Laser damage resistance evaluation method for paramagnetic garnet-type transparent ceramics

Paramagnetic garnet-type transparent ceramics with specific compositions address the vulnerability of terbium-containing aluminum garnet ceramics to laser damage by enhancing laser damage resistance and thermal stability, enabling their use in high-power laser processing machines through non-destructive luminescence lifetime evaluation.

JP7567920B2Active Publication Date: 2024-10-16SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022547489
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-09
Filing Date
2021-08-26
Publication Date
2024-10-16
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

Existing Faraday rotators in optical isolators, particularly those made from terbium-containing aluminum garnet ceramics, are prone to damage from high-power pulsed lasers due to absorption and scattering, which affects their laser damage threshold and thermal stability, making them unsuitable for high-power laser processing machines.

Method used

Development of paramagnetic garnet-type transparent ceramics with specific compositions, such as (Tb1-x-yYxScy)3(Al1-zScz)5O12, characterized by a luminescence lifetime of 346 μs or more for Tb(III) ions, which allows for non-destructive evaluation of laser damage resistance through luminescence lifetime measurement, ensuring high laser damage thresholds and reduced thermal lens effects.

Benefits of technology

The paramagnetic garnet-type transparent ceramics exhibit a laser damage threshold of 10 J/cm² at 1,064 nm and 5 ns, suitable for constructing optical isolators with improved durability and performance in high-power laser environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567920000004
    Figure 0007567920000004
  • Figure 0007567920000001
    Figure 0007567920000001
  • Figure 0007567920000002
    Figure 0007567920000002
Patent Text Reader

Abstract

A TAG-, TYAG- or TYSAG-based paramagnetic garnet-type transparent ceramic exhibiting a high laser damage threshold, said ceramic being characterized by comprising a sintered body of a garnet-type complex oxide represented by formula (1), wherein the luminescence lifetime from the 5D4→7F5 transition of the Tb(III) ions contained in the sintered body is 346 µs or longer. Formula (1): (Tb1-x-yYxScy)3(Al1-zScz)5O12 (In the formula, 0≤x<0.45, 0≤y<0.08, 0≤z<0.16, and 0.001<y+z<0.20.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a paramagnetic garnet-type transparent ceramic having transparency in the visible and / or near infrared range. Laser damage resistance assessment method More specifically, the present invention relates to a paramagnetic garnet-type transparent ceramic material containing terbium that is suitable for forming magneto-optical devices such as optical isolators. Laser damage resistance assessment method Regarding. [Background technology]

[0002] Industrial laser processing machines are equipped with optical isolators to prevent the return of light, such as reflected light, and inside these machines terbium-doped glass or terbium gallium garnet crystals (TGG crystals) are installed as Faraday rotators (for example, JP 2011-213552 A (Patent Document 1)). The magnitude of the Faraday effect is quantified by the Verdet constant, and the Verdet constant of TGG crystals is 40 rad / (T·m) (0.13 min / (Oe·cm)), while that of terbium-doped glass is 0.098 min / (Oe·cm). Since the Verdet constant of TGG crystals is relatively large, they are widely used as standard Faraday rotators. Another example is terbium aluminum garnet crystal (TAG crystal). The Verdet constant of TAG crystal is about 1.3 times that of TGG crystal, which allows the length of the Faraday rotator to be shortened, making it a good crystal that can be used in fiber lasers (for example, JP 2002-293693 A (Patent Document 2), Patent No. 4107292 A (Patent Document 3)).

[0003] In recent years, methods for producing TAG from transparent ceramics have been disclosed (for example, International Publication No. 2017 / 033618 (Patent Document 4) and “High Verdet constant of Ti-doped terbium aluminum garnet (TAG) ceramics” (Non-Patent Document 1)). In addition, a part of terbium was replaced with yttrium (Tb x Y 1-x )3AlO 12The fabrication method of transparent ceramics (0.2≦x≦0.8, or 0.5≦x≦1.0) (YTAG) has also been reported (see, for example, “Fabrication and properties of (Tb x Y 1-x )3AlO 12 "Transparent ceramics by hot isostatic pressing" (Non-Patent Document 2), "Development of optical grade (Tb x Y 1-x )3AlO 12 Rare earth aluminum garnet containing Tb exhibits higher thermal conductivity than TGG, and is therefore expected to become a Faraday element with a smaller thermal lens effect.

[0004] As mentioned above, TAG-based transparent ceramics are expected to have a small thermal lens effect, but if absorption occurs at the wavelength used due to the inclusion of impurities or an inappropriate manufacturing process, a thermal lens effect corresponding to the amount of heat generated will occur, and the material's original potential will not be realized. Due to the increasing power of pulsed laser processing machines in recent years, even small absorption of less than 0.1% / cm can lead to heat generation, so managing minute absorption is essential to provide an excellent optical isolator with a small thermal lens effect.

[0005] Furthermore, in recent years, the high power and short pulse of pulsed lasers has often caused problems such as damage to the Faraday rotator due to the transmission of high power density laser light. "Optical properties and Faraday effect of ceramic terbium gallium garnet for a room temperature Faraday rotator" (Non-Patent Document 4) shows information on the laser damage threshold of TGG single crystal and TGG transparent ceramics by pulsed laser light with a wavelength of 1,064 nm. If the Faraday rotator is damaged, the transmittance, isolation, and beam quality will deteriorate, and in the worst case, the optical isolator will break down. Possible optical damage caused by pulsed lasers include ionization due to multiphoton absorption, electron avalanche collapse, and absorption by impurities. In particular, materials with a large absorption coefficient tend to have high laser damage resistance, so management of absorption is important in order to provide a Faraday rotator with a high laser damage threshold.

[0006] The simplest method for measuring the amount of absorption is to measure the transmittance, but the transmittance of transparent ceramics is a value that reflects absorption and scattering (and reflection). Because transparent ceramics contain many scattering sources, it can be difficult to accurately determine the amount of absorption, even if it is very small, from the transmittance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-213552 A [Patent Document 2] JP 2002-293693 A [Patent Document 3] Patent No. 4107292 [Patent Document 4] International Publication No. 2017 / 033618 [Non-patent literature]

[0008] [Non-Patent Document 1] “High Verdet constant of Ti-doped terbium aluminum garnet (TAG) ceramics”, Optical Materials Express, Vol. 6, No. 1 191-196 (2016) [Non-Patent Document 2] “Fabrication and properties of (TbxY1-x)3Al5O12 transparent ceramics by hot isostatic pressing”, Optical Materials, 72 58-62 (2017) [Non-Patent Document 3] “Development of optical grade (TbxY1-x)3Al5O12 ceramics as Faraday rotator material”, Journal of American Ceramics Society, 100, 4081-4087 (2017) [Non-Patent Document 4] “Optical properties and Faraday effect of ceramic terbium gallium garnet for a room temperature Faraday rotator”, Optical Materials Express, Vol. 19, No. 16 15181-15187 (2011) [Non-Patent Document 5] “Wavelength Dependence of Laser-Induced Damage: Determining the Damage Initiation Mechanisms”, Physical Review Letters, 91, 127402 (2003) Summary of the Invention [Problem to be solved by the invention]

[0009] As described above, with the trend toward higher power and shorter pulses in pulsed laser processing machines, Faraday rotators with high laser damage thresholds are required. However, when we tested an optical isolator equipped with a Faraday rotator made of Tb-containing aluminum garnet fabricated according to the previous literature, we encountered a problem in which the Faraday rotator was damaged when irradiated with a certain high-power pulsed laser.

