Isotropic nanocomposite iron-based rare earth boron magnet alloy, manufacturing method for isotropic nanocomposite iron-based rare earth boron magnet alloy, and manufacturing method for resin-bonded permanent magnet

The iron-based rare earth boron isotropic nanocomposite magnet alloy addresses the trade-off in magnetic properties by optimizing the grain boundary phase and grain size, achieving high HcJ and Br suitable for electric motors without heavy rare earth elements.

JP7568163B2Active Publication Date: 2024-10-16MURATA MFG CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024507025
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-14
Filing Date
2023-06-22
Publication Date
2024-10-16
Estimated Expiration
2043-06-22

AI Technical Summary

Technical Problem

Existing iron-based rare earth boron isotropic magnets face challenges in achieving high intrinsic coercive force HcJ and residual magnetic flux density Br, particularly for applications in electric vehicles (EVs) and hybrid electric vehicles (HEVs), due to the trade-off relationship between these properties and the presence of non-magnetic additives like Ti, which affect magnetization.

Method used

The development of an iron-based rare earth boron isotropic nanocomposite magnet alloy with a specific composition and manufacturing process, including a unique metal structure with a B-type tetragonal compound as the main phase and a grain boundary phase rich in Fe, optimized through the addition of Zr and controlled grain sizes, to enhance exchange interactions and maintain high magnetic properties.

Benefits of technology

The alloy achieves a high intrinsic coercive force HcJ of 1200 kA/m or more and residual magnetic flux density Br of 0.81T or more, suitable for electric motors, without the need for heavy rare earth elements like Dy and Tb, and maintains excellent magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568163000004
    Figure 0007568163000004
  • Figure 0007568163000005
    Figure 0007568163000005
  • Figure 0007568163000006
    Figure 0007568163000006
Patent Text Reader

Abstract

The present invention provides an iron base rare earth boron-based isotropic nanocomposite magnet alloy which has an alloy composition that has a composition which is represented by the composition formula T100-x-y-z(B1-nCn)xREyZrzMm (wherein: T represents one or more transition metal elements that are selected from the group consisting of Fe, Co and Ni, and necessarily includes Fe; RE represents one or more rare earth elements that are selected from among Nd and Pr, and necessarily includes Nd; and M represents one or more metal elements that are selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb), wherein the compositional ratios x, y, and z respectively satisfy 4.2% by atom ≤ x ≤ 5.0% by atom, 12.5 % by atom ≤ y ≤ 14.0% by atom, 0% by atom < z ≤ 2.0% by atom, 0.0% by atom ≤ m ≤ 5.0% by atom, and 0.0 ≤ n ≤ 0.5. This iron base rare earth boron-based isotropic nanocomposite magnet alloy has a metal structure which has, as a main phase, an RE2Fe14B-type tetragonal compound that has a lower B concentration than the stoichiometric composition of an RE2Fe14B-type tetragonal compound, while having an average crystal grain size of not less than 10 nm but less than 70 nm, the average crystal grain size being smaller than the single domain critical diameter, and which comprises a phase that is richer in Fe than the main phase in the grain boundary phase that surrounds the main phase.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an iron-based rare earth boron isotropic nanocomposite magnet alloy, a method for producing an iron-based rare earth boron isotropic nanocomposite magnet alloy, and a method for producing a resin-bonded permanent magnet. [Background technology]

[0002] In recent years, microcrystalline isotropic magnets composed of hard magnetic phases such as Nd-Fe-B and Sm-Fe-N, which are made up of fine crystal grains with sizes on the order of nanometers to submicrometers, and nanocomposite isotropic magnets (hereinafter referred to as "nanocomposite magnets"), in which hard magnetic phases such as Nd-Fe-B and Sm-Fe-N, which are made up of fine crystal grains, and soft magnetic phases such as Fe-B phase and α-Fe phase exist in the same metal structure, have been developed. It has been clarified by computer simulations using micromagnetics that these rare earth iron-based isotropic magnets composed of crystal grains with sizes on the order of nanometers to submicrometers exhibit excellent magnetic properties because the crystal grains are magnetically bonded by exchange interactions in addition to static magnetic interactions due to their fine crystal grains, and these magnets have been put to practical use as high-performance permanent magnet materials.

[0003] Up until now, fine-crystalline rare earth iron-based isotropic magnets have been used mainly in the electronic parts industry, taking advantage of their isotropic properties, as net-shape magnets with high freedom of shape, which are made by grinding the magnets to an average particle size of 50 μm or more and 200 μm or less and then mixing them with epoxy resin-based thermosetting resins or thermoplastic resins such as nylon and polyphenylene sulfide (PPS) to make resin-bonded magnets (commonly known as bonded magnets), taking advantage of their isotropic properties and used in optical drives, spindle motors for hard disks, vibration motors (pager motors) for mobile phones, various sensors, etc. In recent years, due to the high magnetic properties of fine-crystalline rare earth iron-based isotropic magnets, they are expected to be used in brushless DC motors of about 1 horsepower (750 W) or less for automobiles (including electric vehicles and hybrid vehicles) and white goods.

[0004] In particular, in order to achieve high performance and efficiency in small motors of the several hundred watts class, there is a shift from brushed motors using conventional ferrite magnets to brushless DC motors using bonded magnets, and there is a demand for magnetic materials for bonded magnets with superior residual magnetic flux density Br, intrinsic coercive force HcJ, and maximum energy product (BH)max compared to the bonded magnets using fine crystal rare earth iron-based isotropic magnetic materials that have been used in spindle motors, vibration motors, etc.

[0005] To meet these magnetic property requirements, it is necessary to maximize the volume ratio of the ferromagnetic phase, which exhibits hard or soft magnetic properties and is responsible for the magnetic properties, and to minimize the volume ratio of the non-magnetic phase, which forms the grain boundary of the hard magnetic phase. For example, in isotropic rare earth iron boron magnet materials, the hard magnetic phase RE2Fe 14 The main phase is a B-type (RE is a rare earth element) compound, and the presence of a non-magnetic grain boundary phase containing boron surrounding the main phase adjusts the magnetic interdependence between the main phase particles, resulting in the expression of an intrinsic coercivity HcJ of 700 kA / m or more, which is applicable to various high-performance motors. 14 In order to increase the volume ratio of B-type compounds, it is necessary to reduce the boron content, but if the boron content is reduced too much, the residual magnetic flux density Br and maximum energy product (BH)max will decrease due to a decrease in the squareness of the demagnetization curve, so there are no practical materials with a boron content of 0.9 mass% or less, and isotropic rare earth iron boron magnet materials that can reduce the boron content and achieve excellent magnetic properties are expected. In particular, isotropic rare earth iron boron magnet materials that can be applied to various electric motors such as EVs and HEVs are required to have an intrinsic coercivity HcJ≧1200kA / m, which has been difficult to achieve with isotropic rare earth iron boron magnet materials to date, in order to meet customer demands for improved heat resistance and smaller motors.

[0006] Nd2Fe with fine crystal grains is expected to have high magnetic properties. 14Isotropic magnets with B-type tetragonal compound as the main phase have a stoichiometric composition of Nd:Fe:B=11.76:balance:5.88 as the basic composition. However, in order to realize the intrinsic coercivity HcJ≧1200kA / m applicable to various electric motors such as the above-mentioned EV and HEV, RE2Fe 14 It is necessary to increase the main phase ratio of B, and RE2Fe 14 A higher RE concentration of Nd≧12.5 atomic % is required than the stoichiometric composition of B. However, by simply increasing the main phase ratio, it is necessary to obtain a residual magnetic flux density Br≧0.8T required to generate magnet torque in the electric motor. However, with Nd≧12.5 atomic %, Fe and B become surplus components in the alloy composition, which leads to a decrease in magnetization in the magnet alloy. Therefore, a maximum energy product (BH)max≧110kJ / m2 with a squareness of demagnetization polarity that is practical enough to obtain a high magnet torque is required. 3 It is not possible to simultaneously obtain HcJ≧1200kA / m and Br≧0.81T.

[0007] Also, Nd2Fe 14 In isotropic iron-based rare earth nanocomposite magnet alloys with B-type tetragonal compounds as the main phase, Nd2Fe 14 The B phase and the α-Fe phase or the Fe-B phase are mixed in the same metal structure with nanometer-order crystal grain size, and the exchange interaction between each crystal grain makes them behave as if they were a single magnet, resulting in excellent permanent magnet properties. 14 Since the proportion of the B type compound cannot be increased, no RE-Fe-B based isotropic permanent magnet material exhibiting sufficient magnetic properties has been found.

[0008] Patent Document 1 describes RE2Fe 14 The paper discloses an anisotropic sintered magnet with a B tetragonal crystal structure as the main phase, but the magnet is made of REFe 14 The metal structure is composed of RE2Fe tetragonal crystal grains, and the magnetic moment is increased by magnetic orientation. 14This magnet exhibits good magnetic properties by aligning the C-axis direction of the B tetragonal crystals, but as an isotropic magnet in which the magnetic moments are randomly arranged, good magnetic properties cannot be obtained and it cannot be used as a practical magnet.

