Moisture-curable polyurethane resin composition, adhesive, and laminate
The moisture-curable polyurethane hot melt resin composition addresses the issue of poor adhesion to water-repellent fabrics by using a urethane prepolymer with a specific compound, ensuring strong adhesion and wash resistance while being environmentally friendly.
Patent Information
- Application Number
- JP2023548656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-01
AI Technical Summary
Existing moisture-curable polyurethane resin compositions fail to exhibit high adhesion to super water-repellent fabrics and have poor wash resistance.
A moisture-curable polyurethane hot melt resin composition containing a urethane prepolymer with a specific compound (a1) having a hydroxyl group at both ends, a silicone chain, and a long-chain alkyl group, which is produced by reacting a polyol (A) and a polyisocyanate (B), ensuring excellent adhesion to water-repellent fabrics and wash resistance.
The composition achieves excellent adhesion to various fabrics, particularly water-repellent fabrics, and demonstrates superior wash resistance without using solvents, making it environmentally friendly.
Smart Images

Figure 0007568124000001 
Figure 0007568124000002 
Figure 0007568124000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a moisture-curable polyurethane resin composition, an adhesive, and a laminate. [Background technology]
[0002] Moisture-permeable, waterproof functional clothing, which has both moisture permeability and waterproofness, is a structure in which a moisture-permeable film is bonded to a fabric with an adhesive, and as the adhesive, a urethane-based adhesive is generally used because of its good adhesion to both the moisture-permeable film and the fabric. Among the urethane-based adhesives, the amount of use of solvent-free moisture-curable polyurethane resin compositions is gradually increasing due to recent global regulations on solvent emissions and residual solvents (see, for example, Patent Document 1).
[0003] On the other hand, the fabrics used are becoming lighter and more functional, with finer denier fabrics and improved water repellency, which poses the issue of reduced adhesion between the water-repellent treated fabric and the adhesive. However, no current moisture-curing polyurethane resin compositions have been found that exhibit high adhesion, particularly to ultra-water-repellent fabrics. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-202608 A Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved by the present invention is to provide a moisture-curable polyurethane resin composition that has excellent adhesion to fabrics (particularly water-repellent fabrics) and washing resistance. [Means for solving the problem]
[0006] The present invention relates to a moisture-curable polyurethane hot-melt resin composition containing a urethane prepolymer (i) having an isocyanate group, which is a reaction product of a polyol (A) and a polyisocyanate (B), wherein the polyol (A) contains a compound (a1) represented by the following general formula (1):
[0007] [ka] (In formula (1), R1 and R2 each represent an alkylene group having 1 to 6 carbon atoms, m and n each represent an integer of 10 to 40 in total, and a represents an integer of 5 to 30.)
[0008] The present invention also provides an adhesive comprising the moisture-curable polyurethane resin composition. The present invention also provides a laminate comprising at least a substrate (i) and a cured product of the moisture-curable polyurethane resin composition. Effect of the Invention
[0009] The moisture-curable polyurethane hot-melt resin composition of the present invention does not contain a solvent and is an environmentally friendly material. In addition, the moisture-curable polyurethane hot-melt resin composition of the present invention has excellent adhesion to various fabrics, has excellent adhesion to water-repellent fabrics, and is also excellent in washing resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The moisture-curable polyurethane hot-melt resin composition used in the present invention is a reaction product of a polyol (A) containing a specific compound and a polyisocyanate (B), and contains a urethane prepolymer (i) having an isocyanate group.
[0011] It is essential that the polyol (A) contains the compound (a1) represented by the general formula (1) described above in order to obtain excellent adhesion to fabrics (particularly water-repellent fabrics) and washing resistance.
[0012] It is believed that by introducing a compound having hydroxyl groups at both ends, a silicone chain, and a long-chain alkyl group, such as the compound (a1), into the polyol (A), the permeability (affinity) to water-repellent fabrics is improved, and excellent adhesion and washing resistance are exhibited.