[0010] By the way, Tb-containing rare earth aluminum garnets, which have Tb(III) ions as a constituent element, also emit green light due to terbium(III) ions when excited. When Tb-containing rare earth aluminum garnets are used as luminescent materials, it is important that the emission wavelength does not overlap with the absorption bands of other elements in order to increase the luminescence efficiency. For example, ions of first transition metals often have dd transition absorption or charge transfer absorption bands with oxide ions in the visible range, so if they are included as impurities in Tb-containing rare earth aluminum garnets, the emission of Tb ions is reabsorbed by the impurity ions, inhibiting the emission. In addition, when metal oxides are exposed to high temperatures and low oxygen partial pressure, oxygen is removed and defects are formed. Metal oxides with such oxide ion defects often exhibit a gray to black color, which also inhibits the emission of Tb ions. As mentioned above, Tb-containing rare earth aluminum garnets with few colored impurity ions and few lattice defects in the lattice of the garnets themselves are excellent luminescent materials.

[0011] Luminescence efficiency (or luminescence quantum yield) is an index that indicates whether a substance emits strong light, and its value is determined by the ratio of the rate constant of the radiative transition from the lowest excited state accompanied by light emission to the rate constant of the non-radiative transition without light emission. Specifically, it is defined as the probability that the excited state returns to the ground state by a radiative transition. If the lifetime of the excited state (the time until the number of excited states decreases to 1 / e) is τ, there is a proportional relationship between the luminescence quantum yield and the lifetime of the excited state. In other words, if the Tb-containing rare earth aluminum garnet has the same composition, the amount of impurity ions and defects that cause quenching (non-radiative transition) can be indirectly estimated by measuring the lifetime of the excited state. In addition, since luminescence is a phenomenon that occurs within the crystals of the base material, it is not easily affected by scattering that is unique to ceramics.

[0012] The present invention has been made in view of the above circumstances, and provides a paramagnetic garnet-type transparent ceramic material having a high laser damage threshold, such as a TAG-based, a TYAG-based, or a TYSAG-based material. Laser damage resistance assessment method The purpose is to provide. [Means for solving the problem]

[0013] As mentioned above, it has been difficult to separate the scattering and the absorption that is the cause of the optical loss in Faraday rotators using transparent ceramics. In addition, since testing for laser damage involves destruction of the sample, a non-destructive, indirect evaluation method was required. Therefore, although the emission intensity of the light emitter and the laser damage of the Faraday rotator are essentially completely unrelated phenomena, the inventors of the present invention have conducted a study on the absorption of Tb(III) ions in Tb-containing rare earth aluminum garnets (TAG, TYAG, or TYSAG). 5 D4 → 7 As a result of thorough investigation of the luminescence lifetime derived from the F5 transition and the laser damage threshold as a Faraday rotator, it was found that Tb-containing rare earth aluminum garnet (paramagnetic garnet-type transparent ceramics) with a long luminescence lifetime has a high laser damage threshold, while Tb-containing rare earth aluminum garnet (paramagnetic garnet-type transparent ceramics) with a short luminescence lifetime has a low laser damage threshold. In other words, the Tb(III) ion in paramagnetic garnet-type transparent ceramics 5 D4 →7 It was discovered that there is a correlation between the luminescence lifetime derived from the F5 transition and the laser damage threshold. In addition, it was discovered that since the luminescence lifetime can be measured non-destructively, it is possible to easily evaluate the laser damage resistance of a Faraday rotator. Based on these findings, the inventors have conducted extensive research and have completed the present invention.

[0014] That is, the present invention provides the following paramagnetic garnet-type transparent ceramics: Laser damage resistance assessment method to provide. 1. The following formula ( 1’ The sintered body of the garnet-type composite oxide represented by Paramagnetic garnet-type transparent ceramics The Tb(III) ions contained in the sintered body 5 D4 → 7 The lifetime of the emission due to the F5 transition is more than 346 μs. At this time, the damage threshold of a laser with a wavelength of 1,064 nm and a pulse width of 5 ns is 10 J / cm 2 It is judged to have a laser damage resistance of or above Paramagnetic garnet-type transparent ceramics characterized by Laser damage resistance assessment method . (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 ( 1’ ) (In the formula, 0≦x<0.45, 0≦y<0.08, 0≦z<0.1 In 6 be.) 2 . The strongest emission intensity due to excitation light with a wavelength of 350 nm is between 500 and 600 nm. 1 to Paramagnetic garnet-type transparent ceramics described Laser damage resistance assessment method . 3 . The sintered body further contains a sintering aid. or 2 Paramagnetic garnet-type transparent ceramics according to Laser damage resistance assessment method . 4 . The above sintered body is subjected to HIP treatment and further annealing treatment in an oxidizing atmosphere. 3 The paramagnetic garnet-type transparent ceramic according to any one of claims 1 to 5, Laser damage resistance assessment method . 5 . The titanium content in the sintered body is less than 2,000 ppm. 4 The paramagnetic garnet-type transparent ceramic according to any one of claims 1 to 5, Laser damage resistance assessment method . Effect of the Invention

[0015] According to the present invention, the radiation dose is 10 J / cm at a wavelength of 1,064 nm and a pulse width of 5 ns. 2 It is possible to provide paramagnetic garnet-type transparent ceramics having a laser damage threshold of or above this value, which are suitable for forming magneto-optical devices such as optical isolators. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view showing an example of the configuration of an optical isolator using the paramagnetic garnet-type transparent ceramic according to the present invention as a Faraday rotator. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Paramagnetic garnet-type transparent ceramics] The paramagnetic garnet-type transparent ceramics according to the present invention will now be described. The paramagnetic garnet-type transparent ceramic according to the present invention is made of a sintered body of a garnet-type composite oxide represented by the following formula (1), and the Tb(III) ions contained in the sintered body 5 D4 → 7 It is characterized by the lifetime of the emission derived from the F5 transition being 346 μs or more. (T 1-x-y Y x Sc y )3(Al 1-z Sc z )5O 12 (1) (In the formula, 0≦x<0.45, 0≦y<0.08, 0≦z<0.16, 0.001 <y+z<0.20である。)

[0018] In the garnet crystal structure represented by formula (1), the site mainly occupied by Tb, i.e., the first half of the brackets in formula (1), is referred to as the A site, and the site mainly occupied by Al, i.e., the second half of the brackets in formula (1), is referred to as the B site.

[0019] In the A site of formula (1), terbium (Tb) is an element with the largest Verdet constant among trivalent rare earth ions, and has extremely low absorption in the 1,070 nm region (wavelength band 0.9 μm to 1.1 μm) used in fiber lasers, making it the most suitable element for use as an optical isolator material in this wavelength range. However, Tb(III) ions are easily oxidized to produce Tb(IV) ions. When Tb(IV) ions are produced in metal oxides, they absorb light over a wide range of wavelengths from ultraviolet to near infrared, so it is desirable to eliminate them as much as possible. One strategy to prevent the generation of Tb(IV) ions is to adopt a crystal structure in which Tb(IV) ions are unstable, i.e., a garnet structure.

[0020] Yttrium (Y) has an ionic radius about 2% smaller than that of terbium, and when it combines with aluminum to form a composite oxide, it is a material that can stably form a garnet phase rather than a perovskite phase and reduce residual strain in the crystallite, which can prevent scattering due to different phases, deterioration of the extinction ratio due to internal stress, and ff transition absorption of terbium ions, making it an important constituent element in the present invention.Furthermore, by replacing a part of the terbium ions with yttrium ions, the sinterability is leveled, making it possible to limit the amount of remaining pores in the ceramic sintered body to 1 ppm or less, making it an element that can be preferably used in the present invention.

