Method for producing microwires or nanowires
The method enhances the production of microwires and nanowires by controlling gaseous precursors and reactor conditions to achieve precise geometry, uniform position, and single crystal structure, addressing limitations in density and polarity for industrial-scale manufacturing.
Patent Information
- Application Number
- JP2021577636
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-06-26
AI Technical Summary
Existing methods for producing microwires and nanowires made of III-V compounds face limitations in controlling geometry, position, crystallographic properties, density, and polarity, with low density and single crystal structure formation, particularly in industrial-scale production at low cost.
A method involving precise control of gaseous precursors for Group III-V compounds, including a first and second precursor for Group V and III elements, with optional dopant precursors, and specific reactor conditions to form microwires or nanowires with uniform dopant concentration and controlled crystallographic properties, allowing for higher dopant concentrations and varying polarity.
Enables the production of microwires and nanowires with precise geometry, uniform position, and single crystal structure, achieving high density and controlled polarity, suitable for industrial-scale manufacturing at lower costs.
Smart Images

Figure 0007568300000002 
Figure 0007568300000003 
Figure 0007568300000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates generally to devices formed from semiconductor materials and methods of manufacturing the same, and more particularly to devices comprising three-dimensional semiconductor elements of nanometer or micrometer size, in particular microwires or nanowires. [Background technology]
[0002] Examples of microwires or nanowires comprising semiconductor materials are those made of compounds mainly containing elements of groups III and V, such as gallium nitride GaN (hereafter referred to as III-V compounds). Such microwires or nanowires make it possible to produce semiconductor devices, such as optoelectronic devices. The term optoelectronic device is used to mean a device capable of converting an electrical signal into electromagnetic radiation or vice versa, in particular a device for the detection, measurement or emission of electromagnetic radiation or for photovoltaic applications. Summary of the Invention [Problem to be solved by the invention]
[0003] A method for fabricating microwires / nanowires of semiconductor material should enable the fabrication of microwires / nanowires with precise and uniform control over the geometry, position and crystallographic properties of each microwire / nanowire.
[0004] US Patent No. 9,245,948 describes a method for producing microwires / nanowires made of III-V compounds by metalorganic chemical vapor deposition (MOCVD), which allows the production of microwires / nanowires with good control over the geometric structure, position and crystallographic properties of each microwire / nanowire, but only microwires / nanowires with polarity of group V elements, with a density of microwires / nanowires of less than 20%, in particular less than 10%, corresponding to the ratio of the surface area occupied by the microwires / nanowires on the support to the total surface area of the support.
[0005] It is therefore an object of the embodiments to at least partially overcome the disadvantages of the above-mentioned methods of manufacturing microwires / nanowires formed of III-V compounds.
[0006] Another object of the embodiment is that the density of the microwires / nanowires can be less than 10%.
[0007] Another object of the embodiment is that each microwire / nanowire can be formed with Group V element polarity or Group III element polarity.
[0008] It is another object of the embodiment that each microwire / nanowire has substantially a single crystal structure.
[0009] Another embodiment offers the possibility to precisely and uniformly control the position, geometric structure and crystallographic properties of each microwire / nanowire.
[0010] Another object of the embodiments is that the microwires / nanowires can be manufactured on an industrial scale and at low cost. [Means for solving the problem]
[0011] An embodiment is a method of fabricating a device with a micrometer- or nanometer-sized wire comprising a III-V compound, comprising: a first gaseous precursor of a group V element; a second gaseous precursor of a group III element; and a 5×10 ions dopant concentration in a portion of the wire, where the portion of the wire has a uniform dopant concentration. 19 atoms / cm 3 , e.g. 1×10 20 atoms / cm 3 forming at least a portion of the wire for each wire by a process of metalorganic vapor phase epitaxy that includes injecting into the reactor a gas capable of obtaining a higher dopant concentration and a third gas precursor of an additional element that is a dopant of the III-V compound.
[0012] According to an embodiment, the dopant concentration at the surface of the portion of the wire is 1×10 20 atoms / cm 3 Higher and / or covering a portion of the wire with a layer of a material different from the III-V compound and containing the additional element.
