixed solvent of 0.2 g of dichloromethane and 0.2 g of petroleum ether was slowly added to 2 g of bio-oil A, and then the mixture was allowed to stand for 5 min to obtain bio-oil B. Bio-oil B was then separated to obtain an upper mixed solution and a lower lignin oligomer. The upper mixed solution was distilled under reduced pressure at room temperature to obtain lignin monomer. (2) 4 g of the lignin oligomers obtained in (1) and 4 g of catechol were placed in 40 g of 60 °C water and stirred to obtain solution C. 2 g of 78% H2SO4 solution was added dropwise to solution C to obtain solution D. Solution D was reacted at 30 °C for 1 h, then repeatedly washed with deionized water until pH = 5, and then vacuum dried at 40 °C for 24 h to obtain tannin lignin oligomers. (3) 2 g of the lignin monomer obtained in (1) was dissolved in 20 g of a 40% NaOH solution, heated to 60 °C and stirred at 300 rpm, then 6 g of ethylenediamine and 2 g of glyoxal were added to obtain a solution E, and the solution E was reacted at 70 °C for 6 h to obtain a product, the product was centrifuged to obtain a precipitate, the precipitate was repeatedly washed with deionized water until the pH value was 5, and then dried at 60 °C for 12 h to obtain a phenolamine lignin monomer curing agent; (4) Add 2 g of the tannin oligomer obtained in (2) to 10 g of epoxidized soybean oil, stir evenly at 70 °C and 400 rpm, then add 0.5 g of citric acid and react for 30 min, then add 3 g of tannin oligomer and stir evenly, then add 1.5 g of citric acid and react for 8 h. After the reaction is completed, cool to room temperature to obtain a biomass-based epoxy resin. (5) 5 g of the biomass-based epoxy resin obtained in (4) and 0.25 g of the phenolamine lignin monomer curing agent obtained in (3) were uniformly mixed, and then 1.5 g of dialdehyde starch and 0.5 g of tannin lignin oligomer obtained in (2) were added in sequence and uniformly stirred to obtain a biomass-based underwater adhesive.
[0019] The biomass-based underwater adhesive obtained based on the above preparation method can be used for bonding underwater wood substrates. After curing for 1 h at room temperature, the bonding strength reaches 8 MPa. It can withstand 100 cycles of stretching, and after being immersed in water for one month, the bonding strength can still reach 63%.
[0020] Embodiment 2: The method for preparing the all-biomass-based green and environmentally friendly underwater adhesive in this embodiment comprises the following steps: (1) 5 g of cellulose ethanol residue enzymatic hydrolysis lignin powder was mixed with 90 g of isopropanol solution (75 g of isopropanol and 15 g of water) and placed in a microwave reactor. The temperature was raised to 300 °C at a power of 1500 W and a heating rate of 200 °C / min for a reaction time of 0.5 min to obtain a reaction product. The reaction product was filtered to obtain a liquid product. The isopropanol solution was removed from the liquid product under reduced pressure at 55 °C to obtain bio-oil A. A mixed solvent of 0.8 g of dichloromethane and 1.2 g of petroleum ether was slowly added to 4 g of bio-oil A, and then the mixture was allowed to stand for 10 min to obtain bio-oil B. Bio-oil B was then separated to obtain an upper mixed solution and a lower lignin oligomer. The upper mixed solution was distilled under reduced pressure at room temperature to obtain lignin monomer. (2) 6 g of the lignin oligomers obtained in (1) and 18 g of gallic acid were placed in 60 g of 60 °C water and stirred to obtain solution C. 4.8 g of 78% H2SO4 solution was added dropwise to solution C to obtain solution D. Solution D was reacted at 50 °C for 1 h, then repeatedly washed with deionized water until pH = 6, and then vacuum dried at 40 °C for 24 h to obtain tannin lignin oligomers. (3) 4 g of the lignin monomer obtained in (1) was dissolved in 40 g of a 40% NaOH solution, heated to 60 °C and stirred at 300 rpm, then 24 g of triethylenetetramine and 8 g of glyoxal were added to obtain a solution E, and the solution E was reacted at 90 °C for 3 h to obtain a product, the product was centrifuged to obtain a precipitate, the precipitate was repeatedly washed with deionized water to pH = 6, and then dried at 80 °C for 12 h to obtain a phenolamine lignin monomer curing agent; (4) Add 6 g of the tannin oligomer obtained in (2) to 20 g of epoxidized soybean oil, stir evenly at 70 °C and 400 rpm, then add 2 g of fumaric acid and react for 30 min, then add 8 g of tannin oligomer and stir evenly, then add 4 g of fumaric acid and react for 12 h. After the reaction is completed, cool to room temperature to obtain a biomass-based epoxy resin. (5) 12 g of the biomass-based epoxy resin obtained in (4) and 1.2 g of the phenolamine lignin monomer curing agent obtained in (3) were uniformly mixed, and then 6 g of dialdehyde starch and 2.4 g of tannin lignin oligomer obtained in (2) were added in sequence and uniformly stirred to obtain a biomass-based underwater adhesive.