[0021] In the B site of formula (1), aluminum (Al) is a material having the smallest ionic radius among trivalent ions that can exist stably in an oxide having a garnet structure, and is an element that can minimize the lattice constant of a paramagnetic garnet-type oxide containing Tb. If the lattice constant of the garnet structure can be reduced without changing the content of Tb, it is preferable because the Verdet constant per unit length can be increased. Furthermore, since aluminum is a light metal, it has weak diamagnetism compared to gallium, and is expected to have the effect of relatively increasing the magnetic flux density generated inside the Faraday rotator, which is also preferable because it can increase the Verdet constant per unit length. In fact, the Verdet constant of TAG ceramics is improved to 1.25 to 1.5 times that of TGG. Therefore, even if the relative concentration of terbium is reduced by replacing some of the terbium ions with yttrium ions, it is possible to keep the Verdet constant per unit length equal to or slightly lower than that of TGG, so it is a suitable constituent element in the present invention.

[0022] Here, a composite oxide whose constituent elements are only Tb, Y and Al may not have a garnet structure due to a subtle weighing error, and it is difficult to stably manufacture transparent ceramics that can be used for optical applications. Therefore, in the present invention, scandium (Sc) is added as a constituent element to eliminate the composition deviation due to a subtle weighing error. Sc is a material with an intermediate ionic radius that can be dissolved in both the A site and the B site in an oxide having a garnet structure, and is a buffer material that can adjust the distribution ratio to the A site (rare earth site consisting of Tb and Y) and the B site (aluminum site) to exactly match the stoichiometric ratio and thereby minimize the energy of crystallite formation when the compounding ratio of rare earth elements consisting of Tb and Y and Al deviates from the stoichiometric ratio due to variations in weighing. In addition, it is an element that can limit the presence ratio of the alumina heterophase in the garnet parent phase to 1 ppm or less, and the presence ratio of the perovskite-type heterophase in the garnet parent phase to 1 ppm or less, and is an element that can be added to improve product yields.

[0023] In formula (1), the range of x is 0≦x<0.45, preferably 0.1≦x≦0.4, and more preferably 0.2≦x≦0.4. When x is in this range, the Verdet constant at room temperature (23±15℃) and wavelength of 1,064 nm is 30 rad / (T·m) or more, and it can be used as a Faraday rotator. In addition, the larger x is in this range, the smaller the thermal lens effect tends to be, which is preferable. In addition, when x is 0.45 or more, the Verdet constant at wavelength of 1,064 nm is less than 30 rad / (T·m), which is not preferable. In other words, if the relative concentration of Tb is excessively diluted, when using a general magnet, the total length required to rotate the laser light of wavelength 1,064 nm by 45 degrees exceeds 30 mm, which is not preferable because it becomes difficult to manufacture.

[0024] In formula (1), the range of y is 0≦y<0.08, preferably 0.002≦y≦0.07, and more preferably 0.003≦y≦0.06. When y is in this range, the perovskite-type heterophase can be reduced to a level that is not detectable by X-ray diffraction (XRD) analysis. Furthermore, it is preferable because the number of perovskite-type heterophases (typically 1 to 1.5 μm in diameter and granular, light brown in color) present in a 150 μm×150 μm field of view observed under an optical microscope is 1 or less. In this case, the ratio of the perovskite-type heterophase to the garnet parent phase is 1 ppm or less.

[0025] When y is 0.08 or more, the risk of antisite defect absorption, in which Tb and Y occupy the B site and Al occupies the A site, increases, which is undesirable. Also, when y is 0.1 or more, in addition to substituting a part of Tb with Y, Sc also substitutes a part of Tb, which results in an unnecessary decrease in the solid solution concentration of Tb, which is undesirable because the Verdet constant becomes small. Also, since the raw material cost of Sc is high, unnecessary excessive doping of Sc is undesirable from the viewpoint of manufacturing costs.

[0026] In formula (1), the range of z is 0 ≦ z < 0.16, preferably 0.01 ≦ z ≦ 0.15, and more preferably 0.03 ≦ z ≦ 0.15. When z is within this range, a perovskite-type heterogeneous phase is not detected by XRD analysis. Furthermore, it is preferable because the abundance of the perovskite-type heterogeneous phase (granular ones with a typical size of 1 to 1.5 μm in diameter and appearing lightly brownish in color) in a 150 μm × 150 μm field of view by optical microscope observation becomes 1 or less. At this time, the abundance ratio of the perovskite-type heterogeneous phase to the garnet matrix phase is 1 ppm or less.

[0027] When z is 0.16 or more, the risk of anti-site defect absorption in which Tb and Y enter the B site and Al enters the A site increases, which is not preferable. Also, since the value of y, that is, the substitution ratio of Tb by Sc, increases in conjunction with the increase in the value of z, as a result, the solid solution concentration of Tb decreases unnecessarily, and the Verdet constant becomes small, which is not preferable. Furthermore, since Sc is expensive as a raw material, it is not preferable from the viewpoint of manufacturing cost to dopantly Sc excessively and unnecessarily.

[0028] In formula (1), the range of y + z is 0.001 < y + z < 0.20. When y + z is within this range, a perovskite-type heterogeneous phase is not detected by XRD analysis. Furthermore, it is preferable because the abundance of the perovskite-type heterogeneous phase (granular ones with a typical size of 1 to 1.5 μm in diameter and appearing lightly brownish in color) in a 150 μm × 150 μm field of view by optical microscope observation becomes 1 or less. At this time, the abundance ratio of the perovskite-type heterogeneous phase to the garnet matrix phase is 1 ppm or less. Although the effects of the present invention can be obtained even when the range of y + z is 0 ≦ y + z ≦ 0.001, it is not preferable because heterogeneous phases are likely to occur due to weighing errors of raw materials, resulting in a decrease in yield.

[0029] In addition, in the paramagnetic garnet-type transparent ceramics of the present invention, the sintered body preferably further contains a sintering aid. Specifically, it is preferable that the sintering aid contains more than 0 mass% and 0.1 mass% or less (more than 0 ppm and 1,000 ppm or less) of SiO2. If the content exceeds 0.1 mass% (1,000 ppm), there is a risk of slight light absorption occurring due to crystal defects caused by the excessive Si content. The titanium content in the sintered body is preferably less than 2,000 ppm.

[0030] The paramagnetic garnet-type transparent ceramics of the present invention exhibits Tb luminescence. 5 D4 → 7 The lifetime of the emission due to the F5 transition is 346 μs or more, and preferably 500 μs or more. 5 D4 → 7 The method for measuring the "lifetime of luminescence derived from the F5 transition" involves irradiating the target paramagnetic garnet-type transparent ceramic with excitation light of 350 nm wavelength, and measuring the luminescence lifetime of the 545 nm wavelength component in the emitted light with a fluorescence spectrophotometer. In more detail, the time dependence of the luminescence decay of the 545 nm wavelength luminescence component is measured, and assuming that this is a single luminescence lifetime, the time at which the luminescence intensity at the start of the emission becomes 1 / e (approximately 37%) is taken as the luminescence lifetime. It is also preferable that the maximum intensity of the emission emitted by excitation light with a wavelength of 350 nm is between 500 and 600 nm.