[0013] According to an embodiment, the ratio of the flow rate of the first gas precursor to the flow rate of the third gas precursor is less than 1,000, for example 130.
[0014] According to an embodiment, the temperature in the reactor during the forming of the part is 950° C. or higher.
[0015] According to an embodiment, the temperature in the reactor in the step of forming the part is 1,000° C. or higher.
[0016] According to an embodiment, the V / III ratio in the step of forming the portion is 100 or less.
[0017] According to an embodiment, the V / III ratio in the forming step is 50 or less, for example 5.
[0018] According to an embodiment, in the method, the ratio of the flow rate of the neutral gas to the flow rate of the second gas precursor in the step of injecting a neutral gas into the reactor and forming the portion is less than 100, for example 10.
[0019] According to an embodiment, the ratio of the flow rate of the third gas precursor to the flow rate of the second gas precursor is less than 1,000, for example 130.
[0020] According to an embodiment, the ratio of the flow rate of the third gas precursor to the flow rate of the neutral gas is less than 1,000,000, for example 1,300. [Brief description of the drawings]
[0021] The above and other features and advantages are explained in more detail in the following particular embodiments, given as non-limiting illustrations of the invention with reference to the accompanying drawings, in which: FIG.
[0022] [Figure 1] 1A-1D are schematic partial cross-sectional views showing structures obtained at steps of an embodiment of a method for manufacturing a device comprising nanowires or microwires. [Diagram 2] 5A-5C are cross-sectional views illustrating the structure obtained at different steps of the method; [Diagram 3] 5A-5C are cross-sectional views illustrating the structure obtained at different steps of the method; [Figure 4] FIG. 1 shows images of devices with nanowires or microwires obtained by scanning electron microscopy. [Diagram 5] FIG. 2 shows another image of a device with nanowires or microwires obtained by scanning electron microscopy (SEM). [Figure 6] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 7] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 8]FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 9] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 10] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 11] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 12] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 13] FIG. 13 shows another SEM image of a device with nanowires or microwires. [Figure 14] 1 is a schematic partial cross-sectional view illustrating an embodiment of an optoelectronic device comprising microwires or nanowires. [Figure 15] 1 is a schematic partial cross-sectional view illustrating another embodiment of an optoelectronic device comprising microwires or nanowires. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Similar features are indicated by similar reference numerals in the various drawings. In particular, structural and / or functional features common to various embodiments may bear the same reference numerals and may have the same structural, dimensional and material characteristics. For clarity, only those steps and elements useful for understanding the embodiments described herein are shown and described in detail.
[0024] In the following description, when referring to terms defining absolute positions such as "front", "back", "top", "bottom", "left", "right" or relative positions such as "up", "down", "upper", "lower" or orientations such as "horizontal" and "vertical", the terms refer to the device in its orientation in the drawing or in its normal position of use. Unless otherwise specified, the terms "about", "approximately", "substantially" and "to the extent" mean within 10% of the relevant value, preferably within 5%. When the terms "about", "approximately", "substantially" and "to the extent" are used in relation to orientation, these terms mean within 10% of the relevant value, preferably within 5%. Further, in this specification, the terms "insulating" and "conducting" are deemed to mean "electrically insulating" and "electrically conducting", respectively.
[0025] The present invention relates to the production of three-dimensional elements of nanometer or micrometer size, in particular microwires or nanowires.
[0026] The term "microwire" or "nanowire" refers to a three-dimensional structure having an elongated shape in a desired direction, with at least two dimensions, referred to as minor dimensions, in the range of 5 nm to 5 μm, preferably in the range of 50 nm to 2 μm, more preferably in the range of 50 nm to 1.5 μm, and a third dimension, referred to as major dimension or height, that is equal to or greater than the maximum of the minor dimensions, preferably equal to or greater than three times the maximum, more preferably equal to or greater than five times the maximum. In an embodiment, the height of each microwire or nanowire may be equal to or greater than 500 nm, preferably in the range of 1 μm to 50 μm. In the following description, the term "wire" is used to mean "microwire" or "nanowire".