[0021] The biomass-based underwater adhesive obtained based on the above preparation method can be used for bonding underwater plastic substrates. It can be cured at room temperature for 40 min, and the bonding strength reaches 12 MPa. It can withstand 120 cycles of stretching, and after being immersed in water for one month, the bonding strength can still reach 68%.
[0022] Embodiment 3: The method for preparing the all-biomass-based green and environmentally friendly underwater adhesive in this embodiment comprises the following steps: (1) 4 g of ground wood lignin powder extracted in the laboratory was mixed with 64 g of isopropanol solution (including 48 g of isopropanol and 16 g of water) and placed in a microwave reactor. The temperature was raised to 260 °C at a power of 1300 W and a heating rate of 150 °C / min for 1 min to obtain a reaction product. The reaction product was filtered to obtain a liquid product. The isopropanol solution was removed from the liquid product under reduced pressure at 50 °C to obtain bio-oil A. A mixed solvent of 0.45 g of dichloromethane and 0.6 g of petroleum ether was slowly added to 3 g of bio-oil A, and then the mixture was allowed to stand for 7 min to obtain bio-oil B. Bio-oil B was then separated to obtain an upper mixed solution and a lower lignin oligomer. The upper mixed solution was distilled under reduced pressure at room temperature to obtain lignin monomer. (2) 5 g of the lignin oligomers obtained in (1) and 10 g of pyrogallol were placed in 50 g of 60 °C water and stirred to obtain solution C. 3 g of 78% H2SO4 solution was added dropwise to solution C to obtain solution D. Solution D was reacted at 40 °C for 1 h, then repeatedly washed with deionized water until the pH value was 5.5, and then vacuum dried at 40 °C for 24 h to obtain tannin lignin oligomers. (3) 3 g of the lignin monomer obtained in (1) was dissolved in 30 g of a 40% NaOH solution, heated to 60 °C and stirred at 300 rpm, then 15 g of triethylenetetramine and 4.5 g of glyoxal were added to obtain a solution E, and the solution E was reacted at 80 °C for 4 h to obtain a product, the product was centrifuged to obtain a precipitate, the precipitate was repeatedly washed with deionized water until the pH value was 5.5, and then dried at 70 °C for 12 h to obtain a phenolamine lignin monomer curing agent; (4) 3.75 g of the tannin oligomer obtained in (2) was added to 15 g of epoxidized soybean oil, and the mixture was stirred uniformly at 70 °C and 400 rpm. Then, 0.9 g of malic acid was added to react for 30 min, and then 5.25 g of tannin oligomer was added to stir uniformly. Then, 2.4 g of malic acid was added to react for 10 h. After the reaction was completed, the mixture was cooled to room temperature to obtain a biomass-based epoxy resin. (5) 8 g of the biomass-based epoxy resin obtained in (4) and 0.56 g of the phenolamine lignin monomer curing agent obtained in (3) were uniformly mixed, and then 3.2 g of dialdehyde starch and 1.2 g of tannin lignin oligomer obtained in (2) were added in sequence and uniformly stirred to obtain a biomass-based underwater adhesive.
[0023] The biomass-based underwater adhesive obtained based on the above preparation method can be used for bonding underwater metal substrates. It can be cured at room temperature for 20 min, and the bonding strength reaches 18 MPa. It can withstand 180 cycles of stretching, and after being immersed in water for one month, the bonding strength can still reach 72%.
