Flotation combined reagent and application thereof in lepidolite flotation

By using a combination agent of metal ion activator and an anion-cation combination collector in lithium mica flotation, the problems of poor selectivity and poor capture ability of lithium mica in the prior art are solved, and the efficiency of lithium mica is achieved Recycling and green utilization of resources.

CN119034950APending Publication Date: 2024-11-29KUNMING UNIV OF SCI & TECH

Patent Information

Application Number
CN202411466978.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing lithium mica flotation process has problems such as poor selectivity, poor capture ability, weak adaptability and poor controllability of flotation foam, resulting in a low recycling rate of lithium mica and a large corrosion and environmental pollution of equipment and environmental pollution.

Method used

Using a flotation combination agent, including metal ion activator and an anion-cation combination collector, the adsorption selectivity and capture of lithium mica are improved through the directional adsorption function of metal ions and the synergistic effect of anion-cation collector. The harvesting capacity simplifies the process flow and achieves efficient recycling of lithium mica under near-neutral conditions.

Benefits of technology

It improves the concentrate grade and recovery rate of lithium mica, reduces the cost of ore dressing agents, improves the stability of flotation foam, reduces equipment corrosion and environmental pollution, and realizes clean and efficient recycling of lithium mica resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034950A_ABST
    Figure CN119034950A_ABST
Patent Text Reader

Abstract

The invention discloses a flotation combined reagent and application thereof in lepidolite flotation, and belongs to the technical field of mineral processing. According to the invention, the metal ions are used as the activating agent and are matched with the combined collecting agent prepared from the cationic amine collecting agent and the long-chain alkyl anion collecting agent in proportion for use, so that the selectivity and collecting capacity of the collecting agent are improved in the application of lepidolite flotation, and the problems of environmental pollution and equipment corrosion are avoided; the stability of flotation froth is improved, the reagent system and the technological process are simplified, and clean recovery and utilization of low-grade lepidolite ore resources are efficiently achieved under the nearly neutral condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a flotation combination reagent and an application thereof in lepidolite flotation. Background Art

[0002] As a key energy storage material, the application of lithium in high-energy batteries, atomic energy industry and new energy industry has increased significantly. In particular, the booming electric vehicle market has led to a rapid increase in demand for lithium resources.

[0003] Lepidolite is one of the mineral raw materials for lithium extraction. Most of the lepidolite resources mined in China are fine-grained and embedded, with low ore grade, many associated components and complex composition. In industry, amine flotation process is often used for separation and purification, and the recovery rate of lithium is low. Reagents are an important factor in achieving mineral flotation separation. Cationic collectors such as dodecylamine, coconut amine and mixed amines can float lepidolite, but there are problems such as poor solubility, high foam viscosity and difficulty in transporting products after sorting. At the same time, the amine flotation process needs to be carried out under acidic conditions, which is easy to corrode equipment and pollute the environment, restricting the high-value utilization of lepidolite.

[0004] Therefore, there is an urgent need for a flotation agent with strong adaptability, good selectivity and strong collection ability to achieve the separation and enrichment of lithium mica, and provide technical support for the green and efficient recovery of lithium mica resources. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a flotation combination reagent and its application in lepidolite flotation.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a flotation combination reagent, comprising a metal ion activator and an anion-cation combination collector; the anion-cation combination collector comprises a cationic amine collector and a long-chain hydrocarbon anion collector.

[0008] Preferably, the mass ratio of the metal ion activator, the cationic amine collector and the long-chain hydrocarbon anion collector is (1-8):(0.6-1.8):(1.2-4.8).

[0009] Preferably, the metal ion in the metal ion activator is Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+ , Mn 2+ , Fe 2+ , Fe 3+ and Al 3+ At least one of .

[0010] Preferably, the cationic amine collector includes at least one of a primary amine, a secondary amine, a tertiary amine and a quaternary amine;

[0011] The structural formula of the primary amine is R'-NH2 or R0'-N(CH2CH2O) n H2, the structural formula of secondary amine is R1'R2'-NH, the structural formula of tertiary amine is R3'R4'R5'-N, and the structural formula of quaternary amine is [R6'R7'R8'R9'N] + ·X - , wherein R', R0', R1', R2', R3', R4', R5', R6', R7', R8', R9' are independently selected from C 12 ~C 18 Straight-chain or branched hydrocarbon group, n=2.

[0012] Preferably, the cationic amine collector includes at least one of dodecylamine, dodecyltrimethylammonium chloride, dodecylamine polyoxyethylene ether, dodecyl tertiary amine, mixed amines, coconut amine and octadecylamine.

