Display medium, its manufacturing method, and display article
The display medium with a highly regular arrangement of small piece layers and controlled light polarization properties enhances security against counterfeiting while enabling diverse display modes.
Patent Information
- Application Number
- JP2022503372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-28
- Filing Date
- 2021-02-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Display media utilizing polarized light are difficult to counterfeit, and there is a need to enhance their security against counterfeiting.
A display medium is designed with a base material and a display layer comprising small piece layers arranged with high regularity, featuring specific in-plane retardation, shape, and orientation, which can reflect and transmit circularly polarized light in controlled directions, and may include a selective reflection layer for enhanced security.
The display medium is more difficult to counterfeit due to its high regularity of arrangement and controlled light polarization properties, allowing for various display modes and improved security features.
Smart Images

Figure 0007567900000008 
Figure 0007567900000009 
Figure 0007567900000010
Abstract
Description
[Technical field]
[0001] The present invention relates to a display medium, a manufacturing method thereof, and a display article including the display medium. [Background technology]
[0002] From the viewpoint of diversifying the display modes of articles, display modes using polarized light are sometimes adopted. In order to realize such display modes using polarized light, liquid crystal materials have been used in the past. Liquid crystal materials have also been used for identifying authenticity. Examples of such techniques include the techniques described in Patent Documents 1 to 3. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-105327 A [Patent Document 2] JP 2014-174471 A [Patent Document 3] Patent No. 4630465 Summary of the Invention [Problem to be solved by the invention]
[0004] Display media that utilize polarized light are generally difficult to counterfeit, but there is a demand for further enhancements in the difficulty of counterfeiting. The present invention has been devised in view of the above-mentioned problems, and aims to provide a display medium and a manufacturing method thereof that are more difficult to counterfeit, and a display article equipped with the display medium. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be solved by providing a highly regularly arranged fragment layer in a display layer, thereby completing the present invention. That is, the present invention includes the following.
[0006] [1] A display device comprising a substrate and a display layer provided on the substrate, the display layer includes a plurality of flake layers separated by cracks; A display medium, wherein the plurality of small fragment layers are arranged side by side in two or more directions when viewed in the thickness direction. [2] The display medium according to [1], wherein the flake layer has a thickness of 10 μm or less. [3] The display medium according to [1] or [2], wherein the flake layer is formed of a cured liquid crystal composition. [4] The display medium according to any one of [1] to [3], wherein the in-plane retardation of the fragment layer at a measurement wavelength of 550 nm is greater than or equal to "{(2n1+1) / 4}×550 nm-30 nm" and less than or equal to "{(2n1+1) / 4}×550 nm+30 nm" (wherein n1 represents an integer greater than or equal to 0). [5] The display medium described in any one of [1] to [3], wherein the in-plane retardation of the fragment layer at a measurement wavelength of 550 nm is equal to or greater than "{(2n2+1) / 2}×550 nm-30 nm" and equal to or less than "{(2n2+1) / 2}×550 nm+30 nm" (wherein n2 represents an integer of 0 or greater). [6] The display medium described in any one of [1] to [5], wherein the small flake layer is one or more types selected from the group consisting of a positive A plate, a positive C plate, a tilted O plate, and a tilted hybrid alignment plate. [7] The small piece layer is rotated in one direction D D The display medium according to any one of [1] to [3], having a display wavelength range capable of reflecting circularly polarized light having a rotation direction of one and transmitting circularly polarized light having an opposite rotation direction. [8] The substrate is rotated in one direction D S The display medium according to any one of [1] to [7], further comprising a selective reflection layer having a substrate reflection range that can reflect circularly polarized light in a direction of rotation and transmit circularly polarized light in the opposite direction. [9] The substrate is rotated in one direction D Sa selective reflection layer having a substrate reflection range capable of reflecting circularly polarized light having a rotation direction of 1 and transmitting circularly polarized light having an opposite rotation direction; The display medium according to [7], wherein the wavelength width of the substrate reflection range is wider than the wavelength width of the display wavelength range.
[10] The display medium according to [8] or [9], wherein the wavelength width of the substrate reflection range is 70 nm or more.
[11] The display medium according to any one of [1] to
[10] , comprising a plurality of the display layers.
[12] The display medium according to any one of [1] to
[11] , wherein the shape of the small fragment layer when viewed in the thickness direction is rectangular.
[13] The display medium according to any one of [1] to
[12] , wherein the flake layer has a width of 100 μm or less as viewed in the thickness direction.
[14] The display medium according to any one of [1] to
[13] , wherein the substrate has a colored layer.
[15] The display medium according to any one of [1] to
[14] , further comprising an adhesive layer between the substrate and the display layer.
[16] A method for producing the display medium according to any one of [1] to
[15] , A step of preparing a web member including a temporary support and a transfer material layer formed on the temporary support and including the small particle layer; forming an adhesive layer on the substrate, the adhesive layer having the same shape as the display layer when viewed in a thickness direction; a step of bonding the transfer material layer and the adhesive layer; A step of peeling off the temporary support; A method for manufacturing a display medium, comprising:
[17] A display article comprising a base article and the display medium according to any one of [1] to
[15] provided on the base article. Effect of the Invention
[0007] According to the present invention, it is possible to provide a display medium and a manufacturing method thereof that are more difficult to counterfeit; and a display article equipped with the display medium. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic plan view of a display medium according to a first embodiment of the present invention, as viewed from the thickness direction. [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a cross section of the display medium according to the first embodiment of the invention, taken along the II-II plane shown in FIG. [Diagram 3] FIG. 3 is an enlarged plan view that illustrates a schematic enlargement of a portion III shown in FIG. 1 of the display medium according to the first embodiment of the present invention. [Figure 4] FIG. 4 is a cross-sectional view that typically shows a cross section of the display medium according to the first embodiment of the invention taken along the IV-IV plane shown in FIG. [Diagram 5] FIG. 5 is a schematic plan view, seen from the thickness direction, of a web member prepared in the display medium manufacturing method according to the first embodiment of the present invention. [Figure 6] FIG. 6 is a cross-sectional view that typically shows a cross section of an original web member prepared in the display medium manufacturing method according to the first embodiment of the invention, cut along the VI-VI plane shown in FIG. [Figure 7] FIG. 7 is an enlarged plan view that shows a schematic enlargement of a portion VII shown in FIG. 5 of a raw material member prepared in the manufacturing method for a display medium according to the first embodiment of the present invention. [Figure 8] FIG. 8 is a cross-sectional view that typically shows a cross section of a raw material member prepared in the display medium manufacturing method according to the first embodiment of the invention, cut along the VIII-VIII plane shown in FIG. [Figure 9] FIG. 9 is a perspective view that illustrates an example of a processing tool that can be used in the method for producing a web member in the method for producing a display medium according to the first embodiment of the present invention. [Figure 10] FIG. 10 is a perspective view that typically shows the processing tool shown in FIG. [Figure 11] FIG. 11 is a plan view showing a schematic development of the processing tool shown in FIG. 10 after cutting it along line XI-XI. [Figure 12] FIG. 12 is a partial cross-sectional view that shows a schematic cross section of a part in the vicinity of the surface of the processing tool, cut along a plane perpendicular to the direction in which the protrusions extend. [Figure 13] FIG. 13 is a perspective view that illustrates an example of a processing tool that can be used in the method for producing a web member in the method for producing a display medium according to the first embodiment of the present invention. [Figure 14] FIG. 14 is a perspective view diagrammatically showing the processing tool shown in FIG. [Figure 15] FIG. 15 is a plan view showing a schematic development of the processing tool shown in FIG. 14 after cutting it along line XV-XV. [Figure 16] FIG. 16 is a schematic plan view of a display medium according to the second embodiment of the invention, as viewed from the thickness direction. [Figure 17] FIG. 17 is a cross-sectional view that typically shows a cross section of a display medium according to a second embodiment of the invention, taken along the XVII-XVII plane shown in FIG. [Figure 18] FIG. 18 is an enlarged plan view illustrating a schematic enlargement of a portion XVIII shown in FIG. 16 of a display medium according to a second embodiment of the invention. [Figure 19] FIG. 19 is a schematic plan view of a display medium according to a third embodiment of the invention, as viewed from the thickness direction. [Figure 20] FIG. 20 is a cross-sectional view that typically shows a cross section of a display medium according to a third embodiment of the invention, taken along the XX-XX plane shown in FIG. [Figure 21] FIG. 21 is an enlarged plan view that illustrates a schematic enlargement of a portion XXI shown in FIG. 19 of a display medium according to a third embodiment of the invention. [Figure 22] FIG. 22 is a plan view diagrammatically illustrating the display medium produced in Example 101. As shown in FIG. [Figure 23] FIG. 23 is a cross-sectional view illustrating the display medium produced in Example 101. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples described below, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0010] In the following description, unless otherwise specified, the in-plane direction refers to a direction perpendicular to the thickness direction.
[0011] In the following description, the in-plane retardation Re of a layer is a value expressed by Re=(nx-ny)×d, unless otherwise specified. Here, nx represents the refractive index in a direction perpendicular to the thickness direction of the layer (in-plane direction) that gives the maximum refractive index. ny represents the refractive index in the in-plane direction perpendicular to the direction of nx. nz represents the refractive index in the thickness direction. d represents the thickness of the layer. The measurement wavelength is 550 nm, unless otherwise specified.
[0012] In the following description, "circularly polarized light" also includes elliptically polarized light as long as the effects of the present invention are not significantly impaired.
[0013] In the following description, unless otherwise specified, the directions of elements as "parallel," "vertical," and "orthogonal" may include an error within a range that does not impair the effects of the present invention, for example, within a range of ±4°, preferably ±3°, and more preferably ±1°.
[0014] In the following description, the "visible wavelength range" refers to the wavelength range of 400 nm or more and 780 nm or less, unless otherwise specified.
[0015] In the following description, "long" refers to a shape having a length 5 times or more than the width, preferably 10 times or more, specifically a film shape having a length long enough to be wound into a roll for storage or transportation. There is no particular upper limit to the length, and it can be, for example, 100,000 times or less than the width.
[0016] [1. Display medium according to the first embodiment] Fig. 1 is a schematic plan view of a display medium 10 according to a first embodiment of the present invention, as viewed from the thickness direction. Fig. 2 is a schematic cross-sectional view of the display medium 10 according to the first embodiment of the present invention, taken along the II-II plane shown in Fig. 1. As shown in FIGS. 1 and 2, a display medium 10 according to a first embodiment of the present invention includes a substrate 100 and a display layer 200 provided on the substrate 100. The display medium 100 includes a substrate 100 and a display layer 200 disposed on the substrate 100.
[0017] [1.1. Base material 100] The substrate 100 is a member capable of supporting the display layer 200, and typically includes a support layer 110. There are no particular limitations on the material from which the support layer can be formed, and organic materials, inorganic materials, and composite materials combining these materials can be used. Specific examples of materials for the support layer include resin, paper, cloth, leather, metal, alloy, glass, and the like. Among these, resin is preferred because the display medium 10 can be easily manufactured and has excellent flexibility.
[0018] As the resin, a thermoplastic resin is usually used. This thermoplastic resin may contain a polymer and, if necessary, any component. Examples of the polymer include polycarbonate, polyethersulfone, polyethylene terephthalate, polyimide, polymethyl methacrylate, polysulfone, polyarylate, polyethylene, polyphenylene ether, polystyrene, polyvinyl chloride, cellulose diacetate, cellulose triacetate, and alicyclic structure-containing polymers. In addition, the polymer may be used alone or in combination of two or more types at any ratio. Among them, from the viewpoints of transparency, low moisture absorption, dimensional stability, and processability, alicyclic structure-containing polymers are suitable. The alicyclic structure-containing polymer is a polymer having an alicyclic structure in the main chain and / or side chain, and for example, those described in JP-A-2007-057971 can be used.
[0019] There is no limitation on the in-plane retardation of the support layer 110. In this embodiment, an example using an optically isotropic support layer 110 with small in-plane retardation will be described. The in-plane retardation of this optically isotropic support layer 110 at a measurement wavelength of 550 nm may be preferably 0 to 20 nm, more preferably 0 to 10 nm, and particularly preferably 0 to 5 nm.
[0020] The substrate 100 may be a transparent material that transmits light, or may be a non-transparent material that does not transmit light. In this embodiment, a transparent substrate 100 that can transmit light will be described as an example.
[0021] The shape of the substrate 100 is not limited. The substrate 100 may be in the form of a plate, a sheet, a film, or the like. Among them, a film-shaped substrate 100 is preferable from the viewpoint of making the display medium 10 thin. In particular, when a long film is used as the substrate 100, the display medium 10 can be efficiently manufactured using a roll-to-roll method.
[0022] The thickness of the substrate 100 is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, particularly preferably 20 μm or more, and is preferably 1 mm or less, more preferably 500 μm or less, particularly preferably 200 μm or less.
[0023] [1.2. Display layer 200] The display layer 200 is provided directly or indirectly on the substrate 100. The display layer 200 being provided "directly" on the substrate 100 means that there is no other layer between the substrate 100 and the display layer 200. Moreover, the display layer 200 being provided "indirectly" on the substrate 100 means that there is another layer between the substrate 100 and the display layer 200.
[0024] The display layer 200 may be provided on the entire surface 100U of the substrate 100, but is usually provided on a part of the surface 100U of the substrate 100. For example, the display layer 200 may be provided in an area of the surface 100U that has a specific shape when viewed from the thickness direction. In this case, the display layer 200 can have a specific shape when viewed from the thickness direction. Therefore, an observer who observes the display medium 10 can visually recognize the shape. Also, for example, the display layer 200 may be provided in an area other than the area of the surface 100U having a specific shape when viewed from the thickness direction. In this case, the area where the display layer 200 is not provided can have a specific shape when viewed from the thickness direction. Therefore, an observer who observes the display medium 10 can visually recognize the shape. Therefore, in either case, the design of the display medium 10 can be improved.
[0025] Examples of the specific shape include letters, numbers, symbols, pictures, etc. However, the specific shape is not limited to the above examples. In this embodiment, as shown in FIG. 1, an example in which a display layer 200 having a shape of the letter "T" when viewed from the thickness direction is provided will be described.
[0026] Fig. 3 is an enlarged plan view showing a schematic enlargement of a portion III of the display medium 10 according to the first embodiment of the present invention shown in Fig. 1. Fig. 4 is a cross-sectional view showing a schematic cross-section of the display medium 10 according to the first embodiment of the present invention taken along the IV-IV plane shown in Fig. 3. 3 and 4, the display layer 200 includes a plurality of small piece layers 220 separated by cracks 210. In detail, each small piece layer 220 is provided at a different position on the surface 100U of the substrate 100, and the small piece layers 220 are separated from each other by cracks 210 formed throughout the entire thickness of the display layer 200. A group of the plurality of small piece layers 220 forms one display layer 200.
[0027] The small piece layers 220 included in one display layer 200 are arranged in two or more directions when viewed from the thickness direction. In the following description, the direction in which the small piece layers 220 are arranged in this way may be referred to as the "arrangement direction". All of these arrangement directions are perpendicular to the thickness direction, and therefore may be parallel to the layer plane of the display layer. Therefore, usually, when a line segment is drawn connecting the adjacent small piece layers 220 across the crack 210, the line segment is parallel to one of the two or more arrangement directions. The number of arrangement directions is usually two or more, preferably four or less, and more preferably three or less. For example, when the shape of the small piece layer 220 viewed from the thickness direction is an equilateral triangle, the number of arrangement directions of the small piece layers 220 included in one display layer 200 may be three. Also, for example, when the shape of the small piece layer 220 viewed from the thickness direction is a rectangle, the number of arrangement directions of the small piece layers 220 included in one display layer 200 may be two. Furthermore, for example, when the shape of the small piece layer 220 viewed from the thickness direction is a regular hexagon, the number of small piece layers 220 included in one display layer 200 in the arrangement direction can be three.