[0027] The cross-sectional shape of the wire may be different and may be, for example, elliptical, circular or polygonal, in particular triangular, rectangular, square or hexagonal. The term "average diameter" used in connection with the cross-section of a wire denotes a quantity related to the surface area of the wire in this cross-section, which corresponds for example to the diameter of a disk having the same surface area as the cross-section of the wire.
[0028] The wire mainly comprises at least one III-V compound, such as a III-N compound, preferably at least 60% by weight, more preferably at least 80% by weight. Examples of III elements are gallium (Ga), indium (In) or aluminum (Al). Examples of III-N compounds are GaN, AlN, InN, InGaN, AlGaN or AlInGaN. Other V elements may also be used, such as phosphorus or arsenic. In general, the elements in the III-V compounds may be combined in different mole fractions. The semiconductor material of the wire may contain dopants, such as silicon to ensure N-type doping of the III-N compound, or magnesium to ensure P-type doping of the III-N compound.
[0029] That a III-V compound has group III polarity or group V polarity means that the material will grow in the desired crystallographic direction and that the final atomic plane, e.g., the highest plane when growth occurs from bottom to top, will essentially comprise atoms of group III element in the case of group III polarity or atoms of group V element in the case of group V polarity.
[0030] 1-3 show structures obtained at successive steps of an embodiment of a method for manufacturing an optoelectronic device with wires formed from III-V compounds.
[0031] Figure 1 shows - forming a seed layer 14 on the surface 12 of the substrate 10, for example by a conformal chemical vapor deposition (CVD) or physical vapor deposition (PVD) type method, - forming a grown passivation layer 16 on the seed layer 14, for example by CVD; and forming openings 18 (three openings 18 are shown by way of example in FIGS. 1 to 3 ) in the grown passivation layer 16, for example by anisotropic etching, in particular reactive ion etching, i.e. RIE, inductively coupled plasma etching, i.e. ICP etching or chemical etching; The resulting structure is shown after
[0032] The cross-section of the openings 18 may correspond to the desired cross-section of the wire 22 or may differ from the resulting cross-section of the wire 22. The average diameter of the wire 22 may be equal to or greater than the average diameter of the openings 18.
[0033] The substrate 10 may represent a monoblock structure or a layer covering a support made of another material. The substrate 10 is preferably a semiconductor substrate, for example a substrate made of silicon, germanium, silicon carbide, a III-V compound such as GaN or GaAs, or a ZnO substrate. The substrate 10 is preferably a monocrystalline silicon substrate. The substrate is preferably a semiconductor substrate compatible with the manufacturing methods implemented in microelectronics. The substrate 10 may represent a multilayer structure of the silicon-on-insulator type, also called SOI. As a variant, the substrate may be insulating and may be made of, for example, sapphire or spinel.
[0034] The seed layer 14 is formed of a material that favors wire growth. By way of example, the material forming the seed layer 14 may be a nitride, carbide or boride of a transition metal from columns IV, V or VI of the periodic table of the elements, or a combination of these compounds. By way of example, the seed layer 14 may be formed of aluminum nitride (AlN), boron (B), boron nitride (BN), titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), hafnium (Hf), hafnium nitride (HfN), niobium (Nb), niobium nitride (NbN), zirconium (Zr), zirconium boride (ZrB2), zirconium nitride (ZrN), silicon carbide (SiC), tantalum carbonitride (TaCN), Mg x N y(where x is about 3 and y is about 2, e.g. magnesium nitride in the form of Mg3N2), magnesium gallium nitride (MgGaN), tungsten (W), tungsten nitride (WN), or combinations thereof. The seed layer 14 may have a monolayer structure or may correspond to a stack of at least two layers, each formed, for example, of one of the aforementioned materials.
[0035] According to an embodiment, the seed layer 14 may not be provided. According to another embodiment, the seed layer 14 may be replaced by a seed pad formed, for example, in the opening 18.
[0036] The material forming the seed layer 14 may be formed of a material that favors wire growth depending on the polarity of group III elements or wire growth depending on the polarity of group V elements.