[0013] Preferably, the long-chain hydrocarbon anion collector comprises at least one of long-chain alkyl fatty acid salts, long-chain alkyl sulfates and long-chain alkyl sulfonates;

[0014] The structural formula of the long-chain alkyl fatty acid salt is R1-COO - ·Me + , the structural formula of long-chain alkyl sulfate is R2-OSO3 - ·Me + , the structural formula of long-chain alkyl sulfonate is R3-SO3 - ·Me + , wherein R1, R2, and R3 are independently selected from C 12 ~C 22 Straight or branched chain hydrocarbon group.

[0015] Preferably, the long-chain hydrocarbon anion collector includes at least one of sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium oleate, sodium dibutylnaphthalene sulfonate and oxidized paraffin soap.

[0016] The present invention also provides the application of the flotation combination reagent described in the above technical solution in the flotation of lepidolite.

[0017] Preferably, the application of the flotation combination reagent in the flotation of lithium mica includes the following steps: crushing, grinding and slurrying the lithium mica ore to obtain raw ore pulp; desludging the raw ore pulp, and then adding the flotation combination reagent described in the above technical solution to carry out flotation to obtain lithium concentrate and flotation tailings.

[0018] Preferably, the crushing is to crush the lithium mica ore to less than 2 mm;

[0019] The grinding is grinding to a fineness of -200 mesh, and the mass of the ore accounts for 50-70%;

[0020] The mass concentration of the raw ore slurry is 25-35%, and the pH value is 7.6-8.4;

[0021] The desludging method is screening desludging or sedimentation desludging;

[0022] The flotation comprises a roughing process or a roughing process, a cleaning process and a scavenging process.

[0023] Compared with the prior art, the present invention has the following advantages and technical effects:

[0024] (1) The present invention fundamentally improves the adsorption selectivity of collector organic matter to lithium mica in the complex and difficult-to-select mineral flotation system through the directional adsorption function and bridging effect of metal ions. The metal ion synergistic combination collector shows excellent selectivity and collection ability in the lithium mica flotation process, and reduces the dosage of the combination collector.

[0025] (2) The present invention enhances the reactivity of the combined collector by the synergistic effect produced by the association between the cationic amine collector and the long-chain hydrocarbon anion collector, thereby reducing the repulsive effect or thickness between the liquid films, and effectively improving the problem of over-stability of the flotation foam.

[0026] (3) The present invention utilizes and integrates the two enhanced separation technologies by using a combination of metal ion activators and anionic-cationic combined collectors, thereby avoiding the technical difficulties of poor selectivity, poor collection capacity, weak adaptability, and poor flotation foam controllability in the traditional acid-amine lithium mica flotation process, simplifying the reagent system and process flow, and efficiently realizing the clean recovery of low-grade lithium mica ore resources under near-neutral conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0028] Figure 1 The process flow chart of the application of the flotation combination reagent in the flotation of lepidolite in Examples 12-35 of the present invention;

[0029] Figure 2 This is a process flow chart for the application of the flotation combination reagent in lithium mica flotation in Example 36 of the present invention. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0032] The embodiment of the present invention provides a flotation combination reagent, comprising a metal ion activator and an anion-cation combination collector; the anion-cation combination collector comprises a cationic amine collector and a long-chain hydrocarbon anion collector.

[0033] The flotation combination reagent provided by the present invention, firstly, utilizes the directional adsorption function of metal ions, takes metal ions as a bridge, and strengthens the adsorption selectivity of the collector on the surface of lithium mica; secondly, utilizes the "synergistic effect" produced by the anion-cation combination collector, which is easy to realize the regulation of flotation foam, avoids the problem that the foam of the traditional amine flotation process is difficult to control, and reduces the corrosion of the equipment and environmental pollution during the mineral sorting process, and can also promote the separation effect of lithium mica and gangue minerals (such as quartz, feldspar, etc.). Compared with a single collector, the metal ion synergistic combination collector improves the Li2O grade and recovery rate of lithium concentrate, simplifies the process flow, reduces the cost of mineral processing reagents, improves the stability of flotation foam, and efficiently realizes the clean recovery and utilization of low-grade lithium ore resources under near-neutral conditions.

