Magnetic core and coil parts

A tailored Ni-based ferrite composition and manufacturing process stabilize magnetic permeability and inductance against temperature changes, addressing communication stability and size constraints in automotive applications.

JP7568008B2Active Publication Date: 2024-10-16PROTERIAL LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023125212
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-01
Publication Date
2024-10-16
Estimated Expiration
2039-03-19

AI Technical Summary

Technical Problem

Ni-based ferrite materials exhibit significant fluctuations in magnetic permeability and inductance due to temperature changes, particularly in automotive applications, leading to communication failures and increased component size, necessitating a material with high initial magnetic permeability and a relative temperature coefficient of 0/°C or less.

Method used

A Ni-based ferrite composition with specific molar ratios of Fe2O3, ZnO, CuO, and MnO, along with a manufacturing process involving wet mixing, calcination, and sintering, results in a material with an initial magnetic permeability of 465 or more and a relative temperature coefficient of -3.0×10-6/°C or less, stabilizing inductance under temperature variations.

Benefits of technology

The solution provides a Ni-based ferrite with minimal magnetic permeability fluctuations, ensuring stable inductance and reduced component size, suitable for applications requiring precise communication performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568008000003
    Figure 0007568008000003
  • Figure 0007568008000004
    Figure 0007568008000004
  • Figure 0007568008000001
    Figure 0007568008000001
Patent Text Reader

Abstract

To provide a Ni-based ferrite magnetic core with a large initial permeability and a small relative temperature coefficient.SOLUTION: A magnetic core is made of Ni-based ferrite. The Ni-based ferrite has an initial permeability μi equal to or higher than 465 at a temperature of 20°C and at a frequency of several 100 kHz. The Ni-based ferrite has a relative temperature coefficient αμir of the initial permeability at a frequency of 100 kHz that is equal to or higher than -3.0×10-6 / °C and equal to or lower than 0 / °C in a temperature range of 20 to 85°C and equal to or higher than -2.0×10-6 / °C and equal to or lower than 0 / °C in a temperature range of 20 to 120°C. The composition is represented as Fe2O3 equal to or higher than 47.0 mol% and equal to or lower than 47.5 mol%, ZnO equal to or higher than 28.0 mol% and equal to or lower than 32.0 mol%, MnO equal to or higher than 0.3 mol% and equal to or lower than 1.2 mol%, and the balance being CuO and NiO. The total amount of Fe2O3 and MnO is equal to or higher than 47.5 mol% and equal to or lower than 48.2 mol%. ZnO / Fe2O3 is between 0.628 and 0.631.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to Ni-based ferrite used in coil components using magnetic ferrite, and to coil components using the same. [Background technology]

[0002] Magnetic ferrite has a spinel crystal structure, and it is known that its stoichiometric composition is an equimolar mixture of trivalent and divalent compounds. For example, the stoichiometric composition of Ni-based ferrite spinel crystals (general formula Fe2O3·MeO) is a 50:50 ratio of Fe2O3 and MeO (Me:Ni,Zn).

[0003] In a typical manufacturing method for such Ni-based ferrite, oxides of elements constituting the Ni-based ferrite are prepared as raw materials, which are mixed to obtain a predetermined composition and sintered to form a spinel. From the viewpoint of obtaining a uniform spinelization reaction, a manufacturing method is often adopted in which the raw materials are sintered at a temperature lower than that of the main sintering to form a spinel, and the resulting calcined powder is solidified into a predetermined shape to form a compact, which is then sintered to form a magnetic core.

[0004] It is known that the magnetic properties of Ni-based ferrites are strongly dependent on their composition. The properties required of Ni-based ferrites for coil components and the like include a high initial permeability μi in the frequency and temperature range in which they are used, and a small relative temperature coefficient αμir, which indicates the temperature dependence of the initial permeability μi.

[0005] An example of a coil component is an antenna used in a keyless entry system or a TPMS (Tire Pressure Monitoring System), and a configuration example of such an antenna is shown in Fig. 1. Coil component (antenna) 1 is composed of a coil 5 and a magnetic core 7 inserted into the hollow core of the coil 5. Furthermore, at least a part of the coil 5 and magnetic core 7 may be covered with a resin material 8 composed of a thermosetting resin such as an epoxy resin or a thermoplastic resin such as a liquid crystal polymer that has heat resistance and insulating properties.