[0037] The grown passivation layer 16 is made of a dielectric material, such as silicon oxide (SiO2), silicon nitride (Si x N y , where x is about 3 and y is about 4, e.g., Si3N4), (particularly of the general formula SiO x N yThe grown passivation layer 16 may be made of silicon oxynitride (e.g. Si2ON2), aluminum oxide (Al2O3), hafnium oxide (HfO2) or diamond. The grown passivation layer 16 may have a monolayer structure or may correspond to a stack of two or more layers. If the grown passivation layer 16 corresponds to a stack of at least two layers, the upper layer of the stack is insulating and is made, for example, of a dielectric material. One or more lower layers of the stack between the seed layer 14 and the insulating upper layer may be made of a dielectric material. By way of example, the underlayer(s) may be formed of a semiconductor or metallic material, such as aluminum nitride (AlN), boron (B), boron nitride (BN), titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), hafnium (Hf), hafnium nitride (HfN), niobium (Nb), niobium nitride (NbN), zirconium (Zr), zirconium boride (ZrB2), zirconium nitride (ZrN), silicon carbide (SiC), tantalum carbonitride (TaCN), tungsten (W), or tungsten nitride (WN).
[0038] FIG. 2 shows the structure obtained after a seed 20 made of the same III-V compound as the wires has been grown in opening 18, for example by MOCVD, in contact with seed layer 14.
[0039] 3 shows the resulting structure after growing wires 22 from seeds 20, with each wire 22 extending from substrate 10 through one of the openings 18. Each wire 22 extends along a substantially straight axis A that is substantially perpendicular to surface 12.
[0040] Each wire 22 may have a lower portion 24 that is closest to the substrate 10 and extends to an upper portion 26. The lower portion 24 has a core 28 including a III-V material doped with a dopant of a first conductivity type, e.g., N-type, and a layer 30 covering the sidewalls of the core 28, possibly including 30% or more by weight of a dopant along with a group III or V element. The upper portion 26 is formed of an unintentionally doped III-V material. In some embodiments, the upper portion 26 may not be provided. The lower portion 24 of the wire 22 is formed in a first growth step, and the upper portion 26 of the wire 22 is formed in a second growth step.
[0041] The method for growing the seeds 20 and wires 22 is the MOCVD method, also known as metalorganic vapor phase epitaxy (MOVPE) method. The growth conditions of the seeds 20 are different from those of the wires 22, and the growth conditions of the seeds 20 favor the growth of III-V compounds on the seed layer 14 without favoring a particular growth direction. According to an alternative embodiment, there is no step of growing the seeds 20, and the wires 22 are formed directly on the seed layer 14 in the openings 18.
[0042] For example, the method may include injecting a precursor of a group III element and a precursor of a group V element into a reactor. Examples of precursors of group III elements include trimethylgallium (TMGa), triethylgallium (TEGa), trimethylindium (TMIn), or trimethylaluminum (TMAl). Examples of precursors of group V elements include ammonia (NH3), tertiary butyl phosphine (TBP), arsine (AsH3), or unsymmetrical dimethylhydrazine (UDMH).
[0043] According to an embodiment, the temperature in the reactor during the growth of the seeds 20 is below 1,000°C, preferably below 820°C.
[0044] According to an embodiment, the ratio of the flow rate of the group V element precursor gas to the flow rate of the group III element precursor gas, ie, the V / III ratio, for forming the seeds 20 is 1,000 or more, and preferably 5,000 or more.
[0045] The temperature in the reactor in the step of forming the seed 20 is preferably lower than the temperature in the reactor in the step of forming the wire 22. The V / III ratio in the step of forming the seed 20 is preferably higher than the V / III ratio in the step of forming the wire 22.
[0046] According to an embodiment, the temperature in the reactor during the process of forming the wire 22 is 950°C or higher, preferably 1,000°C or higher, more preferably 1,050°C or higher, for example approximately 1,095°C.
[0047] According to an embodiment, the V / III ratio in the step of forming the wire 22 is 100 or less, preferably 50 or less, more preferably 20 or less, more preferably 10 or less, for example about 5.
[0048] According to the embodiment, the pressure in the reactor in the process of forming the wire 22 is within the range of 666 Pa (5 Torr) to 199,984 (1,500 Torr).
[0049] According to an embodiment of the present invention, at least in the first stage of growing the III-V compound wire 22, a precursor of an additional element is added in excess in addition to the III-V compound precursor. The additional element may be silicon (Si). Examples of silicon precursors include silane (SiH4), disilane (S2H6) and dichlorosilane (SiH2Cl2).