[0031] In addition, the paramagnetic garnet-type transparent ceramics of the present invention have a laser damage threshold of 10 J / cm with a wavelength of 1,064 nm and a pulse width of 5 ns. 2 The paramagnetic garnet-type transparent ceramics of the present invention are intended to be used as Faraday rotators, and therefore it is preferable that they are not damaged by pulsed lasers (have laser damage resistance). The damage threshold is preferably as high as possible, and is 10 J / cm when the wavelength λ is 1,064 nm and the pulse width is 5 ns. 2 More than 15 J / cm is preferable. 2More preferably, the damage threshold of the laser with a wavelength of 1,064 nm and a pulse width of 5 ns is 10 J / cm. 2 The method for determining whether or not the energy density is 10 J / cm is to apply an energy density of 10 J / cm to any multiple points (five points or more, preferably ten points or more) of the target paramagnetic garnet-type transparent ceramic. 2 The target area is irradiated with a laser beam with a wavelength of 1,064 nm and a pulse width of 5 ns, and the target area is observed with an optical (polarized) microscope, etc. If the area is completely undamaged, it is said to have a "laser damage threshold of 10 J / cm 2 The laser damage threshold is defined as 10 J / cm or more, and damage at even one point is defined as "laser damage threshold is 10 J / cm or more." 2 It is determined that the above is not the case.

[0032] Incidentally, the laser damage threshold (LIDT) depends on the wavelength, pulse width, and beam spot diameter of the irradiated laser light. 2 If it is not possible to perform a laser damage test at a wavelength of 1,064 nm and a pulse width of 5 ns, the laser damage threshold may be determined by scaling the LIDT. According to "Wavelength Dependence of Laser-Induced Damage: Determining the Damage Initiation Mechanisms" (Non-Patent Document 5), the formula (S1) can be applied as a general rule for scaling (converting) the initial conditions of wavelength (λ1), pulse width (τ1), and irradiation beam diameter (φ1) to new wavelength (λ2), pulse width (τ2), and irradiation beam diameter (φ2). LIDT(λ2,τ2,φ2)=LIDT(λ1,τ1,φ1)×(λ1 / λ2)×(τ2 / τ1) 1 / 2 ×(φ1 / φ2) 2 (S1) Therefore, according to the following formula (S2), the wavelength is 1,064 nm, the wavelength is 5 ns, and the irradiation beam diameter is 100 μm (Gaussian distribution 1 / e 2From the laser damage threshold (LIDT) measured under different conditions of wavelength (λ1 (nm)), pulse width (τ1 (ns)), and irradiation beam diameter (φ1 (μm)), it is possible to convert the laser damage threshold for a wavelength of 1,064 nm and a pulse width of 5 ns (irradiation beam diameter of 100 μm). LIDT(1064,5,100)=LIDT(λ1,τ1,φ1)×(λ1 / 1064)×(5 / τ1) 1 / 2 ×(φ1 / 100) 2 (S2)

[0033] In addition, in the paramagnetic garnet-type transparent ceramics which are sintered bodies of the garnet-type composite oxide represented by the above formula (1), the Tb(III) ions contained in the sintered body are 5 D4 → 7 The lifetime of the emission from the F5 transition is measured. If the lifetime is 346 μs or longer, the laser damage threshold at a wavelength of 1,064 nm is 10 J / cm 2 It can be determined that this is equal to or greater than this.

[0034] Moreover, the paramagnetic garnet-type transparent ceramics of the present invention is preferably obtained by subjecting the above-mentioned sintered body to HIP treatment and further to annealing treatment in an oxidizing atmosphere, as described later.

[0035] Here, the paramagnetic garnet-type transparent ceramics of the present invention may be produced by the following procedure. (raw powder for sintering) First, a raw powder for sintering containing the garnet-type composite oxide powder (ceramic powder) represented by the above formula (1) is prepared.

[0036] The method for producing the raw powder for sintering of the garnet-type composite oxide used in the present invention is not particularly limited, but may be a coprecipitation method, a pulverization method, a spray pyrolysis method, a sol-gel method, an alkoxide hydrolysis method, or any other synthesis method. In some cases, the obtained ceramic raw material of rare earth composite oxide may be appropriately processed by a wet ball mill, a bead mill, a jet mill, a dry jet mill, a hammer mill, or the like to obtain a desired particle size. For example, the raw powder for sintering may be prepared by a solid-phase reaction method in which a plurality of oxide particles are mixed and fired to produce uniformity by thermal diffusion of ions, or a coprecipitation method in which hydroxides, carbonates, etc. are precipitated from an ion-containing solution in which oxide particles are dissolved, and then fired to produce oxides, thereby producing uniformity.

[0037] In the case of the solid-phase reaction method in which a plurality of oxide particles are mixed and fired to produce uniformity by thermal diffusion of ions, metal powders consisting of terbium, yttrium, scandium, and aluminum, or the above metal powders dissolved in an aqueous solution of nitric acid, sulfuric acid, uric acid, or the like, or oxide powders of the above elements, etc. can be suitably used as starting materials. The purity of the above raw materials is preferably 99.9% by mass or more, and particularly preferably 99.99% by mass or more. The starting materials are weighed in a predetermined amount so as to have a composition corresponding to formula (1), mixed, and then fired to obtain a fired raw material mainly composed of a cubic garnet-type oxide of a desired structure. The firing temperature at this time is preferably 950°C or more and lower than the sintering temperature to form a garnet structure, and more preferably 1,100°C or more and lower than the sintering temperature to be performed thereafter. The firing time may be 1 hour or more, and the heating rate at this time is preferably 100°C / h or more and 500°C / h or less. The firing atmosphere is preferably air or an oxygen-containing atmosphere, and nitrogen, argon, hydrogen, etc. are not suitable. The firing apparatus is not particularly limited as long as it can reach the target temperature and oxygen flow, and may be a vertical muffle furnace, a horizontal tubular furnace, a rotary kiln, etc. The term "main component" used here means that the main peak obtained from the powder X-ray diffraction results of the firing raw material is a diffraction peak derived from the garnet structure. When the ratio of the perovskite-type heterophase to the garnet parent phase is 1 ppm or less, the powder X-ray diffraction pattern will essentially only detect a single garnet phase pattern.

[0038] In addition, the raw powder for sintering preferably contains a sintering aid. For example, tetraethoxysilane (TEOS) is added as a sintering aid together with the above starting raw material in an amount of more than 0 ppm and not more than 1,000 ppm (more than 0 mass% and not more than 0.1 mass%) in terms of SiO2 in the entire raw powder (garnet-type complex oxide powder + sintering aid), or SiO2 powder is added in an amount of more than 0 ppm and not more than 1,000 ppm (more than 0 mass% and not more than 0.1 mass%) in the entire raw powder (garnet-type complex oxide powder + sintering aid), mixed and fired to obtain a sintering raw material. If the amount added exceeds 1,000 ppm, there is a risk of slight light absorption occurring due to crystal defects caused by the excessive Si contained. The purity is preferably 99.9 mass% or more. The sintering aid may be added when preparing the raw powder slurry described later. In addition, if no sintering aid is added, it is preferable to select a raw powder for sintering (i.e., the above complex oxide powder) whose primary particles have a nano-sized particle size and have extremely high sintering activity. Such a selection may be made as appropriate.

[0039] Next, the obtained firing raw material is pulverized to obtain a raw material powder for sintering. Either a dry or wet pulverization method can be selected, but it is necessary to pulverize so that the target ceramics become highly transparent. For example, in the case of wet pulverization, the firing raw material is slurried by various pulverization (dispersion) methods such as a ball mill, a bead mill, a homogenizer, a jet mill, and ultrasonic irradiation, and then pulverized (dispersed) to primary particles. The dispersion medium of this wet slurry is not particularly limited as long as it can make the final ceramics highly transparent, and examples of the dispersion medium include alcohols such as lower alcohols having 1 to 4 carbon atoms and pure water. In addition, various organic additives may be added to this wet slurry for the purpose of improving the quality stability and yield in the subsequent ceramic manufacturing process. In the present invention, these are also not particularly limited. That is, various dispersants, binders, lubricants, plasticizers, etc. can be suitably used. However, it is preferable to select high-purity types of organic additives that do not contain unnecessary metal ions. In the case of wet pulverization, the dispersion medium of the slurry is finally removed to obtain a raw material powder for sintering.