[0006] Since Ni-based ferrite has a temperature characteristic of magnetic permeability, the inductance of the coil component may vary with changes in the environmental temperature. When the coil component is used as an antenna, the resonant frequency of the parallel resonant circuit of the coil component and a capacitor (not shown) is set to match the communication frequency of the antenna. If the inductance of the coil component varies, a deviation occurs between the resonant frequency and the communication frequency, which may cause problems such as communication not being possible or the communication distance being shortened. In addition, if the magnetic permeability of Ni-based ferrite is low, it is necessary to increase the number of turns of the coil to obtain the desired inductance, and the external dimensions of the coil component tend to become large accordingly, and it may be difficult to fit it into a limited space.

[0007] In relation to the temperature characteristics of the magnetic permeability of Ni-based ferrite, Patent Document 1 discloses a ferrite sintered body in which the relative temperature coefficient αμir of the initial magnetic permeability μi is small, being −2 to 2 ppm / °C in the temperature range of −40 to 150°C. This ferrite sintered body contains 46.0 to 50.0 mol% Fe2O3, 20.0 to 30.0 mol% ZnO, 1.0 to 9.0 mol% CuO, and 0.1 to 1.0 mol% Mn2O3, and is composed of a composition in which the remainder excluding Fe2O3, ZnO, CuO, and Mn2O3 is mainly NiO, and the ZnO / Fe2O3 (molar ratio) satisfies 0.54 to 0.67. The relative temperature coefficient αμir is calculated by the formula described below. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2006-282437 A Summary of the Invention [Problem to be solved by the invention]

[0009] Usually, the temperature change that occurs in the environment to which an antenna is exposed tends to be more toward the high temperature side than the low temperature side, for example, with 20°C as the base temperature. In particular, the temperature change tends to be large in in-vehicle applications. For this reason, Ni-based ferrite with a small relative temperature coefficient αμir on the high temperature side is required.

[0010] In addition, since Ni-based ferrite has a negative magnetostriction constant, it is known that the initial permeability μi increases according to compressive stress, passes a maximum value, and then decreases. When compressive stress is applied to the magnetic core due to the difference in linear expansion coefficient between the ferrite magnetic core and the resin material that coats it, the inductance of the coil component tends to increase. Therefore, it is also desirable for the relative temperature coefficient αμir of Ni-based ferrite to be 0 / ℃ or less.

[0011] The ferrite sintered body of Patent Document 1 has a small relative temperature coefficient αμi in the temperature range of -40 to 150°C, but the initial permeability μi of the one disclosed in the embodiment is at most about 460, and further improvement of the initial permeability μi is required to miniaturize coil components. In addition, the fluctuation of the initial permeability μi may be a monotonous increase or decrease with respect to temperature change, or an extreme value of the initial permeability μi may be obtained by turning from an increase to a decrease or from a decrease to an increase. In such a case, the relative temperature coefficient αμir of the initial permeability μi may be calculated as a seemingly small value. This is likely to occur when the relative temperature coefficient αμir is calculated under conditions with a wide temperature range. In other words, even if the relative temperature coefficient αμir is small, when it is specified in a wide temperature range, it may include a large fluctuation of the initial permeability μi with respect to temperature change.

[0012] Therefore, the present invention aims to provide a Ni-based ferrite having a large initial permeability μi, small fluctuations in the initial permeability μi relative to temperature changes on the high-temperature side, and a relative temperature coefficient αμir of 0 / ℃ or less, and a coil component using the same. [Means for solving the problem]

[0013] The first invention is a magnet that has an initial permeability μi of 465 or more at a temperature of 20° C. and a frequency of 100 kHz, and a relative temperature coefficient of initial permeability αμir of −3.0×10 in a temperature range of 20 to 85° C. -6 / ℃ or more and 0 / ℃ or less, and in the temperature range of 20 to 120℃, -2.0×10 -6 The Ni-based ferrite has a temperature of from 47.0 mol% to 47.5 mol% Fe2O3, from 28.0 mol% to 32.0 mol% ZnO, from 6.0 mol% to 9.0 mol% CuO, from 0.3 mol% to 1.2 mol% MnO, and the balance NiO, and the total amount of Fe2O3 and MnO is from 47.5 mol% to 48.2 mol%.