[0034] In a preferred embodiment, the mass ratio of the metal ion activator, the cationic amine collector and the long-chain hydrocarbon anion collector is (1-8): (0.6-1.8): (1.2-4.8). If no metal ion activator is added and only an anion-cation combination collector is used, the selectivity is poor and the concentrate grade is low; if a cationic amine collector is used alone, it is easy to cause a large amount of non-selective floating of minerals, and it is difficult to separate lithium mica from gangue minerals; when the amount of metal ion activator and anion collector is too high or too low, it will lead to a decrease in the recovery rate of Li2O in lithium concentrate.

[0035] In a preferred embodiment, the metal ion in the metal ion activator is Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+ , Mn 2 + , Fe 2+ , Fe 3+ and Al 3+The metal ion activator of the present invention exists in the form of metal ion hydroxy complex, metal ion surface precipitate and metal ion-organic multi-ligand complex generated with collector during the flotation process, which further strengthens the adsorption behavior of collector on the surface of lepidolite.

[0036] In a preferred embodiment, the cationic amine collector comprises at least one of a primary amine, a secondary amine, a tertiary amine and a quaternary amine; the structural formula of the primary amine is R'-NH2 or R0'-N(CH2CH2O) n H2, the structural formula of secondary amine is R1'R2'-NH, the structural formula of tertiary amine is R3'R4'R5'-N, and the structural formula of quaternary amine is [R6'R7'R8'R9'N] + ·X - , wherein R', R0', R1', R2', R3', R4', R5', R6', R7', R8', R9' are independently selected from C 12 ~C 18 Straight or branched hydrocarbon group, n = 2, X - Cl - The cationic amine collector in the present invention is mainly adsorbed on the surface of lepidolite by electrostatic force and hydrogen bond, making the mineral surface hydrophobic, thereby achieving flotation separation from gangue minerals (such as quartz and albite).

[0037] In a preferred embodiment, the cationic amine collector includes dodecylamine, dodecyltrimethylammonium chloride, dodecylamine polyoxyethylene ether (CH3-(CH2) 11 -N(CH2CH2O)2H2), at least one of dodecyl tertiary amine, mixed amine, coconut amine and octadecyl amine. In a preferred embodiment, the mixed amine is composed of primary amine, secondary amine and tertiary amine with a hydrocarbon chain length of 12.

[0038] In a preferred embodiment, the long-chain hydrocarbon anion collector comprises at least one of a long-chain alkyl fatty acid salt, a long-chain alkyl sulfate and a long-chain alkyl sulfonate; the structural formula of the long-chain alkyl fatty acid salt is R1-COO - ·Me + , the structural formula of long-chain alkyl sulfate is R2-OSO3 - ·Me + , the structural formula of long-chain alkyl sulfonate is R3-SO3 - ·Me + , wherein R1, R2, and R3 are independently selected from C 12 ~C 22 Straight or branched hydrocarbon group, Me + Represents Na +The long-chain hydrocarbon-based anion collector of the present invention can be adsorbed in a small amount on the weakly positively charged micro-region on the surface of lepidolite, and can interact with the mineral again using metal ions as a bridge, thereby strengthening the flotation recovery of lepidolite.

[0039] In a preferred embodiment, the long-chain hydrocarbon anion collector includes at least one of sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium oleate, sodium dibutylnaphthalene sulfonate and oxidized paraffin soap.

[0040] The present invention also provides the application of the flotation combination reagent described in the above technical solution in the flotation of lepidolite.

[0041] In a preferred embodiment, the application of the flotation combination reagent in the flotation of lithium mica includes the following steps: crushing, grinding and slurrying the lithium mica ore to obtain raw ore pulp; desliming the raw ore pulp, and then adding the flotation combination reagent described in the above technical solution to carry out flotation to obtain lithium concentrate and flotation tailings.

[0042] In a preferred embodiment, the crushing is to crush the lepidolite ore to less than 2 mm;

[0043] The grinding is grinding to a fineness of -200 mesh, and the mass of the ore accounts for 50-70%;

[0044] The mass concentration of the raw ore slurry is 25-35%, and the pH value is 7.6-8.4;

[0045] The desludging method is screening desludging or sedimentation desludging; the mesh number of the standard sieve used for the screening desludging is 600 meshes.

[0046] In a preferred embodiment, the flotation includes one roughing selection or one roughing selection, one cleaning selection and one scavenging selection; the flotation combination reagent is added during the roughing selection and scavenging selection process, and the amount of the metal ion activator in the flotation combination reagent is 100-800 g / t, the amount of the anion-cation combination collector is 150-660 g / t per ton of lithium mica ore, and the mass ratio of the cationic amine collector and the long-chain hydrocarbon anion collector in the anion-cation combination collector is (0.6-1.8):(1.2-4.8).