[0024] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a fully biomass-based green and environmentally friendly underwater adhesive, characterized in that: The steps include: S1, mixing lignin powder and isopropanol solution, placing in a reactor and heating to obtain a reaction product, filtering the reaction product to obtain a liquid product, performing reduced pressure distillation on the liquid product to remove the isopropanol solution to obtain bio-oil A, adding a mixed solvent of dichloromethane and petroleum ether to the bio-oil A, and then standing to obtain bio-oil B, and then separating the bio-oil B to obtain an upper layer mixed solution and a lower layer lignin oligomers, and performing reduced pressure distillation on the upper layer mixed solution at room temperature to obtain lignin monomer; S2, taking the lignin oligomers obtained in S1 and polyphenols, mixing them in water, and stirring them evenly to obtain a solution C, adding a sulfuric acid solution dropwise to the solution C to obtain a solution D, heating the solution D for reaction, and then repeatedly washing it with deionized water, and then vacuum drying it to obtain a tannin lignin oligomer; S3, dissolving the lignin monomer obtained in S1 in a sodium hydroxide solution, heating to 60°C and stirring, then adding aliphatic polyamine and glyoxal to obtain a solution E, heating the solution E to react to obtain a product, centrifuging the product to obtain a precipitate, repeatedly washing the precipitate with deionized water, and then drying to obtain a phenolamine lignin monomer curing agent; S4, adding 0.2 to 0.3 parts of tannin oligomer obtained in S2 to epoxy soybean oil and stirring them uniformly, then adding a nucleophilic reagent to react, then adding 0.3 to 0.4 parts of tannin oligomer to stir them uniformly, then adding a nucleophilic reagent to react, and cooling to room temperature after the reaction is completed to obtain a biomass-based epoxy resin; S5, uniformly mixing the biomass-based epoxy resin obtained in S4 and the phenolamine lignin monomer curing agent obtained in S3, and then sequentially adding dialdehyde starch and 0.1 to 0.2 parts of tannin lignin oligomer obtained in S2 and uniformly stirring to obtain a biomass-based underwater adhesive.
2. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The lignin powder in S1 is any one of kraft lignin powder, cellulose ethanol residue enzymatic hydrolysis lignin powder or laboratory extracted ground wood lignin powder; the mass ratio of isopropanol to water in the isopropanol solution is (1-5):1; the mass ratio of the lignin powder to the isopropanol solution is 1:(15-18).
3. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The specific heating in S1 is: heating to 200-300 °C at a power of 1200-1500 W and a heating rate of 50-200 °C / min, and the reaction time is 0.5-2 min; the reduced pressure distillation is carried out at 45-55 °C; the mass ratio of the bio-oil A to dichloromethane and petroleum ether is 1: (0.1-0.2): (0.1-0.3); the standing time is 5-10 min.
4. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The mass ratio of lignin oligomers to polyphenols in the S2 is 1:(1-3); the temperature of mixing in water is 60°C; the polyphenol is any one of catechol, gallic acid or pyrogallol; the mass ratio of water to lignin oligomers in the solution C is 10:
1.
5. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The mass fraction of the sulfuric acid solution in the S2 is 78%; the mass ratio of the lignin oligomers to the sulfuric acid solution in the solution D is 1:(0.5-0.8); the heating reaction is carried out at 30-50°C for 1 h; the deionized water is repeatedly washed until the pH value is 5-6; and the vacuum drying is carried out at 40°C for 24 h.
6. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The mass fraction of the sodium hydroxide solution in S3 is 40%; the stirring speed is 300 rpm; and the aliphatic polyamine is any one of ethylenediamine, diethylenetriamine or triethylenetetramine.
7. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The mass ratio of lignin monomer, sodium hydroxide solution, aliphatic polyamine and glyoxal in solution E in S3 is 1:10:(3-6):(1-2); the heating reaction is carried out at 70-90°C for 3-6 hours; the deionized water is repeatedly washed until the pH value is 5-6; and the drying is carried out at 60-80°C for 12 hours.
8. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The S4 is specifically as follows: according to the mass fraction, 0.2 to 0.3 parts of tannin oligomers obtained in S2 are added to 1 part of epoxidized soybean oil, and stirred evenly at a temperature of 70 ° C and a rotation speed of 400 rpm, and then 0.05 to 0.1 parts of nucleophilic reagents are added to react for 30 min, and then 0.3 to 0.4 parts of tannin oligomers are added to stir evenly, and then 0.15 to 0.2 parts of nucleophilic reagents are added to react for 8 to 12 h. After the reaction is completed, the reaction is cooled to room temperature to obtain a biomass-based epoxy resin; the nucleophilic reagent is any one of citric acid, malic acid or fumaric acid.
9. The method for preparing a fully biomass-based green and environmentally friendly underwater adhesive according to claim 1, characterized in that: The mass ratio of the biomass-based epoxy resin to the phenolamine lignin monomer curing agent in S5 is 1:(0.05-0.1); the mass ratio of the biomass-based epoxy resin, dialdehyde starch and tannin lignin oligomer is 1:(0.3-0.5):(0.1-0.2).
10. A fully biomass-based green and environmentally friendly underwater adhesive, characterized in that: The invention is obtained based on the preparation method of a fully biomass-based green and environmentally friendly underwater adhesive described in any one of claims 1-9.
Citation Information
Cited By
Environment-friendly waterproof adhesive for furniture wood board and preparation method of environment-friendly waterproof adhesive
CN119592271A
Preparation and use method of biomass super-strong universal adhesive
CN119614148A
Green, low-cost and high-performance lignin adhesive as well as preparation method and application thereof
CN120290136A
Environment-friendly insole adhesive and preparation method thereof
CN121022345A