[0014] In the first invention, by evaluating the relative temperature coefficient αμir calculated in two temperature ranges, 20 to 85°C and 20 to 120°C, in the higher temperature range, it is possible to evaluate with high accuracy the fluctuation of the initial permeability μi with respect to the temperature change on the higher temperature side.

[0015] In the first invention, the relative temperature coefficient αμir of the initial permeability at a frequency of 100 kHz is −3.0×10 in the temperature range of −40 to 20° C. -6 Preferably, the Ni-based ferrite has a temperature of from 0.3 mol% to 0.7 mol% and the total amount of Fe2O3 and MnO is from 47.5 mol% to 47.9 mol%. Such Ni-based ferrite has a small relative temperature coefficient αμir in the temperature range of -40 to 120°C, and the change is negative, so that the inductance fluctuation with respect to temperature change is further reduced.

[0016] The second invention is a coil component using the Ni-based ferrite of the first invention, the coil component including a coil and a magnetic core made of the Ni-based ferrite of the first invention arranged in the magnetic path of the coil, at least a part of which is coated with resin. According to the coil component of the present invention, the variation of inductance is small with respect to the compressive stress generated between the coating resin and the Ni-based ferrite. Effect of the Invention

[0017] According to the present invention, it is possible to provide an Ni-based ferrite having a large initial permeability μi, small fluctuation in the initial permeability μi with respect to temperature changes, and a relative temperature coefficient αμir of 0 / °C or less, and a coil component using the same. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a perspective view showing an example of a coil component of the present invention. [Diagram 2] 1 is a graph showing the relationship between the total molar amount of Fe2O3 and MnO and the relative temperature coefficient αμir in a Ni-based ferrite according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The following is a description of an Ni-based ferrite according to one embodiment of the present invention and a coil component using the same. However, the present invention is not limited to this, and the scope of the technical idea is The above can be changed as appropriate.

[0020] (A) Composition The Ni-based ferrite of this embodiment is composed of a composition in which the total amount of Fe2O3, ZnO, CuO, MnO, and NiO is 100 mol%, Fe2O3 is 47.0 mol% to 47.5 mol%, ZnO is 28.0 mol% to 32.0 mol%, CuO is 6.0 mol% to 9.0 mol%, MnO is 0.3 mol% to 1.2 mol%, and the balance is NiO, and the total amount of Fe2O3 and MnO is 47.5 mol% to 48.2 mol%. Each raw material may contain unavoidable impurity elements of about several ppm to several hundred ppm. Specific examples of unavoidable impurity elements include Si, Ca, B, C, S, Cl, Se, Br, Te, I, Li, Na, Mg, Al, K, Ga, Ge, Sr, In, Sn, Sb, Ba, Bi, Sc, Ti, V, Cr, Y, Nb, Mo, Pd, Ag, Hf, and Ta, but the total amount of unavoidable impurities in Ni-based ferrite is preferably 1 part by mass or less per 100 parts by mass of Fe2O3, ZnO, CuO, MnO, and NiO, and is preferably kept as low as possible. Of the unavoidable impurities, Na, S, Cl, P, Cr, and B are preferably as low as possible, and the industrially acceptable range is preferably 0.1 parts by mass or less in total, more preferably 0.05 parts by mass or less.

[0021] The composition of this embodiment will be described below. In general, the relative temperature coefficient αμir tends to increase as the amount of Fe2O3 increases. In the Ni-based ferrite of the present invention, Fe2O3 is set to 47.0 mol% or more and 47.5 mol% or less so that the relative temperature coefficient αμir is negative in the high-temperature range, particularly in the temperature range of 20 to 120°C. By adjusting the relative temperature coefficient αμir by setting MnO to 0.3 mol% or more and 1.2 mol% or less, and setting the total amount with Fe2O3 to 47.5 mol% or more and 47.9 mol% or less, the relative temperature coefficient αμir is set to -2.0×10 in the two temperature ranges of 20 to 85°C and 20 to 120°C. -6 The temperature must be between 0 / ℃ and 20 / ℃.