[0047] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0048] In the following examples, the metal ion Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+ , Mn 2+ , Fe 2+ , Fe 3+ 、Al 3+The metal ion sources are calcium chloride, magnesium chloride, lead nitrate, zinc sulfate, manganese chloride, ferrous chloride, ferric chloride, and aluminum sulfate;

[0049] Mixed amine and coconut amine were purchased from Kunming Liangfan Technology Co., Ltd.

[0050] Examples 1-5

[0051] A lithium mica mine in Jiangxi Province was selected. The ore is composed of lithium mica, iron lithium mica, quartz, albite and biotite, and the Li2O grade of the original ore is 0.21%.

[0052] The flotation reagent combination is composed of a cationic amine collector, dodecylamine, and a long-chain hydrocarbon anion collector in a mass ratio of 1.2:1.2; the long-chain hydrocarbon anion collectors used in Examples 1-5 are sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium dibutylnaphthalene sulfonate, oxidized paraffin soap, and sodium oleate, respectively.

[0053] The steps of applying the flotation combination reagent in the flotation of lepidolite are as follows:

[0054] (1) The lithium mica ore is crushed to less than 2 mm, and the crushed ore is ground in a ball mill for 3 minutes, with a grinding concentration of 67%, to obtain a slurry with a fineness of -200 mesh and a mass proportion of 57%, and then passed through a 20-mesh sieve, discarding the material on the sieve, and adding water to the material under the sieve to prepare the slurry to obtain a lithium mica slurry with a pH value of 7.6-7.8 and a mass concentration of 28%, and stirring for 1 minute; then, two sedimentation and desliming operations are carried out, with the sedimentation time being 5 minutes each, to obtain deslimed slurry and fine-grained slurry.

[0055] (2) The deslimed slurry obtained in step (1) was stirred for 2 minutes, and then 120 g / t of dodecylamine and 120 g / t of long-chain hydrocarbon anion collector were added per ton of lithium mica ore, and stirred for 4 minutes; then, aeration roughing was started, and the scraping time was 6 minutes. The lithium mica was scraped to the receiving basin along with the foam to become lithium concentrate, and the unfloated product in the flotation tank was tailings. After the lithium concentrate and tailings were filtered, dried and weighed, the lithium concentrate was taken for testing the Li2O grade, and the concentrate yield and Li2O recovery rate were calculated. The results are shown in Table 1.

[0056] Table 1 Effect of flotation reagent combination in Examples 1-5 on flotation index of lithium concentrate

[0057]

[0058] As shown in Table 1, when the long-chain hydrocarbon anion collector sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium oleate, sodium dibutylnaphthalene sulfonate or oxidized paraffin soap is combined with dodecylamine as a collector for flotation of lithium mica, the Li2O grade in the obtained lithium concentrate is higher than that of the original ore.

[0059] Embodiment 6-11

[0060] The same batch of lepidolite ore was used as in Example 1.

[0061] The flotation combination reagent is composed of a cationic amine collector and a long-chain hydrocarbon anion collector sodium dibutylnaphthalene sulfonate in a mass ratio of 1.2:1.2. The cationic amine collectors used in Examples 6-11 are dodecyltrimethylammonium chloride, dodecylamine polyoxyethylene ether, dodecyl tertiary amine, mixed amines, coconut amine, and octadecylamine, respectively.

[0062] The steps of applying the flotation combination reagent in the flotation of lepidolite are as follows:

[0063] Step (1) is the same as in Example 1.

[0064] (2) The deslimed slurry obtained in step (1) was stirred for 2 minutes, and then 120 g / t of a cationic collector and 120 g / t of a long-chain hydrocarbon anionic collector sodium dibutylnaphthalenesulfonate were added per ton of lithium mica ore, and stirred for 4 minutes; then, aeration roughing was started, and the foam scraping time was 6 minutes. The lithium mica was scraped to the receiving basin along with the foam to become lithium concentrate, and the unfloated product in the flotation tank was tailings. After the lithium concentrate and tailings were filtered, dried, and weighed, the lithium concentrate was taken for testing the Li2O grade, and the concentrate yield and Li2O recovery rate were calculated. The results are shown in Table 2.

[0065] Table 2 Effect of flotation reagent combination in Examples 6-11 on flotation index of lithium concentrate

[0066]

[0067]

[0068] As shown in Table 2, when the cationic amine collectors such as dodecyltrimethylammonium chloride, dodecylamine polyoxyethylene ether, dodecyl tertiary amine, mixed amines, coconut amine or octadecylamine are combined with sodium dibutylnaphthalene sulfonate as collectors for flotation of lithium mica, the Li2O grade in the lithium concentrate is higher than that of the original ore.