[0013] In the compound (a1), R1 is preferably an alkylene group having 1 to 2 carbon atoms, more preferably an ethylene group, from the viewpoint of obtaining even better adhesiveness and wash resistance. R2 is preferably an alkylene group having 3 to 6 carbon atoms, more preferably a propylene group. m is preferably an integer of 5 to 20, more preferably an integer of 5 to 15, and n is preferably an integer of 0 to 40, more preferably an integer of 0 to 20. a is preferably an integer of 5 to 30, more preferably an integer of 10 to 20.
[0014] The amount of the compound (a1) used is preferably from 0.5 to 30% by mass, and more preferably from 1.0 to 15% by mass, in the polyol (A) in terms of obtaining even better adhesiveness and washing resistance.
[0015] The polyol (A) may be used in combination with other polyols than the compound (a1). As the other polyols, for example, polyester polyols, polyether polyols, polycarbonate polyols, polyacrylic polyols, etc. may be used. These polyols may be used alone or in combination of two or more. Among these, polyester polyols and / or polyether polyols are preferred because they provide even better mechanical strength.
[0016] As the polyester polyol, for example, a reaction product of a polybasic acid and a compound having two or more hydroxyl groups can be used.
[0017] Examples of the polybasic acid include oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedicarboxylic acid, glutaric acid, pimelic acid, suberic acid, dimer acid, sebacic acid, undecanedicarboxylic acid, hexahydroterephthalic acid, and phthalic acid compounds (phthalic acid, phthalic anhydride, isophthalic acid, and terephthalic acid). These polybasic acids may be used alone or in combination of two or more. Among these, adipic acid and / or phthalic acid compounds are preferred because they provide even better adhesion and mechanical strength.
[0018] Examples of the reaction products with the compound having two or more of the above groups include ethylene glycol, diethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, hexamethylene glycol, glycerin, trimethylolpropane, bisphenol A, bisphenol F, and their alkylene oxide adducts, 2-methyl-1,3-propanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 2,2,4 -trimethyl-1,3-pentanediol, 1,2-butanediol, 1,3-butanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-propanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-isopropyl-1,4-butanediol, 2,4-dimethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-ethyl-1,6-hexanediol, 3,5-heptanediol, 2-methyl-1,8-octanediol, neopentyl glycol, trimethylolpropane, etc. can be used. These compounds may be used alone or in combination of two or more.
[0019] The number average molecular weight of the polyester polyol is preferably 500 to 10,000, and more preferably 700 to 5,000, in terms of obtaining even better adhesiveness and mechanical strength. The number average molecular weight of the polyester polyol is a value measured by gel permeation chromatography (GPC).
[0020] When the polyester polyol is used, the amount used is preferably from 10 to 100% by mass, and more preferably from 30 to 100% by mass, in the polyol (A) in terms of obtaining even better mechanical strength.
[0021] As the polyether polyol, for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, etc. can be used. These may be used alone or in combination of two or more. Among these, polypropylene glycol is preferred because it provides even more excellent adhesiveness and mechanical strength.
[0022] The number average molecular weight of the polyether polyol is preferably 500 to 10,000, and more preferably 700 to 5,000, in terms of obtaining even better adhesiveness and mechanical strength. The number average molecular weight of the polyether polyol is a value measured by gel permeation chromatography (GPC).
[0023] When the polyether polyol is used, the amount used is preferably from 0 to 90% by mass, more preferably from 0 to 70% by mass, in the polyol (A) in terms of obtaining even better mechanical strength.
[0024] As the polyisocyanate (B), aromatic polyisocyanates such as polymethylene polyphenyl polyisocyanate, diphenylmethane diisocyanate, carbodiimide-modified diphenylmethane diisocyanate isocyanate, xylylene diisocyanate, phenylene diisocyanate, tolylene diisocyanate, and naphthalene diisocyanate; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and tetramethylxylylene diisocyanate can be used. These polyisocyanates may be used alone or in combination of two or more. Among these, aromatic polyisocyanates are preferably used, and diphenylmethane diisocyanate is more preferably used, because they have better reactivity and adhesion to fabrics.
[0025] The amount of the polyisocyanate (B) used is preferably from 5 to 40 mass %, more preferably from 10 to 30 mass %, based on the total mass of the raw materials constituting the urethane prepolymer (i).