[0028] Conventionally, it has been difficult to form a display layer as a collection of small layers arranged with high regularity. For example, when a display layer is formed by applying paint containing a pigment corresponding to the small layer to a substrate, the pigment contained in the resulting display layer is arranged randomly, and high regularity cannot be achieved. The display layer 200 of the display medium 10 according to this embodiment is formed by small piece layers 220 arranged with high regularity in two or more directions, so that it is difficult to manufacture using conventional techniques. Therefore, it is possible to increase the difficulty of counterfeiting the display medium 10.
[0029] The angle between the arrangement directions of the small fragment layers 220 included in one display layer 200 is usually 5° or more, more preferably 10° or more, even more preferably 30° or more, particularly preferably 40° or more, and is usually 90° or less. In this embodiment, an example will be described in which the small fragment layers 220 included in the display layer 200 are arranged side by side in a first arrangement direction X perpendicular to the thickness direction and a second arrangement direction Y perpendicular to both the thickness direction and the arrangement direction X, as shown in Fig. 3.
[0030] It is preferable that each small piece layer 220 included in one display layer 200 has the same shape when viewed in the thickness direction. Since forming the display layer 200 from a group of small piece layers 220 having the same shape is particularly difficult in manufacturing, it can effectively increase the difficulty of counterfeiting the display medium 10.
[0031] The shape of each small piece layer 220 as viewed in the thickness direction is not particularly limited. Preferred examples include polygons such as triangles, squares, and hexagons. Among them, equilateral triangles, squares, and regular hexagons are preferred, squares are more preferred, parallelograms are even more preferred, rectangular shapes such as squares and rectangles are even more preferred, and squares are particularly preferred.
[0032] The width of each small piece layer 220 as viewed in the thickness direction is preferably within a specific range. Specifically, the width of the small piece layer 220 is preferably 150 μm or less, more preferably 125 μm or less, even more preferably 100 μm or less, and particularly preferably 80 μm or less. There is no particular lower limit, and the width is usually greater than 0 μm, and preferably 10 μm or more. The width of the small piece layer 220 refers to the longest distance among the distances between multiple parallel lines drawn to be tangent to the outline of the small piece layer 220. Since such small small piece layers 220 are difficult to see with the naked eye, the difficulty of counterfeiting the display medium 10 can be effectively increased.
[0033] Since the small piece layers 220 are arranged in two or more arrangement directions, the cracks 210 that divide the small piece layers 220 usually include indentations 211 and 212 that extend in two or more directions. When viewed from the thickness direction, the cracks 210 preferably include a plurality of indentations 211 that extend linearly in one direction and a plurality of indentations 212 that extend linearly in a different direction. Furthermore, it is more preferable that the indentations 211 and 212 each extend linearly continuously throughout the entire display layer 200. When such indentations 211 and 212 are employed, the small piece layer 220 can be manufactured particularly smoothly.
[0034] When the indentations 211 and 212 extend continuously and linearly over the entire display layer 200, the cracks 210 may be provided in a lattice shape as a whole. The small piece layer 220 divided by the cracks 210 may be aligned in the direction in which the indentations 211 and 212 extend. In this embodiment, an example will be described in which a rectangular small piece layer 220 is divided by lattice-shaped cracks 210 including a first group of indentations 211 extending continuously and linearly in a first arrangement direction X over the entire display layer 200 and a second group of indentations 212 extending continuously and linearly in a second arrangement direction Y over the entire display layer 200, as shown in FIG. 3.
[0035] Of the indentations 211 and 212 included in the crack 210 formed in one display layer 200, it is preferable that the intervals between the indentations extending in the same direction are substantially the same. Therefore, in the example shown in this embodiment, the interval P 211 It is preferable that the intervals P between the notches 212 extending in the arrangement direction Y are substantially the same. 212 are preferably substantially the same. Here, "a certain interval (first interval) between the indentations is substantially the same as another interval (second interval)" means that the second interval is 90% or more and 110% or less of the first interval. In this case, the shape of each small piece layer 220 viewed from the thickness direction can usually be made the same, which effectively increases the difficulty of counterfeiting the display medium 10.
[0036] Of the indentations 211 and 212 included in the crack 210 formed in one display layer 200, it is preferable that the intervals between the indentations extending in different directions are substantially the same. Therefore, in the example shown in this embodiment, the interval P 211 and the interval P between the notches 212 extending in the arrangement direction Y. 212 In this case, the regularity of the arrangement of the small piece layers 220 when viewed from the thickness direction can usually be increased, which effectively increases the difficulty of counterfeiting the display medium 10.
[0037] In the case where the lattice-like cracks 210 divide the rectangular small piece layer 220 as in the example shown in this embodiment, the interval P between the indentations 211 is 211 and the interval P between the notches 212 212 may correspond to the length of the corresponding side of the flake layer 220. 211 and P 212 Even if the distance P does not match the length of the side of the small piece layer 220, 211 and P 212 can be correlated to the size of the particle layer 220. 211 and P 212 is preferably set according to the size of the small piece layer 220.
[0038] In general, the interval P 211 and P 212 The smaller the distance P, the smaller the size of the small piece layer 220. Also, the smaller the size of the small piece layer 220, the more difficult it is to see with the naked eye, and therefore the greater the difficulty of counterfeiting the display medium 10. Therefore, from the viewpoint of improving the difficulty of counterfeiting the display medium 10, the distance P 211 and P 212 It is preferable that the interval P is in a certain small range. 211 and P 212 are each preferably 150 μm or less, more preferably 125 μm or less, further preferably 115 μm or less, and particularly preferably 100 μm or less. There is no particular lower limit, and it is usually larger than 0 μm, and preferably 10 μm or more.
[0039] The thickness of the small piece layer 220 is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 2 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 6 μm or less, and particularly preferably 5 μm or less. The thicknesses of the small piece layers 220 included in one display layer 200 may be different, but are preferably the same. When the small piece layer 220 is thin, the size of the small piece layer 220 viewed from the thickness direction can be reduced, effectively increasing the difficulty of counterfeiting the display medium 10.
[0040] The fragment layer 220 may have an in-plane retardation. The fragment layer 220 having an in-plane retardation and the display layer 200 including the fragment layer 220 can function as a retardation plate, and therefore can adjust the polarization state of transmitted light. Therefore, by utilizing the adjustment of the polarization state by the fragment layer 220 and the display layer 200, the display medium 10 can realize various display modes.
[0041] For example, the small piece layer 220 may have an in-plane retardation that can function as a quarter wave plate. The specific in-plane retardation of the small piece layer 220 that can function as a quarter wave plate is preferably "{(2n1+1) / 4}×550nm-30nm" or more, more preferably "{(2n1+1) / 4}×550nm-20nm" or more, particularly preferably "{(2n1+1) / 4}×550nm-10nm" or more, and is preferably "{(2n1+1) / 4}×550nm+30nm" or less, more preferably "{(2n1+1) / 4}×550nm+20nm" or less, particularly preferably "{(2n1+1) / 4}×550nm+10nm" or less, at a measurement wavelength of 550nm. Here, n1 represents an integer of 0 or more. The fragment layer 220 having an in-plane retardation Re in the above range at a measurement wavelength of 550 nm can usually function as a quarter-wave plate in a wide range of the visible wavelength range. Therefore, the fragment layer 220 and the display layer 200 including it can appropriately adjust the polarization state of transmitted light of a wide range of colors. Therefore, the degree of freedom of the color of the display layer 200 can be increased, and a display medium 10 with high designability can be realized.
[0042] For example, the small piece layer 220 may have an in-plane retardation that can function as a 1 / 2 wavelength plate. The specific in-plane retardation of the small piece layer 220 that can function as a 1 / 2 wavelength plate is preferably "{(2n2+1) / 2}×550nm-30nm" or more, more preferably "{(2n2+1) / 2}×550nm-20nm" or more, particularly preferably "{(2n2+1) / 2}×550nm-10nm" or more, and is preferably "{(2n2+1) / 2}×550nm+30nm" or less, more preferably "{(2n2+1) / 2}×550nm+20nm" or less, particularly preferably "{(2n2+1) / 2}×550nm+10nm" or less, at a measurement wavelength of 550nm. Here, n2 represents an integer of 0 or more. The fragment layer 220 having an in-plane retardation Re in the above range at a measurement wavelength of 550 nm can usually function as a half-wave plate in a wide range of the visible wavelength range. Therefore, the fragment layer 220 and the display layer 200 including it can appropriately adjust the polarization state of transmitted light of a wide range of colors. Therefore, the degree of freedom of the color of the display layer 200 can be increased, and a display medium 10 with high designability can be realized.
[0043] The in-plane retardation of the flake layers 220 included in one display layer 200 may be different, but is preferably the same.
[0044] There is no particular limit to the wavelength dispersion of the fragment layer 220. Therefore, the fragment layer 220 may have forward wavelength dispersion or reverse wavelength dispersion. Forward wavelength dispersion means that the in-plane retardation Re(450) and Re(550) at measurement wavelengths of 450 nm and 550 nm satisfy the following formula (R1). The fragment layer 220 having forward wavelength dispersion usually has a smaller in-plane retardation as the measurement wavelength is longer. In addition, reverse wavelength dispersion means that the in-plane retardation Re(450) and Re(550) at measurement wavelengths of 450 nm and 550 nm satisfy the following formula (R2). The fragment layer 220 having reverse wavelength dispersion usually has a larger in-plane retardation as the measurement wavelength is longer. Re(450)>Re(550) (R1) Re(450) <Re(550) (R2)
[0045] The small piece layer 220 can adjust the transmitted light in the visible wavelength range to different polarization states depending on the wavelength dispersion of the small piece layer 220. For example, when the small piece layer 220 capable of functioning as a quarter-wave plate at a certain wavelength has a reverse wavelength dispersion, the small piece layer 220 can give the transmitted light a quarter-wave in-plane retardation in the entire visible wavelength range. On the other hand, when the small piece layer 220 capable of functioning as a quarter-wave plate at a certain wavelength has a forward wavelength dispersion, the small piece layer 220 can give the transmitted light an in-plane retardation that deviates from the quarter-wave in a part of the visible wavelength range. Therefore, when the wavelength dispersion of the small piece layer 220 is different, the polarization state of the polarized light transmitted through the small piece layer 220 can be different. Therefore, the color of the small piece layer 220 and the display layer 200 including it may be adjusted by utilizing the difference in the polarization state. By adjusting the color by using differences in wavelength dispersion in this way, the degree of freedom in the color of the display layer 200 can be increased, and a display medium 10 with excellent design properties can be realized.
[0046] The wavelength dispersion properties of the fragment layers 220 included in one display layer 200 may be different, but are preferably the same.
[0047] When the fragment layer 220 has an in-plane retardation, the fragment layer 220 may have a direction that exhibits the maximum refractive index. Hereinafter, this direction may be referred to as the "optical axis direction". This optical axis direction may be parallel to the layer plane, perpendicular to the layer plane, or inclined in a direction that is neither parallel nor perpendicular to the layer plane. The fragment layer 220 and the display layer 200 including the fragment layer 220 may adjust the polarization state of the transmitted light in various ways depending on the optical axis direction and the traveling direction of the transmitted light. Therefore, by appropriately selecting the optical axis direction of the fragment layer 220, the color of the display layer 200 according to the observation direction can be changed with a wide degree of freedom, thereby realizing a display medium 10 with high designability.
[0048] When the small fragment layer 220 is formed of a liquid crystal composition or a cured product thereof, the optical axis direction of the small fragment layer 220 can be represented by the substantial maximum tilt angle of the molecules of the liquid crystal compound contained in the small fragment layer 220. The "substantial maximum tilt angle" of the molecules of the liquid crystal compound contained in a certain layer refers to the maximum value of the tilt angle of the molecules of the liquid crystal compound when it is assumed that the tilt angle of the molecules on one surface of the layer is 0° and the tilt angle of the molecules changes at a constant rate in the thickness direction. The "tilt angle" of the molecules of the liquid crystal compound refers to the angle that the molecules of the liquid crystal compound make with the layer plane of the layer containing the liquid crystal compound. This tilt angle corresponds to the maximum angle among the angles that the direction of the maximum refractive index in the refractive index ellipsoid of the molecules of the liquid crystal compound makes with the layer plane. Specifically, consider the case where the tilt angle of the molecules of the liquid crystal compound in the thickness direction of the layer containing the liquid crystal compound is smaller closer to one side of the layer and larger farther from the one side. The effective maximum tilt angle represents the maximum tilt angle calculated on the assumption that the rate of change of the tilt angle in the thickness direction (i.e., the rate of change that decreases toward one side and increases toward the other side) is constant. To give a specific example, in a liquid crystal cured layer obtained by curing a layer of a liquid crystal composition formed on a temporary support, the effective maximum tilt angle usually represents the maximum tilt angle of the molecules of the liquid crystal compound on the surface of the temporary support side of the liquid crystal cured layer, assuming that the tilt angle of the molecules is 0° and changes at a constant rate in the thickness direction. Usually, the larger the effective maximum tilt angle of a layer, the larger the tilt angle of the molecules of the liquid crystal compound contained in the layer as a whole tends to be. Therefore, it is possible to know whether the optical axis direction of the small fragment layer 220 is parallel, perpendicular, or neither parallel nor perpendicular to the layer plane, based on this effective maximum tilt angle. For example, if the effective maximum tilt angle is 0° to 4°, the optical axis direction can be parallel to the layer plane. Also, for example, if the effective maximum tilt angle is 86° to 90°, the optical axis direction can be perpendicular to the layer plane. Furthermore, for example, if the substantial maximum tilt angle is greater than 4° and smaller than 86°, the optical axis direction can be inclined with respect to the layer plane.
[0049] The optical axis directions of the fragment layers 220 included in one display layer 200 may be different, but are preferably the same. Therefore, when the fragment layers 220 are formed of a liquid crystal composition or a cured product thereof, the substantial maximum tilt angles may be different, but are preferably the same.
[0050] When the small piece layer 220 has an in-plane retardation, the type of the small piece layer 220 as a retarder can be classified into several types according to the relationship between the optical axis direction of the small piece layer 220 and the layer plane. There is no particular limitation on the type of the small piece layer 220 as a retarder. As a suitable type, the small piece layer 220 is preferably one or more types selected from the group consisting of a positive A plate, a positive C plate, an inclined O plate, and an inclined hybrid alignment plate. The positive A plate refers to a layer whose optical axis direction is parallel to the layer plane. The positive C plate refers to a layer whose optical axis direction is perpendicular to the layer plane. The inclined O plate refers to a layer whose optical axis direction is neither parallel nor perpendicular to the layer plane. The inclined hybrid alignment plate refers to a layer whose optical axis direction is different from the layer plane on one side and the other side. The small piece layer 220 of the suitable type and the display layer 200 including it can adjust the polarization state of the transmitted light in various ways according to the type and the traveling direction of the transmitted light. Therefore, by appropriately selecting the type of the small fragment layer 220, the color of the display layer 200 can be changed with a wide degree of freedom according to the observation direction, thereby realizing a display medium 10 with excellent design.
[0051] The types of flake layers 220 included in one display layer 200 may be different, but are preferably the same.