[0069] Examples 12-19

[0070] A lithium mica mine in Hebei Province was selected. The ore is mainly composed of lithium mica, albite, potassium feldspar, quartz, biotite, chabazite and other minerals. The Li2O grade of the original ore is 0.185%.

[0071] The flotation reagent combination is composed of dodecylamine, sodium dibutylnaphthalene sulfonate and a metal ion activator in a mass ratio of 1.2:1.8:2; the metal ions in the metal ion activator used in Examples 12-19 are Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+, Mn 2 + , Fe 2+ , Fe 3+ 、Al 3+ .

[0072] The steps of applying the flotation reagent combination in the flotation of lithium mica are as follows. The process flow is shown in Figure 1 :

[0073] (1) The lithium mica ore is crushed to less than 1 mm, and the crushed ore is ground in a rod mill for 90 seconds, with a grinding concentration of 50%, to obtain a slurry in which the ore mass of the ore with a fineness of -200 mesh accounts for 60%; water is added to adjust the slurry to obtain a lithium mica slurry with a pH value of 8.0-8.4 and a mass concentration of 28%, and stirred for 1 minute; then a 600-mesh standard sieve is used for screening and desliming to obtain a deslimed slurry and fine-grained slurry.

[0074] (2) The deslimed slurry obtained in step (1) was stirred for 2 min, and then 200 g / t of metal ion activator was added per ton of lithium mica ore, and stirred for 3 min, and then 120 g / t of dodecylamine and 180 g / t of sodium dibutylnaphthalene sulfonate were added, and stirred for 3 min; then, aeration roughing was started, and the scraping time was 6 min. The lithium mica was scraped to the receiving basin with the foam to become lithium concentrate, and the unfloated product in the flotation tank was tailings. After the lithium concentrate and tailings were filtered, dried and weighed, the lithium concentrate was taken for testing the Li2O grade, and the concentrate yield and Li2O recovery rate were calculated. The results are shown in Table 3.

[0075] Table 3 Effect of flotation reagent combination in Examples 12-19 on flotation index of lithium concentrate

[0076] Metal ions Concentrate yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Example 12 <![CDATA[Ca 2+ ]]> 10.45 1.39 78.50 Embodiment 13 <![CDATA[Mg 2+ ]]> 9.61 1.50 77.92 Embodiment 14 <![CDATA[Pb 2+ ]]> 11.52 1.27 79.08 Embodiment 15 <![CDATA[Zn 2+ ]]> 11.38 1.29 79.35 Example 16 <![CDATA[Mn 2+ ]]> 9.90 1.61 86.13 Embodiment 17 <![CDATA[Fe 2+ ]]> 10.81 1.18 68.96 Embodiment 18 <![CDATA[Fe 3+ ]]> 8.15 1.82 80.18 Embodiment 19 <![CDATA[Al 3+ ]]> 9.82 1.71 90.74

[0077] It can be seen from Table 3 that the use of metal ions Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+ , Mn 2+ , Fe 2+ , Fe 3+ 、Al 3+ The metal ion activator is combined with dodecylamine and sodium dibutylnaphthalene sulfonate to form a flotation combination reagent, which is used for the flotation of lithium mica ore and improves the Li2O grade of lithium concentrate.

[0078] Examples 20-26

[0079] The same batch of lithium mica ore was used as in Example 12.

[0080] The flotation reagent combination is composed of a metal ion activator, dodecylamine and sodium dibutylnaphthalene sulfonate in a mass ratio of 1:1.2:1.8, 3:1.2:1.8, 4:1.2:1.8, 5:1.2:1.8, 6:1.2:1.8, 7:1.2:1.8 and 8:1.2:1.8, respectively. The metal ion in the metal ion activator is Fe 3+ .

[0081] The steps of applying the flotation reagent combination in the flotation of lithium mica are as follows. The process flow is shown in Figure 1 :

[0082] Step (1) is the same as in Example 12.