[0009] Patent Document 2 discloses RE2Fe alloys that contain at least 10 atomic % of rare earth elements, about 0.5 atomic % or more and about 10 atomic % or less of boron, and the remainder being iron. 14 The authors have disclosed an isotropic permanent magnet with a hard magnetic phase having a B tetragonal crystal structure as the main phase, which has a high intrinsic coercivity HcJ of up to 1460 kA / m. 14 The grain size of B-type crystal grains is 20 nm or more and 400 nm or less. 14 It contains crystal grains that exceed the single magnetic domain crystal grain size of B-type crystal grains. As a result, magnetization is reduced, and even in the example that has the best magnetic properties, the residual magnetic flux density Br is a maximum of 0.83 T and the maximum energy product (BH)max is a maximum of 103 kJ / m 3 Therefore, magnetic properties that can be applied to various electric motors for EVs, HEVs, etc. have not been realized.

[0010] Patent Document 3 and Patent Document 4 disclose iron-based rare earth isotropic nanocomposite magnets. These iron-based rare earth isotropic nanocomposite magnets contain mainly α-Fe phase as the soft magnetic phase, and therefore may have a high residual magnetic flux density Br of 0.9 T or more, but are not suitable as permanent magnet materials for use in automobiles and white goods because they have poor squareness of the demagnetization curve and are inferior in demagnetization resistance and heat resistance.

[0011] On the other hand, Patent Document 5 reports that in an iron-based rare earth isotropic nanocomposite magnet that mainly contains an iron-based boride phase as the soft magnetic phase, the addition of Ti suppresses the precipitation and growth of the α-Fe phase during the cooling process of the molten alloy, and Nd2Fe 14 However, Ti easily combines with boron (B) and crystallizes to form TiB2 phase during the crystallization process, so the precipitation and growth of the main phase Nd2Fe 14The absolute amount of boron required for the formation of the B phase is reduced, and the intrinsic coercivity HcJ expected from the rare earth element concentration cannot be obtained.

[0012] Patent Document 6 discloses an iron-based rare earth-based isotropic nanocomposite magnet that contains mainly an iron-based boride phase as the soft magnetic phase, and teaches that the following effects can be obtained by adding Ti and carbon (C).

[0013] 1. The liquidus temperature of the molten alloy is lowered by 5°C or more (for example, by about 10°C or more and about 40°C or less). When the liquidus temperature of the molten alloy is lowered by adding carbon, the molten alloy viscosity hardly increases even if the molten alloy temperature is lowered by that amount, because the crystallization of coarse TiB2 phases and the like is suppressed. As a result, it becomes possible to continuously form a stable molten alloy flow during the quenching process of the molten alloy.

[0014] 2. When the temperature of the molten metal is low, sufficient cooling can be achieved on the surface of the chill roll, which prevents the metal from wrapping around the chill roll and makes it possible to uniformly refine the rapidly solidified alloy structure.

[0015] 3. Because of the high (B+C) concentration and high amorphous formation ability, it is easy to obtain a fine metal structure even if the molten metal cooling rate is relatively low, at 100°C / sec or more and 10,000°C / sec or less. Therefore, it is possible to obtain Nd2Fe without precipitating coarse α-Fe phase. 14 It is possible to produce a rapidly solidified alloy containing 60% or more of phase B by volume.

[0016] As described above, the iron-based rare earth isotropic nanocomposite magnet described in Patent Document 6, which requires the addition of Ti, has a uniform fine Nd2Fe 14 It is said that excellent permanent magnet properties are obtained by the coexistence of a hard magnetic phase with a B-type crystal structure and a soft magnetic phase consisting of an Fe phase and an Fe-B phase in the same metal structure. However, Ti, an essential element, is a non-magnetic element, and Nd2Fe 14Since these compounds do not enter either the B phase, the Fe phase, or the Fe-B phase, but are scattered at the grain boundaries, this results in a decrease in magnetization and makes it impossible to achieve magnetic properties suitable for use in various electric motors for EVs, HEVs, etc. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] Japanese Patent Application Publication No. 59-46008 [Patent Document 2] Japanese Patent Application Publication No. 60-9852 [Patent Document 3] Japanese Patent Application Publication No. 8-162312 [Patent Document 4] Japanese Patent Application Publication No. 10-53844 [Patent Document 5] JP 2002-175908 A [Patent Document 6] JP 2003-178908 A Summary of the Invention [Problem to be solved by the invention]

[0018] To enable application to various electric motors for EVs, HEVs, etc., an intrinsic coercivity HcJ≧1200kA / m is required, and a maximum energy product (BH)max≧110kJ / m, which provides the excellent demagnetization curve squareness required for the minimum required magnet torque, is required. 3 In order to obtain a residual magnetic flux density Br of 0.81 T, the use of non-magnetic additive elements such as Ti that do not form compounds must be minimized while making the most of the interactions between particles. In order to make the exchange interactions work effectively, the size of the crystal grains must be refined to an average grain size of 10 nm or more and less than 70 nm, while at the same time adjusting the interactions between particles to maximize the coercivity.

[0019] In addition, there is a trade-off between the intrinsic coercivity HcJ and the residual magnetic flux density Br. 14Increasing the volume ratio of the main phase consisting of B-type hard magnetic compounds leads to a decrease in the remanence Br. Therefore, in order to suppress the decrease in the remanence Br, in addition to increasing the exchange interaction acting between each grain by forming the above-mentioned uniform and fine metal structure, it is necessary to make the grain boundary phase adjacent to the main phase a hard or semi-hard magnetic phase that is highly magnetized and has a certain degree of anisotropic magnetic field.

[0020] The inventors have 14 It was thought that by making the grain boundary phase adjacent to the main phase consisting of the B-type hard magnetic compound hard or semi-hard, it might be possible to obtain a permanent magnet material with excellent magnetic properties not previously available. However, as mentioned above, it was found that it is difficult to suppress the decrease in remanence Br while maintaining a high intrinsic coercivity HcJ with the added elements such as Ti.

[0021] The present invention has been made in consideration of the above circumstances, and its main object is to provide an iron-based rare earth boron-based isotropic nanocomposite magnet alloy that can secure the magnet alloy properties necessary for application to various electric motors for EVs, HEVs, etc., and that can improve the residual magnetic flux density, intrinsic coercivity HcJ, and maximum energy product (BH)max compared to existing iron-based rare earth boron-based isotropic magnet alloys, a manufacturing method for the iron-based rare earth boron-based isotropic nanocomposite magnet alloy, and a manufacturing method for a resin-bonded permanent magnet containing the iron-based rare earth boron-based isotropic nanocomposite magnet alloy. [Means for solving the problem]

[0022] The iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention has the composition formula T 100-x-y-z (B 1-n C n ) x RE y Zr z M m(T is at least one element selected from the group consisting of Fe, Co, and Ni, a transition metal element that necessarily contains Fe, RE is at least one rare earth element that necessarily contains at least Nd of Nd and Pr, M is one or more metal elements selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), and the composition ratios x, y, and z are 4.2 atomic % ≤ x ≤ 5.0 atomic %, 12.5 atomic % ≤ y ≤ 14.0 atomic %, 0 atomic % < z ≤ 2.0 atomic %, 0.0 atomic % ≤ m ≤ 5.0 atomic %, and 0.0 ≤ n ≤ 0.5, respectively, and has an alloy composition having a composition that satisfies these conditions. RE2Fe 14 Although it has a B content concentration lower than the stoichiometric composition of the RE2Fe 14 type tetragonal compound, it is finer than the single-domain critical diameter with an average crystal grain size of 10 nm or more and less than 70 nm. RE2Fe 14 Based on the RE2Fe 14 type tetragonal compound as the main phase, Fe is present in the grain boundary phase surrounding the main phase. 17 It has a metal structure containing a phase richer in Fe than the main phases such as the RE2 phase and the α-Fe phase.

[0023] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy, the width of the thickest part of the grain boundary phase can be 1 nm or more and less than 150 nm. Also, in the composition ratio of the main phase and the grain boundary phase, it can have a metal structure in which the ratio of the main phase is 70% by volume or more and less than 99% by volume, and the ratio of the grain boundary phase is 1% by volume or more and less than 30% by volume.

[0024] The method for producing the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention has the composition formula T 100-x-y-z (B 1-n C n ) x RE y Zr z M m(T is at least one element selected from the group consisting of Fe, Co, and Ni, which is a transition metal element necessarily containing Fe, RE is at least one rare earth element necessarily containing at least Nd among Nd and Pr, and M is one or more metal elements selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), and the composition ratios x, y, and z satisfy 4.2 atomic % ≤ x ≤ 5.0 atomic %, 12.5 atomic % ≤ y ≤ 14.0 atomic %, 0 atomic % < z ≤ 2.0 atomic %, 0.0 atomic % ≤ m ≤ 5.0 atomic %, and 0.0 ≤ n ≤ 0.5, respectively. A step of preparing a molten alloy having a composition, and the above molten alloy is arranged at the tip of a nozzle at an average pouring rate of 200 g / min or more and less than 2000 g / min per orifice, and is sprayed onto the surface of a rotating roll mainly composed of an alloy containing Cu, Mo, W, or at least one of these metals, whereby RE2Fe 14 A step of producing a rapidly solidified alloy having either a crystalline phase containing the B phase or an amorphous phase in an amount of 1% by volume or more.

[0025] In the method for producing the resin-bonded permanent magnet, a step of preparing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder produced by the method for producing the iron-based rare earth boron-based isotropic nanocomposite magnet alloy, adding a thermosetting resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder, filling it into a molding die, and then subjecting it to compression molding to form a compression molded body, and then heat-treating it at a temperature equal to or higher than the polymerization temperature of the thermosetting resin.