[0052] The small fragment layer 220 may have a circularly polarized light separation function. The "circularly polarized light separation function" means a function of reflecting circularly polarized light having one of the rotation directions, clockwise and counterclockwise, and transmitting circularly polarized light having the opposite rotation direction. Therefore, the small fragment layer 220 and the display layer 200 including it can exhibit the circularly polarized light separation function by reflecting circularly polarized light having one rotation direction D D The circularly polarized light is reflected and rotated in the direction D. DThe small fragment layer 220 may be capable of transmitting circularly polarized light having a rotation direction opposite to that of the small fragment layer 220. In the following description, the wavelength range in which the small fragment layer 220 can exhibit the circularly polarized light separation function may be referred to as the "display wavelength range" as appropriate. The reflectance of the small fragment layer 220 for unpolarized light in the display wavelength range is usually 35% to 50%, and preferably 40% to 50%. The small fragment layer 220 having the circularly polarized light separation function and the display layer 200 including the small fragment layer 220 can transmit circularly polarized light having a rotation direction D in the display wavelength range. D By utilizing the function of selectively transmitting and reflecting specific circularly polarized light of a specific wavelength, it is possible to realize a variety of display modes on the display medium 10.
[0053] The rotation direction D of the circularly polarized light that the small piece layer 220 included in one display layer 200 can reflect D may be different, but are preferably the same.
[0054] From the viewpoint of realizing a display mode that can be seen by the human eye, the display wavelength range is preferably in the visible wavelength range. The display wavelength ranges of the fragment layers 220 included in one display layer 200 may be different, but are preferably the same.
[0055] The material of the small piece layer 220 is not particularly limited. Examples of the material of the small piece layer 220 include inorganic materials and organic materials. Examples of the inorganic material include metals such as aluminum and silver; and metal compounds such as titanium oxide, silicon oxide, niobium oxide, tantalum oxide, and magnesium fluoride. Examples of the organic material include acrylic polymers, polystyrene, polyester, polyamide, polyvinyl chloride, polyvinyl acetate, cellulose-based polymers (e.g., triacetyl cellulose), polycarbonate, polyurethane, polyolefin, alicyclic structure-containing polymers, epoxy resins, melamine resins, and phenolic resins. The material of the small piece layer 220 may be used alone or in combination of two or more types. In addition, when one small piece layer 220 contains two or more types of materials, the small piece layer 220 may have a single layer structure that uniformly contains two or more types of materials, or may have a multilayer structure having two or more layers containing one or more types of materials.
[0056] In particular, the fragment layer 220 is preferably formed of a cured liquid crystal composition containing a liquid crystal compound. The cured liquid crystal composition makes it possible to efficiently manufacture the fragment layer 220 having in-plane retardation and the fragment layer 220 having a circularly polarized light separation function. Here, for convenience, the material referred to as the "liquid crystal composition" includes not only a mixture of two or more substances, but also a material consisting of a single substance. In the following description, a layer formed of a cured liquid crystal composition may be referred to as the "liquid crystal cured layer".
[0057] For example, a small piece layer 220 having in-plane retardation can be formed by curing a liquid crystal composition in a state in which the liquid crystal compound contained in the liquid crystal composition is aligned. As a specific example, the liquid crystal compound contained in the liquid crystal composition is aligned to make the liquid crystal composition have a liquid crystal phase such as a nematic phase or a smectic phase. When a liquid crystal composition in such a liquid crystal phase is cured, the alignment direction of the liquid crystal compound can be fixed. Therefore, the liquid crystal cured layer containing the cured product obtained by the curing can contain a liquid crystal compound aligned as described above, and can have an in-plane retardation according to factors such as the type of liquid crystal compound, the alignment state of the liquid crystal compound, and the thickness. Therefore, a small piece layer 220 having in-plane retardation can be obtained as the liquid crystal cured layer. The "liquid crystal compound" contained in the cured product of the liquid crystal compound includes not only unreacted liquid crystal compounds, but also liquid crystal compounds that have undergone reactions such as polymerization and crosslinking reactions.
[0058] In this case, the type of the small piece layer 220 as a retardation plate can be adjusted by adjusting the alignment direction of the liquid crystal compound in the thickness direction of the liquid crystal cured layer. For example, when the alignment direction of the liquid crystal compound is parallel to the layer plane, the small piece layer 220 as a positive A plate can be obtained. Also, when the alignment direction of the liquid crystal compound is perpendicular to the layer plane, the small piece layer 220 as a positive C plate can be obtained. Furthermore, when the alignment direction of the liquid crystal compound is neither parallel nor perpendicular to the layer plane, the small piece layer 220 as an inclined O plate can be obtained. Also, when the liquid crystal compound is aligned in such a manner that the angle of the alignment direction of the liquid crystal compound with respect to the layer plane is smaller the closer to one side of the layer and larger the farther from the one side, the small piece layer 220 as an inclined hybrid alignment plate can be obtained.
[0059] Also, for example, a small piece layer 220 having a circularly polarized light separation function can be formed by curing a liquid crystal composition in a state in which the liquid crystal compound contained in the liquid crystal composition is aligned to have cholesteric regularity. Cholesteric regularity is a structure in which the molecular axes are aligned in a certain direction on a certain plane, but the direction of the molecular axes is shifted at a slight angle on the next plane that overlaps it, and the angle is further shifted on the next plane, and so on. As the light passes through the overlapping and arranged planes in sequence, the angle of the molecular axes in the plane shifts (twists). That is, when molecules inside a certain layer have cholesteric regularity, the molecules are aligned so that the molecular axes are in a certain direction on a first plane inside the layer. On a second plane that overlaps the first plane inside the layer, the direction of the molecular axes shifts at a slight angle from the direction of the molecular axes on the first plane. On a third plane that further overlaps the second plane, the direction of the molecular axes shifts at an angle from the direction of the molecular axes on the second plane. In this way, in the plane where the molecules are arranged in an overlapping manner, the angle of the molecular axis in the plane is gradually shifted (twisted). A structure in which the direction of the molecular axis is twisted in this way is usually a helical structure, which is an optically chiral structure. Usually, a liquid crystal cured layer containing a liquid crystal compound having such cholesteric regularity reflects circularly polarized light while maintaining its chirality.
[0060] As a specific example, the liquid crystal compound contained in the liquid crystal composition is aligned to make the liquid crystal composition into a cholesteric phase. When the liquid crystal composition in the cholesteric phase is cured, the alignment direction of the liquid crystal compound can be fixed. Therefore, the liquid crystal cured layer containing the cured product obtained by the curing can contain the liquid crystal compound aligned to have cholesteric regularity as described above, and can have a circularly polarized light separation function according to factors such as the type of liquid crystal compound, the alignment state of the liquid crystal compound, and the thickness. Therefore, a fragment layer 220 having a display wavelength range can be obtained as the liquid crystal cured layer.
[0061] The materials of the flake layers 220 included in one display layer 200 may be different, but are preferably the same.
[0062] [1.3. Optional Layer] The display medium 10 may further include any layer in combination with the substrate 100 and the display layer 200. For example, the display medium 10 may include an adhesive layer (not shown) between the substrate 100 and the display layer 200. By using the adhesive layer, the display medium 10 can be efficiently manufactured.
[0063] The adhesive layer is a layer that bonds the substrate 100 and the display layer 200, and can be formed of an adhesive. The adhesive includes not only adhesives in the narrow sense (adhesives having a shear storage modulus of 1 MPa to 500 MPa at 23°C after irradiation with energy rays or after heat treatment), but also pressure-sensitive adhesives (such as pressure-sensitive adhesives) having a shear storage modulus of less than 1 MPa at 23°C. One type of adhesive may be used alone, or two or more types may be used in combination.
[0064] The adhesive layer may be a transparent layer that transmits light, or may be a non-transparent layer that does not transmit light. In addition, when the adhesive layer is transparent, the adhesive layer may have in-plane retardation, but is preferably an optically isotropic layer with small in-plane retardation. For example, the in-plane retardation of the adhesive layer at a measurement wavelength of 550 nm is preferably 0 to 20 nm, more preferably 0 to 10 nm, and particularly preferably 0 to 5 nm.
[0065] Further examples of the optional layer include a matte layer that improves the slipperiness of the display medium 10; a hard coat layer such as an impact-resistant polymethacrylate resin layer; an anti-reflection layer; an anti-fouling layer; and the like.
[0066] [1.4. Display medium manufacturing method] There is no particular limitation on the manufacturing method of the display medium 10 according to the first embodiment of the present invention, and any manufacturing method that can obtain the above-mentioned display medium 10 can be adopted. From the viewpoint of efficiently manufacturing the display medium 10, the display medium 10 is A step (A) of preparing a web member including a temporary support and a transfer material layer including a small piece layer 220 formed on the temporary support; A step (B) of forming an adhesive layer having the same shape as the display layer 200 when viewed in the thickness direction on the substrate 100; A step (C) of bonding the transfer material layer and the adhesive layer; A step (D) of peeling off the temporary support; It is preferable to produce the composition by a production method including the steps of:
[0067] This preferred manufacturing method will be described below with reference to the drawings. Fig. 5 is a schematic plan view of a web member 300 prepared in the manufacturing method for display medium 10 according to the first embodiment of the present invention, as viewed from the thickness direction. Fig. 6 is a cross-sectional view showing a cross section of web member 300 prepared in the manufacturing method for display medium 10 according to the first embodiment of the present invention, cut along the VI-VI plane shown in Fig. 5. Fig. 7 is an enlarged plan view showing a schematic enlargement of part VII shown in Fig. 5 of web member 300 prepared in the manufacturing method for display medium 10 according to the first embodiment of the present invention.
[0068] As shown in FIGS. 5 and 6, in step (A), a web member 300 including a temporary support 310 and a transfer material layer 320 formed on the temporary support 310 is prepared.
[0069] For example, a plate, sheet, film, or the like formed of an appropriate material can be used as the temporary support 310. From the viewpoint of efficient manufacturing of the display medium 10, it is preferable that the temporary support 310 has an elongated shape.
[0070] For example, a resin can be used as the material of the temporary support 310. Examples of the resin include the same resins as those exemplified as the material of the base material 100. Among them, a resin containing an alicyclic structure-containing polymer is preferable.
[0071] The temporary support 310 may or may not be subjected to a stretching treatment. In addition, the surface of the temporary support 310 may be subjected to a surface treatment such as a rubbing treatment.
[0072] The temporary support 310 may have a single-layer structure having only one layer, or may have a multi-layer structure having two or more layers. For example, the temporary support 310 may have a resin film layer formed of the above-mentioned resin and an alignment film formed on the resin film layer. When the temporary support 310 having such an alignment film is used, the liquid crystal compound contained in the layer of the liquid crystal composition formed on the alignment film can be well aligned. The alignment film can be formed of a resin containing a polymer such as polyimide, polyvinyl alcohol, polyester, polyarylate, polyamideimide, polyetherimide, or polyamide.
[0073] The thickness of the temporary support 310 is preferably 12 μm or more, more preferably 25 μm or more, even more preferably 50 μm or more, and is preferably 250 μm or less, more preferably 200 μm or less, even more preferably 188 μm or less.
[0074] As shown in FIG. 7, the transfer material layer 320 is a layer including a fragment layer 330 that is the same as the fragment layer 220 included in the display medium 10. In detail, the transfer material layer 320 includes a plurality of fragment layers 330 separated by cracks 340, and the fragment layers 330 are the same as the fragment layers 220 included in the display medium 10. Therefore, each fragment layer 330 is provided at a different position on the surface 310U of the temporary support 310, and the fragment layers 330 are separated from each other by cracks 340 formed throughout the entire thickness of the transfer material layer 320. The transfer material layer 320 is formed by a group of the plurality of fragment layers 330.
[0075] The fragment layer 330 included in the transfer material layer 320 is the same as the fragment layer 220 included in the display medium 10, and is therefore usually formed of the same material as the fragment layer 220 included in the display medium 10. Furthermore, the fragment layer 330 included in the transfer material layer 320 usually has the same arrangement direction, shape as viewed from the thickness direction, size, and characteristics (in-plane retardation, wavelength dispersion, type as a phase difference plate, circular polarization separation function, etc.) as the fragment layer 220 included in the display medium 10.
[0076] In addition, since the small piece layer 330 included in the transfer material layer 320 is the same as the small piece layer 220 included in the display medium 10, the cracks 340 dividing the small piece layer 330 usually have the same shape, size and interval as the cracks 210 dividing the small piece layer 220 when viewed from the thickness direction. Furthermore, the cracks 340 dividing the small piece layer 330 usually include indentations 341 and 342 extending in two or more directions, and the directions in which these indentations 341 and 342 extend and the shape, size and interval as viewed from the thickness direction are the same as the indentations 211 and 212 included in the cracks 210 dividing the small piece layer 220.
[0077] However, the transfer material layer 320 does not have to have the same shape as the display layer 200 when viewed in the thickness direction. The transfer material layer 320 is usually formed larger than the display layer 200. In detail, the transfer material layer 320 is usually formed large enough to cover the display layer 200. In this embodiment, an example will be described in which the transfer material layer 320 is formed on most of a surface 310U of a temporary support 310 that is larger than the display layer 200, as shown in Figs. 5 and 6.
[0078] The transfer material layer 320 is usually disposed on the outermost side of the original web member 300. Disposed on the outermost side means that the transfer material layer 320 is disposed on the outermost side in the thickness direction of the original web member 300. Therefore, a surface 320U of the transfer material layer 320 can be exposed on one side of the original web member 300. The original web member 300 may have an arbitrary layer between the temporary support 310 and the transfer material layer 320.
[0079] The raw fabric member 300 can be manufactured, for example, by a manufacturing method including forming a layer of the material of the small piece layer 330 on the temporary support 310 and forming the cracks 340 in the formed layer. In the following description, the layer before the cracks 340 formed of the material of the small piece layer 330 are formed may be referred to as a "material layer". This material layer is usually a layer formed of the same material as the small piece layers 220 and 330 and to the same thickness as the small piece layers 220 and 330, and can have the same optical properties (e.g., in-plane retardation, circular polarization separation function, etc.) as the small piece layers 220 and 330.
[0080] There is no limitation on the method of forming the material layer. For example, when forming a material layer by a cured product of a liquid crystal composition, a layer of the liquid crystal composition is formed on the temporary support 310, and after orienting the liquid crystal compound contained in the liquid crystal composition as necessary, the liquid crystal composition is cured to obtain a material layer as a liquid crystal cured layer. For example, when it is desired to form a material layer having in-plane retardation, the method described in International Publication No. 2014 / 069515, International Publication No. 2015 / 064581, International Publication No. 2019 / 163611, International Publication No. 2019 / 146468, etc. may be adopted. In addition, for example, when it is desired to form a material layer having a circularly polarized light separation function, the method described in JP-A-2014-174471 may be adopted. By forming a material layer on the temporary support 310, a multilayer member including the temporary support 310 and the material layer is obtained.
[0081] Fig. 8 is a cross-sectional view showing a cross section of an original web member 300 prepared in the manufacturing method of the display medium 10 according to the first embodiment of the present invention, cut along the VIII-VIII plane shown in Fig. 7. By forming cracks 340 in a material layer of a multi-layer member (not shown), an original web member 300 having a transfer material layer 320 including a small piece layer 330 is obtained as shown in Fig. 8. The cracks 340 are usually formed throughout the thickness of the material layer, dividing the small piece layer 330 throughout the thickness.