[0026] The hot-melt urethane prepolymer (i) is obtained by reacting the polyol (A) with the polyisocyanate (B), and has an isocyanate group that can form a crosslinked structure by reacting with moisture present in the air or in the substrate to which the moisture-curable polyurethane hot-melt resin composition is applied.
[0027] The hot-melt urethane prepolymer (i) can be produced, for example, by adding the polyisocyanate (B) to a reaction vessel containing the polyol (A) and reacting them under conditions in which the isocyanate groups of the polyisocyanate (B) are in excess of the hydroxyl groups of the polyol (A).
[0028] In producing the hot-melt urethane prepolymer (i), the equivalent ratio (isocyanate group / hydroxyl group) of the isocyanate group in the polyisocyanate (B) to the hydroxyl group in the polyol (A) is preferably 1.1 to 5, and more preferably 1.5 to 3.0, in order to obtain even better adhesion to fabrics.
[0029] The isocyanate group content (hereinafter abbreviated as "NCO%) of the hot-melt urethane prepolymer (i) obtained by the above method is preferably in the range of 1.7 to 5, more preferably 1.8 to 3.0, in order to obtain even better adhesiveness. The NCO% of the hot-melt urethane prepolymer (i) is a value measured by potentiometric titration in accordance with JIS K1603-1:2007.
[0030] The moisture-curable polyurethane hot-melt resin composition used in the present invention contains the urethane prepolymer (i) as an essential component, but may contain other additives as necessary.
[0031] Examples of the other additives that can be used include light resistance stabilizers, curing catalysts, tackifiers, plasticizers, stabilizers, fillers, dyes, pigments, fluorescent brighteners, silane coupling agents, waxes, thermoplastic resins, etc. These additives may be used alone or in combination of two or more.
[0032] As described above, the moisture-curable polyurethane hot melt resin composition of the present invention does not contain a solvent and is an environmentally friendly material. In addition, the moisture-curable polyurethane hot melt resin composition of the present invention has excellent adhesion to various fabrics, has excellent adhesion to water-repellent fabrics, and is also excellent in washing resistance.
[0033] Next, the laminate of the present invention will be described.
[0034] The laminate of the present invention comprises at least a base material (i) and a cured product of the moisture-curable polyurethane hot-melt resin composition.
[0035] Examples of the fabric (i) that can be used include fiber substrates such as nonwoven fabrics, woven fabrics, knitted fabrics, etc. made of polyester fibers, polyethylene fibers, nylon fibers, acrylic fibers, polyurethane fibers, acetate fibers, rayon fibers, polylactic acid fibers, cotton, hemp, silk, wool, glass fibers, carbon fibers, and blends thereof; nonwoven fabrics impregnated with resins such as polyurethane resin; nonwoven fabrics further provided with a porous layer; and resin substrates.
[0036] In addition, the present invention also provides a fabric (i) that has been subjected to a water-repellent treatment (hereinafter, abbreviated as "water-repellent fabric") and shows excellent adhesiveness. In the present invention, the "water-repellent" of the water-repellent fabric is defined as a fabric having a surface free energy of 50 mJ / m2 calculated as follows: 2 Show that:
[0037] The contact angles of the test liquids (water and diiodomethane) on the fabric (i) were measured using a contact angle meter ("DM500" manufactured by Kyowa Interface Science Co., Ltd.) Based on the results, the surface free energy of the fabric (i) was calculated using the following formula (1). (1+cosA)·γL / 2=(γsd·γLd)1 / 2+(γsp·γLp)1 / 2
[0038] A: Contact angle of the test liquid on the fabric (i) γL: Surface tension of the liquid to be measured γLd: Dispersion force component of the surface free energy of the liquid to be measured γLp: Polar component of the surface free energy of the liquid to be measured γsd: Dispersion force component of the surface free energy of the fabric (i) γsp; the polar component of the surface free energy of substrate (i)
[0039] Examples of a method for applying the moisture-curable polyurethane hot-melt resin composition include methods using a roll coater, a knife coater, a spray coater, a gravure roll coater, a comma coater, a T-die coater, an applicator, a dispenser, and the like.