[0026] In the method for producing the resin-bonded permanent magnet, a step of preparing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder produced by the method for producing the iron-based rare earth boron-based isotropic nanocomposite magnet alloy, adding a thermoplastic resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder to produce a compound for injection molding, and then injection molding.

Advantages of the Invention

[0027] According to the present invention, it is possible to provide a rare earth boron-based isotropic nanocomposite magnet alloy that can ensure magnetic properties such as residual magnetic flux density Br, intrinsic coercivity HcJ, and maximum energy product (BH)max required for a permanent magnet for various electric motors for EVs, HEVs, etc. Also, according to the present invention, it is possible to provide a method for manufacturing the rare earth boron-based isotropic nanocomposite magnet alloy. Furthermore, according to the present invention, it is possible to provide a method for manufacturing a resin-bonded permanent magnet including the rare earth boron-based isotropic nanocomposite magnet alloy. [Brief description of the drawings]

[0028] [Figure 1] 1 is a cross-sectional view showing a schematic diagram of an example of an iron-based rare earth boron-based isotropic magnet alloy according to the present invention. [Diagram 2] (a) is a diagram showing the equipment configuration of a heat treatment furnace that realizes flash annealing, and (b) is a diagram showing the state of the rapidly solidified alloy moving inside the furnace tube. [Diagram 3] FIG. 2 is a conceptual diagram of a thermal history by flash annealing carried out in the present invention. [Figure 4] 1 is a powder X-ray diffraction profile of the rapidly solidified alloy obtained in Example 9. [Diagram 5] 1 shows a powder X-ray diffraction profile of the rapidly solidified alloy obtained in Example 9 after flash annealing (crystallization heat treatment). [Figure 6] 1 is an elemental mapping image obtained in Example 24. [Figure 7] 1 shows an X-ray powder diffraction profile of the rapidly solidified alloy obtained in Comparative Example 7 after flash annealing (crystallization heat treatment). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] Hereinafter, the rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, the method for manufacturing the rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, the method for manufacturing a powder composed of the rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, and the method for manufacturing a resin-bonded permanent magnet of the present invention will be described. Note that the present invention is not limited to the following configurations, and may be appropriately changed without departing from the gist of the present invention. In addition, a combination of a plurality of the individual preferred configurations described below is also the present invention.

[0030] The rare earth boron-based isotropic nanocomposite magnet alloy of the present invention has a composition formula T 100-x-y-z (B 1-n C n ) x RE y Zr z M m (T is at least one element selected from the group consisting of Fe, Co, and Ni, and is a transition metal element that necessarily contains Fe, RE is at least one rare earth element that necessarily contains at least Nd among Nd and Pr, and M is one or more metal elements selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), and the composition ratios x, y, and z satisfy 4.2 atomic % ≤ x ≤ 5.0 atomic %, 12.5 atomic % ≤ y ≤ 14.0 atomic %, 0 atomic % < z ≤ 2.0 atomic %, 0.0 atomic % ≤ m ≤ 5.0 atomic %, and 0.0 ≤ n ≤ 0.5, respectively, and has an alloy composition. It has a B content concentration lower than the stoichiometric composition of the RE2Fe 14 B-type tetragonal crystal compound, and has an average crystal grain size of 10 nm or more and less than 70 nm, and is finer than the single-domain critical diameter. The RE2Fe 14 B-type tetragonal crystal compound is the main phase, and the grain boundary phase surrounding the main phase has a metal structure containing a phase richer in Fe than the main phases such as the Fe 17 RE2 phase and the α-Fe phase.

[0031] The width of the thickest part of the grain boundary phase is preferably 1 nm or more and less than 150 nm. An example of such an iron-based rare earth boron-based isotropic magnet alloy of the present invention is shown in FIG. 1.

[0032] The composition ratio of the main phase and the grain boundary phase is not necessarily limited, but it is preferable that the ratio of the main phase is 70 volume % or more and less than 99 volume %, and the ratio of the grain boundary phase is 1 volume % or more and less than 30 volume %.

[0033] The rare earth boron based isotropic nanocomposite magnet alloy of the present invention is characterized by a low boron content concentration, RE2Fe 14 The boron (B) content in the alloy composition range in which a magnet alloy with the B phase as the main phase can be obtained is defined as RE2Fe 14 The rare earth boron-based isotropic nanocomposite magnet alloy of the present invention has a rare earth element (RE) and iron (Fe) in a surplus state in the same alloy structure, and the rare earth element (RE) and iron (Fe) in the main phase are in a surplus state in the rare earth boron-based nanocomposite magnet alloy of the present invention. 14 The grain boundary phase is formed from the excess RE and Fe that are not required for the formation of the B phase. As a result, the iron-based rare earth boron isotropic magnet alloy of the present invention has an average crystal grain size of, for example, 10 nm or more and less than 70 nm. 14 Fe, which surrounds the B phase 17 The alloy can have a unique fine metal structure in which there is a grain boundary phase, the thickest part of which is 1 nm or more and less than 150 nm wide, which contains a phase that is richer in Fe than the main phase, such as the RE2 phase or the α-Fe phase.

[0034] By realizing the above-mentioned unique uniform fine metal structure, the inventors have 14 The B phase and the grain boundary phase, which is uniformly present around the main phase and is mainly composed of RE and Fe, are connected by a strong exchange interaction in addition to the static magnetostatic interaction. If the exchange interaction (exchange coupling) becomes too strong, it will result in a decrease in the intrinsic coercivity HcJ of the magnet alloy. However, by adjusting the RE-Fe-B composition and the concentration of Zr, it is possible to reduce the Fe 17 By forming a unique metal structure in which the grain boundary phase contains a phase richer in Fe than the main phases such as the RE2 phase and α-Fe phase, 14It was discovered that this suppresses the decrease in HcJ of the B phase and achieves a high maximum energy product (BH)max by improving the residual magnetic flux density Br and the squareness of the demagnetization curve, which are applicable to various electric motors for EVs, HEVs, etc. In particular, by using the metal structure configuration described above, it is believed that a high HcJ that could not be achieved with conventional rare earth iron boron isotropic magnets can be achieved without adding extremely rare and expensive heavy rare earth elements such as Dy and Tb.

[0035] When the boron content is less than 4.2 atomic %, the main phase RE2Fe 14 Since the formation of the B phase is inhibited, both the intrinsic coercivity HcJ and the residual magnetic flux density Br are significantly reduced. In addition, when the boron content exceeds 5.0 atomic %, Fe 17 Since phases richer in Fe than the main phases such as RE2 phase and α-Fe phase do not precipitate, a residual magnetic flux density of Br: 0.81 T or more can be achieved, but the maximum energy product (BH) max: 110 kJ / m 3 It is not possible to obtain an intrinsic coercivity HcJ of 1200 kA / m or more while maintaining the above.

[0036] On the other hand, when the boron content is 4.2 atomic % or more and 5.0 atomic % or less, the RE2Fe required to obtain the intrinsic coercivity HcJ ≥ 1200 kA / m is 14 Without impairing the formation of B phase, 17 It is believed that the above magnetic properties are obtained because the grain boundary phase, which is mainly composed of RE and Fe and includes a phase that is richer in Fe than the main phase such as the RE2 phase and the α-Fe phase, is uniformly formed.

[0037] Patent Documents 2, 3, 4, 5 and 6 all report that the intrinsic coercivity HcJ is RE2Fe 14 The paper discloses a microcrystalline isotropic permanent magnet material made of B-type tetragonal compounds, and the magnitude of the intrinsic coercivity HcJ is mainly determined by the RE2Fe 14 It depends largely on the volume ratio of B-type tetragonal compounds, RE2Fe 14 If the volume ratio of the B phase is high, the intrinsic coercivity HcJ will be high, and RE2Fe 14 If the volume ratio of the B phase is low, the intrinsic coercivity HcJ is low.

[0038] On the other hand, the anisotropic RE2Fe described in Patent Document 1 14 In B sintered magnets, heavy rare earth elements such as Dy and Tb are used in the main phase, RE2Fe 14 B-type tetragonal compounds include RE2Fe 14 By increasing the anisotropic magnetic field of the B-type tetragonal compound, the intrinsic coercivity HcJ is improved. The above fine isotropic permanent magnet material and anisotropic sintered magnet are both RE2Fe 14 Although the main phase is a B-type tetragonal compound, the size of the main phase of anisotropic sintered magnets is approximately 1 μm or more and 10 μm or less. 14 This is greater than the critical diameter for the single domain of B-type tetragonal compounds. Therefore, although anisotropic sintered magnets are in a multi-domain state before magnetization, the magnetic moments are aligned in the magnetization direction (C-axis direction) by magnetization, and the magnetization results in a single domain state, which allows the magnet to exhibit permanent magnet properties. Therefore, the intrinsic coercivity HcJ of anisotropic sintered magnets represents the ability to keep the magnetic moments aligned in the same direction, and therefore RE2Fe 14 By increasing the anisotropic magnetic field of the B-type tetragonal compound, the intrinsic coercivity HcJ is improved.