[0082] Furthermore, the crack 340 is formed at a thickness T 330 In particular, the cracks 340 are preferably formed deeper than the thickness T 330 In this case, the tip 340C of the crack 340 reaches a position deeper than the surface 310U of the temporary support 310 on the side of the small piece layer 330. 340 is the thickness T of the small piece layer 330 330 When the cracks 340 are deep in this way, the shape conformity of the small piece layers 330 separated by the cracks 340 can be improved.
[0083] However, the depth of the crack 340, T 340It is preferable to set the depth T of the crack 340 so as not to completely cut the temporary support 310. 340 is the thickness T of the small piece layer 330 330 and the thickness T 300 Smaller is preferable.
[0084] The crack 340 can be formed, for example, by pressing a processing tool having an uneven shape against the material layer side of the multi-layered member. Preferably, the crack 340 is formed by pressing the multi-layered member between the support tool and the processing tool while the multi-layered member is supported by the support tool.
[0085] As the processing tool, a member having a convex portion on its surface corresponding to the shape of the crack 340 as viewed from the thickness direction of the multi-layered member can be used. For example, if the shape of the crack as viewed from the thickness direction of the multi-layered member is a lattice shape, a member having a lattice-shaped convex portion on its surface can be used.
[0086] Only one processing tool may be used, or two or more may be used in combination. For example, a processing tool having a convex portion on its surface corresponding to a part of the crack 340 and a processing tool having a convex portion on its surface corresponding to another part of the crack 340 may be used in combination. When forming a crack including the indentations 341 and 342 extending in different directions as in the example shown in this embodiment, the crack 340 may be formed by pressing a first processing tool having a convex portion on its surface corresponding to the indentation 341 extending in one direction and a second processing tool having a convex portion on its surface corresponding to the indentation 342 extending in another direction against the multi-layer member.
[0087] The same tool may be pressed against the multi-layer member multiple times in different orientations to form cracks 340 .
[0088] Also, a cylindrical tool may be used to form continuous cracks in the multi-layered member.
[0089] The material of the processing tool may be one that has a strength that does not break even when the multi-layered member is pressed and can form an uneven structure. Examples of such materials include carbon steel and stainless steel. In addition, the processing tool may have a multi-layer coating of one or more layers on the surface from the viewpoint of increasing corrosion resistance, strength, and thermal conductivity. Examples of such coatings include plating films of nickel, nickel phosphorus, silicon, copper, etc.; coatings formed by ceramic spraying; and the like. Furthermore, the processing tool may be provided with, for example, a heating device using a heater, a heat medium, dielectric heating, induction heating, etc.; a static eliminator for static electricity countermeasures; an earth; and the like. Such a processing tool can be manufactured, for example, by forming an uneven shape on a cylindrical metal roll by cutting with a cutting tool such as a diamond bit or processing with a laser processing device.
[0090] The pressure when pressing the processing tool against the material layer side of the multi-layered member is preferably 0.5 MPa or more, more preferably 1 MPa or more, even more preferably 5 MPa or more, and preferably 100 MPa or less, more preferably 75 MPa or less. When the pressure is equal to or greater than the lower limit, a crack 340 of sufficient depth can be formed. When the pressure is equal to or less than the upper limit, damage to the raw fabric member 300 can be suppressed. When the same or different processing tools are pressed against the multi-layered member multiple times to form the crack 340, the multiple pressings may be performed at the same pressure or at different pressures. Preferably, the multiple pressings are performed at the same pressure.
[0091] The support usually has a support surface capable of supporting the surface opposite to the side of the material layer included in the multi-layered member. The hardness of the support surface of the support is preferably D40 or more, more preferably D60 or more, even more preferably D70 or more, and preferably D99 or less, more preferably D97 or less, even more preferably D95 or less. Here, the hardness represents a value measured by a durometer (type D) according to JIS K-6253. When the hardness of the support surface of the support is within the above range, a crack of an appropriate depth can be easily formed. Examples of the material of the surface of the support include rubber and resin.
[0092] An example of a method for forming the crack 340 using a processing tool will be described below with reference to the drawings. Fig. 9 is a perspective view showing an example of a processing tool 400 that can be used in a method for manufacturing a raw fabric member 300 in a method for manufacturing a display medium 10 according to the first embodiment of the present invention. Fig. 10 is a perspective view showing the processing tool 400 shown in Fig. 9. Fig. 11 is a plan view showing the processing tool 400 shown in Fig. 10 cut along line XI-XI and developed. Fig. 12 is a partial cross-sectional view showing a cross section of a part of the vicinity of the surface of the processing tool 400 cut along a plane perpendicular to the extension direction of the protrusions 410.
[0093] As shown in FIG. 9, the processing tool 400 is arranged to contact the surface 360U of the multi-layered member 350 on the material layer 360 side so that the multi-layered member 350 can be pressed. As shown in FIG. 10, the processing tool 400 has a cylindrical shape and is rotatably provided. The outer surface of the processing tool 400 (the surface that contacts the multi-layered member 350) is provided with an uneven shape. As shown in FIG. 11, the uneven shape includes a convex portion 410 and a concave portion 420 extending in a direction that forms an angle θx with respect to a certain reference direction L1. Here, an example is shown in which the axial direction of the processing tool 400 perpendicular to the conveying direction of the multi-layered member 350 is adopted as the reference direction L1. The convex portions 410 and the concave portions 420 of the processing tool 400 are alternately and repeatedly formed in a direction perpendicular to the direction in which the convex portions 410 extend. The angle θx is not particularly limited, but an example is shown in which the angle θx is 45°. The uneven shape of the processing tool 400 is a shape of straight lines when viewed from above the paper surface, as shown in Fig. 11. As shown in Fig. 12, the distance P between two adjacent protrusions 410 is 410 10 and 11, reference numerals 430 and 440 denote ends of the processing tool 400.
[0094] As shown in FIG 12, the protrusion 410 may have a mountain shape with an acute-angled apex 410T in cross section. 410 The smaller the apex angle θ, the better. 410may be, for example, 10° or more, 20° or more, or 30° or more, and may be, for example, 90° or less, 80° or less, 70° or less, or 60° or less. The apex shape of the protrusion 410 may be rounded or chamfered as long as it is possible to form the crack 340 in the material layer 360.
[0095] 9, a cylindrical support 450 is rotatably provided opposite the processing tool 400. The support 450 is provided so as to be able to press the surface of the multilayer member 350 on the temporary support 310 side. Thus, the multilayer member 350 is pressed between the support 450 and the processing tool 400.
[0096] Fig. 13 is a perspective view showing an example of a processing tool 500 that can be used in a method for manufacturing a raw fabric member 300 in a method for manufacturing a display medium 10 according to the first embodiment of the present invention. Fig. 14 is a perspective view showing the processing tool 500 shown in Fig. 13. Fig. 15 is a plan view showing the processing tool 500 shown in Fig. 14 cut along line XV-XV and developed.
[0097] As shown in FIG. 13 to FIG. 15, the processing tool 500 is arranged to contact the surface 360U of the multilayer member 350 on the material layer 360 side so that the multilayer member 350 can be pressed. The processing tool 500 is provided in the same manner as the processing tool 400, except that the directions in which the convex portion 510 and the concave portion 520 extend are different. The processing tool 500 includes the convex portion 510 and the concave portion 520, but the angle θy that the convex portion 510 and the concave portion 520 make with respect to the reference direction L2 is different from the angle θx of the processing tool 400. Here, an example is shown in which the axial direction of the processing tool 500 perpendicular to the conveying direction of the multilayer member 350 is adopted as the reference direction L2. The angle θy is not particularly limited, but an example is shown in which the angle θy is 135°. 15, when viewed from above the paper, the uneven shape of the processing tool 500 is a shape in which straight lines are arranged in a direction intersecting the direction in which the convex portions 410 and the concave portions 420 of the processing tool 400 extend. In FIGS. 14 and 15, reference numerals 530 and 540 denote ends of the processing tool 500.
[0098] 13, a cylindrical support 550 is rotatably provided opposite the processing tool 500. The support 550 is provided so as to be able to press the surface of the multilayer member 350 on the temporary support 310 side. Thus, the multilayer member 350 is pressed between the support 550 and the processing tool 500.
[0099] When forming a crack 340 in a material layer 360 of a multi-layer member 350 using the processing tools 400 and 500 and the support tools 450 and 550, a step of forming one notch 341 using one processing tool 400 and support tool 450, and a step of forming the other notch 342 using the other processing tool 500 and support tool 550 are performed.
[0100] In the process using the processing tool 400 and the support tool 450, as shown in Fig. 9, the multilayer member 350 is passed between the processing tool 400 and the support tool 450, and the convex portion 410 of the processing tool 400 is brought into contact with the material layer 360. Then, by pressing the multilayer member 350 between the processing tool 400 and the support tool 450 in this state, the convex portion 410 of the processing tool 400 is caused to penetrate into the material layer 360, and an indentation 341 reflecting the shape of the convex portion 410 can be formed. When the degree of pressing is adjusted so that the convex portion 410 of the processing tool 400 penetrates into the temporary support 310, the indentation 341 is formed in a thickness T of the small piece layer 330. 330 It is formed deeper, reaching a position deeper than the surface 310U of the temporary support 310 on the side of the small piece layer 330 (see FIG. 8).
[0101] 13, the multilayer member 350 is passed between the processing tool 500 and the support tool 550, and the protruding portion 510 of the processing tool 500 is brought into contact with the material layer 360. In this state, the multilayer member 350 is pressed between the processing tool 500 and the support tool 550, so that the protruding portion 510 of the processing tool 500 penetrates into the material layer 360, and the indentations 342 reflecting the shape of the protruding portion 510 can be formed. When the degree of pressing is adjusted so that the protruding portion 510 of the processing tool 500 penetrates into the temporary support 310, the indentations 342 are formed in a thickness T of the small piece layer 330. 330It is formed deeper, reaching a position deeper than the surface 310U of the temporary support 310 on the side of the small piece layer 330 (see FIG. 8).
[0102] Therefore, by the method including the step of forming the incision 341 and the step of forming the incision 342 as described above, the crack 340 including the incision 341 and the incision 342 can be formed in the material layer 360 to obtain the raw fabric member 300. The order of forming the incision 341 by the processing tool 400 and the incision 342 by the processing tool 500 is not particularly limited. For example, the multilayer member 350 may be pressed by the processing tool 400 and then pressed by the processing tool 500. Also, the multilayer member 350 may be pressed by the processing tool 500 and then pressed by the processing tool 400.
[0103] In step (B), an adhesive layer having the same shape as the display layer 200 when viewed from the thickness direction is formed on the substrate 100. The adhesive layer thus formed can function as a latent image of the display layer 200. There is no limitation on the method of forming the adhesive layer. For example, when a liquid adhesive is used, the adhesive may be applied to the substrate to form an adhesive layer. As the application method, for example, a printing method such as a screen printing method or an inkjet printing method is preferable. Also, for example, when a film-like or sheet-like adhesive is used, the adhesive may be processed into an appropriate shape, and the processed adhesive may be attached to the substrate. Examples of the processing method include cutting, punching, and the like. Among them, the printing method is preferable from the viewpoint of suppressing the manufacturing cost.
[0104] After the steps (A) and (B), a step (C) is performed in which the transfer material layer 320 of the original web member 300 and the adhesive layer formed on the substrate 100 are bonded together. The bonding is usually performed by pressing the original web member 300 and the substrate 100 with a pressing tool such as a nip roll, with the surface of the original web member 300 on the transfer material layer 320 side facing the surface of the substrate 100 on the adhesive layer side. As a result, in the area where the adhesive layer is present, the substrate 100 and the transfer material layer 320 are bonded together via the adhesive layer.
[0105] After the step (C), a step (D) of peeling off the temporary support 310 is performed. When the temporary support 310 is peeled off, in the area on the substrate 100 where the adhesive layer is formed, the transfer material layer 320 is separated from the temporary support 310 and remains on the substrate 100. Thus, the display layer 200 is formed by the part of the transfer material layer 320 remaining on the substrate 100. This display layer 200 includes a group of small piece layers 220 as a part of the many small piece layers 330 contained in the transfer material layer 320. Thus, the display layer 200 is formed by this group of small piece layers 220. On the other hand, in the area on the substrate 100 where there is no adhesive layer, the transfer material layer 320 cannot be separated from the temporary support 310. Thus, the transfer material layer 320 is peeled off together with the temporary support 310, so that the small piece layer 330 does not remain in the area on the substrate 100 where there is no adhesive layer. Therefore, the display layer 200 having the shape of the adhesive layer when viewed in the thickness direction can be formed on the substrate 100 to obtain the display medium 10.
[0106] In the above-described method for producing the display medium 10, the order of steps (A), (B), (C) and (D) is not limited as long as the display medium 10 is obtained.
[0107] The above-mentioned manufacturing method of the display medium 10 is preferably carried out using a long substrate 100 and a long original web member 300. In this case, the display medium 10 can be manufactured with high productivity using a roll-to-roll method.
[0108] The above-mentioned method for manufacturing the display medium 10 may further include any optional step in addition to the steps (A), (B), (C) and (D). For example, when a curable adhesive is used, the above-described manufacturing method of the display medium 10 may include a step of curing the adhesive. The curing of the adhesive is usually performed after the step (C) and before the step (D). Furthermore, when a long substrate 100 and a long original web member 300 are used, a long display medium 10 is usually obtained. Therefore, the manufacturing method of the display medium 10 described above may include a step of trimming the long display medium 10 into an appropriate shape.
[0109] [1.5. Main effects of display media] The display medium 10 described above can realize a variety of display modes by using the display layer 200. For example, the display layer 200 can be formed in various colors and shapes, allowing a variety of images to be visually recognized by an observer who observes the display layer 200. Therefore, the display medium 10 can contribute to increasing the degree of freedom in display modes.
[0110] In particular, the display layer 200 including the fragment layer 220 having in-plane retardation is usually transparent, and therefore may be difficult to see when observed with the naked eye. However, when the display medium 10 is placed between two linear polarizing plates arranged in a crossed Nicol or parallel Nicol configuration and observed through transmission, the display layer 200 can be seen depending on the installation angle of the display medium 10. Therefore, the display layer 200 can contribute to the realization of various display modes according to the observation method. "Crossed Nicol" refers to an arrangement in which the absorption axes of the two linear polarizing plates are orthogonal when viewed from the thickness direction. Also, "parallel Nicol" refers to an arrangement in which the absorption axes of the two linear polarizing plates are parallel when viewed from the thickness direction.
[0111] In particular, the display layer 200 including the small fragment layer 220 having the circularly polarized light separation function can be seen when observed with the naked eye under non-polarized light. In addition, when observed through a circular polarizing plate that can transmit the circularly polarized light that the small fragment layer 220 can reflect, the display layer 200 can be seen. However, when observed through a circular polarizing plate that does not transmit the circularly polarized light that the small fragment layer 220 can reflect, the display layer 200 may be difficult to see. In addition, when observed by irradiating only circularly polarized light that the small fragment layer 220 cannot reflect, the display layer 200 may be difficult to see. Therefore, the display layer 200 can contribute to the realization of various display modes according to the observation method. In particular, the display layer 200 including the small fragment layer 220 having the circularly polarized light separation function can reflect circularly polarized light of a color corresponding to the display wavelength range of the small fragment layer 220, so that the display layer 200 can be displayed with a color corresponding to the display wavelength range. Therefore, it can effectively contribute to increasing the degree of freedom of the display mode.