[0050] According to an embodiment of the invention, the ratio of the flow rate of the gas precursor of the group V element to the flow rate of the gas precursor of the additional element is less than 1,000, preferably less than 500, more preferably less than 200, for example about 140. According to an embodiment, the ratio of the flow rate of the gas precursor of the additional element to the flow rate of the gas precursor of the group III element is less than 3×10 -4 The flow rate of the gas precursor is 5×10 ions / cm 2 into the core 28 of the lower portion 24 of the wire 22 if all the dopant is incorporated into the core 28 of the lower portion 24 of the wire 22.19 atoms / cm 3 Higher, preferably 10 20 atoms / cm 3 However, the growth step of the lower portion 24 produces a layer 30 that contains a significant proportion of dopant, so that the actual dopant concentration in the core 28 is 10 20 atoms / cm 3 is less than.
[0051] According to an embodiment, a carrier gas may be used that ensures the diffusion of the metalorganic precursors up to the reactor during the growth of the seeds 20 and the wires 22. The carrier gas may comprise a neutral gas or a mixture of neutral gases, in particular a mixture of nitrogen (N2) and hydrogen (H2). The carrier gas may be filled together with the metalorganic precursors in a bubbler. According to an embodiment, the volume concentration of hydrogen in the carrier gas is in the range of 0% to 100%, for example approximately 20%.
[0052] The ratio of the flow rate of the carrier gas to the flow rate of the precursor gas of the group III element is less than 100, for example 10. The ratio of the flow rate of the precursor gas of the additional element to the flow rate of the carrier gas is less than 1,000,000, for example 1,300.
[0053] The presence of silane as a precursor gas incorporates silicon into the GaN compound, which in turn causes a layer of silicon nitride 30 to form during growth of the lower portion 24 of the wire 22, covering the periphery of the lower portion 24 except for the top portion.
[0054] To grow the upper portion 26, the above-mentioned operating conditions of the MOCVD reactor are maintained as an example, except that the flow of silane in the MOCVD reactor is reduced, for example by a factor of 10 or stopped. Even when the silane flow is stopped, the active portion may be doped N-type by diffusion of dopants from adjacent passivated portions into the active portion or by residual doping of the GaN.
[0055] Tests were carried out. A first substrate, a second substrate or a third substrate was used. The first substrate corresponds to a sapphire support covered with GaN, which favours the growth of GaN depending on the metal polarity. The second substrate corresponds to a silicon support covered with an AlN seed layer, which favours the growth of GaN depending on the metal polarity. The third substrate corresponds to a substrate favouring the growth of GaN depending on the nitrogen polarity. The growth passivation layer 16 included a stack of a Si3N4 layer with a thickness of 80 nm and a SiO2 layer with a thickness of 50 nm. The cross section of the openings 18 was circular. The openings 18 were arranged in rows and columns. Three MOCVD methods with different parameters were carried out. If not indicated otherwise, in the following tests, the values of the parameters of the method are the values indicated in Table 1 below.
[0056] [Table 1]
[0057] Comparison method P1 Method P1 corresponds to a known nanowire formation method called the low flow method, or LF method. This method is an MOCVD method that can only form Ga-polar GaN wires. Thus, during method P1, the seed layer 14 favors the growth of Ga-polar wires.
[0058] Figure 4 shows an image obtained by scanning electron microscopy of wires 22 produced according to method P1 when the average diameter of each wire 22 was 350 nm and when the spacing between two adjacent openings 18 in the same row was 800 nm. A third substrate was used. As shown in Figure 4, the size of the obtained wires 22, in particular the average diameter and height, is not uniform.
[0059] 5, 6 and 7 are respectively plan views obtained by scanning electron microscopy of wires 22 produced according to method P1 when the average diameter of the openings 18 was 100 nm, 150 nm and 200 nm, respectively, and when the spacing between two adjacent openings 18 in the same row was 400 nm, 330 nm and 800 nm, respectively. A first substrate was used. As can be seen in the figures, the number of defects increases with increasing average diameter of the openings 18.