[0039] In the low boron content and iron-based rare earth boron isotropic nanocomposite magnet alloy of the present invention, the addition of Zr within a certain range makes the metal structure of the magnet alloy uniform and fine, and the exchange coupling between particles is optimized to obtain excellent squareness of the demagnetization curve. At the same time, the composition ratio and metal structure of each phase contained in the alloy change, resulting in the formation of Fe. 17 We were able to realize a unique metal structure with grain boundary phases that contain phases richer in Fe than the main phase, such as RE2 and α-Fe phases. 14 RE2Fe, which can suppress the decrease in the intrinsic coercivity HcJ of B-type tetragonal compounds 14It has been found that an isotropic nanocomposite magnet composed of Fe and B with a B-type cubic compound as the main phase and a ferromagnetic compound containing a phase richer in Fe than the main phase as the secondary phase can be obtained. As a result, according to the iron-based rare-earth boron-based isotropic nanocomposite magnet of the present invention, while suppressing a significant decrease in the residual magnetic flux density Br, a high intrinsic coercive force HcJ that could not be achieved with conventional iron-based rare-earth boron-based isotropic magnets can be obtained without adding heavy rare earths such as Dy and Tb.

[0040] In addition, it has been found that the iron-based rare-earth boron-based isotropic nanocomposite magnet alloy characterized by a low boron content concentration of the present invention can improve the intrinsic coercive force HcJ without causing a decrease in the residual magnetic flux density Br by substituting a part of boron (B) with carbon (C). Furthermore, by combining carbon (C) substitution and heavy rare-earth element addition, the improvement effect of the intrinsic coercive force HcJ can be increased.

[0041] [Alloy composition] The alloy composition of the iron-based rare-earth boron-based isotropic nanocomposite magnet alloy of the present invention has a composition formula T 100-x-y-z (B 1-n C n ) x RE y Zr z M m (T is at least one element selected from the group consisting of Fe, Co, and Ni, which is a transition metal element necessarily containing Fe; RE is at least one rare-earth element necessarily containing at least Nd among Nd and Pr; M is one or more metal elements selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), and the composition ratios x, y, and z satisfy 4.2 atomic% ≤ x ≤ 5.0 atomic%, 12.5 atomic% ≤ y ≤ 14.0 atomic%, 0 atomic% < z ≤ 2.0 atomic%, 0.0 atomic% ≤ m ≤ 5.0 atomic%, and 0.0 ≤ n ≤ 0.5, respectively. For the analysis of the composition of the entire magnet alloy according to the present invention, ICP mass spectrometry or fluorescent X-ray analysis is used. Additionally, the combustion-infrared absorption method may be used in combination as necessary.

[0042] The transition metal element T, which contains Fe as an essential element, occupies the remainder of the above-mentioned elements. The desired hard magnetic properties can be obtained even if a part of Fe is replaced with one or two of Co and Ni, which are ferromagnetic elements like Fe. However, if the amount of replacement with respect to Fe exceeds 30%, it will cause a significant decrease in magnetic flux density, so the amount of replacement is preferably in the range of 0% or more and 30% or less. In addition, since the addition of Co not only contributes to improving magnetization, but also has the effect of reducing the viscosity of the molten metal and stabilizing the melt discharge rate from the nozzle during quenching of the molten metal, the amount of replacement with Co is more preferably 0.5% or more and 30% or less, and from the viewpoint of cost-effectiveness, the amount of replacement with Co is even more preferably 0.5% or more and 10% or less.

[0043] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, when the composition ratio x of B+C is less than 4.2 atomic %, RE2Fe 14 The amount of B+C required to generate B-type tetragonal compounds cannot be secured, and the magnetic properties and amorphous generation ability are greatly reduced. This causes the α-Fe phase to precipitate during rapid solidification of the molten metal, resulting in a loss of squareness in the demagnetization curve. In addition, when the composition ratio x of B+C exceeds 5.0 atomic %, the Fe 17 Since the grain boundary phase mainly composed of RE and Fe, which includes a phase richer in Fe than the main phase such as the RE2 phase and the α-Fe phase, is not generated, the intrinsic coercivity HcJ decreases, and the above-mentioned magnetic properties may not be ensured. Therefore, the composition ratio x is limited to a range of 4.2 atomic % or more and 5.0 atomic % or less. The composition ratio x is preferably 4.4 atomic % or more and 4.9 atomic % or less, and more preferably 4.5 atomic % or more and 4.9 atomic % or less.

[0044] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, by substituting a part of B with C, the melting point of the molten alloy is lowered and the amount of wear of the refractory material used during rapid solidification is reduced, so that the process cost related to rapid solidification can be reduced and the intrinsic coercivity HcJ can be improved. However, if the substitution rate of C for B exceeds 50%, the amorphous generation ability is greatly reduced, which is not preferable. Therefore, the substitution rate of C for B is limited to a range of 0% or more and 50% or less, that is, 0.0≦n≦0.5. From the viewpoint of the effect of improving the intrinsic coercivity HcJ, the substitution rate of C for B is preferably 2% or more and 30% or less, and more preferably 3% or more and 15% or less.

[0045] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, when the composition ratio y of at least one rare earth element RE, which must include at least Nd among Nd and Pr, is less than 12.5 atomic %, Fe 17 There is a possibility that the grain boundary phase mainly composed of RE and Fe, which includes a phase richer in Fe than the main phase such as the RE2 phase and the α-Fe phase, is not generated, and the above-mentioned magnetic properties cannot be ensured. In addition, when the composition ratio y exceeds 14.0 atomic %, the magnetization decreases significantly. Therefore, the composition ratio y is limited to a range of 12.5 atomic % or more and 14.0 atomic % or less. In addition, from the viewpoint of stably ensuring the intrinsic coercivity HcJ, the composition ratio y is preferably 12.6 atomic % or more and 14.0 atomic % or less, and from the viewpoint of ensuring a high residual magnetic flux density Br, it is more preferably 12.8 atomic % or more and 13.5 atomic % or less.

[0046] The above rare earth elements RE are y =(Nd 1-l Pr l ) y In this case, l is limited to 0.05 or more and 0.7 or less. If the ratio l of Pr to Nd is too low, the effect of improving HcJ is small, and if l is too high, the absolute value of the temperature coefficient β related to the coercivity of the magnet alloy becomes small, which may cause a decrease in heat resistance, so l is preferably 0.15 or more and 0.6 or less, and more preferably 0.2 or more and 0.5 or less.

[0047] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, Zr is an essential additive element for uniformly refining the magnet alloy and for generating a phase richer in Fe than the main phase at the grain boundaries, and since a Zr composition ratio z exceeding 2.0 atomic % leads to a decrease in magnetization and a residual magnetic flux density Br of 0.81 T or more cannot be obtained, the composition ratio z is limited to a range of 2.0 atomic % or less. From the viewpoint of improving the squareness of the demagnetization curve, the composition ratio z is preferably 0.6 atomic % or more and 2.0 atomic % or less, and from the viewpoint of ensuring a high residual magnetic flux density Br, it is more preferable that the composition ratio z is 0.7 atomic % or more and 1.5 atomic % or less.

[0048] In the iron-based rare earth boron isotropic magnet alloy of the present invention, one or more metal elements M selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au and Pb may be added. The addition of the metal element M improves the amorphous generation ability, improves the intrinsic coercive force HcJ by uniformly refining the metal structure after crystallization heat treatment, improves the squareness of the demagnetization curve, and improves the magnetic properties. However, if the composition ratio m of these metal elements M exceeds 5.0 atomic %, it will cause a decrease in magnetization, so the composition ratio m is limited to a range of 0.0 atomic % or more and 5.0 atomic % or less. In addition, the composition ratio m is preferably 0.0 atomic % or more and 3.0 atomic % or less, and more preferably 0.0 atomic % or more and 2.0 atomic % or less.

[0049] [Metal structure] In the iron-based rare earth boron isotropic nanocomposite magnet alloy of the present invention, the main phase RE2Fe 14 If the average crystal grain size of B-type tetragonal compounds is less than 10 nm, the intrinsic coercivity HcJ decreases, and if it is more than 70 nm, the squareness of the demagnetization curve decreases due to the decrease in the exchange interaction between the crystal grains. Therefore, the remanence Br is 0.81 T or more, the intrinsic coercivity HcJ is 1200 kA / m or more but less than 1700 kA / m, and the maximum energy product (BH)max is 110 kJ / m. 3 In order to achieve the above magnetic properties, RE2Fe 14The average crystal grain size of the B-type tetragonal compound is limited to the range of 10 nm or more and less than 70 nm. 14 The average crystal grain size of the B-type tetragonal compound is preferably 15 nm or more and 60 nm or less, and more preferably 15 nm or more and 50 nm or less.

[0050] RE2Fe 14 The average crystal grain size of a B-type tetragonal compound means the average value of the equivalent circle diameters of each grain present in a field of view when the grain size of each grain is measured at three or more points by the line segment method using a transmission electron microscope (TEM).

[0051] In addition, the above RE2Fe 14 The main phase is made of B-type tetragonal compounds, and is surrounded by Fe 17 When the width of the grain boundary phase, which is mainly composed of RE and Fe and includes a phase richer in Fe than the main phase such as the RE2 phase or the α-Fe phase, is less than 1 nm, the bonding force acting between the main phase particles increases, resulting in a decrease in the intrinsic coercivity HcJ. In addition, when the width of the thickest part of the grain boundary phase is 150 nm or more, the interparticle bonding is weakened and the squareness of the demagnetization curve decreases. Therefore, the width of the thickest part of the grain boundary phase is not necessarily limited, but is preferably 1 nm or more and less than 150 nm, more preferably 2 nm or more and 100 nm or less, and even more preferably 2 nm or more and 10 nm or less. The width of the grain boundary phase was obtained by performing image analysis on a bright-field image taken using a scanning transmission electron microscope under conditions of an accelerating voltage of 200 kV and an observation magnification of 900,000 times.