[0040] After the moisture-curable polyurethane hot-melt resin composition is applied, it can be dried and cured by a known method.
[0041] The thickness of the cured product of the moisture-curable urethane hot-melt resin composition is, for example, in the range of 5 to 300 μm.
[0042] In addition, when the moisture-curable polyurethane hot melt resin composition of the present invention is used as an adhesive for moisture-permeable waterproof functional clothing, the moisture-curable polyurethane hot melt resin composition is preferably intermittently applied by a gravure roll coater or a dispenser, and the fabric (i) is bonded to a known moisture-permeable film. In such a case, the thickness of the cured product of the moisture-curable polyurethane hot melt resin composition is, for example, in the range of 5 to 50 μm.
[0043] A mesh fabric may be laminated onto the moisture-permeable film by intermittently applying a moisture-curable polyurethane hot-melt resin composition. EXAMPLES
[0044] The present invention will now be described in more detail with reference to examples.
[0045] [Example 1] A four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet, and a reflux condenser was charged with 495 parts by mass of polyester polyol 1 (a reaction product of adipic acid and 2-methyl-1,3-propanediol, number average molecular weight: 2,000), 495 parts by mass of polyester polyol 2 (a reaction product of phthalic anhydride, diethylene glycol, and neopentyl glycol, number average molecular weight: 1,000), and 10 parts by mass of a compound in which R1 is an ethylene group, m is 20, n is 0, and a is 15 in formula (1) (hereinafter abbreviated as "a1-1"). The mixture was then dried under reduced pressure at 110°C to dehydrate it until the water content was 0.05% by mass or less. Next, after cooling to 60°C, 331 parts by mass of diphenylmethane diisocyanate (hereinafter abbreviated as "MDI") was added, the temperature was raised to 110°C, and the reaction was carried out for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (1), which was used as a moisture-curable polyurethane hot-melt resin composition (1).
[0046] [Example 2] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 150 parts by mass of polyester polyol 3 (1,6-hexanediol and phthalic anhydride reacted, number average molecular weight: 2,000), 700 parts by mass of polyester polyol 4 (phthalic anhydride, adipic acid, terephthalic acid, and ethylene glycol reacted, number average molecular weight: 3,500), and 30 parts by mass of a compound in which R1 is an ethylene group, m is 15, n is 5, and a is 15 in the formula (1) (hereinafter abbreviated as "a1-2"). The mixture was dried under reduced pressure at 110 ° C. and dehydrated until the water content was 0.05% by mass or less. Next, after cooling to 60 ° C., 200 parts by mass of MDI was added, the temperature was raised to 110 ° C., and the mixture was reacted for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (2), which was a moisture-curable polyurethane hot melt resin composition (2).
[0047] [Example 3] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 295 parts by mass of polypropylene glycol 1 (number average molecular weight: 400), 295 parts by mass of polypropylene glycol 2 (number average molecular weight: 1,000), and 30 parts by mass of a compound in which R1 is an ethylene group, m is 10, n is 10, and a is 15 in the formula (1) (hereinafter abbreviated as "a1-3"). The mixture was dried under reduced pressure at 110 ° C. and dehydrated until the water content was 0.05% by mass or less. Next, after cooling to 60 ° C., 459 parts by mass of MDI was added, the temperature was raised to 110 ° C., and the mixture was reacted for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (3), which was a moisture-curable polyurethane hot melt resin composition (3).
[0048] [Comparative Example 1] In a four-neck flask equipped with a thermometer, a stirrer, an inert gas inlet and a reflux condenser, 495 parts by mass of polyester polyol 1 (adipic acid and 2-methyl-1,3-propanediol reacted, number average molecular weight: 2,000), 495 parts by mass of polyester polyol 2 (phthalic anhydride, diethylene glycol and neopentyl glycol reacted, number average molecular weight: 1,000), and dried under reduced pressure at 110 ° C. to dehydrate until the water content was 0.05 mass% or less. Next, after cooling to 60 ° C., 331 parts by mass of diphenylmethane diisocyanate (hereinafter abbreviated as "MDI") was added, the temperature was raised to 110 ° C., and the mixture was reacted for 2 hours until the isocyanate group content became constant, thereby obtaining a urethane prepolymer (R1), which was used as a moisture-curable polyurethane hot melt resin composition (R1).