[0060] Figure 8 shows an image obtained by scanning electron microscopy of wires 22 produced according to method P1 when the average diameter of each wire 22 was 420 nm and when the spacing between two adjacent openings 18 in the same row was 800 nm. A second substrate was used. As shown in Figure 8, as the mesh spacing increases, blocks 32 of GaN result.
[0061] 9 and 10 are respectively images obtained by scanning electron microscopy of wires 22 produced according to method P1 when the average diameter of the openings 18 was 100 nm, the spacing between two adjacent openings 18 in the same row was 300 nm, and the processing times were 2 and 30 minutes, respectively. A first substrate was used. As shown in Figs. 9 and 10, beyond a given time of about 5 minutes, there is almost no increase in the length of the wires 22 and blocks 32 of GaN are formed. Thus, wires with heights of more than 800 nm cannot be obtained by method P1.
[0062] Comparison method P2 Method P2 corresponds to known nanowire formation methods such as the method described in US Pat. No. 9,245,948. Method P2 is an MOCVD method capable of forming only N-polarity GaN wires. A third substrate was used. Thus, the seed layer favors the growth of N-polarity wires 22. Method P2 gives satisfactory results, especially for low densities of wires 22 below 5%, but is not adapted to higher wire densities. For method P2, the flow rate of the precursor of the additional element, here SiH4, is set to 1000 μm at the lower portion 24 of the wire 22 when the lower portion 24 has a uniform composition.19 atoms / cm 3 is selected to obtain a Si dopant concentration of
[0063] Figure 11 shows an image obtained by scanning electron microscopy of wires obtained according to method P2 when the average diameter of each wire was 350 nm and the spacing between two adjacent openings 18 in the same row was 800 nm, corresponding to a target density of wires of approximately 20%. As shown in Figure 11, many openings 18 do not have wires 22 growing in them. A filling rate of less than 50% is obtained.
[0064] Method P3 Method P3 corresponds to an embodiment of the method according to the invention.
[0065] FIG. 12 shows a scanning electron microscope image of wires obtained with method P3 when using the first substrate. The first substrate favors the growth of Ga-polar wires. The average diameter of each wire was 220 nm and the spacing between two adjacent openings 18 in the same row was 400 nm. There are no visible defects.
[0066] Figure 13 shows a scanning electron microscope image of wires obtained with method P3 when using a third substrate, and thus a substrate favoring the growth of N-polarity wires. The average diameter of each wire was 540 nm, and the spacing between two adjacent openings 18 in the same row was approximately 800 nm. There were few visible defects, and the growth rate, corresponding to the number of wires grown in each opening, was greater than 95%.
[0067] Examples of applications of devices comprising said wires are optoelectronic devices, examples of which are optoelectronic devices comprising light emitting diodes, devices for detecting or measuring electromagnetic radiation or devices for photovoltaic applications.
[0068] FIG. 14 is a schematic partial cross-sectional view illustrating an embodiment of an optoelectronic device 35 comprising a light emitting diode.
[0069] Figure 14 shows, from bottom to top, a semiconductor substrate 10; a seed layer 14 arranged on the surface 12 and made of a material that promotes wire growth; a growth passivation layer 16 covering the seed layer 14 and having an opening 18 exposing a portion of the seed layer 14; - wires 22 (one wire shown) each protruding from one of the openings 18; a shell 40 having a stack of semiconductor layers covering the side and top surfaces of each wire 22; an insulating layer 42 extending over the sides of the lower part of the shell 40 and over the grown passivation layer 16 between the wires 22; a layer 44 forming an electrode covering each shell 40 and extending further on the insulating layer 42; The structure shown is:
[0070] The assembly formed by each wire 22 and associated shell 40 forms a light emitting diode. The shell 40 may include a stack of layers including, among others, an active layer 46 and a bonding layer 48. The active layer is the layer from which the majority of the light emitted by the light emitting diode DEL is emitted. By way of example, the active layer 46 may include a confinement means such as multiple quantum wells. The bonding layer may include a stack of semiconductor layers of the same III-V material as the wires 22, but of opposite conductivity type.