[0083] (2) The deslimed slurry obtained in step (1) was stirred for 2 min, and then different amounts of metal ion activator (Fe 3+ The dosage is 100g / t, 300g / t, 400g / t, 500g / t, 600g / t, 700g / t, 800g / t respectively), and stirred for 3min; then 120g / t of dodecylamine and 180g / t of sodium dibutylnaphthalenesulfonate are added, and stirred for 3min; then aeration roughing is started, and the scraping time is 6min. The lithium mica is scraped out with the foam to become lithium concentrate, and the unfloated product in the flotation tank is the tailings. After the lithium concentrate and tailings are filtered, dried and weighed, the lithium concentrate is sampled for testing the Li2O grade, and the concentrate yield and Li2O recovery rate are calculated. The results are shown in Table 4.

[0084] Table 4 Effect of flotation reagent combination in Examples 18, 20-26 on flotation index of lithium concentrate

[0085]

[0086] It can be seen from Table 4 that when the dosage of the metal ion activator is 100-800 g / t, the Li2O grade and recovery rate in the lithium concentrate are both high, and an appropriate amount of metal ion activator realizes the flotation recovery of lithium mica.

[0087] Examples 27-31

[0088] The same batch of lithium mica ore was used as in Example 12.

[0089] The flotation reagent combination is composed of a metal ion activator, dodecylamine and sodium dibutylnaphthalene sulfonate in a mass ratio of 5:1.2:1.2, 5:1.2:2.4, 5:1.2:3, 5:1.2:3.6 and 5:1.2:4.8, respectively. The metal ion in the metal ion activator is Fe 3+ .

[0090] The steps of applying the flotation reagent combination in the flotation of lithium mica are as follows. The process flow is shown in Figure 1 :

[0091] Step (1) is the same as in Example 12.

[0092] (2) The deslimed slurry obtained in step (1) was stirred for 2 min, and 500 g / t of metal ion activator was added per ton of lithium mica ore, and stirred for 3 min; then 120 g / t of dodecylamine and sodium dibutylnaphthalene sulfonate (in amounts of 120 g / t, 240 g / t, 300 g / t, 360 g / t and 480 g / t, respectively) were added and stirred for 3 min; then aeration flotation was started, and the foam scraping time was 6 min. The lithium mica was scraped out with the foam to become lithium concentrate, and the unfloated product in the flotation tank was tailings. After the lithium concentrate and tailings were filtered, dried and weighed, the lithium concentrate was sampled for testing the Li2O grade, and the concentrate yield and Li2O recovery rate were calculated. The results are shown in Table 5.

[0093] Table 5 Effect of flotation reagent combination in Examples 23, 27-31 on flotation index of lithium concentrate

[0094]

[0095] From Table 5, we know that Fe 3+ As a metal ion activator, when the dosage of sodium dibutylnaphthalene sulfonate in the anion-cation combined collector is 120-480 g / t, the lithium concentrate obtains a higher Li2O grade, but too high or too low anion collector dosage will lead to a decrease in the Li2O recovery rate of the concentrate.

[0096] Examples 32-35

[0097] The same batch of lithium mica ore was used as in Example 12.

[0098] The flotation reagent combination is composed of a metal ion activator, dodecylamine and sodium dibutylnaphthalene sulfonate in a mass ratio of 5:0.6:1.8, 5:0.9:1.8, 5:1.5:1.8 and 5:1.8:1.8, respectively. The metal ion in the metal ion activator is Fe 3 + .

[0099] The steps of applying the flotation reagent combination in the flotation of lithium mica are as follows. The process flow is shown in Figure 1 :

[0100] (1) This step is the same as step (1) of Example 3.

[0101] Step (1) is the same as in Example 12.

[0102] (2) The deslimed slurry obtained in step (1) was stirred for 2 min, and 500 g / t of metal ion activator was added per ton of lithium mica ore, and stirred for 3 min; then dodecylamine (in amounts of 60 g / t, 90 g / t, 150 g / t and 180 g / t, respectively) and 180 g / t of sodium dibutylnaphthalene sulfonate were added, and stirred for 3 min; then aeration flotation was started, and the foam scraping time was 6 min. The lithium mica was scraped out with the foam to become lithium concentrate, and the unfloated product in the flotation tank was tailings. After the lithium concentrate and tailings were filtered, dried and weighed, the lithium concentrate was sampled for testing the Li2O grade, and the concentrate yield and Li2O recovery rate were calculated. The results are shown in Table 6.

[0103] Table 6 Effect of flotation reagent combination in Examples 23, 32-35 on flotation index of lithium concentrate

[0104]

[0105]

[0106] It can be seen from Table 6 that Fe 3+ As a metal ion activator, when the dosage of dodecylamine in the anion-cation combined collector is 60-180 g / t, a higher Li2O recovery rate is obtained in the lithium concentrate, but an excessive amount of cationic collector will cause a significant decrease in the Li2O grade in the concentrate.