[0052] In the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, the ratio of the main phase to the grain boundary phase is preferably 70% by volume or more and less than 99% by volume, and the ratio of the grain boundary phase is 1% by volume or more and less than 30% by volume. This results in a residual magnetic flux density Br of 0.81 T or more, an intrinsic coercivity HcJ of 1200 kA / m or more and less than 1700 kA / m, and a maximum energy product (BH)max of 110 kJ / m. 3The above magnetic properties are easily achieved. The main phase ratio is preferably 80 volume % or more and less than 99 volume %, and more preferably 90 volume % or more and less than 98 volume %. The composition ratio of the main phase and the grain boundary phase was determined by performing image analysis on bright-field images taken with a scanning transmission electron microscope under conditions of an accelerating voltage of 200 kV and an observation magnification of 900,000 times.

[0053] [Magnetic properties] As described below, the iron-based rare earth boron isotropic nanocomposite magnet alloy of the present invention has a residual magnetic flux density Br of 0.81 T or more and a maximum energy product (BH)max of 110 kJ / m 3 While ensuring the above, it is possible to realize an extremely high intrinsic coercivity HcJ of 1200kA / m or more and less than 1700kA / m, which has not been realized so far as an iron-based rare earth boron isotropic magnet alloy, but since the intrinsic coercivity HcJ of conventional iron-based rare earth boron isotropic magnets is a permanent magnet characteristic of 1200kA / m or less, which is difficult to apply to various electric motors such as EVs and HEVs, which require high heat resistance along with miniaturization, the intrinsic coercivity HcJ is preferably 1200kA / m or more, and more preferably 1250kA / m or more. Note that if the intrinsic coercivity HcJ is 1700kA / m or more, the magnetization significantly decreases, so the intrinsic coercivity HcJ is preferably 1700kA / m or less, and more preferably 1600kA / m or less. Regarding the residual magnetic flux density Br, when an embedded magnet rotor (IPM type rotor) or the like is used, it becomes possible to operate at a higher operating point (permeance) compared to the SPM type, so it is better to have as high a residual magnetic flux density Br as possible; however, taking into consideration the balance with heat resistance and intrinsic coercivity HcJ, the residual magnetic flux density Br is preferably 0.81 T or more, and more preferably 0.82 T or more.

[0054] The reason why the residual magnetic flux density Br is set to 0.81T or more is that when used as an isotropic bonded magnet in a DC brushless motor, the operating point (permeance Pc) of the magnet is between 3 and 10, so if the residual magnetic flux density Br is 0.81T or more, within this Pc range, the maximum energy product (BH)max is 300kJ / m 3 This is because it is possible to obtain an effective magnetic flux Bm at the same level as that of the above-mentioned anisotropic Nd-Fe-B sintered magnet at 120° C. It is more preferable that the residual magnetic flux density Br is 0.82 T or more.

[0055] The reason for setting the intrinsic coercivity HcJ at 1200kA / m or more is that if the intrinsic coercivity HcJ is less than 1200kA / m and it is used as an isotropic bonded magnet in a DC brushless motor, the heat resistance temperature of the motor cannot be guaranteed to be 120°C, and there is a possibility that the desired motor characteristics will not be obtained due to thermal demagnetization.In addition, the reason for setting the intrinsic coercivity HcJ at less than 1700kA / m is that if the intrinsic coercivity HcJ is 1700kA / m or more, the magnetization will decrease significantly, and in magnet specifications where the magnetic path is long, such as polar anisotropic magnetization, the magnetic path will not be connected and the required effective magnetic flux Bm will not be obtained.

[0056] Furthermore, the maximum energy product (BH) is 110 kJ / m 3 The reason for this is that the maximum energy product (BH) is 110kJ / m 3 Below this, the squareness ratio of the demagnetization curve (residual magnetization Jr / saturation magnetization Js) will be 0.8 or less, and if used in a DC brushless motor as an isotropic bonded magnet, the magnetic properties will decrease due to the reverse magnetic field that is generated when the motor is in operation, and it may not be possible to obtain the desired motor characteristics.

[0057] The method for producing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy according to the present invention comprises the steps of: 100-x-y-z (B 1-n C n ) x RE y Zr z M m(T is at least one element selected from the group consisting of Fe, Co, and Ni, which is a transition metal element necessarily containing Fe, RE is at least one rare earth element necessarily containing at least Nd among Nd and Pr, and M is one or more metal elements selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), and the composition ratios x, y, and z satisfy 4.2 atomic % ≤ x ≤ 5.0 atomic %, 12.5 atomic % ≤ y ≤ 14.0 atomic %, 0 atomic % < z ≤ 2.0 atomic %, 0.0 atomic % ≤ m ≤ 5.0 atomic %, and 0.0 ≤ n ≤ 0.5, respectively, to prepare a molten alloy having such a composition; and the above molten alloy is sprayed onto the surface of a rotating roll mainly composed of an alloy containing Cu, Mo, W, or at least one of these metals at an average pouring rate of 200 g / min or more and less than 2000 g / min per orifice arranged at the tip of the nozzle, whereby RE2Fe 14 A step of producing a rapidly solidified alloy having either a crystalline phase containing the RE2Fe 14 B phase or an amorphous phase in an amount of 1% by volume or more. The present invention is characterized by comprising this step. Note that RE is at least one rare earth element substantially free of La and Ce. As an example, as described above, it can be at least one rare earth element necessarily containing at least Nd among Nd and Pr. The details are as described above.

[0058] [Molten metal rapid cooling] In the method for producing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, after melting raw materials prepared to have a predetermined alloy composition to obtain a molten alloy, the above molten alloy is sprayed onto the surface of a rotating roll mainly composed of an alloy containing Cu, Mo, W, or at least one of these metals at an average pouring rate of 200 g / min or more and less than 2000 g / min per orifice arranged at the tip of the nozzle, whereby RE2Fe 14A rapidly solidified alloy having 1% by volume or more of either the crystalline phase including the B phase or the amorphous phase is produced, but if the average tapping rate is less than 200 g / min, the productivity is poor, and if it is more than 2000 g / min, the molten alloy structure will be a coarse α-Fe phase, so that the above-mentioned magnetic properties may not be obtained even if the crystallization heat treatment is performed. Therefore, the average tapping rate per orifice located at the nozzle tip is limited to a range of 200 g / min or more and less than 2000 g / min. The average tapping rate is preferably 300 g / min or more and 1500 g / min or less, and more preferably 400 g / min or more and 1300 g / min or less.

[0059] The hole at the nozzle tip through which the molten metal is discharged does not have to be a circular orifice, and may be any shape such as a square, triangle, ellipse, etc., and may be a slit-shaped hole as long as it can ensure a predetermined discharge rate. In addition, the nozzle material is permissible as long as it is a refractory material that does not or is difficult to react with the molten alloy, but ceramic materials, SiC, C, or BN that cause little wear of the nozzle orifice due to the molten metal during discharge are preferred, BN is more preferred, and hard BN containing an additive is even more preferred.

[0060] When producing the above-mentioned rapidly solidified alloy, the rapid solidification atmosphere is preferably an oxygen-free or low-oxygen atmosphere, since the increase in the viscosity of the molten alloy can be suppressed by preventing oxidation of the molten alloy, and a stable melt tapping rate can be maintained. In order to realize this atmosphere, it is necessary to evacuate the inside of the rapid solidification apparatus to 20 Pa or less, preferably 10 Pa or less, more preferably 1 Pa or less, and then introduce an inert gas into the rapid solidification apparatus to set the oxygen concentration in the rapid solidification apparatus to 500 ppm or less, preferably 200 ppm or less, more preferably 100 ppm or less, and then perform rapid solidification. As the inert gas, rare gases such as helium and argon, and nitrogen can be used, but since nitrogen is relatively reactive with rare earth elements and iron, rare gases such as helium and argon are preferable, and argon gas is more preferable from the viewpoint of cost.

[0061] In the process of producing a rapidly solidified alloy, the rotating roll for rapidly cooling the molten alloy is mainly composed of Cu, Mo, W or an alloy containing at least one of these metals, and preferably has a base material containing such a main component. This is because these base materials have excellent thermal conductivity and durability. In addition, by plating the base material surface of the rotating roll with Cr, Ni or a combination thereof, the heat resistance and hardness of the base material surface of the rotating roll can be increased, and melting and deterioration of the base material surface of the rotating roll during rapid solidification can be suppressed. The diameter of the rotating roll is, for example, Φ200 mm or more and Φ20000 mm or less. If the rapid solidification time is a short time of 10 seconds or less, there is no need to water-cool the rotating roll, but if the rapid solidification time exceeds 10 seconds, it is preferable to flow cooling water inside the rotating roll to suppress the temperature rise of the rotating roll base material. It is preferable that the water-cooling capacity of the rotating roll is calculated according to the latent heat of solidification and the melting rate per unit time, and appropriately adjusted optimally.

[0062] [Flash Annealing] The method for producing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention further comprises a step of performing flash annealing on the rapidly solidified alloy, in which the alloy is heated at a rate of 10°C / sec or more and less than 200°C / sec to a constant temperature range of not less than the crystallization temperature and not more than 850°C, and then quenched after a lapse of 0.1 sec or more and less than 7 min., and the step of performing flash annealing produces RE2Fe 14 RE2Fe has a lower B content than the stoichiometric composition of the B-type tetragonal compound, but has an average crystal grain size of 10 nm or more and less than 70 nm. 14 The main phase is a B-type tetragonal compound, and the Fe 17 RE2Fe contains a grain boundary phase with a width of 1 nm or more and less than 10 nm, which is mainly composed of RE and Fe including the RE2 phase. 14 It is preferable to form a metal structure finer than the single magnetic domain critical diameter of a B-type tetragonal compound.