[0040] [Manufacturing process] In the present invention, the above-mentioned raw powder for sintering is used to press-mold into a predetermined shape, followed by degreasing and then sintering to produce a sintered body with a relative density of at least 94%. It is preferable to carry out hot isostatic pressing (HIP) as a post-process. If hot isostatic pressing (HIP) is carried out directly, the paramagnetic garnet-type transparent ceramics will be reduced and some oxygen deficiency will occur. For this reason, it is preferable to carry out a slight oxidation HIP process or an annealing process in an oxidizing atmosphere after the HIP process to recover the oxygen deficiency. This makes it possible to obtain a transparent garnet-type oxide ceramics without defect absorption.

[0041] (molding) In the manufacturing method of the present invention, a normal press molding process can be suitably used. That is, a very common press process in which a mold is filled and pressurized from a certain direction, or a cold isostatic pressing (CIP) process or a warm isostatic pressing (WIP) process in which the molded body is sealed and stored in a deformable waterproof container and pressurized with hydrostatic pressure can be suitably used. The applied pressure can be appropriately adjusted while checking the relative density of the obtained molded body, and is not particularly limited. For example, the manufacturing cost can be reduced by controlling the pressure within a pressure range of about 300 MPa or less that can be handled by a commercially available CIP device. Alternatively, a hot press process, a discharge plasma sintering process, a microwave heating process, etc., in which not only the molding process but also sintering is performed at once during molding can also be suitably used. Furthermore, it is possible to produce a molded body by a casting molding method instead of a press molding method. A molding method such as pressurized casting molding, centrifugal casting molding, and extrusion molding can also be adopted by optimizing the combination of the shape and size of the oxide powder as the starting material and various organic additives.

[0042] (Degreasing) In the manufacturing method of the present invention, a normal debinding process can be suitably used. That is, a heating debinding process using a heating furnace can be used. The type of atmospheric gas used at this time is not particularly limited, and air, oxygen, hydrogen, etc. can be suitably used. There is no particular limit to the debinding temperature, but if a raw material containing an organic additive is used, it is preferable to heat the raw material to a temperature at which the organic component can be decomposed and eliminated.

[0043] (Sintering) In the manufacturing method of the present invention, a general sintering process can be preferably used. That is, a heat sintering process such as a resistance heating method or an induction heating method can be preferably used. The atmosphere at this time is not particularly limited, and sintering can be performed in various atmospheres such as an inert gas, oxygen gas, hydrogen gas, helium gas, or under reduced pressure (vacuum). However, since it is preferable to prevent the occurrence of oxygen deficiency in the end, more preferable atmospheres include an oxygen gas atmosphere and a reduced pressure oxygen gas atmosphere.

[0044] The sintering temperature in the sintering step of the present invention is preferably 1,500 to 1,780°C, and particularly preferably 1,550 to 1,750°C. This range of sintering temperature is preferable because it promotes densification while suppressing heterophase precipitation. A sintering holding time of about several hours in the sintering step of the present invention is sufficient, but the relative density of the sintered body must be densified to at least 94%.

[0045] (Hot Isostatic Pressing (HIP)) In the manufacturing method of the present invention, a step of performing a hot isostatic pressing (HIP) process can be additionally provided after the sintering process. The type of pressurized gas medium that can be used at this time is preferably an inert gas such as argon or nitrogen, or Ar-O2. The pressure applied by the pressurized gas medium is preferably 50 to 300 MPa, more preferably 100 to 300 MPa. If the pressure is less than 50 MPa, the transparency improvement effect may not be obtained, and if the pressure exceeds 300 MPa, even if the pressure is increased, no further transparency improvement is obtained, and the load on the device becomes excessive, which may damage the device. It is convenient and preferable that the applied pressure is 196 MPa or less, which can be processed by a commercially available HIP device.

[0046] The treatment temperature (predetermined holding temperature) is set in the range of 1,000 to 1,780°C, preferably 1,100 to 1,730°C. If the treatment temperature exceeds 1,780°C, the risk of oxygen deficiency increases, which is not preferable. If the treatment temperature is less than 1,000°C, the effect of improving the transparency of the sintered body is hardly obtained. The holding time of the treatment temperature is not particularly limited, but if it is held for too long, the risk of oxygen deficiency increases, which is not preferable. Typically, it is preferably set in the range of 1 to 3 hours. The heater material, heat insulating material, and treatment container for the HIP treatment are not particularly limited, but graphite, molybdenum (Mo), tungsten (W), and platinum (Pt) can be preferably used, and yttrium oxide and gadolinium oxide can also be preferably used as the treatment container. In particular, when the treatment temperature is 1,500°C or less, platinum (Pt) can be used as the heater material, heat insulating material, and treatment vessel, and Ar-O2 can be used as the pressurized gas medium, which is preferable because it prevents the occurrence of oxygen vacancies during HIP treatment. When the treatment temperature exceeds 1,500°C, graphite is preferable as the heater material and heat insulating material, but in this case, it is preferable to select graphite, molybdenum (Mo), or tungsten (W) as the treatment vessel, and further select either yttrium oxide or gadolinium oxide as a double vessel inside, and fill the vessel with an oxygen release material, since this minimizes the amount of oxygen vacancies during HIP treatment.

[0047] (Anneal) In the manufacturing method of the present invention, after the HIP treatment, oxygen deficiency may occur in the obtained transparent ceramic sintered body, which may have a gray appearance. In that case, it is preferable to perform oxygen annealing treatment (oxygen deficiency recovery treatment) in an oxygen atmosphere at a temperature equal to or lower than the HIP treatment temperature, typically 1,000 to 1,500 ° C. In this case, the holding time is not particularly limited, but it is preferable to select a time that is sufficient to recover the oxygen deficiency and is not too long to waste electricity. By the oxygen annealing treatment, even if the transparent ceramic sintered body has a faint light gray appearance in the HIP treatment process, it can be made into a colorless, transparent paramagnetic garnet-type transparent ceramic with little defect absorption.

[0048] (optical polishing) In the manufacturing method of the present invention, it is preferable to optically polish both end faces on the optically utilized axis of the paramagnetic garnet-type transparent ceramics that has undergone the above-mentioned series of manufacturing steps. In this case, the optical surface accuracy is preferably λ / 2 or less, and particularly preferably λ / 8 or less, when the measurement wavelength λ=633 nm. It is also possible to further reduce optical loss by appropriately forming an anti-reflection film on the optically polished surface.

[0049] As described above, a sintered body of the paramagnetic garnet-type composite oxide containing terbium represented by the above formula (1) was obtained, and the Tb(III) ions contained in the sintered body were 5 D4 → 7 It is possible to provide a paramagnetic garnet-type transparent ceramic having a lifetime of 346 μs or more of luminescence derived from the F5 transition. In addition, it is preferable that the laser damage threshold is 10 J / cm at a wavelength of 1,064 nm and a pulse width of 5 ns. 2 It can be more than one.