[0112] Furthermore, the above-mentioned display medium 10 allows the display layer 200 to be visually recognized without magnification observation using a loupe or a microscope. However, the small piece layer 220 included in the display layer 200 is small, so it is difficult to visually recognize it without magnification observation, and it is difficult to recognize its shape, size, and arrangement. In particular, the small piece layer 220 whose width is within the above-mentioned specific range is difficult to visually recognize unless a high-magnification microscope is used, and it is difficult for an observer to know that the small piece layer 220 is included in the display layer 200. Therefore, according to the above-mentioned display medium 10, it is possible to increase the difficulty of counterfeiting while contributing to the realization of various display modes by the display layer 200.
[0113] Moreover, the small piece layers 220 of the display medium 10 are arranged side by side in two or more directions in one display layer 200. The small piece layers 220 arranged side by side in two or more directions in this manner have a high degree of regularity in their arrangement. By arranging the small piece layers 220 with a high degree of regularity, the difficulty of manufacturing the display medium 10 is increased. Therefore, according to the display medium 10 described above, it is possible to increase the difficulty of counterfeiting.
[0114] The above-described display medium 10 can be efficiently manufactured using a roll-to-roll method, and therefore can be manufactured at low cost, which is commercially advantageous.
[0115] [2. Second embodiment] In the first embodiment, the display medium 10 including the transparent substrate 100 has been described as an example, but the display medium may include a non-transparent substrate. For example, the display medium may include a substrate including a colored layer. Hereinafter, an embodiment of a display medium including a colored layer will be described.
[0116] Fig. 16 is a schematic plan view of a display medium 20 according to a second embodiment of the present invention, as viewed from the thickness direction. Fig. 17 is a schematic cross-sectional view of the display medium 20 according to the second embodiment of the present invention, cut along the XVII-XVII plane shown in Fig. 16. Fig. 18 is an enlarged plan view of the display medium 20 according to the second embodiment of the present invention, enlarging the XVIII portion shown in Fig. 16. In the second embodiment, the same elements as those described in the first embodiment will be described with the same reference numerals as those used in the first embodiment.
[0117] 16 to 18, the display medium 20 according to the second embodiment of the present invention is provided in the same manner as the display medium 10 according to the first embodiment, except that it has a non-transparent substrate 600 instead of the transparent substrate 100. Thus, the display medium 20 has the substrate 600 and a display layer 200 formed on the substrate 600, and the display layer 200 includes a plurality of small fragment layers 220 formed with high regularity.
[0118] The substrate 600 includes a colored layer 610 combined with a support layer 110. The colored layer 610 does not transmit light in a part or all of the visible wavelength range, so the substrate 600 is non-transparent. In this embodiment, an example will be described in which the substrate 600 includes the support layer 110 and the colored layer 610 in this order from the display layer 200 side. However, the substrate 600 may include the colored layer 610 and the support layer 110 in this order from the display layer 200 side. In addition, the substrate 600 may be provided so that the colored layer 610 itself can support the display layer 200, omitting the support layer 110.
[0119] The colored layer 610 can be formed of a material that can block a part or all of the light in the visible wavelength range. Examples of materials for the colored layer 610 include resins containing colorants such as pigments and dyes, paper, leather, cloth, wood, metals, and metal compounds. These materials may be used alone or in combination of two or more.
[0120] The display medium 20 according to the second embodiment of the present invention can obtain the same advantages as the display medium 10 described in the first embodiment. Furthermore, the colored layer 610 allows the substrate 600 having the colored layer 610 to express various designs. This effectively contributes to increasing the degree of freedom of the display mode. Furthermore, the colored layer 610 can block a part or all of the light passing through the substrate 600, thereby improving the visibility of the display layer 200. Even if the visibility of the display layer 200 is improved in this way, the fragment layer 220 is difficult to view without magnified observation, so the display medium 20 can increase the difficulty of counterfeiting.
[0121] [3. Third embodiment] The substrate of the display medium may have a circularly polarized light separation function. Such a substrate having a circularly polarized light separation function usually has a selective reflection layer having a circularly polarized light separation function. Hereinafter, an embodiment of a display medium having a selective reflection layer will be described.
[0122] Fig. 19 is a schematic plan view of a display medium 30 according to a third embodiment of the present invention, as viewed from the thickness direction. Fig. 20 is a schematic cross-sectional view of the display medium 30 according to the third embodiment of the present invention, cut along the XX-XX plane shown in Fig. 19. Fig. 21 is an enlarged plan view of the display medium 30 according to the third embodiment of the present invention, enlarging the XXI portion shown in Fig. 19. In the third embodiment, the same elements as those described in the first embodiment will be described with the same reference numerals as those used in the first embodiment.
[0123] 19 to 21, the display medium 30 according to the third embodiment of the present invention is provided in the same manner as the display medium 10 according to the first embodiment, except that it includes a substrate 700 having a circularly polarized light separation function instead of the substrate 100. Thus, the display medium 30 includes the substrate 700 and a display layer 200 formed on the substrate 700, and the display layer 200 includes a plurality of small fragment layers 220 formed with high regularity.
[0124] The substrate 700 includes a selective reflection layer 710 in combination with the support layer 110. Since the selective reflection layer 710 has a circularly polarized light separation function, the substrate 700 can acquire the circularly polarized light separation function. In this embodiment, an example will be described in which the substrate 700 includes the selective reflection layer 710 and the support layer 110 in this order from the display layer 200 side. However, the substrate 700 may also include the support layer 110 and the selective reflection layer 710 in this order from the display layer 200 side. Furthermore, the substrate 700 may be provided so that the selective reflection layer 710 itself can support the display layer 200, omitting the support layer 110.
[0125] The selective reflection layer 710 has a circularly polarized light separation function, and therefore, in the wavelength range in which the circularly polarized light separation function can be exerted, one rotation direction D S The circularly polarized light is reflected and rotated in the direction D. S It can transmit circularly polarized light having a rotation direction opposite to that of the selective reflection layer 710. In the following description, the wavelength range in which the selective reflection layer 710 can exhibit the circularly polarized light separation function is sometimes referred to as the "substrate reflection range" as appropriate. The reflectance of the selective reflection layer 710 in the substrate reflection range for unpolarized light is usually 35% to 50%, and preferably 40% to 50%.
[0126] When the small piece layer 220 included in the display layer 200 has a circularly polarized light separation function, the rotation direction D of the circularly polarized light that the selective reflection layer 710 can reflect is S is the rotation direction D of the circularly polarized light that the flake layer 220 can reflect. D It may be the same as or vice versa.
[0127] The wavelength width of the substrate reflection range of the selective reflection layer 710 is preferably wide. The specific wavelength width of the substrate reflection range is preferably 70 nm or more, more preferably 100 nm or more, even more preferably 200 nm or more, and particularly preferably 400 nm or more. The wide wavelength width of the substrate reflection range can widen the range of circularly polarized colors that can be reflected by the selective reflection layer 710. Since such a selective reflection layer 710 can be viewed in a low saturation color, when a display layer 200 with a high saturation color is formed, the visibility of the display layer 200 can be improved. The upper limit of the wavelength width of the substrate reflection range is not particularly limited, but can be, for example, 600 nm or less.
[0128] When the small fragment layer 220 included in the display layer 200 has a circularly polarized light separation function, the substrate reflection range of the selective reflection layer 710 may or may not overlap with the display wavelength range of the small fragment layer 220 included in the display layer 200. When overlapping, a part of the substrate reflection range may overlap with a part of the display wavelength range, a part of the substrate reflection range may overlap with the entire display wavelength range, the entire substrate reflection range may overlap with a part of the display wavelength range, or the entire substrate reflection range may overlap with the entire display wavelength range. Among them, it is preferable that the substrate reflection range includes the display wavelength range by overlapping a part of the substrate reflection range with the entire display wavelength range. In this case, the visibility of the display layer 200 under circularly polarized light can be increased while the visibility of the display layer 200 under non-polarized light can be reduced. For example, the rotation direction D of the circularly polarized light that the selective reflection layer 710 can reflect may be set to 1. S and the rotation direction D of the circularly polarized light that the flake layer 220 included in the display layer 200 can reflect. D Assume that the above is reversed. In this case, when non-polarized light is irradiated onto the display layer 200 side of the display medium 30, both the selective reflection layer 710 and the display layer 200 reflect circularly polarized light. In this case, if the substrate reflection range includes the display wavelength range, both areas with and without the display layer 200 can be visually recognized as the color of the selective reflection layer 710. Therefore, the visibility of the display layer 200 is low to an observer observing the display layer 200 side of the display medium 30. However, if the display medium 30 has a rotation direction D D When the display medium 30 is irradiated with circularly polarized light, the selective reflection layer 710 does not reflect the circularly polarized light, but the display layer 200 reflects the circularly polarized light. Therefore, an observer who observes the display layer 200 side of the display medium 30 can clearly see the circularly polarized light reflected by the display layer 200, thereby improving the visibility of the display layer 200.
[0129] When the small fragment layer 220 included in the display layer 200 has a circularly polarized light separation function, it is preferable that the wavelength width of the substrate reflection range of the selective reflection layer 710 is wider than the wavelength width of the display wavelength range of the small fragment layer 220. In this case, since the display wavelength range can be included in the substrate reflection range, it is possible to increase the visibility of the display layer 200 under circularly polarized light while decreasing the visibility of the display layer 200 under unpolarized light.
[0130] The substrate reflection range of the selective reflection layer 710 preferably includes the entire visible wavelength range. Therefore, the lower limit of the substrate reflection range is preferably 400 nm or less, and the upper limit of the substrate reflection range is preferably 780 nm or more.
[0131] The display medium 30 according to the third embodiment of the present invention can provide the same advantages as the display medium 10 described in the first embodiment. Furthermore, the selective reflection layer 710 allows the substrate 700 having the selective reflection layer 710 to express a variety of designs. This can effectively contribute to increasing the degree of freedom in display modes. Furthermore, the selective reflection layer 710 allows the substrate 700 to reflect light in a specific rotation direction D when the substrate 700 is irradiated with light. S Therefore, when the display layer 200 includes the small piece layer 220 having in-plane retardation, the display layer 200 can adjust the polarization state of the circularly polarized light to realize various display modes.
[0132] For example, assume that the display medium 30 is illuminated with unpolarized light when the fragment layer 220 included in the display layer 200 has an in-plane retardation that can function as a quarter-wave plate. In this case, it is difficult for an observer who observes the display medium 30 with the naked eye to see the display layer 200. However, an observer who observes the display layer 200 side of the display medium 30 through a linear polarizing plate can see the display layer 200 if the angle between the absorption axis of the linear polarizing plate and the slow axis of the fragment layer 220 included in the display layer 200 is appropriate.
[0133] Also, for example, assume that the flake layer 220 included in the display layer 200 has an in-plane retardation that can function as a quarter-wave plate, and the display layer 200 side of the display medium 30 is illuminated with circularly polarized light. The rotation direction of the circularly polarized light that illuminates the display medium 30 is the rotation direction D of the circularly polarized light that can be reflected by the selective reflection layer 710. S If the reflectance of the circularly polarized light is equal to the reflectance of the circularly polarized light, the selective reflection layer 710 can reflect the circularly polarized light with a strong intensity in the area where the display layer 200 is not provided. However, in the area where the display layer 200 is provided, the circularly polarized light is converted to linearly polarized light by the display layer 200, and the selective reflection layer 710 can only reflect the linearly polarized light with a weak intensity. Therefore, the display layer 200 can be visually recognized as an area with a weaker reflection than the surrounding area. On the other hand, the rotation direction of the circularly polarized light illuminating the display medium 30 is the rotation direction D of the circularly polarized light that can be reflected by the selective reflection layer 710. S In the opposite case, in the area where the display layer 200 is not provided, the selective reflection layer 710 cannot reflect the circularly polarized light. However, in the area where the display layer 200 is provided, the circularly polarized light is converted into linearly polarized light by the display layer 200, and the selective reflection layer 710 can reflect the linearly polarized light. Therefore, the display layer 200 can be visually recognized as a part that is more reflective than the surrounding area.
[0134] Furthermore, for example, assume that the flake layer 220 included in the display layer 200 has an in-plane retardation that can function as a half-wave plate, and the display medium 30 is illuminated with unpolarized light. In this case, it is difficult for an observer who observes the display medium 30 with the naked eye to see the display layer 200. However, an observer who observes the display layer 200 side of the display medium 30 through an appropriate circular polarizer can see the display layer 200.
[0135] Also, for example, assume that the flake layer 220 included in the display layer 200 has an in-plane retardation that can function as a half-wave plate, and the display layer 200 side of the display medium 30 is illuminated with circularly polarized light. The rotation direction of the circularly polarized light that illuminates the display medium 30 is the rotation direction D of the circularly polarized light that can be reflected by the selective reflection layer 710. SIf the rotation direction of the circularly polarized light is equal to or greater than the rotation direction of the display layer 200, the selective reflection layer 710 can reflect the circularly polarized light in areas where the display layer 200 is not provided. However, in areas where the display layer 200 is provided, the rotation direction of the circularly polarized light is reversed by passing through the display layer 200, and the selective reflection layer 710 cannot reflect the circularly polarized light. Therefore, the display layer 200 can be visually recognized as an area that has weaker or no reflection than the surrounding area. On the other hand, the rotation direction of the circularly polarized light illuminating the display medium 30 is the rotation direction D of the circularly polarized light that can be reflected by the selective reflection layer 710. S If the opposite is true, the selective reflection layer 710 cannot reflect the circularly polarized light in areas where the display layer 200 is not provided. However, in areas where the display layer 200 is provided, the rotation direction of the circularly polarized light is reversed by passing through the display layer 200, and the selective reflection layer 710 can reflect the circularly polarized light. Therefore, the display layer 200 can be visually recognized as a part that is more reflective than the surrounding area.
[0136] As described above, the display medium 30 according to the present embodiment can contribute to the realization of various display modes. Even when the display modes are diversified in this way, the small fragment layer 220 is difficult to see without magnified observation, so the display medium 30 can increase the difficulty of counterfeiting.
[0137] In the third embodiment, the substrate 700 does not include a colored layer (see the second embodiment), but the substrate 700 may include a colored layer in combination with the selectively reflective layer 710.
[0138] [4. Other embodiments] In the above-mentioned embodiment, an example in which only one display layer is provided on one substrate has been shown and described, but multiple display layers may be provided on one substrate. In addition, the multiple display layers may be the same or different. Therefore, for example, (i) the shape of the display layer as viewed from the thickness direction, (ii) the size of the display layer as viewed from the thickness direction, (iii) the arrangement direction of the small piece layer as viewed from the thickness direction, (iv) the shape of the small piece layer as viewed from the thickness direction, (v) the size of the small piece layer as viewed from the thickness direction, (vi) the thickness of the small piece layer, (vii) the in-plane retardation of the small piece layer, (viii) the wavelength dispersion of the small piece layer, (ix) the type of the small piece layer as a retardation plate, (x) the slow axis direction of the small piece layer, (xi) the display wavelength range of the small piece layer, (xii) the rotation direction D of the circularly polarized light that the small piece layer can reflect. D Elements such as (xiii) the material of the flake layer may be the same or different among multiple display layers.
[0139] Thus, for example, the display medium may have a first display layer including a first group of small fragment layers having a slow axis in a certain direction, and a second display layer including a second group of small fragment layers having a slow axis in a direction non-parallel to the slow axis. Also, for example, the display medium may have a first display layer including a first group of flake layers having a first display wavelength range capable of reflecting circularly polarized light in a certain rotation direction, and a second display layer including a second group of flake layers having a second display wavelength range capable of reflecting circularly polarized light in the opposite rotation direction.