[0063] If the heating rate during flash annealing (crystallization heat treatment) is less than 10°C / sec, excessive grain growth will prevent a fine metal structure from being obtained, resulting in a decrease in intrinsic coercivity HcJ and residual magnetic flux density Br. If the heating rate is 200°C / sec or more, grain growth will not be able to keep up, resulting in RE2Fe with an average grain size of 10nm or more and less than 70nm, which is necessary for the development of a permanent magnet. 14 RE2Fe has a B-type tetragonal compound as its main phase, and a grain boundary phase mainly composed of RE and Fe and having a width of 1 nm or more and less than 10 nm is present surrounding the main phase. 14 The metal structure does not become finer than the single domain critical diameter of the B-type tetragonal compound, and the magnetic properties deteriorate as in the case of heating at a rate of less than 10° C. / sec. Therefore, the heating rate is preferably 10° C. / sec or more and less than 200° C. / sec, more preferably 30° C. / sec or more and 200° C. / sec or less, and even more preferably 40° C. / sec or more and 180° C. / sec or less.

[0064] In the flash annealing (crystallization heat treatment) in the manufacturing method of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, it is preferable to immediately quench after reaching a crystallization heat treatment temperature (holding temperature) in a constant temperature range of not less than the crystallization temperature and not more than 850°C in order to obtain good magnetic properties. In detail, the holding time from reaching the crystallization heat treatment temperature to quenching is substantially 0.1 sec or more, and holding for 7 min or more is not preferable because it damages the uniform fine metal structure and leads to a deterioration of various magnetic properties. Therefore, the holding time is preferably 0.1 sec or more and less than 7 min, more preferably 0.1 sec or more and 2 min or less, and even more preferably 0.1 sec or more and 30 sec or less.

[0065] In the flash annealing (crystallization heat treatment) in the manufacturing method of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention, it is preferable to cool the rapidly solidified alloy to 400°C or less at a temperature drop rate of 2°C / sec or more and 200°C / sec or less. If the temperature drop rate is less than 2°C / sec, the crystal structure will become coarse, and if it exceeds 200°C / sec, the alloy may be oxidized. Therefore, the temperature drop rate is preferably 2°C / sec or more and 200°C / sec or less, more preferably 5°C / sec or more and 200°C / sec or less, and even more preferably 5°C / sec or more and 150°C / sec or less.

[0066] The flash annealing (crystallization heat treatment) is preferably performed in an inert gas atmosphere to prevent oxidation of the rapidly solidified alloy. As the inert gas, rare gases such as helium and argon, and nitrogen can be used, but since nitrogen reacts relatively easily with rare earth elements and iron, rare gases such as helium and argon are preferred, and argon gas is more preferred from the viewpoint of cost.

[0067] [Crushing and molding] The method for producing a powder of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy of the present invention may further include a step of producing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder by pulverizing the rapidly solidified alloy or the rapidly solidified alloy that has been subjected to the flash annealing.

[0068] The rapidly solidified alloy obtained through the above process may be roughly cut or crushed into a ribbon shape, for example, to 50 mm or less, before flash annealing (crystallization heat treatment). Furthermore, the magnetic alloy of the present invention after flash annealing (crystallization heat treatment) can be crushed into magnetic alloy powder having an appropriate average powder particle size in the range of 20 μm or more and 200 μm or less, and various resin-bonded permanent magnets (commonly known as plastic magnets or bonded magnets) can be manufactured using the magnetic alloy powder by known processes.

[0069] The manufacturing method of the resin-bonded permanent magnet of the present invention can include the steps of preparing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder manufactured by the manufacturing method of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy, and adding a thermosetting resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder, filling the mixture into a molding die, and compressing the mixture to form a compressed body, followed by heat treatment at a temperature equal to or higher than the polymerization temperature of the thermosetting resin.

[0070] The manufacturing method of the resin-bonded permanent magnet of the present invention can include the steps of: preparing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder produced by the manufacturing method of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy; and adding a thermoplastic resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder to prepare an injection molding compound, and then injection molding the compound.

[0071] When producing the above resin-bonded permanent magnet, the iron-based rare earth nanocomposite magnet powder is mixed with epoxy, polyamide, polyphenylene sulfide (PPS), liquid crystal polymer, acrylic, polyether, etc., and molded into a desired shape. In this case, for example, a hybrid magnet powder mixed with a permanent magnet powder such as SmFeN magnet powder or hard ferrite magnet powder may be used.

[0072] Using the resin-bonded permanent magnets described above, it is possible to manufacture brushless DC motors that require small size and heat resistance, such as various electric motors for EVs, HEVs, etc.

[0073] When the magnet alloy powder of the present invention is used for injection molded bonded magnets, it is preferable to pulverize it to an average grain size of 100 μm or less, and more preferably, the average grain size of the powder is 20 μm or more and 100 μm or less. When the magnet alloy powder of the present invention is used for compression molded bonded magnets, it is preferable to pulverize it to an average grain size of 200 μm or less, and more preferably, the average grain size of the powder is 50 μm or more and 150 μm or less. Even more preferably, the grain size distribution has two peaks, and the average grain size is 80 μm or more and 130 μm or less.

[0074] By subjecting the surface of the magnet alloy powder of the present invention to surface treatment such as coupling treatment, chemical conversion treatment (including phosphate treatment and glass coating treatment), it is possible to improve the moldability during molding of the resin-bonded permanent magnet and the corrosion resistance and heat resistance of the resulting resin-bonded permanent magnet, regardless of the molding method. In addition, when the surface of the resin-bonded permanent magnet after molding is subjected to surface treatment such as resin painting, chemical conversion treatment, plating, etc., it is possible to improve the corrosion resistance and heat resistance of the resin-bonded permanent magnet in the same way as the surface treatment of the magnet alloy powder.

[0075] The manufacturing method of the iron-based rare earth boron isotropic nanocomposite magnet alloy of the present invention is not limited to the above, and other manufacturing methods can be adopted as long as they can produce an iron-based rare earth boron isotropic magnet alloy having the above-mentioned composition, average crystal grain size, etc. For example, by using flash annealing, it is possible to produce RE2Fe 14 A fine metal structure having a B-type tetragonal compound as the main phase can be formed, but the method for forming such a fine metal structure is not limited to flash annealing, and other methods can also be used. For example, even when a normal annealing process is used instead of flash annealing, good magnetic properties can be obtained by adjusting the surface speed of the rotating roll for quenching the molten alloy to form a homogeneous fine metal structure consisting of crystal grains that are 5% to 20% smaller than the alloy structure that provides optimal magnetic properties. EXAMPLES

[0076] EXAMPLES Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.

[0077] (Example) In order to obtain the alloy composition shown in Table 1, 100 g of raw material containing the main elements Nd, Pr, B, Co, C, Zr, and Fe with a purity of 99.5% or more, as well as additive elements such as Si, Ti, Cu, Zn, Ga, Nb, and Hf, was placed in an alumina melting crucible and then set in the work coil in a vacuum melting furnace. The vacuum melting furnace was then evacuated to 0.02 Pa or less, and argon gas was introduced to normal pressure, after which the alloy was molten by high-frequency induction heating. The molten alloy was then cast into a water-cooled copper mold to produce a master alloy.

[0078] Next, the obtained mother alloy was divided into appropriate sizes, and 40 g of the alloy was inserted into a transparent quartz nozzle having an orifice with a suitable diameter (0.7 mm or more, 1.2 mm or less) at the bottom so as to obtain the average melting rate shown in Table 1 (in Table 1, it is simply indicated as "melting rate"). The nozzle was then set in the work coil in the single roll quenching device. The vacuum melting furnace was then evacuated to 0.02 Pa or less, and argon gas was introduced until the quenching atmosphere pressure shown in Table 1 was reached. The mother alloy was remelted by high-frequency induction heating, and the molten alloy was discharged from the nozzle orifice at a spray pressure of 30 kPa onto the surface of the rotating roll rotating at the roll surface speed (Vs) shown in Table 1, to produce a rapidly solidified alloy. At this time, the distance between the nozzle tip and the rotating roll surface was set to 0.8 mm. The main component of the rotating roll was copper. The rapidly solidified alloy obtained was Nd2Fe 14 The material contained 1% by volume or more of either a crystalline phase including phase B or an amorphous phase.

[0079] As a representative example, FIG. 4 shows the powder X-ray diffraction profile of the rapidly solidified alloy obtained in Example 9. As shown in FIG. 4, Nd2Fe 14 The presence of phase B was confirmed.

[0080] The rapidly solidified alloy obtained in the above process was coarsely pulverized to a few mm or less to obtain rapidly solidified alloy powder, and then the coarse powder of the rapidly solidified alloy was put into a raw material hopper using a flash annealing furnace (crystallization heat treatment furnace, furnace tube: transparent quartz, outer diameter 15 mm x inner diameter 12.5 mm x length 1000 mm, heating zone 300 mm, cooling zone by cooling fan 500 mm), and heat treatment was performed at a work cutting speed of 20 g / min. The inclination angle of the furnace tube, the rotation speed of the furnace tube, and the vibration frequency of the furnace tube were appropriately adjusted along with the heat treatment temperature and heat treatment time shown in Table 2 so as to obtain the heating rate shown in Table 2. As a result, the rapidly solidified alloy powder passed through the furnace tube while undergoing a movement that combines stirring due to the rotational motion of the furnace tube and hopping phenomenon due to the vibration of the furnace tube, and the rapidly solidified alloy powder was placed under unique heat treatment conditions in which the powder individually receives a thermal history rather than as a whole. An example of a heat treatment furnace and a thermal history in the step of performing flash annealing are shown in FIG. 2 and FIG. 3, respectively.