[0022] If Fe2O3 is less than 47.0 mol%, the relative temperature coefficient αμir becomes large on the negative side, and if it exceeds 47.5 mol%, it becomes large on the positive side, and even by adjusting the relative temperature coefficient αμir with MnO, the desired relative temperature coefficient αμir may not be obtained in the two temperature ranges of 20 to 85°C and 20 to 120°C.

[0023] MnO is considered to form Mn ferrite [Fe2O3·(Mn,Zn)O], and is also effective in improving the initial magnetic permeability μi. If the MnO content is less than 0.3 mol%, the desired relative temperature coefficient αμir may not be obtained, or the effect of improving the initial magnetic permeability μi may not be obtained. Alternatively, if the MnO content exceeds 1.2 mol%, the desired relative temperature coefficient αμir may not be obtained. The more preferable MnO content is 0.3 mol% or more and 0.7 mol% or less.

[0024] If the ZnO content is less than 28.0 mol%, the desired initial permeability cannot be obtained, and if it exceeds 32.0 mol%, the Curie temperature decreases and the desired relative temperature coefficient αμir may not be obtained. Note that the Curie temperature Tc calculated from the molar amounts of Fe2O3 and ZnO is in the range of approximately 110 to 190°C if the Fe content and Zn content are within the above ranges, and there is no practical problem even if the temperature exceeds 100°C.

[0025] If the CuO content is less than 6.0 mol%, the densification is insufficient and it is difficult to obtain the desired initial permeability. On the other hand, if it exceeds 9.0 mol%, many coarse grains exceeding 20 μm appear in the crystal structure, and the preferable stress characteristics may not be obtained. The preferable CuO content is 6.5 mol% or more, more preferably 7.0 mol% or more, and even more preferably 7.5 mol% or more. Also, 8.5 mol% or less is preferable.

[0026] The balance is NiO, which is preferably 10.3 mol% or more and 18.7 mol% or less. Preferably, NiO is 12.0 mol% or more, and more preferably 13.0 mol% or more. Preferably, NiO is 17.0 mol% or less, and more preferably 16.0 mol% or less.

[0027] The amount of each component can be determined by X-ray fluorescence analysis and ICP atomic emission spectrometry. The qualitative analysis of the contained elements is first performed by X-ray fluorescence analysis, and then the contained elements are quantified by a calibration curve method that compares them with standard samples.

[0028] (B) Manufacturing method of Ni-based ferrite core When manufacturing the magnetic core of the Ni-based ferrite of this embodiment, it is preferable to wet mix Fe2O3, ZnO, CuO, MnO, and NiO in a predetermined ratio, dry them, and calcinate them at 800 to 1000°C to obtain a calcined powder that has been converted into a spinel. The calcined powder obtained is then put into a ball mill together with ion-exchanged water, and pulverized to an average pulverized particle size (air permeation method) of 1.7 to 2.1 μm to obtain a slurry. Polyvinyl alcohol is added as a binder to the obtained slurry, and the mixture is granulated using a spray dryer, followed by pressure molding to obtain a molded body of a predetermined shape.

[0029] The obtained compact is sintered in a sintering furnace to obtain a Ni-based ferrite magnetic core. The sintering process includes a temperature increase process, a high-temperature holding process, and a temperature decrease process. The atmosphere in the sintering process may be an inert gas atmosphere or an air atmosphere. Here, the compact passes through the temperature increase process, reaches the high temperature set in the high-temperature holding process, and is sintered. In this high-temperature holding process, the set temperature of the sintering furnace is preferably 1050 to 1200°C. If the temperature is less than 1050°C, sintering is insufficient, the initial permeability μi is small, and the strength of the magnetic core may not be obtained. Also, if the temperature exceeds 1200°C, sintering becomes excessive, and the energy consumption of the sintering furnace increases, which is not preferable because it leads to an increase in manufacturing costs.