[0140] Furthermore, the display medium may include elements other than those described above, so long as the effects of the present invention are not significantly impaired. For example, the display medium may include a metal reflective layer. Such a metal reflective layer may be provided, for example, between the substrate and the display layer. Furthermore, the metal reflective layer may be provided not only in the area where the display layer is provided, but also in the area where the display layer is not provided.
[0141] For example, the display medium may also include a cover layer that protects each of the above-mentioned layers. These cover layers are preferably provided on the outside of the above-mentioned layers. As a specific example, the display medium may include a cover layer, a substrate, a display layer, and another cover layer in this order in the thickness direction. Such a cover layer may be formed of a transparent material, for example, a resin.
[0142] Furthermore, for example, the display medium may have any layer with small in-plane retardation between the above-mentioned layers and as the outermost layer of the display medium, as long as the effect of the present invention is not significantly impaired. Such any layer with small in-plane retardation may be referred to as a "low Re layer" hereinafter. The specific in-plane retardation of this low Re layer is usually 0 nm or more and 5 nm or less. The low Re layer preferably has high light transmittance, and the total light transmittance of the low Re layer is preferably 80% or more, more preferably 85% or more. Examples of materials for such low Re layers include hard polyvinyl chloride, soft polyvinyl chloride, acrylic resin, glass, polycarbonate (PC), and polyethylene terephthalate (PET). Specific materials can be appropriately selected depending on the use of the display medium, the required texture, durability, and mechanical strength.
[0143] [5.Displayed items] A display article according to one embodiment of the present invention includes a base article and the display medium provided on the base article. By providing the display medium on the support article, the display aspect of the display medium can be imparted to the support article, so that a display article with excellent design can be obtained.
[0144] The support article is an object on which the display medium is provided, and there is no limitation on the scope of the support article. Examples of the support article include, but are not limited to, cloth products such as clothing, leather products such as bags and shoes, metal products such as screws, paper products such as price tags, plastic products such as cards and plastic banknotes, and rubber products such as tires. EXAMPLES
[0145] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto. In the following description, the units "%" and "parts" that represent amounts are by weight unless otherwise specified. Furthermore, the following operations were carried out in air at room temperature and normal pressure unless otherwise specified. In the following description, unless otherwise specified, the commercially available adhesive used was a transparent adhesive tape "LUCIACS CS9621T" (thickness 25 μm, visible light transmittance 90% or more, in-plane retardation 3 nm or less) manufactured by Nitto Denko Corporation.
[0146] [Method of measuring in-plane retardation and slow axis direction] The in-plane retardation and the slow axis direction were measured at a measurement wavelength of 550 nm using a phase difference meter (Axoscan, manufactured by Axometrics).
[0147] [Method of measuring the actual maximum tilt angle] The retardation of the cured liquid crystal layer was measured at a wavelength of 590 nm using a phase difference meter (Axometrics' "AxoScan"). This measurement was performed multiple times by changing the incident angle to the cured liquid crystal layer in the range of -50° to 50°. In each measurement, the measurement direction was set perpendicular to the fast axis of the cured liquid crystal layer.
[0148] From the measured retardation, the substantial maximum tilt angle of the molecules of the liquid crystal compound contained in the cured liquid crystal layer was analyzed using analysis software attached to the phase difference meter (AxoMetrics' analysis software "Multi-Layer Analysis"; analysis conditions were analysis wavelength of 590 nm and number of layers divided into 20 layers).
[0149] [Method for measuring reflectance of cholesteric liquid crystal layer] The temporary support was peeled off from the multilayer member to obtain a liquid crystal cured layer. The reflectance of this liquid crystal cured layer when non-polarized light (wavelength 400 nm to 800 nm) was incident thereon was measured using an ultraviolet-visible spectrophotometer (manufactured by JASCO Corporation, "UV-Vis 550").
[0150] [Manufacturing Example 1: Manufacturing of multi-layered member (Q1)] According to Example 1 of WO 2017 / 057005, a multilayer member (Q1) was produced, which includes a temporary support as a long film formed of a thermoplastic norbornene resin and a liquid crystal cured layer as a positive A plate formed on the temporary support. The in-plane retardation Re of the liquid crystal cured layer was 138 nm, the thickness of the liquid crystal cured layer was 2.3 μm, and the angle of the slow axis of the liquid crystal cured layer with respect to the longitudinal direction of the temporary support was 45°. The liquid crystal cured layer had a reverse wavelength dispersion characteristic in which the in-plane retardation gradually increased as the measured wavelength increased.
[0151] [Manufacturing Example 2: Manufacturing of multi-layered material (Q2)] According to Example 1 of WO 2019 / 188519, a multilayer member (Q2) was produced comprising a temporary support as a long film formed of a thermoplastic norbornene resin and a liquid crystal cured layer as an inclined hybrid alignment plate formed on the temporary support. The in-plane retardation Re of the cured liquid crystal layer was 138 nm, the thickness of the cured liquid crystal layer was 4.0 μm, and the angle of the slow axis of the cured liquid crystal layer with respect to the longitudinal direction of the temporary support was 45 °. In addition, since the actual maximum inclination angle of the cured liquid crystal layer was 63 °, it was confirmed that the optical axis direction of the cured liquid crystal layer was neither parallel nor perpendicular to the layer plane. Furthermore, the cured liquid crystal layer had a reverse wavelength dispersion characteristic in which the in-plane retardation gradually increased as the measured wavelength increased.
[0152] [Manufacturing Example 3: Manufacturing of multi-layered member (Q3)] A multilayer member (Q3) including a temporary support as a long film formed of a thermoplastic norbornene resin and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 1, except that the type of liquid crystal compound was changed to "LC242" manufactured by BASF and the thickness was changed so as to obtain an in-plane retardation capable of functioning as a quarter-wave plate. The in-plane retardation Re of the cured liquid crystal layer was 143 nm, the thickness of the cured liquid crystal layer was 1.2 μm, and the angle of the slow axis of the cured liquid crystal layer with respect to the longitudinal direction of the temporary support was 45 °. The cured liquid crystal layer had a forward wavelength dispersion characteristic in which the in-plane retardation gradually decreased as the measurement wavelength increased.
[0153] [Manufacturing Example 4: Manufacturing of multi-layered member (H1)] A multilayer member (H1) including a temporary support as a long film formed of a thermoplastic norbornene resin and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 3, except that the thickness was changed so as to obtain an in-plane retardation capable of functioning as a 1 / 2 wavelength plate. The in-plane retardation Re of the cured liquid crystal layer was 280 nm, the thickness of the cured liquid crystal layer was 2.4 μm, and the angle of the slow axis of the cured liquid crystal layer with respect to the longitudinal direction of the temporary support was 45°. The cured liquid crystal layer had forward wavelength dispersion characteristics in which the in-plane retardation gradually decreased as the measurement wavelength increased.
[0154] [Manufacturing Example 5: Manufacturing of multi-layered member (H2)] A multilayer member (H2) including a temporary support as a long film formed of a thermoplastic norbornene resin and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 4, except that the type of liquid crystal compound was changed to that shown in the following formula (X1) and the thickness was changed so as to obtain an in-plane retardation capable of functioning as a 1 / 2 wavelength plate. The in-plane retardation Re of the liquid crystal cured layer was 275 nm, the thickness of the liquid crystal cured layer was 1.2 μm, and the angle of the slow axis of the liquid crystal cured layer with respect to the longitudinal direction of the temporary support was 45 °. The liquid crystal cured layer had a forward wavelength dispersion characteristic in which the liquid crystal cured layer gradually decreased as the measurement wavelength increased.
[0155] [ka]
[0156] [Manufacturing Example 6: Manufacturing of multi-layered material (CLC_W)] A liquid crystal composition was prepared by mixing 100 parts of the photopolymerizable liquid crystal compound represented by the above formula (X1), 25 parts of the photopolymerizable non-liquid crystal compound represented by the following formula (X2), 8 parts of a chiral agent ("LC756" manufactured by BASF), 5 parts of a photopolymerization initiator ("Irgacure 907" manufactured by Ciba Japan), 0.15 parts of a surfactant ("S-420" manufactured by AGC Seimi Chemical Co., Ltd.), and 320 parts of cyclopentanone as a solvent.
[0157] [ka]
[0158] A long polyethylene terephthalate film ("A4100" manufactured by Toyobo Co., Ltd.; thickness 100 μm) was prepared as a temporary support. This temporary support was attached to a feeding section of a film transport device, and the following operations were performed while the temporary support was transported in the longitudinal direction.
[0159] The surface of the temporary support was subjected to a rubbing treatment in the longitudinal direction parallel to the transport direction. Next, a liquid crystal composition was applied to the rubbed surface of the temporary support using a die coater to form a layer of the liquid crystal composition. This layer of the liquid crystal composition was subjected to an alignment treatment in which the liquid crystal composition was heated at 120°C for 4 minutes, and aligned so that the liquid crystal composition exhibited a cholesteric liquid crystal phase. Thereafter, the layer of the liquid crystal composition was subjected to a band broadening treatment. In this band broadening treatment, 5 mJ / cm 2 ~30mJ / cm 2 By repeatedly irradiating the film with weak ultraviolet light at 800 mJ / cm and heating the film at 100 to 120 °C, the wavelength range capable of exhibiting the circularly polarized light separation function was controlled to have a desired wavelength width. 2The layer of the liquid crystal composition was irradiated with ultraviolet light of 100 nm to cure the layer of the liquid crystal composition. As a result, a multilayer member (CLC_W) was obtained that included a temporary support and a cured liquid crystal layer having a circularly polarized light separation function. The reflectance of the cured liquid crystal layer of this multilayer member (CLC_W) was measured by the above-mentioned measurement method. As a result of the measurement, the cured liquid crystal layer had a wavelength range of 450 nm to 700 nm in which the reflectance for unpolarized light was 40% or more. The thickness of the cured liquid crystal layer was 5.2 μm.
[0160] [Manufacturing Example 7: Manufacturing of composite material (CLC_R)] A multilayer member (CLC_R) including a temporary support and a liquid crystal cured layer having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 6, except that the amount of the chiral agent (BASF "LC756") was changed to 7 parts and the band-widening treatment was not performed. The reflectance of the liquid crystal cured layer of this multilayer member (CLC_R) was measured by the above-mentioned measurement method. As a result of the measurement, the liquid crystal cured layer had a central wavelength near 650 nm, a half-width of about 20 nm, and a wavelength range in which the reflectance for unpolarized light was 40% or more. When this liquid crystal cured layer was visually observed under natural light, it was visually recognized as red. The thickness of the liquid crystal cured layer was 3.5 μm.
[0161] [Manufacturing Example 8: Manufacturing of multi-layered material (CLC_G)] A multilayer member (CLC_G) including a temporary support and a liquid crystal cured layer having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 6, except that the band-widening treatment was not performed. The reflectance of the liquid crystal cured layer of this multilayer member (CLC_G) was measured by the above-mentioned measurement method. As a result of the measurement, the liquid crystal cured layer had a central wavelength near 550 nm, a half-width of about 20 nm, and a wavelength range in which the reflectance for unpolarized light was 40% or more. When this liquid crystal cured layer was visually observed under natural light, it was visually recognized as green. The thickness of the liquid crystal cured layer was 3.5 μm.
[0162] [Manufacturing Example 9: Manufacturing of multi-layered material (CLC_rG)] A multilayer member (CLC_rG) having a temporary support and a liquid crystal cured layer having a circularly polarized light separation function was produced by the same method as in Production Example 6, except that 16 parts of a compound (X3) represented by the following formula (X3) was used instead of 8 parts of a chiral agent (BASF "LC756"), and that a band-widening treatment was not performed. The reflectance of the liquid crystal cured layer of this multilayer member (CLC_rG) was measured by the above-mentioned measurement method. As a result of the measurement, the liquid crystal cured layer had a central wavelength near 550 nm, a half-width of about 20 nm, and a wavelength range in which the reflectance for unpolarized light was 40% or more. When this liquid crystal cured layer was visually observed under natural light, it was visually recognized as green. The thickness of the liquid crystal cured layer was 3.5 μm.
[0163] [ka] (compound name) D-Mannitol, 1,4:3,6-dihydro-, 2,5-bis[4-[[[6-[[[4-[(1-oxo-2-propen-1-yl)oxy]butoxy]carbonyl]oxy]-2-naphthalenyl]carbonyl]oxy]benzoate]
[0164] [Manufacturing Example 10: Manufacturing of composite material (CLC_B)] A multilayer member (CLC_B) including a temporary support and a liquid crystal cured layer having a circularly polarized light separation function was manufactured by the same method as in Manufacturing Example 6, except that the amount of the chiral agent (BASF "LC756") was changed to 10 parts and the band-widening treatment was not performed. The reflectance of the liquid crystal cured layer of this multilayer member (CLC_B) was measured by the above-mentioned measurement method. As a result of the measurement, the liquid crystal cured layer had a central wavelength near 450 nm, a half-width of about 20 nm, and a wavelength range in which the reflectance for unpolarized light was 40% or more. When this liquid crystal cured layer was visually observed under natural light, it was visually recognized as blue. The thickness of the liquid crystal cured layer was 3.5 μm.
[0165] [Production Example 11: Production of Retardation Film (R1)] A resin film formed from a thermoplastic norbornene resin (ZEONOR film manufactured by Zeon Corporation; a film manufactured by extrusion molding; unstretched product) was prepared. This resin film was stretched in one direction at a stretching temperature of 130°C to obtain a retardation film (R1) having an in-plane retardation capable of functioning as a 1 / 2 wavelength plate. The thickness of this retardation film (R1) was 38 μm, and the in-plane retardation was 280 nm.
[0166] [Production Example 12: Production of Retardation Film (R2)] A retardation film (R2) was produced in the same manner as in Production Example 11, except that the stretching ratio was changed so as to obtain an in-plane retardation capable of functioning as a quarter-wave plate. The thickness of this retardation film (R2) was 47 μm, and the in-plane retardation was 143 nm.
[0167] [Production Example 13: Production of circularly polarized selective reflective film (D)] The retardation film (R2) produced in Production Example 12 was laminated onto a linearly polarized selective reflection film "DBEF" manufactured by 3M Co., Ltd., via a commercially available adhesive, to produce a circularly polarized selective reflection film (D). The lamination was performed by adjusting the direction of the slow axis of the retardation film (R2) so that the circularly polarized selective reflection film (D) could selectively reflect right-handed circularly polarized light.
[0168] [Example 101] (Outline of display media) Fig. 22 is a plan view diagrammatically illustrating the display medium 800 manufactured in Example 101. Fig. 23 is a cross-sectional view diagrammatically illustrating the display medium 800 manufactured in Example 101. 22 and 23, the display medium 800 produced in Example 101 had a display layer 830 on a substrate 810 via an adhesive layer 820. When viewed in the thickness direction, the display layer 830 had a shape of a block letter "T" with a thickness of approximately 7 mm. A method for producing the display medium 800 will be described below.
[0169] (Manufacturing of raw material materials) In the cured liquid crystal layer of the multilayer member (Q1) produced in Production Example 1, a 3 mm square notch was formed by the following cross-cut method. <3mm square cross-cut method> In the 3 mm square cross-cut method, a processing device (TQC's "Cross Cut Adhesion TestKIT CC3000") was used to form multiple linear indentations in the liquid crystal cured layer in accordance with a method conforming to JIS-K5600-5-6. The indentations were formed in two mutually perpendicular directions at 3 mm intervals. The depth of the indentations was adjusted to be deeper than the thickness of the liquid crystal cured layer and not to cut the temporary support completely. The depth of the indentations was adjusted by adjusting the cutting depth of the blade of the processing device.