[0050] [Magneto-optical devices] Furthermore, since the paramagnetic garnet-type transparent ceramic of the present invention is intended to be used as a magneto-optical material, it is preferable to apply a magnetic field parallel to the optical axis of the paramagnetic garnet-type transparent ceramic, and then set a polarizer and an analyzer so that their optical axes are shifted by 45 degrees from each other to form a magneto-optical device. That is, the magneto-optical material of the present invention is suitable for use in magneto-optical devices, and is particularly suitable for use as a Faraday rotator for an optical isolator with a wavelength of 0.9 to 1.1 μm.

[0051] FIG. 1 is a schematic cross-sectional view showing an example of an optical isolator, which is an optical device having a Faraday rotator made of the magneto-optical material of the present invention as an optical element. 1, an optical isolator 100 includes a Faraday rotator 110 made of the magneto-optical material of the present invention, and a polarizer 120 and an analyzer 130, which are polarizing materials, are provided in front of and behind the Faraday rotator 110. Moreover, in the optical isolator 100, the polarizer 120, the Faraday rotator 110, and the analyzer 130 are arranged in this order on the optical axis 112, and it is preferable that a magnet 140 is placed on at least one of the side surfaces of these elements.

[0052] The optical isolator 100 can be suitably used in industrial fiber laser devices, that is, to prevent the reflected light of the laser light emitted from the laser light source from returning to the light source, causing the oscillation to become unstable.

[0053] [Method for determining laser damage resistance of paramagnetic garnet-type transparent ceramics] The method for judging the laser damage resistance of a paramagnetic garnet-type transparent ceramic of the present invention is to determine the amount of Tb(III) ions contained in a paramagnetic garnet-type transparent ceramic made of a sintered body of a garnet-type composite oxide represented by the following formula (1'): 5 D4 → 7 This method is characterized by judging the laser damage resistance based on the lifetime of the emission derived from the F5 transition. (T 1-x-y Y x Sc y )3(Al 1-zSc z )5O 12 (1’) (where 0 ≦ x < 0.45, 0 ≦ y < 0.08, 0 ≦ z < 0.16.)

[0054] Here, when the lifetime of the luminescence derived from the 5 D4→ 7 F5 transition of the above Tb(III) ion is 346 μs or more, the laser damage threshold value of wavelength 1,064 nm and pulse width 5 ns is 10 J / cm 2 or more, it is preferable to determine that it has laser damage resistance of Details of the sintered body of the garnet-type composite oxide represented by the formula (1’) and its manufacturing method are the same as those of the above-described paramagnetic garnet-type transparent ceramics of the present invention and its manufacturing method, except for the condition of “0.001 < y + z < 0.20”. [Examples]

[0055] Hereinafter, the present invention will be described more specifically with reference to Examples, Reference Examples, and Comparative Examples, but the present invention is not limited to these Examples.

[0056] [Example 1] Example 1 shows the case where y = 0.004 and z = 0.03 (y + z = 0.034) in the formula (1) are fixed and the value of x is 0 ≦ x ≦ 0.396. Yttrium oxide powder manufactured by Shin-Etsu Chemical Co., Ltd., terbium oxide powder, scandium oxide powder, and aluminum oxide powder manufactured by Daming Chemical Co., Ltd. were obtained. Further, tetraethyl orthosilicate (TEOS) manufactured by Kishida Chemical Co., Ltd. and polyethylene glycol 200 liquid manufactured by Kanto Chemical Co., Ltd. were obtained. The purity of all the powder raw materials was 99.9 mass% or more, and the purity of the liquid raw materials was 99.999 mass% or more. Using the above raw materials, the mixing ratios were adjusted as follows to produce four types of raw material powders having the final compositions shown in Table 1. The titanium content in each raw material powder was less than 1 ppm.

[0057] (Raw materials for Example 1-1 and Comparative Example 1-1) The moles of terbium, yttrium, aluminum, and scandium were weighed out so that Tb:Y:Sc:Al=1.794:1.194:0.162:4.850, respectively (Tb 0.598 Y 0.398 Sc 0.004 )3(Al 0.97 Sc 0.03 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0058] (Materials for Examples 1-2 and Comparative Examples 1-2) The moles of terbium, yttrium, aluminum, and scandium were weighed out so that Tb:Y:Sc:Al=2.091:0.897:0.162:4.850, respectively (Tb 0.697 Y 0.299 Sc 0.004 )3(Al 0.97 Sc 0.03 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0059] (Materials for Examples 1-3 and Comparative Examples 1-3) The moles of terbium, yttrium, aluminum, and scandium were weighed out so that Tb:Y:Sc:Al=2.391:0.597:0.162:4.850, respectively (Tb 0.797 Y 0.199 Sc 0.004 )3(Al 0.97 Sc 0.03 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0060] (Materials for Examples 1-4 and Comparative Examples 1-4) The moles of terbium, aluminum, and scandium were weighed out so that Tb:Sc:Al was 2.988:0.162:4.850, respectively (Tb0.996 Sc 0.004 )3(Al 0.97 Sc 0.03 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0061] Next, each was placed in a polyethylene pot, taking care to prevent mixing, and polyethylene glycol 200 was added as a dispersant to the oxide powder at 0.5% by mass. Each was dispersed and mixed in ethanol using a ball mill. The processing time was 24 hours. After that, a spray drying process was carried out to produce granular raw materials with an average particle size of 20 μm.

[0062] Next, these granular raw materials were placed in an yttria crucible and sintered in a high-temperature muffle furnace at 1,100°C for 3 hours to obtain sintered raw material powders with each composition. The four types of powder raw materials obtained were each subjected to uniaxial press molding and isostatic pressing at a pressure of 198 MPa to obtain CIP compacts. The obtained compacts were degreased in a muffle furnace at 1,000°C for 2 hours.

[0063] As an example, the degreased molded body was placed in an oxygen atmosphere furnace and treated at 1,730°C for 3 hours to obtain a total of four types of sintered bodies. At this time, the sintered relative density of each sample was 94% or more. Each of the obtained sintered bodies was placed in a HIP furnace made of a carbon heater and HIP-treated under conditions of Ar, 200 MPa, 1,700°C, and 2 hours. Next, the HIP-treated sintered bodies were placed again in the oxygen atmosphere furnace and each was subjected to oxidation annealing treatment under conditions of 1,450°C for 6 hours.

[0064] As a comparative example, the degreased green body was placed in a vacuum furnace and treated at 1,600°C for 3 hours to obtain a total of four types of sintered bodies. At this time, the sintered relative density of each sample was 94% or more. Each of the obtained sintered bodies was placed in a HIP furnace made of a carbon heater and HIP-treated under conditions of 200 MPa, 1,600°C, and 3 hours in Ar. In accordance with the prior art, the HIP-treated sintered bodies were not subjected to oxidation annealing treatment.

[0065] Each transparent ceramic thus obtained was cylindrically ground to a diameter of 10 mm, and then ground and polished to a length of 10 mm. Furthermore, both optical end faces of each sample were subjected to final optical polishing with an optical surface precision of λ / 8 (when the measurement wavelength λ=633 nm). Next, the optically polished samples were coated with an anti-reflection film designed to set the center wavelength at 1,064 nm.

[0066] Each sample obtained as described above was evaluated by measuring the emission lifetime and performing a laser damage test as described below.