[0107] Embodiment 36

[0108] The same batch of lithium mica ore was used as in Example 12.

[0109] The flotation reagent combination is composed of a metal ion activator, dodecylamine and sodium dibutylnaphthalene sulfonate in a mass ratio of 5:1.2:1.8. The metal ion in the metal ion activator is Fe 3+ .

[0110] The steps of applying the flotation reagent combination in the flotation of lithium mica are as follows. The process flow is shown in Figure 2 :

[0111] (1) The lithium mica ore is crushed to less than 1 mm, and three groups of crushed ore materials are respectively ground in a rod mill for 90 seconds, with a grinding concentration of 50%, to obtain a slurry in which the mass of the ore material with a fineness of -200 mesh accounts for 60%; after adding water to adjust the slurry, the three groups of materials are combined into one group to obtain a lithium mica raw ore slurry with a pH value of 8.0-8.4 and a mass concentration of 28%, which is stirred for 1 minute; then, a 600-mesh standard sieve is used for screening and desliming to obtain flotation slurry and fine mud.

[0112] (2) The deslimed slurry obtained in step (1) is stirred for 2 minutes, and 500 g / t of metal ion activator is added per ton of lithium mica ore, and stirred for 3 minutes; then 120 g / t of dodecylamine and 180 g / t of sodium dibutylnaphthalene sulfonate are added, and stirred for 3 minutes; then aeration is started for roughing, and the scraping time is 6 minutes to obtain a roughing concentrate and a roughing tailing.

[0113] (3) After stirring the roughing concentrate obtained in step (2) for 2 minutes, aeration is started for concentration, and no reagent is added during the concentration stage. The scraping time is 6 minutes to obtain lepidolite concentrate and concentrated tailings.

[0114] (4) stirring the roughing tailings obtained in step (2) for 2 minutes, adding 250 g / t of metal ion activator per ton of lithium mica ore, and stirring for 3 minutes; then adding 60 g / t of dodecylamine and 90 g / t of sodium dibutylnaphthalene sulfonate, and stirring for 3 minutes; then starting to aerate for scavenging, the scraping time is 6 minutes, and obtaining scavenging concentrate and flotation tailings.

[0115] (5) The selected tailings in step (3) and the scavenged concentrate in step (4) are combined into a middling ore. After the lithium mica concentrate and the middling ore are filtered, dried and weighed, the mica concentrate and the middling ore are sampled and tested for Li2O grade, and the concentrate yield and Li2O recovery rate are calculated. The results are shown in Table 7.

[0116] Table 7 Sorting index of lithium mica activated flotation process in Example 36

[0117] Flotation products Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Fine mud 15.85 0.09 7.71 Lepidolite Concentrate 5.93 2.68 85.85 Zhongkuang 5.13 0.133 2.34 Flotation tailings 73.10 0.007 2.78 Ore 100.0 0.185 100.0

[0118] It can be seen from Table 7 that under natural pH conditions, after the “one coarse, one fine, one sweep” lithium mica activation flotation process, the lithium mica concentrate has a high Li2O grade and a low Li loss rate in the tailings, which can achieve green and efficient recovery of lithium mica resources.

[0119] Comparative Example 1

[0120] The only difference from Example 1 is that only the cationic collector dodecylamine is used as the collector, and no long-chain hydrocarbon anionic collector is added.

[0121] The flotation indexes of the products in Comparative Example 1 are shown in Table 8.

[0122] Table 8 Sorting index of flotation lithium mica in comparative example 1

[0123] Flotation products Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Fine-grained mud 21.69 0.10 10.64 Lithium Concentrate 16.30 0.70 54.19 Tailings 62.01 0.12 35.18 Ore 100.0 0.21 100.0

[0124] As shown in Table 8, in Comparative Example 1, a single cationic collector, dodecylamine, was used to float lithium mica. The mineral floated non-selectively, the obtained lithium concentrate Li2O had a low grade, and the lithium mica flotation recovery was difficult.

[0125] Comparative Example 2

[0126] The only difference from Example 12 is that no metal ion activator is added.

[0127] The flotation indexes of the products in Comparative Example 2 are shown in Table 9.