[0030] An example of the configuration of an antenna used in an antenna circuit, suitable for using such a Ni-based ferrite core, is shown in Fig. 1. Antenna 1 is a coil component including coil 5, magnetic core 7 passing through the air-core portion of coil 5, and resin material 8 (shown by dashed lines) that covers at least a portion of coil 5 and magnetic core 7, and is also called a resin molded antenna. From the viewpoints of heat resistance, insulation, moldability, etc., the resin used for molding is a thermosetting resin such as epoxy resin or a thermoplastic resin such as liquid crystal polymer.

[0031] An antenna circuit using an antenna made of the coil component of the present invention can be configured with a resonant circuit in which a capacitor is connected in parallel with the antenna, and a control circuit. The resonant frequency determined by the inductance of the antenna and the capacitance of the capacitor is set according to the communication frequency, but according to the present invention, the fluctuation of the initial permeability μi due to temperature changes is suppressed, so the inductance is stable and the communication function as an antenna is not impaired.

[0032] The present invention will be described in more detail by the following examples, but the present invention is not limited thereto. EXAMPLES

[0033] The raw materials were wet mixed so that the components Fe2O3, ZnO, CuO, MnO and NiO were in the proportions shown in Table 1, then dried and calcined at 900°C for 1 hour. The calcined powder obtained was put into a ball mill together with ion-exchanged water and pulverized to an average pulverized particle size of 1.9 μm to produce a slurry. Polyvinyl alcohol was added as a binder to the obtained slurry, which was then granulated using a spray dryer and pressed to produce a ring-shaped compact.

[0034] The obtained compact was sintered in a sintering furnace in air at 1120°C for 2 hours to obtain a ring-shaped Ni-based ferrite core with an outer diameter of 30 mm, an inner diameter of 20 mm, and a height of 10 mm. The average crystal grain size of samples No. 1 to No. 7 was 8 to 12 μm.

[0035] [Table 1]

[0036] The initial permeability μi, relative temperature coefficient αμir, relative loss coefficient tan δ / μi, and sintered density ds of each sample were measured by the following methods. (1) Initial permeability μi Each sample was used as the object to be measured, and a conductor was wound 20 turns to form a coil component. The inductance was measured using an LCR meter (Agilent Technologies 4285A) at a temperature of 20°C, a frequency of 100 kHz, and a current of 1 mA in a thermostatic chamber, and the inductance was calculated using the following formula. Initial permeability μi=(le×L) / (μ0×Ae×N 2 ) (le: magnetic path length, L: inductance of the sample (H), μ0: magnetic permeability of vacuum = 4π×10 -7 (H / m), Ae: cross-sectional area of ​​the magnetic core, N: number of turns of the conductor) ll

[0037] (2) Relative loss factor tanδ / μi In measuring the initial magnetic permeability μi, the loss factor tanδ was calculated by determining the inductance L (H) and resistance (Ω) of the sample measured using an LCR meter (4285A manufactured by Agilent Technologies) at a temperature of 20°C, a frequency of 100 kHz, and a current of 1 mA, and dividing the loss factor by the initial magnetic permeability μi.

[0038] (3) Relative temperature coefficient αμir αμir = [(μi2-μi1) / μi1 2 〕 / (T2-T1) (where T1 and T2 are measurement temperatures, μi1 is the initial permeability at temperature T1, and μi2 is the initial permeability at temperature T2.) The initial magnetic permeability μi was measured by the above-mentioned method and conditions for the coil components adjusted to -40°C to 120°C in an electronic thermostatic bath. In the case of the relative temperature coefficient αμir of -40°C to 20°C, T1=20°C, T2=-40°C, μi1 is the initial magnetic permeability at 20°C, and μi2 is the initial magnetic permeability at -40°C. In the case of 20°C to 85°C, T1=20°C, T2=85°C, μi1 is the initial magnetic permeability at 20°C, and μi2 is the initial magnetic permeability at 85°C. In the case of 20°C to 120°C, T1=20°C, T2=120°C, μi1 is the initial magnetic permeability at 20°C, and μi2 is the initial magnetic permeability at 120°C.

[0039] (4) Sintered density ds The sintered density of each sample was calculated by the underwater displacement method using Archimedes' principle.