[0067] (Luminescence lifetime measurement) The luminescence lifetime was measured using a modular fluorescence spectrophotometer, Fluorolog-3 (manufactured by HORIBA). The measurement was performed on a cylindrically ground rough surface. The excitation light was 350 nm, and the lifetime was measured for the luminescence component with a wavelength of 545 nm. When the excitation light was applied, the measurement sample was in an excited state, and the lowest excited state was 545 nm. 5 The electrons return to the ground state via D4, releasing energy. At this time, light is emitted. In all samples, light emission with maximum intensity was observed between 500 and 600 nm. In this case, the time change in emission intensity F(t) is given by the following formula: F(t) = F0 × exp(-t / τ) (In the formula, F0 is the emission intensity at t=0, and τ is the emission lifetime (μs).) In other words, the time when F(t) = 1 / eF0 (approximately 37%) occurs is the luminescence lifetime. The luminescence lifetime τ was determined by measuring the time dependence of luminescence decay and by the least squares method using the above formula, assuming a single luminescence lifetime.

[0068] (Laser damage test) The laser damage threshold was measured using a Nd:YAG laser with a wavelength of 1,064 nm and a pulse width of 5 ns. The irradiation angle was perpendicular to the polished surface (optical end surface of the sample), and the irradiation size was a beam diameter of 100 μm (Gaussian distribution 1 / e 2 Intensity) and energy density is 10-11 J / cm 2 The sample was irradiated so that the laser beam was emitted at a constant angle of 1000 nm. 10 shots were irradiated while changing the position within the optically effective area of ​​the optical end face of the sample, and the number of damages was counted using a polarizing microscope. Specifically, a polarizing microscope with a magnification of 12.5x was used to observe a crossed Nicol image of the entire optically effective area from the optical end face direction, and if Hv (Horizontal-vertical) light scattering was confirmed, it was determined that this was caused by laser damage distortion and that laser damage had occurred at that position. Note that the position of the laser damage (inside the material, on the output end face, etc.) was not important. The above results are summarized in Table 1.

[0069] [Table 1]

[0070] From the above results, the luminescence lifetime of the transparent ceramics that were oxidatively annealed (Examples 1-1 to 1-4) was 346 μs to 751 μs. The luminescence lifetime of the transparent ceramics that were not oxidatively annealed (Comparative Examples 1-1 to 1-4) was 232 μs to 280 μs. That is, it was confirmed that the luminescence lifetime of the transparent ceramics that were oxidatively annealed was longer than that of the transparent ceramics that were not oxidatively annealed, at 346 μs or more. Note that the tendency for the luminescence lifetime to become shorter as x becomes smaller for the transparent ceramics that were oxidatively annealed (Examples 1-1 to 1-4) is thought to be due to concentration quenching of Tb ions. In addition, at an energy density of 10 to 11 J / cm 2When irradiated with laser light, the laser damage numbers of the annealed transparent ceramics (Examples 1-1 to 1-4) were all 0, while the damage numbers of the non-annealed transparent ceramics (Comparative Examples 1-1 to 1-4) were all 10. That is, by performing an annealing treatment after HIP treatment, transparent ceramics with a long emission lifetime of 346 μs or more can be obtained, and it was confirmed that transparent ceramics with a laser damage threshold higher than 10 J / cm 2 were obtained.

[0071] [Example 2] As Example 2, the case where x = 0.4 in Formula (1) was fixed, the value of y was 0 ≤ y ≤ 0.07, the value of z was 0 ≤ z ≤ 0.15, and the value of y + z was 0.001 < y + z < 0.20 is shown. Similar to Example 1, yttrium oxide powder, terbium oxide powder, scandium oxide powder manufactured by Shin-Etsu Chemical Co., Ltd., and aluminum oxide powder manufactured by Daming Chemical Co., Ltd. were obtained. Furthermore, tetraethyl orthosilicate (TEOS) manufactured by Kishida Chemical Co., Ltd. and polyethylene glycol 200 liquid manufactured by Kanto Chemical Co., Ltd. were obtained. The purity of all the powder raw materials was 99.9 mass% or more, and the purity of the liquid raw materials was 99.999 mass% or more. Using the above raw materials, the mixing ratios were adjusted as follows to prepare a total of three types of raw material powders having the final compositions shown in Table 2.

[0072] (Raw materials for Example 2-1) The number of moles of terbium, yttrium, scandium, and aluminum were weighed so that Tb:Y:Sc:Al = 1.797:1.200:0.008:4.995, respectively (Tb 0.599 Y 0.4 Sc 0.001 )3(Al 0.999 Sc 0.001 )5O 12 The mixed powder was prepared. Subsequently, TEOS was weighed and added as a sintering aid so that the added amount was 100 ppm in terms of SiO2, and used as a raw material.

[0073] (Raw materials for Example 2-2) The moles of terbium, yttrium, scandium, and aluminum were weighed out so that Tb:Y:Sc:Al=1.68:1.20:0.52:4.60, respectively (Tb 0.56 Y 0.4 Sc 0.04 )3(Al 0.92 Sc 0.08 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0074] (Materials for Examples 2-3) The moles of terbium, yttrium, scandium, and aluminum were weighed out so that Tb:Y:Sc:Al=1.59:1.20:0.86:4.35, respectively (Tb 0.53 Y 0.4 Sc 0.07 )3(Al 0.87 Sc 0.13 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0075] (Raw material for Reference Example 2-1) The moles of terbium, yttrium, and aluminum were weighed out so that Tb:Y:Al=1.8:1.2:5.0, respectively (Tb 0.6 Y 0.4 )3AlO 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0076] Next, each was placed in a polyethylene pot, taking care to prevent mixing, and polyethylene glycol 200 was added as a dispersant to the oxide powder at 0.5% by mass. Each was dispersed and mixed in ethanol using a ball mill. The processing time was 24 hours. After that, a spray drying process was carried out to produce granular raw materials with an average particle size of 20 μm.

[0077] Next, these granular raw materials were placed in an yttria crucible and sintered in a high-temperature muffle furnace at 1,100°C for 3 hours to obtain sintered raw material powders with each composition. The four types of powder raw materials obtained were each subjected to uniaxial press molding and isostatic pressing at a pressure of 198 MPa to obtain CIP compacts. The obtained compacts were degreased in a muffle furnace at 1,000°C for 2 hours.

[0078] The degreased compacts were placed in an oxygen atmosphere furnace and treated at 1,730°C for 3 hours to obtain a total of four types of sintered compacts. At this time, the sintered relative density of each sample was 94% or more. Each of the obtained sintered compacts was placed in a carbon heater HIP furnace and HIP-treated under Ar conditions of 200 MPa, 1,700°C, and 2 hours. The HIP-treated sintered compacts were then placed again in the oxygen atmosphere furnace and subjected to oxidation annealing treatment at 1,450°C for 6 hours.

[0079] Each transparent ceramic thus obtained was cylindrically ground to a diameter of 10 mm, and then ground and polished to a length of 10 mm. Furthermore, both optical end faces of each sample were subjected to final optical polishing with an optical surface precision of λ / 8 (when the measurement wavelength λ=633 nm). Next, the optically polished samples were coated with an anti-reflection film designed to set the center wavelength at 1,064 nm.

[0080] For each sample obtained as described above, the emission lifetime was measured and a laser damage test was performed in the same manner as in Example 1 to evaluate the sample. The above results are summarized in Table 2.

[0081] [Table 2]

[0082] From the above results, the luminescence lifetime of the transparent ceramics of Examples 2-1 to 2-3 was 705 μs to 729 μs. Also, the number of damages in all of the transparent ceramics of Examples 2-1 to 2-3 was 0. That is, transparent ceramics with luminescence lifetimes of 705 μs to 729 μs and laser damage thresholds of 10 J / cm were obtained. 2 It was confirmed that highly transparent ceramics could be obtained.