[0081] The constituent phases of the rapidly solidified alloy powder after flash annealing (crystallization heat treatment) were confirmed by powder X-ray diffraction. 14 B phase, and Fe 17 The presence of the RE2 phase was confirmed. Figure 5 shows a powder X-ray diffraction profile of the rapidly solidified alloy obtained in Example 9 after flash annealing (crystallization heat treatment) as a representative example. In addition, Fe 17 The peak of the RE2 phase is seen in Fig. 5 after flash annealing (crystallization heat treatment), and Nd2Fe 14 B phase and Fe 17 It was confirmed that the alloy had a composite structure in which the RE2 phase and the RE3 phase were mixed. In addition, elemental mapping was performed using TEM-EDX on the quenched alloy after flash annealing (crystallization heat treatment) obtained in Example 24, and the presence of a phase richer in Fe than the main phase was confirmed. Figure 6 shows an elemental mapping image obtained in Example 24 as a representative example. The left image in Figure 6 is a bright-field STEM image, in which the main phase and the grain boundary phase are visible. Meanwhile, the right image in Figure 6 is an Fe mapping image, in which it can be confirmed that Fe is rich in the position corresponding to the grain boundary phase in the left image.

[0082] The bright-field images and elemental mapping of the rapidly solidified alloys that had been subjected to flash annealing (crystallization heat treatment) were observed using a transmission electron microscope. From the bright-field images, Nd2Fe 14 B phase and NdFe 14 In addition, elemental mapping confirmed the presence of a grain boundary phase in which Nd and Fe were concentrated at the grain boundaries of the main phase, which is made up of the main constituent elements Nd, Fe, and B. Considering the above powder X-ray diffraction results, it was found that Fe 17 It was speculated that the RE2 phase was present at the grain boundaries consisting of Fe and RE. 17 The present inventors have confirmed that the grain boundary phase consisting of Fe and RE, including the RE2 phase, is formed in all the examples. In addition, in all the examples, the width of the thickest part of the grain boundary phase was 1 nm or more and less than 150 nm. For example, the grain boundary phase observed in Example 24 has a mixture of various thicknesses, but the width of the thickest part was 2 nm to 117 nm. In addition, in all the examples, the ratio of the main phase to the grain boundary phase was 70 vol% or more and less than 99 vol%, and the ratio of the grain boundary phase was 1 vol% or more and less than 30 vol%. For example, in Example 1, the ratio of the main phase to the grain boundary phase was 18 vol%, and the ratio of the main phase was 82 vol%.

[0083] The iron-based rare earth boron isotropic magnet alloy obtained by performing the flash annealing (crystallization heat treatment) shown in Table 2 was made into a sample for evaluating magnetic properties with a length of about 7 mm, a width of about 0.9 mm or more and 2.3 mm or less, and a thickness of 18 μm or more and 25 μm or less, and then magnetized in the longitudinal direction with a pulsed magnetic field of 3.2 MA / m. The sample for evaluating magnetic properties was then set in the longitudinal direction to suppress the effects of the demagnetizing field, and the magnetic properties at room temperature were measured using a vibrating sample magnetometer (VSM), with the results shown in Table 3. From Table 3, the remanence Br is 0.81 T or more, the intrinsic coercivity HcJ is 1200 kA / m or more and less than 1700 kA / m, and the maximum energy product (BH)max is 110 kJ / m. 3 It was found that the above magnetic properties were obtained by the alloy compositions and manufacturing methods described in Examples 1-24.

[0084] Next, the flash annealed (crystallization heat treatment) magnetic powder obtained in Example 9 was pulverized in a pin disk mill to an average particle size of 125 μm. Then, 2 mass% of epoxy resin diluted with methyl ethyl ketone (MEK) was added to this pulverized magnetic powder, and after mixing and kneading, 0.1 mass% of calcium stearate was added as a lubricant to prepare a compound for compression molded bonded magnets.

[0085] The above compression molded bonded magnet compound was compressed at 1568MPa (16ton / cm 2 ) to obtain a compression molded body having a diameter of 10 mm and a height of 7 mm, which was then subjected to a hardening heat treatment (curing) at 180°C for 1 hour in an argon gas atmosphere to obtain an isotropic compression molded bonded magnet. The density of the resulting isotropic compression molded bonded magnet was 6.3 g / cm. 3 (The true specific gravity of the magnetic powder is 7.5g / cm 3 ), the magnetic powder filling rate was 84 volume %.

[0086] The magnetic properties of the isotropic compression molded bonded magnet obtained using the magnetic powder of Example 9 were measured using a BH tracer after magnetizing it in the longitudinal direction with a pulsed magnetic field of 3.2 MA / m. The results were as follows: residual magnetic flux density Br: 0.71 T, intrinsic coercivity HcJ: 1223 kA / m, maximum energy product (BH)max: 82.2 kJ / m 3 It was found that the magnetic properties were expressed.

[0087] Next, the magnetic powder obtained in Example 9 after flash annealing (crystallization heat treatment) was pulverized in a pin disk mill to an average particle size of 75 μm. Then, while heating and stirring this pulverized magnetic powder, 0.75 mass% of a titanate coupling agent was sprayed onto the magnetic powder to perform coupling treatment, and 0.5 mass% of stearic acid amide and 4.75 mass% of nylon 12 resin powder were added and mixed as lubricants. Then, a compound for injection-molded bonded magnets was produced using a continuous extrusion kneader at an extrusion temperature of 170°C.

[0088] The compound for injection-molded bonded magnets was used to carry out injection molding at an injection temperature of 250°C to produce an isotropic injection-molded bonded magnet with a diameter of 10 mm and a height of 7 mm. The density of the resulting isotropic injection-molded bonded magnet was 4.6 g / cm. 3 (The true specific gravity of the magnetic powder is 7.5g / cm 3 ), the magnetic powder filling rate was 61 volume %.

[0089] The magnetic properties of the above isotropic injection molded bonded magnet obtained using the magnetic powder of Example 9 were measured with a BH tracer after magnetizing it in the longitudinal direction with a pulsed magnetic field of 3.2 MA / m. The results were as follows: residual magnetic flux density Br: 0.51 T, intrinsic coercivity HcJ: 1218 kA / m, maximum energy product (BH)max: 60.1 kJ / m 3 It was found that, despite being injection molded, it was possible to obtain magnetic properties equivalent to those of a general-purpose isotropic Nd-Fe-B compression molded bonded magnet.

[0090] (Comparative Example) To obtain the alloy composition shown in Table 1, 100 g of raw materials containing the main elements Nd, Pr, Dy, B, and Fe with a purity of 99.5% or more, as well as additive elements such as Co and Nb, were placed in an alumina melting crucible and then set in the work coil in a vacuum melting furnace. The vacuum melting furnace was then evacuated to 0.02 Pa or less, and argon gas was introduced to normal pressure, after which the alloy was molten by high-frequency induction heating. The molten alloy was then cast into a water-cooled copper mold to produce the master alloy.

[0091] Next, the obtained mother alloy was divided into appropriate sizes, and 40 g was inserted into a transparent quartz nozzle having an orifice with a suitable different diameter (0.7 mm or more, 1.2 mm or less) at the bottom so as to obtain the average melting rate shown in Table 1 (simply indicated as "melting rate" in Table 1), and then set in the work coil in the single roll quenching device. Then, the inside of the vacuum melting furnace was evacuated to 0.02 Pa or less, and argon gas was introduced until the quenching atmosphere pressure shown in Table 1 was reached, and the mother alloy was remelted by high-frequency induction heating, and the molten alloy was discharged from the nozzle orifice at a spray pressure of 30 kPa onto the surface of the rotating roll rotating at the roll surface speed (Vs) shown in Table 1, to produce a rapidly solidified alloy. In this case, the distance between the nozzle tip and the rotating roll surface was set to 0.8 mm.

[0092] The rapidly solidified alloy obtained in the above process was coarsely pulverized to a size of a few mm or less to obtain a rapidly solidified alloy powder, and then the rapidly solidified alloy coarse powder was put into a raw material hopper in a flash annealing furnace (crystallization heat treatment furnace, furnace tube: transparent quartz, outer diameter 15 mm x inner diameter 12.5 mm x length 1000 mm, heating zone 300 mm, cooling zone by cooling fan 500 mm), and heat treatment was performed at a workpiece cutting speed of 20 g / min. The inclination angle of the furnace tube, the rotation speed of the furnace tube, and the vibration frequency of the furnace tube were appropriately adjusted along with the heat treatment temperature and heat treatment time listed in Table 2 so as to obtain the heating rate listed in Table 2.

[0093] The constituent phases of the rapidly solidified alloy powder after flash annealing (crystallization heat treatment) were confirmed by powder X-ray diffraction. 14 The presence of B phase was confirmed. As a representative example, FIG. 7 shows the powder X-ray diffraction profile of the rapidly solidified alloy after flash annealing (crystallization heat treatment) obtained in Comparative Example 7. As shown in FIG. 7, Comparative Example 7 is Nd2Fe 14 It was confirmed that the metal structure was a single phase with phase B as the main phase.