[0049] [Method for measuring number average molecular weight] The number average molecular weights of the polyols used in the examples and comparative examples are values measured by gel permeation chromatography (GPC) under the following conditions.
[0050] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene.
[0051] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0052] [How to make the laminate] First, a mixture of solvent-based polyurethane resin "Crisbon S-525 (DIC Corporation)", methyl ethyl ketone, and dimethylformamide was evenly applied onto release paper using a knife coater to a coating amount of 100 g / m2 (wet), and then dried at 70°C for 1 minute and then at 120°C for 2 minutes to produce a moisture-permeable polyurethane film with a thickness of 15 μm. Next, the moisture-curable polyurethane resin compositions (1) to (3) and (R1) which had been heated and melted at 120°C were each applied at a rate of 20 g / m onto the moisture-permeable polyurethane film 1 using a lattice-shaped gravure roll heated to 120°C. 2 After intermittently applying the solution, the mixture was laminated with a 40 denier water-repellent treated nylon taffeta, a fibrous substrate, and left for 3 days in an environment of 23°C and 65% relative humidity to produce a laminate.
[0053] [Method for evaluating adhesion to fabric] A 1-inch-wide hot melt cloth tape was adhered to the moisture-permeable polyurethane film side of the obtained laminate at 130°C for 5 seconds, and then the normal adhesive strength was measured at a temperature of 23°C and a relative humidity of 50% using Shimadzu Corporation's Autograph AG-1 (head speed: 200mm / min) in accordance with JIS K6854-2.Measurements of 6.0N / inch or more were deemed to have excellent adhesion to water-repellent fabric.
[0054] [How to evaluate washability] The obtained laminate was washed 50 times in water in accordance with JIS L 1089-1970, and the appearance after washing was evaluated by visual inspection according to the following criteria. "Good": No peeling was observed at all. "X": More than half of the adhesive area was peeled off.
[0055] [Table 1]
[0056] It was found that the moisture-curable polyurethane hot-melt resin composition of the present invention has excellent adhesion to water-repellent fabrics and washing resistance.
[0057] On the other hand, Comparative Example 1, which is an embodiment in which compound (a1) was not used, had poor adhesion to water-repellent fabric and poor washability.
Claims
1. A moisture-curable polyurethane hot-melt resin composition comprising a urethane prepolymer (i) having an isocyanate group, the urethane prepolymer (i) being a reaction product of a polyol (A) and a polyisocyanate (B), The polyol (A) contains a compound (a1) represented by the following general formula (1) and one or more polyols selected from a polyester polyol, a polyether polyol, a polycarbonate polyol, and a polyacrylic polyol, The amount of the compound (a1) used in the polyol (A) is in the range of 0.5 to 30 mass%. 【Chemistry 1】 (In formula (1), R 1 and R 2 each represents an alkylene group having 1 to 6 carbon atoms, the sum of m and n represents an integer of 10 to 40, and a represents an integer of 5 to 30.
2. The moisture-curable polyurethane hot-melt resin composition according to claim 1 , wherein the polyol (A) contains the polyester polyol and / or the polyether polyol.
3. The polyol (A) contains the polyether polyol, 2. The moisture-curable polyurethane hot-melt resin composition according to claim 1, wherein the polyether polyol is polypropylene glycol.
4. An adhesive comprising the moisture-curable polyurethane hot-melt resin composition according to claim 1.
5. A laminate comprising at least a substrate (i) and a cured product of the moisture-curable polyurethane hot melt resin composition according to claim 1.
6. 6. The laminate according to claim 5, wherein the fabric (i) is a water-repellent fabric.
Citation Information
Patent Citations
Polyether-polysiloxane polyol
JP2008174749A
A mixture of polydiorganosiloxane-containing silylated polyurethane and silylated polyurethane, a substrate containing the same, and a process for producing the substrate.
JP2013528667A