[0170] By forming the indentations by the 3 mm square cross-cut method, cracks were formed in the liquid crystal cured layer, and many small pieces were obtained, which were divided by the cracks. Thus, a raw material member was obtained, which had a temporary support and a transfer material layer including many small pieces formed on the temporary support. The small pieces were arranged in two mutually perpendicular directions, and both were 3 mm squares when viewed from the thickness direction.
[0171] (Formation of a latent image on the surface of the substrate) A long film (thickness 100 μm) made of thermoplastic norbornene resin was prepared as the substrate. An adhesive layer was formed on the surface of this substrate in an area shaped like the letter "T". Specifically, a commercially available adhesive with adhesive strength was cut into the shape of the letter "T", and this cut adhesive layer was attached to the substrate. As a result, a latent image of the letter "T" was formed by the adhesive layer on the surface of the substrate.
[0172] (Formation of display layer) The substrate on which the latent image was formed and the original fabric member were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the substrate and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. In the area on the substrate where there was no adhesive layer, the small piece layer included in the transfer material layer did not remain on the substrate and was peeled off together with the temporary support. In the area on the substrate where the adhesive layer was formed, the small piece layer included in the transfer material layer remained on the substrate and only the temporary support was peeled off. Thus, on the substrate, a plurality of small piece layers were selectively provided via the adhesive layer in the area of the letter "T" shape where the adhesive layer was formed. Then, as a collection of these small piece layers, a display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, as shown in FIG. 22 and FIG. 23, a display medium 800 was obtained, which includes a substrate 810 and a display layer 830 provided on the substrate 810 via an adhesive layer 820.
[0173] [Example 102] In the process (manufacturing the raw material member), the method for forming indentations in the liquid crystal cured layer was changed from the 3 mm square cross-cut method to the 50 μm square roll press method described below. <50μm square roll press method> In the 50 μm square roll press method, a plurality of linear notches were formed in the liquid crystal cured layer by the method described in Example 1 of International Publication No. 2019 / 189246. The notches were formed at 50 μm intervals in two mutually perpendicular directions. The depth of the notches was adjusted so as to be deeper than the thickness of the liquid crystal cured layer and not to completely cut the temporary support. The depth of the notches was adjusted by adjusting the press pressure. The plurality of small piece layers provided in the raw fabric member obtained by the 50 μm square roll press method were arranged in two mutually perpendicular directions, and each was a 50 μm square when viewed from the thickness direction.
[0174] Except for the above, a display medium including a substrate and a display layer provided on the substrate via an adhesive layer was obtained in the same manner as in Example 101.
[0175] [Example 103] In the process (manufacturing the raw material member), the method for forming indentations in the liquid crystal cured layer was changed from the 3 mm square cross-cut method to the 20 μm square roll press method described below. <20μm square roll press method> In the 20 μm square roll press method, multiple notches were formed in the liquid crystal cured layer by the same method as the 50 μm square roll press method, except that the interval between the notches was changed from 50 μm to 20 μm. The multiple small piece layers of the raw fabric member obtained by the 20 μm square roll press method were arranged in two directions perpendicular to each other, and each was a square with a side of 20 μm when viewed from the thickness direction.
[0176] Except for the above, a display medium including a substrate and a display layer provided on the substrate via an adhesive layer was obtained in the same manner as in Example 101.
[0177] [Example 104] Instead of the multilayer member (Q1) manufactured in Manufacturing Example 1, the multilayer member (Q2) manufactured in Manufacturing Example 2 was used. In addition, in the process (manufacturing the raw material member), the method of forming the indentations in the liquid crystal cured layer was changed from the 3 mm square cross-cut method to the 20 μm square roll press method. A display medium including a substrate and a display layer provided on the substrate via an adhesive layer was obtained by the same method as in Example 101, except for the above.
[0178] [Examples 105 to 112] Instead of the multilayer member (Q1) manufactured in Manufacturing Example 1, the multilayer member shown in Table 1 was used. In addition, in the process (manufacturing the original fabric member), the method of forming the indentations in the liquid crystal cured layer was changed from the 3 mm square cross-cut method to the 50 μm square roll press method. A display medium including a substrate and a display layer provided on the substrate via an adhesive layer was obtained by the same method as in Example 101 except for the above.
[0179] [Comparative Example 1] An adhesive layer was formed on one side of the retardation film (R2) produced in Production Example 12. The retardation film (R2) was then cut out to obtain a film piece having a shape of a block letter "T" with a thickness of approximately 7 mm. The surface of this film piece on the adhesive layer side was bonded to the same substrate as used in Example 101 by batch processing. As a result, a display medium was obtained that had a display layer consisting of the substrate and a film piece of the retardation film (R2) provided on the substrate via an adhesive layer.
[0180] [Comparative Example 2] A display medium was obtained by the same method as in Comparative Example 1, except that the retardation film (R1) produced in Production Example 11 was used instead of the retardation film (R2) produced in Production Example 12, and the display layer was made of a film piece of the retardation film (R1) provided on the substrate via an adhesive layer.
[0181] [Comparative Example 3] A display medium was obtained by the same method as in Comparative Example 1, except that the circularly polarized light selective reflection film (D) produced in Production Example 13 was used instead of the retardation film (R2) produced in Production Example 12, and the display layer was made of a film piece of the circularly polarized light selective reflection film (D) provided on the substrate via an adhesive layer.
[0182] [Summary of the configurations of Examples 101 to 112 and Comparative Examples 1 to 3] The configurations of the above-mentioned Examples 101 to 112 and Comparative Examples 1 to 3 are summarized in the following Table 1. In the following Table 1, the meanings of the abbreviations are as follows. Re: In-plane retardation of the display layer and the platelet layer. Dispersion: Wavelength dispersion of the display layer and the flake layer. Reflected color: The color of circularly polarized light reflected by the display layer and the small piece layer having a circularly polarized light separation function. Reflected polarization: The direction of rotation of the circularly polarized light reflected by the display layer and the small piece layer that have a circularly polarized light separation function. Shape:Plate shape. Size: Width of the strip layer. R: Red. G: Green. B: Blue.
[0183] [Table 1]
[0184] [Observation of display media obtained in Examples 101 to 112 and Comparative Examples 1 to 3] The display media obtained in Examples 101 to 112 and Comparative Examples 1 to 3 were observed by the observation methods 1 to 4 described below.
[0185] (Observation method 1: Transmitted crossed Nicol observation of the display layer) Two commercially available linear polarizing plates were placed on top of each other on a backlight equipped with a fluorescent lamp as a non-polarized light source. The two linear polarizing plates were placed in a crossed Nicol arrangement in which the absorption axes of the two linear polarizing plates were orthogonal to each other when viewed from the thickness direction. The display media obtained in Examples 101 to 105 and Comparative Example 1 were placed between these two linear polarizing plates. The display media were set so that the slow axis direction of the display layer and the slow axis direction of the small piece layer contained in the display layer were at an angle of 45° with respect to the absorption axis of the linear polarizing plate. Thereafter, the backlight was turned on, and the light transmitted through the display medium was observed to determine whether the image on the display layer was visible or invisible.
[0186] (Observation method 2: Transmitted paranic observation of the display layer) Two commercially available linear polarizing plates were placed on top of each other on a backlight equipped with a fluorescent lamp as a non-polarized light source. The two linear polarizing plates were placed in a paranicol arrangement in which the absorption axes of the two linear polarizing plates were parallel to each other when viewed from the thickness direction. The display media obtained in Examples 106 to 107 and Comparative Example 2 were placed between these two linear polarizing plates. The display media were set so that the slow axis direction of the display layer and the slow axis direction of the small piece layer contained in the display layer were at an angle of 45° with respect to the absorption axis of the linear polarizing plate. Thereafter, the backlight was turned on and the light transmitted through the display medium was observed to determine whether the image on the display layer was visible or invisible.
[0187] (Observation method 3: Circularly polarizing plate observation of the display layer) The display media obtained in Examples 108 to 112 and Comparative Example 3 were illuminated with a fluorescent lamp as a non-polarized light source, and the light reflected by the display media was observed. The above observations were performed by (i) observation with the naked eye, (ii) observation through a right circular polarizer, and (iii) observation through a left circular polarizer. As the right and left circular polarizers, glasses-shaped right and left circular polarizers (positive and negative circular polarizers) used for watching 3D television were used. In these observations, it was determined whether the image on the display layer was visible or invisible.
[0188] (Observation method 4: Observation of the small-piece layer) The display layer of the display medium was observed (i) with the naked eye and (ii) with a microscope to determine whether the flake layer contained in the display layer was visible or invisible.
[0189] [Results of Examples 101 to 112 and Comparative Examples 1 to 3] The results of Examples 101 to 112 and Comparative Examples 1 to 3 are shown in Table 2 below.
[0190] [Table 2]
[0191] [Study of Examples 101 to 112 and Comparative Examples 1 to 3] From Tables 1 and 2, the display layers of the display media obtained in Examples 101 to 105 and Comparative Example 1 can be seen in crossed Nicols observation, and the display layers of the display media obtained in Examples 106 to 107 and Comparative Example 2 can be seen in parallel Nicols observation. The display layers of the display media obtained in Examples 108 to 112 and Comparative Example 3 are seen when observed through one of a right circular polarizer and a left circular polarizer, and are invisible when observed through the other. Therefore, it is clear that the use of these display media provides a wide variety of display characteristics.
[0192] Among them, the display media obtained in the examples can be manufactured by a cheap transfer method using a roll-to-roll method, whereas the display media obtained in the comparative examples cannot be manufactured by the roll-to-roll method and require lamination by batch processing, which is disadvantageous in terms of cost.
[0193] In addition, the display media obtained in the examples all contain a small fragment layer with a uniform shape and regular arrangement in the display layer, so the difficulty of manufacturing is improved, and therefore the difficulty of counterfeiting is also improved. In particular, the display layer of the display media obtained in Examples 102 to 112 is not visible to the naked eye, so it is difficult to notice the presence of the small fragment layer. Therefore, a display medium containing such a small fragment layer can particularly improve the difficulty of counterfeiting. This effect of improving the difficulty of counterfeiting is useful because it cannot be obtained with the display media of Comparative Examples 1 to 3 that do not contain a small fragment layer.
[0194] [Example 201] (Manufacture of substrate) A black paper was attached to the temporary support side of the multilayer member (CLC_W) produced in Production Example 6 to form a colored layer, thereby obtaining a long substrate having, in that order, a colored layer, a support layer as a temporary support, and a liquid crystal cured layer having a circular polarization separation function.
[0195] (Formation of a latent image on the surface of the substrate) An adhesive layer was formed in the area of the shape of the letter "T" on the surface of the substrate on the side of the liquid crystal cured layer. As a result, a latent image of the letter "T" was formed on the surface of the substrate by the adhesive layer.
[0196] (Formation of display layer) The substrate on which the latent image was formed and the original web member manufactured in Example 102 were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the substrate and the transfer material layer side of the original web member were laminated by a nip roll. Then, the temporary support of the original web member was peeled off. On the substrate, a plurality of small pieces were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small pieces, a first display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium including the substrate and the first display layer provided on the substrate via the adhesive layer was obtained.
[0197] [Example 202] (Production of raw material member for forming second display layer) A multilayer member (Q1-1) including a temporary support and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 1, except that the stretching direction of the long film used as the temporary support was changed. The in-plane retardation Re of the liquid crystal cured layer was 138 nm, the thickness of the liquid crystal cured layer was 2.3 μm, and the angle of the slow axis of the liquid crystal cured layer with respect to the longitudinal direction of the temporary support was 135 °. The liquid crystal cured layer had a reverse wavelength dispersion characteristic in which the in-plane retardation gradually increased as the measurement wavelength increased.
[0198] A 50 μm square roll press method was used to form notches in the liquid crystal cured layer of this multilayer member (Q1-1), to obtain a raw material member having a temporary support and a transfer material layer including a large number of small chip layers formed on this temporary support.
[0199] (Formation of a latent image for a second display layer on the surface of a substrate) A display medium was manufactured in the same manner as in Example 201. An adhesive layer was formed in an area shaped like the letter "T" on the surface of the first display layer side of the substrate included in this display medium. At this time, the adhesive layer was formed so as not to overlap with the first display layer. As a result, a latent image for the second display layer was formed by the adhesive layer on the surface of the substrate.
[0200] (Formation of second display layer) The display medium on which the latent image for the second display layer was formed and the original fabric member were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the display medium and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. On the substrate, a plurality of small piece layers were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small piece layers, a second display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium was obtained that includes a long substrate having a color layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function in this order, and a first display layer and a second display layer provided on the substrate via an adhesive layer.
[0201] [Example 203] (Production of raw material member for forming third display layer) A multilayer member (Q1-2) including a temporary support and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 1, except that the stretching direction of the long film used as the temporary support was changed. The in-plane retardation Re of the liquid crystal cured layer was 138 nm, the thickness of the liquid crystal cured layer was 2.3 μm, and the angle of the slow axis of the liquid crystal cured layer with respect to the longitudinal direction of the temporary support was 180°. The liquid crystal cured layer had a reverse wavelength dispersion characteristic in which the in-plane retardation gradually increased as the measurement wavelength increased.
[0202] A 50 μm square roll press method was used to form notches in the liquid crystal cured layer of this multilayer member (Q1-2), to obtain a raw material member having a temporary support and a transfer material layer including a large number of small chip layers formed on this temporary support.
[0203] (Formation of a latent image for a third display layer on the surface of a substrate) A display medium was manufactured in the same manner as in Example 202. An adhesive layer was formed in an area shaped like the letter "T" on the surface of the first display layer side of the substrate included in this display medium. At this time, the adhesive layer was formed so as not to overlap the first display layer and the second display layer. As a result, a latent image for the third display layer was formed on the surface of the substrate by the adhesive layer.
[0204] (Formation of the third display layer) The display medium on which the latent image for the third display layer was formed and the original fabric member were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the display medium and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. On the substrate, a plurality of small piece layers were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small piece layers, a third display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium was obtained that includes a long substrate having a color layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function in this order, and a first display layer, a second display layer, and a third display layer provided on the substrate via an adhesive layer.
[0205] [Example 204] Except for using the original fabric material produced in Example 106 instead of the original fabric material produced in Example 102, the same method as in Example 201 was used to obtain a display medium comprising a long substrate having, in that order, a colored layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function, and a first display layer provided on this substrate via an adhesive layer.
[0206] [Example 205] (Production of raw material member for forming second display layer) A multilayer member (H1-1) including a temporary support and a liquid crystal cured layer formed on the temporary support was produced by the same method as in Production Example 4, except that the stretching direction of the long film used as the temporary support was changed. The in-plane retardation Re of the liquid crystal cured layer was 280 nm, the thickness of the liquid crystal cured layer was 2.4 μm, and the angle of the slow axis of the liquid crystal cured layer with respect to the longitudinal direction of the temporary support was 135 °. The liquid crystal cured layer had forward wavelength dispersion characteristics in which the in-plane retardation gradually decreased as the measurement wavelength increased.
[0207] A notch was formed in the liquid crystal cured layer of this multilayer member (H1-1) by a 50 μm square roll press method to obtain a raw material member having a temporary support and a transfer material layer including a large number of small chip layers formed on this temporary support.