[0083] [Example 3] In Example 3, x=0, y=0, z=0.002 (y+z=0.002) in formula (1) are used, and the effect of including paramagnetic impurities that absorb the wavelength used is shown. As an example of paramagnetic impurities, the effect of doping with Ti is shown with reference to Non-Patent Document 1. Terbium oxide powder manufactured by Shin-Etsu Chemical Co., Ltd., aluminum oxide powder manufactured by Taimei Chemical Co., Ltd., and titanium oxide powder manufactured by Kojundo Chemical Laboratory Co., Ltd. were obtained. In addition, tetraethyl orthosilicate (TEOS) manufactured by Kishida Chemical Co., Ltd. and polyethylene glycol 200 liquid manufactured by Kanto Chemical Co., Ltd. were obtained. The purity of the powder raw materials was 99.9% by mass or more, and the purity of the liquid raw materials was 99.999% by mass or more. Using the above raw materials, a total of two types of raw material powders with the final composition shown in Table 3 were produced by adjusting the mixing ratio as follows.

[0084] (Materials for Example 3-1) The moles of terbium, scandium, and aluminum were weighed out so that Tb:Sc:Al=3:0.01:4.99, respectively. 0.998 Sc 0.002 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and this was used as the raw material.

[0085] (Raw materials for Comparative Examples 3-1 and 3-2) With reference to Non-Patent Document 1, the mole numbers of terbium, scandium, aluminum, and titanium were weighed out so that Tb:Sc:Al:Ti=3:0.01:4.95:0.04, respectively. 0.990 Sc0.002 Ti 0.008 )5O 12 Next, TEOS was weighed and added as a sintering aid so that the amount added was 100 ppm in terms of SiO2, and the raw material was prepared. The titanium content at this time was 2.4 × 10 3 ppm.

[0086] Next, each was placed in a polyethylene pot, taking care to prevent mixing, and polyethylene glycol 200 was added as a dispersant to the oxide powder at 0.5% by mass. Each was dispersed and mixed in ethanol using a ball mill. The processing time was 24 hours. After that, a spray drying process was carried out to produce granular raw materials with an average particle size of 20 μm.

[0087] Next, these granular raw materials were placed in an yttria crucible and sintered in a high-temperature muffle furnace at 1,100°C for 3 hours to obtain sintered raw material powders with the respective compositions. The two types of powder raw materials obtained were each subjected to uniaxial press molding and isostatic pressing at a pressure of 198 MPa to obtain CIP compacts. The obtained compacts were degreased in a muffle furnace at 1,000°C for 2 hours.

[0088] As an example, Tb3(Al 0.998 Sc 0.002 )5O 12 The degreased molded body was placed in an oxygen atmosphere furnace and treated at 1,650°C for 3 hours to obtain a sintered body. At this time, the sintered relative density of the sample was 98%. The obtained sintered body was placed in a carbon heater HIP furnace and HIP-treated under conditions of Ar, 200 MPa, 1,650°C, and 2 hours. The HIP-treated sintered body was then placed in the oxygen atmosphere furnace again and subjected to oxidation annealing treatment at 1,450°C for 6 hours, which was designated as Example 3-1.

[0089] With reference to Non-Patent Document 1, Tb3(Al 0.990 Sc 0.002 Ti 0.008 )5O 12The degreased green body was placed in a vacuum furnace and sintered at 1,600°C for 8 hours to obtain a sintered body. The sintered relative density of each sample was 99% or more. The sample had a translucent appearance and was brown in color. The sample that was not subjected to the oxidation annealing treatment after vacuum sintering was designated Comparative Example 3-1.

[0090] The vacuum sintered body was then placed in an oxygen atmosphere furnace and subjected to oxidation annealing treatment at 1,450°C for 6 hours to obtain Comparative Example 3-2. The appearance was translucent and the color was brown.

[0091] Each transparent ceramic thus obtained was cylindrically ground to a diameter of 10 mm, and then ground and polished to a length of 10 mm. Furthermore, both optical end faces of each sample were subjected to final optical polishing with an optical surface precision of λ / 8 (when the measurement wavelength λ=633 nm). Next, the optically polished samples were coated with an anti-reflection film designed to set the center wavelength at 1,064 nm.

[0092] For each sample obtained as described above, the emission lifetime was measured and a laser damage test was performed in the same manner as in Example 1 to evaluate the sample. The above results are summarized in Table 3.

[0093] [Table 3]

[0094] From the above results, the luminescence lifetime of the transparent ceramics not doped with titanium (Example 3-1) was 374 μs. Also, the luminescence lifetimes of the transparent ceramics doped with titanium (Comparative Examples 3-1 and 3-2) were 198 μs and 234 μs. That is, it was confirmed that the luminescence lifetime was shorter when doped with titanium than when not doped with titanium, regardless of whether or not oxidation annealing was performed. Also, at an energy density of 10 to 11 J / cm 2When irradiated with a laser beam of 10 J / cm, the number of laser damages in the transparent ceramic not doped with titanium (Example 3-1) was 0, whereas the number of laser damages in the transparent ceramics doped with titanium (Comparative Examples 3-1 and 3-2) was 10. In other words, transparent ceramics with a luminescence lifetime of less than 234 μs, regardless of whether or not they were subjected to oxidation annealing treatment, had a laser damage threshold of 10 J / cm 2 It was confirmed that it was less than

[0095] Although the present invention has been described above using the above-mentioned embodiments, the present invention is not limited to these embodiments, and can be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, deletions, etc., and any aspect is within the scope of the present invention as long as it achieves the effects of the present invention. [Explanation of symbols]

[0096] 100 Optical isolator 110 Faraday Rotator 112 Optical axis 120 Polarizer 130 Analyzer 140 Magnet 150 Case

Claims

1. Regarding a paramagnetic garnet-type transparent ceramics consisting of a sintered body of a garnet-type composite oxide represented by the following formula (1'), 5 D 4 → 7 F 5 A method for determining the laser damage resistance of a paramagnetic garnet-type transparent ceramic, characterized in that when the lifetime of light emission derived from a transition is 346 μs or more, it is determined that the ceramic has a laser damage resistance of 10 J / cm2 or more when the laser damage threshold is 1,064 nm in wavelength and 5 ns in pulse width. (Tb 1-x-y Y x Sc y ) 3 (Al 1-z Sc z ) 5 O 12 (1’) (In the formula, 0≦x<0.45, 0≦y<0.08, and 0≦z<0.16.)

2. 2. The method for judging laser damage resistance of a paramagnetic garnet-type transparent ceramic according to claim 1, wherein the maximum intensity of light emitted by excitation light having a wavelength of 350 nm is between 500 and 600 nm.

3. 3. The method for evaluating laser damage resistance of a paramagnetic garnet-type transparent ceramic according to claim 1, wherein the sintered body further contains a sintering aid.

4. 4. The method for determining laser damage resistance of a paramagnetic garnet-type transparent ceramic according to claim 1, wherein the sintered body is subjected to HIP treatment and further annealing treatment in an oxidizing atmosphere.

5. 5. The method for determining laser damage resistance of a paramagnetic garnet-type transparent ceramic according to claim 1, wherein the titanium content in the sintered body is less than 2,000 ppm.

Citation Information

Patent Citations

  • Terbium-aluminum-garnet single crystal and method of manufacturing for the same

    JP2002293693A

  • Garnet crystal for magnetooptical element

    JP2011213552A

  • Nonlinear absorption measurement method of optical material

    JP2012185081A

  • Paramagnetic garnet transparent ceramic, magnetic optical material and magnetic optical device

    JP2019199386A

  • Terbium-based paramagnetic garnet single crystals and porcelain optical devices

    JP4107292B2