[0071] FIG. 15 is a partial cross-sectional schematic diagram showing an embodiment of an optoelectronic device 50 with a light emitting diode, in which, compared to the optoelectronic device 35 shown in FIG. 14, the shell 40 and the electrode 44 are provided only on the top of the wire 22.
[0072] Various embodiments and variants have been described. Those skilled in the art will understand that certain features of these various embodiments and variants can be combined, and other variants will occur to those skilled in the art. Finally, the actual implementation of the described embodiments and variants is within the skill of those skilled in the art based on the functional representations set forth above.
[0073] This patent application claims priority from French Patent Application No. 19 / 07109, which is incorporated herein by reference.
Claims
1. 1. A method of manufacturing a device comprising micrometer or nanometer sized wires on a substrate comprising a III-V compound, the wires having a polarity corresponding to the substrate on which the wires are grown, whether the substrate is a group V polarity or a group III polarity, comprising the steps of: A first gas precursor of a group V element, a second gas precursor of a group III element, and a third gas precursor of an additional element that is a dopant for a III-V compound are mixed in a gas mixture having a ratio of a flow rate of the third gas precursor of the additional element to a flow rate of the second gas precursor of the group III element of 3×10 -4 forming at least a portion of the wire by a process of metalorganic vapor phase epitaxy, the process including injecting into a reactor a ratio of a flow rate of a first gaseous precursor of the group V element to a flow rate of a third gaseous precursor of the additional element that is equal to or less than 1,000 for each wire, such that when the portion of the wire has a uniform dopant concentration, the portion of the wire has a dopant concentration of 5×10 19 A method for obtaining dopant concentrations higher than atoms / cm 3 .
2. The method of claim 1, obtaining a dopant concentration in a portion of the wire that is greater than 1×10 20 atoms / cm 3 when the portion of the wire has a uniform dopant concentration.
3. The method of claim 1, wherein the ratio of the flow rate of the first gas precursor of the group V element to the flow rate of the third gas precursor of the additional element is 500 or less.
4. The method of claim 3, wherein the ratio of the flow rate of the first gas precursor of the Group V element to the flow rate of the third gas precursor of the additional element is 200 or less.
5. The dopant concentration at the surface of the wire is 1×10 20 atoms / cm 3 The method according to any one of claims 1 to 4, further comprising covering a part of said wire with a layer of a material different from said III-V compound and containing said additional element.
6. The method according to any one of claims 1 to 5, wherein the temperature in the reactor during the forming step is 950°C or higher.
7. 7. The method of claim 6, wherein the temperature in the reactor during the forming step is 1,000° C. or greater.
8. The method according to any one of claims 1 to 7, wherein the V / III ratio in the step of forming a part is 100 or less.
9. 9. The method of claim 8, wherein the V / III ratio in the forming step is 50 or less.
10. Injecting a neutral gas into the reactor; The method of any one of claims 1 to 9, wherein the ratio of the flow rate of the neutral gas to the flow rate of the second gas precursor during the forming of the portion is less than 100.
11. The method of claim 10 , wherein a ratio of a flow rate of the third gas precursor to a flow rate of the second gas precursor is less than 1,000.
12. 12. The method of claim 10 or 11, wherein the ratio of the flow rate of the third gas precursor to the flow rate of the neutral gas is less than 1,000,000.
13. and successively forming at least the first portion of the wire and the second portion of the wire by a process of metalorganic vapor phase epitaxy, the process including injecting into the reactor a first gaseous precursor of a group V element, a second gaseous precursor of a group III element, and a third gaseous precursor of an additional element that is a dopant of a group III-V compound of a gas capable of forming the first portion of the wire, such that when the first portion of the wire has a uniform dopant concentration, the first portion has a dopant concentration of 5×10 19 The method of any one of claims 1 to 12, further comprising reducing or stopping the flow of the third gas precursor to obtain a dopant concentration higher than atoms / cm 3 to form the second portion.
14. The method of claim 13, obtaining a dopant concentration in the first portion of the wire greater than 1×10 20 atoms / cm 3 when the first portion of the wire has a uniform dopant concentration.
Citation Information
Patent Citations
Method for manufacturing an optoelectronic device comprising a light-emitting diode
JP2016535434A