[0208] (Formation of a latent image for a second display layer on the surface of a substrate) A display medium was manufactured in the same manner as in Example 204. An adhesive layer was formed in the area shaped like the letter "T" on the surface of the first display layer side of the substrate included in this display medium. At this time, the adhesive layer was formed so as not to overlap with the first display layer. As a result, a latent image for the second display layer was formed by the adhesive layer on the surface of the substrate.
[0209] (Formation of second display layer) The display medium on which the latent image for the second display layer was formed and the original fabric member were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the display medium and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. On the substrate, a plurality of small piece layers were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small piece layers, a second display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium was obtained that includes a long substrate having a color layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function in this order, and a first display layer and a second display layer provided on the substrate via an adhesive layer.
[0210] [Example 206] Except for using the original web material produced in Example 102 as the original web material for the second display layer, the same method as in Example 205 was used to obtain a display medium comprising a long substrate having, in that order, a colored layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function, and a first display layer and a second display layer provided on this substrate via an adhesive layer.
[0211] [Example 207] (Manufacture of substrate) A black paper was attached to one side of a long optically isotropic film (thickness 100 μm) made of a thermoplastic norbornene resin to form a colored layer, thereby obtaining a long substrate comprising a colored layer and a film layer.
[0212] (Formation of a latent image on the surface of the substrate) An adhesive layer was formed on the surface of the substrate on the film layer side in an area shaped like the letter "T." As a result, a latent image of the letter "T" was formed on the surface of the substrate by the adhesive layer.
[0213] (Formation of display layer) The substrate on which the latent image was formed and the original web member produced in Example 109 were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the substrate and the transfer material layer side of the original web member were laminated by a nip roll. Then, the temporary support of the original web member was peeled off. On the substrate, a plurality of small pieces were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small pieces, a first display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium including the substrate and the first display layer provided on the substrate via the adhesive layer was obtained.
[0214] [Example 208] (Formation of a latent image for a second display layer on the surface of a substrate) A display medium was manufactured in the same manner as in Example 207. An adhesive layer was formed in an area shaped like the letter "T" on the surface of the substrate of this display medium on the side of the first display layer. At this time, the adhesive layer was formed so as not to overlap with the first display layer. As a result, a latent image for the second display layer was formed on the surface of the substrate by the adhesive layer.
[0215] (Formation of second display layer) The display medium on which the latent image for the second display layer was formed and the original fabric member manufactured in Example 110 were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the display medium and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. On the substrate, a plurality of small pieces were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small pieces, a second display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium was obtained that had a long substrate having a color layer and a film layer, and a first display layer and a second display layer provided on the substrate via an adhesive layer.
[0216] [Example 209] A display medium was obtained by the same method as in Example 207, except that the raw fabric member produced in Example 112 was used instead of the raw fabric member produced in Example 109, and the display medium was provided with a long substrate having a colored layer and a film layer, and a first display layer provided on this substrate via an adhesive layer.
[0217] [Example 210] (Formation of a latent image for a second display layer on the surface of a substrate) A display medium was manufactured in the same manner as in Example 209. An adhesive layer was formed in an area shaped like the letter "T" on the surface of the substrate of this display medium on the side of the first display layer. At this time, the adhesive layer was formed so as not to overlap with the first display layer. As a result, a latent image for the second display layer was formed on the surface of the substrate by the adhesive layer.
[0218] (Formation of second display layer) The display medium on which the latent image for the second display layer was formed and the original fabric member manufactured in Example 110 were laminated by the roll-to-roll method while being transported in the longitudinal direction. Specifically, the adhesive layer side of the display medium and the transfer material layer side of the original fabric member were laminated by a nip roll. Then, the temporary support of the original fabric member was peeled off. On the substrate, a plurality of small pieces were selectively provided via the adhesive layer in the area of the shape of the letter "T" where the adhesive layer was formed. Then, as a collection of these small pieces, a second display layer having the shape of the letter "T" when viewed from the thickness direction was formed. As a result, a display medium was obtained that had a long substrate having a color layer and a film layer, and a first display layer and a second display layer provided on the substrate via an adhesive layer.
[0219] [Example 211] Except for using the original fabric material produced in Example 105 instead of the original fabric material produced in Example 102, the same method as in Example 201 was used to obtain a display medium comprising a long substrate having, in that order, a colored layer, a temporary support, and a liquid crystal cured layer having a circularly polarized light separation function, and a first display layer provided on this substrate via an adhesive layer.
[0220] [Example 212] Except for using the original fabric material produced in Example 104 instead of the original fabric material produced in Example 102, the same method as in Example 201 was used to obtain a display medium comprising a long substrate having, in that order, a colored layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function, and a first display layer provided on this substrate via an adhesive layer.
[0221] [Comparative Example 4] An adhesive layer was formed on one side of the retardation film (R2) produced in Production Example 12. The retardation film (R2) was then cut out to obtain a film piece having a shape of a block letter "T" with a thickness of approximately 7 mm. The surface of this film piece on the adhesive layer side and the substrate produced in Example 201 were bonded together by batch processing. As a result, a display medium was obtained that had a substrate having a colored layer, a temporary support, and a liquid crystal cured layer having a circularly polarized light separation function in this order, and a first display layer consisting of a film piece of the retardation film (R2) provided on the substrate via an adhesive layer.
[0222] [Comparative Example 5] Except for using the retardation film (R1) produced in Production Example 11 instead of the retardation film (R2) produced in Production Example 12, a display medium was obtained in the same manner as in Comparative Example 4, which included a substrate having, in this order, a colored layer, a temporary support, and a liquid crystal cured layer having a circular polarization separation function, and a first display layer consisting of a film piece of the retardation film (R1) provided on the substrate via an adhesive layer.
[0223] [Comparative Example 6] An adhesive layer was formed on one side of the circularly polarized selective reflection film (D) produced in Production Example 13. The circularly polarized selective reflection film (D) was then cut out to obtain a film piece having a shape of a block letter "T" with a thickness of approximately 7 mm. The surface of this film piece on the adhesive layer side was bonded to the substrate produced in Example 207 by batch processing. This resulted in a display medium comprising a substrate having a colored layer and a film layer, and a first display layer consisting of a film piece of the circularly polarized selective reflection film (D) provided on the substrate via an adhesive layer.
[0224] [Summary of the configurations of Examples 201 to 212 and Comparative Examples 4 to 6] The configurations of the above-mentioned Examples 201 to 212 and Comparative Examples 4 to 6 are summarized in the following Table 3. In the following Table 3, the meanings of the abbreviations are as follows. CLC: A liquid crystal layer with a circularly polarized light separation function. Re: In-plane retardation of the display layer and the platelet layer. Dispersion: Wavelength dispersion of the display layer and the flake layer. θ: the angle that the slow axes of the display layer and the flake layer make with respect to the longitudinal direction of the substrate. Color: The color of the circularly polarized light reflected by the display layer and the flake layer having a circularly polarized light separation function. Reflected polarization: The direction of rotation of the circularly polarized light reflected by the display layer and the small piece layer that have a circularly polarized light separation function.
[0225] [Table 3]
[0226] [Observation of display media obtained in Examples 201 to 212 and Comparative Examples 4 to 6] The display media obtained in Examples 201 to 212 and Comparative Examples 4 to 6 were observed by the observation methods 5 to 8 described below.
[0227] (Observation method 5: Naked eye observation of the display layer) The display media obtained in Examples 201 to 212 and Comparative Examples 4 to 6 were illuminated with a fluorescent lamp as a non-polarized light source, and the light reflected by the display media was observed with the naked eye. During the observation, it was determined whether the image on the display layer was visible or invisible.
[0228] (Observation method 6: Observing the display layer with polarized sunglasses) The display media obtained in Examples 201 to 206, 211, and 212 and Comparative Examples 4 to 5 were rotated around the axis of rotation in the thickness direction while being illuminated with a fluorescent lamp as a non-polarized light source, and the light reflected by the display medium was observed through a linear polarizer. Commercially available polarized sunglasses were used as the linear polarizer. During the observation, it was determined whether the image on the display layer was visible or invisible. If it was visible at one or more rotation angles, it was determined to be "visible," and if it was not visible at any rotation angle, it was determined to be "invisible."
[0229] (Observation method 7: Observation of the display layer under polarized light irradiation) The display media obtained in Examples 201 to 203, 211 and 212 and Comparative Example 4 were illuminated with linearly polarized light, and the light reflected by the display medium was observed with the naked eye. During the observation, the color of the display layer was judged.
[0230] (Observation method 8: Circularly polarizing plate observation of the display layer) The display media obtained in Examples 204 to 210 and Comparative Examples 5 to 6 were illuminated with a fluorescent lamp as a non-polarized light source, and the light reflected by the display media was observed. The above observations were performed by (i) observing through a right circular polarizer and (ii) observing through a left circular polarizer. As the right and left circular polarizers, glasses-shaped right and left circular polarizers (positive and negative circular polarizers) used for watching 3D television were used. In these observations, it was determined whether the image on the display layer was visible or invisible.
[0231] (Observation method 9: Observation of the small-piece layer) The display layer of the display medium was observed (i) with the naked eye and (ii) with a microscope to determine whether the flake layer contained in the display layer was visible or invisible.
[0232] [Results of Examples 201 to 212 and Comparative Examples 4 to 6] The results of Examples 201 to 212 and Comparative Examples 4 to 6 are shown in Table 4 below. In the columns of "Naked Eyes", "Polarized Sunglasses", "Right Circular Polarizer" and "Left Circular Polarizer" in Table 4, the symbols "I", "II" and "III" indicate that the first display layer, the second display layer and the third display layer were visible, respectively. In addition, in Table 4 below, it is determined that the image of the display layer was visible not only when the image of the display layer was visible because the reflected light from the display layer was visible, but also when the image of the display layer was visible because the reflected light from the display layer was not visible or was only weakly visible while the strong reflected light from the base material in the area without the display layer was visible.
[0233] [Table 4]
[0234] [Study of Examples 201 to 212 and Comparative Examples 4 to 6] From Tables 3 and 4, it is understood that Examples 201 to 203, Examples 206, and Examples 211 to 212, and Comparative Example 4 can be made visible when observed through polarized sunglasses. It was also found that these samples can be made visible to the naked eye when irradiated with polarized light emitted from a liquid crystal display and a smartphone screen.
[0235] In comparing Example 201 and Example 211, it was found that the visible color varies depending on whether the wavelength dispersion of the flake layer contained in the display layer is reverse wavelength dispersion or forward wavelength dispersion.
[0236] Comparing Example 201 and Example 212, it was found that the image viewed can be given different variations for each observation direction depending on the angle (tilt angle) that the optical axis direction of the small fragment layer contained in the display layer makes with respect to the layer plane.
[0237] It was found that in Examples 204 to 205, Examples 207 to 210, and Comparative Examples 5 to 6, the images became visible or switched between visible and invisible when observed through a circular polarizing plate.
[0238] From these series of examples, it is clear that various display modes can be realized by changing the observation method. In addition, the display layer of the example sample contains a small piece layer that is not included in the display layer of the comparative example sample. It can be understood that this small piece layer can improve the difficulty of counterfeiting. [Explanation of symbols]
[0239] 10 Display media 20 Display media 30 Display media 100 Base material 110 Support layer Surface of 100U substrate 200 display layer 210 Crack 211 Notch 212 Notch 220 Small piece layer 300 Raw material 310 Temporary Support 310U Surface of temporary support 320 Transfer material layer 320U Surface of transfer material layer 330 Small piece layer 340 Crack 340C Crack tip 341 Notch 342 Notch 350 Composite Materials 360 material layers 360U Material layer side of composite member 400 Processing tools 410 Convex part of processing tool 410T Apex of the convex part 420 Tool recess 430 Tool ends 440 Tool ends 450 Supports 500 Processing tools 510 Convex part of processing tool 520 Tool recess 530 Tool ends 540 Tool ends 550 Supports 600 Base material 610 Colored layer 700 Base material 710 Selective Reflection Layer 800 Display media 810 Base material 820 Adhesive layer 830 Display layer
Claims
1. A substrate and a display layer provided on the substrate, the display layer includes a plurality of flake layers separated by cracks; The plurality of small piece layers are arranged side by side in two or more directions as viewed in the thickness direction, A display medium, wherein each small piece layer included in the display layer has the same shape when viewed in the thickness direction.
2. The display medium according to claim 1 , wherein the flake layer has a thickness of 10 μm or less.
3. 3. The display medium according to claim 1, wherein the flake layer is formed of a cured liquid crystal composition.
4. The in-plane retardation of the platelet layer at a measurement wavelength of 550 nm is "{(2n 1 +1) / 4}×550nm-30nm” or more, “{(2n 1 +1) / 4}×550 nm+30 nm (where n 1 represents an integer of 0 or more. The display medium according to any one of claims 1 to 3.
5. The in-plane retardation of the platelet layer at a measurement wavelength of 550 nm is "{(2n 2 +1) / 2}×550nm-30nm” or more, “{(2n 2 +1) / 2}×550 nm+30 nm (where n 2 represents an integer of 0 or more. The display medium according to any one of claims 1 to 3.
6. 6. The display medium according to claim 1, wherein the flake layer is one or more selected from the group consisting of a positive A plate, a positive C plate, a tilted O plate, and a tilted hybrid alignment plate.
7. The small piece layer is rotated in one direction D D 4. The display medium according to claim 1, having a display wavelength range capable of reflecting circularly polarized light having a rotation direction of 1 and transmitting circularly polarized light having an opposite rotation direction.
8. The substrate is rotated in one direction D S 8. The display medium according to claim 1, further comprising a selective reflection layer having a substrate reflection range capable of reflecting circularly polarized light in one direction and transmitting circularly polarized light in the opposite direction.
9. The substrate is rotated in one direction D S a selective reflection layer having a substrate reflection range capable of reflecting circularly polarized light having a rotation direction of 1 and transmitting circularly polarized light having an opposite rotation direction; The display medium according to claim 7 , wherein a wavelength width of the substrate reflection range is wider than a wavelength width of the display wavelength range.
10. 10. The display medium according to claim 8, wherein the wavelength width of the substrate reflection range is 70 nm or more.
11. The display medium according to claim 1 , comprising a plurality of the display layers.
12. The display medium according to any one of claims 1 to 11, wherein the small fragment layer has a rectangular shape when viewed in the thickness direction.
13. The display medium according to any one of claims 1 to 12, wherein the width of the small fragment layer as viewed in the thickness direction is 100 µm or less.
14. The display medium according to any one of claims 1 to 13, wherein the substrate has a colored layer.
15. The display medium according to any one of claims 1 to 14, further comprising an adhesive layer between the substrate and the display layer.
16. A method for producing the display medium according to any one of claims 1 to 15, comprising the steps of: A step of preparing a web member including a temporary support and a transfer material layer formed on the temporary support and including the small particle layer; forming an adhesive layer on the substrate, the adhesive layer having the same shape as the display layer when viewed in a thickness direction; a step of bonding the transfer material layer and the adhesive layer; A step of peeling off the temporary support; A method for manufacturing a display medium, comprising:
17. A display article comprising a base article and the display medium according to any one of claims 1 to 15 provided on the base article.
Citation Information
Patent Citations
Patch transferring medium
JP2010105327A
Forgery prevention medium, method for producing the same, and adhesive label and transfer foil having the forgery prevention medium
JP2011128270A
Forgery prevention medium and manufacturing method thereof, and adhesive label having the forgery prevention medium
JP2012083655A
Identification medium, method of identifying articles, and laminated structure body
JP2014174471A
Crack printed or coated article and manufacturing method therefor
JP2016210005A