[0040] The results obtained are summarized in Table 2. Also, Fig. 2 shows a graph showing the relationship between the total molar amount of Fe2O3 and MnO and the relative temperature coefficient αμir.

[0041] [Table 2]

[0042] In the samples No. 1 to 7*, the initial permeability μi was 465 or more. The relative temperature coefficient αμir was −3.0×10 in the temperature range of 20 to 85° C. in the samples No. 1 to 4 (Ni-based ferrite cores) of the embodiment in which the total amount of Fe2O3 and MnO was 47.5 mol % or more and 48.2 mol % or less. -6 / ℃ or more and 0 / ℃ or less, and in the temperature range of 20 to 120℃, -2.0×10 -6 / °C or more and 0 / °C or less, and according to the examples of the present invention, the rate of change of initial permeability with respect to the higher temperature side with 20°C as the reference was small, and the relative temperature coefficient αμir was 0 / °C or less. On the other hand, in the comparative samples No. 5* to 7* in which the total amount of Fe2O3 and MnO exceeds 48.2 mol%, the relative temperature coefficient αμir exceeded 0 / °C and became a positive value. In addition, in the samples No. 1 and 2 in which the total amount of Fe2O3 and MnO is 47.9 mol% or less, the relative temperature coefficient αμir was -3.0×10 -6 / ℃ or more and 0 / ℃ or less. As shown in Figure 2, the relative temperature coefficient αμir showed a positive correlation with the total amount of Fe2O3 and MnO in both the temperature range of 20 to 85℃ and the temperature range of 20 to 120℃, and showed a similar tendency in the temperature range of -40 to 20℃.

[0043] Coil components using such Ni-based ferrite of the present invention have small fluctuations in inductance due to temperature changes, and can be used as small antennas. [Explanation of symbols]

[0044] 1 Antenna 5 Coil 7. Ni-based ferrite core 8 Resin material

Claims

1. The initial permeability μi at a temperature of 20° C. and a frequency of 100 kHz is 465 or more. The relative temperature coefficient αμir of the initial permeability at a frequency of 100 kHz is −3.0×10 in the temperature range of 20 to 85° C. -6 / °C or more and 0 / °C or less, and in the temperature range of 20 to 120°C, -2.0 x 10 -6 A magnetic core using Ni-based ferrite having a temperature of 0°C or higher and a temperature of 10°C or lower, The composition of the Ni-based ferrite is 47.0 mol % or more and 47.5 mol % or less of Fe 2 O 3 , 28.0 mol % to 32.0 mol % ZnO, 0.3 mol % to 1.2 mol % MnO, the balance being CuO and NiO, and Fe 2 O 3 and MnO in a total amount of 47.5 mol % or more and 48.2 mol % or less, and ZnO / Fe 2 O 3 A magnetic core using Ni-based ferrite having a magnetic constant of 0.628 to 0.

631.

2. 2. A magnetic core using the Ni-based ferrite according to claim 1, wherein CuO is 6.0 mol % or more and 9.0 mol % or less.

3. The relative temperature coefficient αμir of the initial permeability at a frequency of 100 kHz is −3.0×10 in the temperature range of −40 to 20° C. -6 A magnetic core using Ni-based ferrite having a temperature of 0°C or higher and a temperature of 10°C or lower, MnO is 0.3 mol % or more and 0.7 mol % or less, Fe 2 O 3 2. A magnetic core using Ni-based ferrite according to claim 1, wherein the total amount of NiO is 47.5 mol % or more and 47.9 mol % or less.

4. 4. A coil component comprising: the magnetic core according to claim 1; and a coil having the magnetic core disposed in a magnetic path, the coil being at least partially coated with resin.

Citation Information

Patent Citations

  • Soft-magnetic nickel-copper-zinc ferrite material and preparation method thereof

    CN102690109A

  • NiCuZn soft magnetic ferrite material used for low temperature co-sintering and preparation method thereof

    CN102690110A

  • Inductor and oxide magnetic material

    JP1994140229A

  • Ferrite material

    JP1998101410A

  • Oxide magnetic material, ferrite core, coil component, and transformer

    JP2002289421A