[0094] The iron-based rare earth boron isotropic magnet alloy obtained in Comparative Example 7 was observed with a transmission electron microscope for bright field images and element mapping. In the bright field images, Nd2Fe 14Although the B phase was confirmed, no clear grain boundary phase was confirmed. In addition, element mapping also revealed that the grain boundary phase in which Fe and RE were concentrated, as seen in Example 9, was not present in the crystal grain boundaries of the main phase consisting of the main constituent elements Nd, Fe, and B. This was also the case in the other comparative examples.

[0095] The iron-based rare earth boron isotropic magnet alloy obtained by performing the flash annealing (crystallization heat treatment) shown in Table 2 was made into a sample for evaluating magnetic properties with a length of about 7 mm, a width of about 0.9 mm or more and 2.3 mm or less, and a thickness of 18 μm or more and 25 μm or less, and then magnetized in the longitudinal direction with a pulsed magnetic field of 3.2 MA / m. The sample for evaluating magnetic properties was then set in the longitudinal direction to suppress the effects of the demagnetizing field, and the magnetic properties at room temperature were measured with a vibrating sample magnetometer (VSM), with the results shown in Table 3. From Table 3, the above-mentioned Br: 0.81 T or more, HcJ: 1200 kA / m or more and less than 1700 kA / m, (BH)max: 110 kJ / m 3 It was found that the above magnetic properties were not obtained with the alloy compositions and manufacturing methods described in Comparative Examples 1-12.

[0096] In general, there is a trade-off between the remanence Br and the intrinsic coercivity HcJ, and it is difficult to achieve both a high remanence Br and a high intrinsic coercivity HcJ. In contrast, in this embodiment, by having an Fe-rich grain boundary phase in which the width of the thickest part of the grain boundary phase is 1 nm or more and less than 150 nm as described above, exchange interaction between the main phase and the grain boundary phase works effectively, and both properties can be improved. For example, Example 11 and Comparative Example 5 have the same high intrinsic coercivity HcJ, but Example 11 achieves a higher remanence Br than Comparative Example 5.

[0097] [Table 1]

[0098] [Table 2]

[0099] [Table 3] [Explanation of symbols]

[0100] 1 Raw material hopper 2. Material supply feeder 3. Core Tube 3a Enlarged view of the furnace tube 3b Enlarged cross-section of the furnace tube 4 tube furnace 5 cooling tower 6 Collection hopper 7 Transducer 8. Furnace tube rotation motor 9. Core tube rotation axis 10. Equipment stand 11. Core tube inclination angle 12 Cooling fan wind 13 Rapidly solidified alloy powder (workpiece) 14 Workpiece movement direction 15 Work hopping phenomenon 16 Heating rate 17 Holding temperature 18 Cooling rate 21 Main phase 22 Grain boundary phase

Claims

1. Composition formula T 100-x-y-z (B 1-n C n ) x R.E. y Zr z M m (T is at least one element selected from the group consisting of Fe, Co, and Ni, and is a transition metal element that necessarily includes Fe; RE is at least one rare earth element of Nd and Pr, which necessarily includes at least Nd; M is at least one metal element selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), The composition ratios x, y and z are 4.2 atomic %≦x≦5.0 atomic %, 13.1 atomic %≦y≦14.0 atomic %, 0 atomic %<z≦2.0 atomic %, 0.5 atomic %≦m≦5.0 atomic %, and 0.0≦n≦0.5 The alloy composition has a composition that satisfies RE 2 Fe 14 The RE has a lower B content than the stoichiometric composition of the B-type tetragonal compound, and has an average crystal grain size of 10 nm or more and less than 70 nm, which is finer than the critical diameter of a single magnetic domain. 2 Fe 14 An iron-based rare earth boron isotropic nanocomposite magnet alloy, characterized in that the main phase is a B-type tetragonal compound, and the grain boundary phase surrounding the main phase contains a phase that is richer in Fe than the main phase and has a width of its thickest part that is 10 nm or more and less than 150 nm.

2. 2. The iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 1, wherein the ratio of the main phase to the grain boundary phase is 70 volume % or more and less than 99 volume %, and the ratio of the grain boundary phase is 1 volume % or more and less than 30 volume %.

3. Residual magnetic flux density Br is 0.81 T or more, intrinsic coercivity HcJ is 1200 kA / m or more and less than 1700 kA / m, and maximum energy product (BH)max is 110 kJ / m 3 3. The iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 1, which exhibits the above magnetic properties.

4. The iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 1 or 2, wherein the RE contains at least Nd and Pr.

5. The composition ratios x, y and z are 4.2 atomic %≦x≦5.0 atomic %, 13.1 atomic %≦y≦14.0 atomic %, 0 atomic %<z≦2.0 atomic %, 3.1 atomic %≦m≦5.0 atomic %, and 0.0≦n≦0.5 3. The iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 1, having an alloy composition satisfying the following:

6. Composition formula T 100-x-y-z (B 1-n C n ) x R.E. y Zr z M m (T is at least one element selected from the group consisting of Fe, Co, and Ni, and is a transition metal element that necessarily includes Fe; RE is at least one rare earth element of Nd and Pr, which necessarily includes at least Nd; M is at least one metal element selected from the group consisting of Al, Si, V, Cr, Ti, Mn, Cu, Zn, Ga, Nb, Mo, Ag, Hf, Ta, W, Pt, Au, and Pb), The composition ratios x, y and z are 4.2 atomic %≦x≦5.0 atomic %, 13.1 atomic %≦y≦14.0 atomic %, 0 atomic %<z≦2.0 atomic %, 0.0 atomic %≦m≦5.0 atomic %, and 0.0≦n≦0.5 preparing a molten alloy having a composition that satisfies the above; The molten alloy is sprayed onto the surface of a rotating roll mainly composed of Cu, Mo, W or an alloy containing at least one of these metals at an average rate of 200 g / min or more and less than 2000 g / min per orifice hole arranged at the tip of the nozzle, thereby forming a RE. 2 Fe 14 A step of preparing a rapidly solidified alloy having 1 volume % or more of either a crystalline phase including a B phase or an amorphous phase; A method for producing an iron-based rare earth boron-based isotropic nanocomposite magnet alloy comprising the steps of:

7. The method further includes a step of performing flash annealing on the rapidly solidified alloy, in which the alloy is heated at a heating rate of 10° C. / sec or more and less than 200° C. / sec to reach a certain temperature range of a crystallization temperature or more and 850° C. or less, and then rapidly cooled after a lapse of 0.1 sec or more and less than 7 min. The flash annealing step provides RE 2 Fe 14 The RE has a lower B content than the stoichiometric composition of the B-type tetragonal compound, and has an average crystal grain size of 10 nm or more and less than 70 nm, which is finer than the critical diameter of a single magnetic domain. 2 Fe 14 7. The method for producing an iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 6, wherein a nanocomposite metal structure is formed in which a B-type tetragonal compound is the main phase, and a grain boundary phase surrounding the main phase includes a phase that is richer in Fe than the main phase and has a width of the thickest part of 10 nm or more and less than 150 nm.

8. 7. The method for producing powder of iron-based rare earth-boron-based isotropic nanocomposite magnet alloy according to claim 6, further comprising the step of producing iron-based rare earth-boron-based isotropic magnet alloy powder by pulverizing the rapidly solidified alloy.

9. A method for producing a powder of the iron-based rare earth boron-based isotropic nanocomposite magnet alloy described in claim 7, further comprising a step of producing an iron-based rare earth boron-based isotropic magnet alloy powder by pulverizing the rapidly solidified alloy that has been subjected to the flash annealing.

10. A step of preparing an iron-based rare earth boron isotropic nanocomposite magnet alloy powder produced by the method for producing an iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 7; A step of adding a thermosetting resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder, filling the powder into a molding die, and forming a compression molded body by compression molding, followed by heat treatment at a temperature equal to or higher than the polymerization temperature of the thermosetting resin; A method for manufacturing a resin-bonded permanent magnet comprising the steps of:

11. A step of preparing an iron-based rare earth boron isotropic nanocomposite magnet alloy powder produced by the method for producing an iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 7; adding a thermoplastic resin to the iron-based rare earth boron-based isotropic nanocomposite magnet alloy powder to prepare an injection molding compound, and then injection molding the compound; A method for manufacturing a resin-bonded permanent magnet comprising the steps of:

12. The molten alloy is The composition ratios x, y and z are 4.2 atomic %≦x≦5.0 atomic %, 13.1 atomic %≦y≦14.0 atomic %, 0 atomic %<z≦2.0 atomic %, 3.1 atomic %≦m≦5.0 atomic %, and 0.0≦n≦0.5 8. The method for producing an iron-based rare earth boron isotropic nanocomposite magnet alloy according to claim 6 or 7, having a composition that satisfies the above.

Citation Information

Patent Citations

  • Permanent magnet

    JP1984046008A

  • High energy stored rare earth-iron magnetic alloy

    JP1985009852A

  • Permanent magnet material, permanent magnet and manufacture of permanent magnet

    JP1996162312A

  • (rare earth)-iron-boron magnetic alloy and its production and bond magnet using the (rare earth)-iron-boron magnetic alloy

    JP1998053844A

  • Permanent magnet having plural ferromagnetic phases, and its manufacturing method

    JP2002175908A