[0128] Table 9 Sorting index of flotation lithium mica in comparative example 2

[0129] Flotation products Yield (%) <![CDATA[Li2O grade (%)]]> <![CDATA[Recovery rate of Li2O (%)]]> Fine-grained mud 14.81 0.09 7.20 Lithium Concentrate 18.64 0.80 80.61 Tailings 66.55 0.03 12.19 Ore 100.0 0.185 100.0

[0130] It can be seen from Table 9 that in Comparative Example 2, when no metal ion activator was added and dodecylamine and sodium dibutylnaphthalenesulfonate were used as combined collectors to float lithium mica, the Li2O grade in the obtained lithium concentrate was low.

[0131] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A flotation combination reagent, characterized in that: It comprises a metal ion activator and an anion-cation combination collector; the anion-cation combination collector comprises a cationic amine collector and a long-chain hydrocarbon anion collector.

2. The flotation reagent combination according to claim 1, characterized in that: The mass ratio of the metal ion activator, the cationic amine collector and the long-chain hydrocarbon anion collector is (1-8):(0.6-1.8):(1.2-4.8).

3. The flotation combination reagent according to claim 1, characterized in that: The metal ion in the metal ion activator is Ca 2+ Mg 2+ , Pb 2+ 、Zn 2+ , Mn 2+ , Fe 2+ , Fe 3+ and Al 3+ At least one of .

4. The flotation combination reagent according to claim 1, characterized in that: The cationic amine collector includes at least one of a primary amine, a secondary amine, a tertiary amine and a quaternary amine; The structural formula of the primary amine is R'-NH2 or R0'-N(CH2CH2O) n H2, the structural formula of secondary amine is R1'R2'-NH, the structural formula of tertiary amine is R3'R4'R5'-N, and the structural formula of quaternary amine is [R6'R7'R8'R9'N] + ·X - , wherein R', R0', R1', R2', R3', R4', R5', R6', R7', R8', R9' are independently selected from C 12 ~C 18 Straight-chain or branched hydrocarbon group, n=2.

5. The flotation combination reagent according to claim 4, characterized in that: The cationic amine collector includes at least one of dodecylamine, dodecyltrimethylammonium chloride, dodecylamine polyoxyethylene ether, dodecyl tertiary amine, mixed amines, coconut oil amine and octadecylamine.

6. The flotation reagent combination according to claim 1, characterized in that: The long-chain hydrocarbon anion collector includes at least one of a long-chain alkyl fatty acid salt, a long-chain alkyl sulfate and a long-chain alkyl sulfonate; The structural formula of the long-chain alkyl fatty acid salt is R1-COO - ·Me + , the structural formula of long-chain alkyl sulfate is R2-OSO3 - ·Me + , the structural formula of long-chain alkyl sulfonate is R3-SO3 - ·Me + , wherein R1, R2, and R3 are independently selected from C 12 ~C 22 Straight or branched chain hydrocarbon group.

7. The flotation combination reagent according to claim 6, characterized in that: The long-chain hydrocarbon anion collector includes at least one of sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium oleate, sodium dibutylnaphthalene sulfonate and oxidized paraffin soap.

8. Use of the flotation combination reagent as claimed in any one of claims 1 to 7 in the flotation of lepidolite.

9. The use according to claim 8, characterized in that: The following steps are involved: The lepidolite ore is crushed, ground and slurried to obtain raw ore pulp; the raw ore pulp is deslimed, and then the flotation combination reagent according to any one of claims 1 to 7 is added for flotation to obtain lithium concentrate and flotation tailings.

10. The use according to claim 9, characterized in that: The crushing is to crush the lithium mica ore to less than 2 mm; The grinding is grinding to a fineness of -200 mesh, and the mass of the ore accounts for 50-70%; The mass concentration of the raw ore slurry is 25-35%, and the pH value is 7.6-8.4; The desludging method is screening desludging or sedimentation desludging; The flotation comprises a roughing process or a roughing process, a cleaning process and a scavenging process.

Citation Information

Patent Citations

  • Combined collecting agent, preparation method of combined collecting agent and application of combined collecting agent in lepidolite flotation

    CN117101876A

  • Composite flotation reagent and application thereof in lepidolite flotation

    CN117282545A

  • Composite flotation reagent for fluorite type lepidolite ore and application of composite flotation reagent

    CN117324125A

  • Method for promoting whole-fraction flotation separation of lepidolite and feldspar through surface pretreatment

    CN118179758A

  • Preparation method of lepidolite collecting agent

    CN118477760A

Cited By

  • Ion regulation inhibitor for preventing slime from covering, application and lepidolite ore beneficiation method

    CN119565767A

  • Combined collecting agent for direct flotation of lepidolite and application of combined collecting agent

    CN119634051A

  • Lepidolite positive flotation combined collector and application thereof