HOLLOW SEMICONDUCTOR PACKAGE, ITS MANUFACTURING METHOD, AND RESIN COMPOSITION SET FOR HOLLOW SEMICONDUCTOR PACKAGE
The use of polysiloxane resin for both spacer and sealant in hollow semiconductor packages addresses reflow resistance and reliability issues by minimizing moisture retention and dimensional changes, ensuring joint integrity.
Patent Information
- Application Number
- JP2020179425
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Hollow semiconductor packages face issues with reflow resistance and reliability due to dimensional changes caused by temperature and humidity, leading to peeling or cracking at the joints between the spacer, substrate, and lid, or at the interface between the spacer and sealant.
A hollow semiconductor package design using a polysiloxane resin for both the spacer and sealant, with a moisture permeability of 0.05 to 0.6 g/m·24h and a glass transition temperature of 30 to 150°C, ensuring the spacer and sealant have similar dimensional changes, reducing moisture retention and enhancing joint reliability.
The polysiloxane resin composition effectively dissipates moisture and minimizes dimensional differences, preventing peeling and cracking, thereby improving the reliability and reflow resistance of the hollow semiconductor package.
Smart Images

Figure 0007568476000005 
Figure 0007568476000006 
Figure 0007568476000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a hollow semiconductor package having a semiconductor element in a hollow structure and a method for producing the same, and also to a resin composition set for a hollow semiconductor package used for forming a spacer and a sealant for the hollow semiconductor package. [Background technology]
[0002] A hollow package structure in which a semiconductor element is disposed in a hollow structure is known as a structure for a light receiving semiconductor device such as a solid-state image sensor or a semiconductor laser. In the hollow structure, a spacer is disposed between a substrate such as a silicon substrate and a lid made of glass or the like, and the joints between the substrate and the spacer and the joints between the lid and the spacer are sealed with a sealant to maintain airtightness.
[0003] Patent Document 1 proposes forming a spacer by applying a photosensitive resin composition having thermocompression bonding properties to the substrate material onto the substrate and patterning the composition into a frame shape by photolithography. Patent Document 2 describes that adding a moisture absorbent to the sealant improves the reliability of the hollow semiconductor package by absorbing moisture inside the hollow structure in which the semiconductor element is arranged. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-116968 A [Patent Document 2] JP 2002-124589 A Summary of the Invention [Problem to be solved by the invention]
[0005] Hollow semiconductor packages require reflow resistance because they must go through a high-temperature reflow process during mounting. In addition, even if the temperature and humidity change in the device's operating environment, peeling or cracks must not occur at the joints between the spacer and the substrate or lid, or at the interface between the spacer and the sealant, and the hollow structure must remain sealed.
[0006] The spacer and sealant that form the hollow structure are made of resin materials, and so are prone to dimensional changes due to humidification and temperature changes. If the hygroscopicity of the sealant is increased as proposed in Patent Document 2, moisture absorption and expansion become significant, and peeling or cracks may occur at the interface due to differences in the amount of dimensional change between the spacer and the sealant.
[0007] In view of the above, an object of the present invention is to provide a hollow semiconductor package in which retention of moisture in the hollow structure is suppressed and the joint between the spacer and the sealant is highly reliable. [Means for solving the problem]
[0008] The hollow semiconductor package includes a semiconductor element in a hollow structure formed by a substrate, a lid, and a frame-shaped spacer disposed between the substrate and the lid. The joint between the substrate and the spacer and the joint between the lid and the spacer are sealed with a sealing part. Both the spacer and the sealing part preferably contain a polysiloxane resin.
[0009] The sealing portion may have a product of moisture permeability and thickness of 0.05 to 0.6 g / m·24 h. The sealing portion may have a glass transition temperature of 30 to 150° C.
[0010] The sealing portion is preferably formed by thermally curing a sealant made of a thermosetting resin composition containing a polysiloxane resin. The polysiloxane resin of the sealing portion (sealant after thermal curing) may contain either a cyclic polysiloxane structure or a chain polysiloxane structure, or may contain both.
[0011] The sealant may contain a polysiloxane polymer having two or more SiH groups in one molecule and a crosslinker having two or more alkenyl groups in one molecule. The polysiloxane polymer of the sealant may contain a cyclic polysiloxane structure, and the crosslinker may contain a linear polysiloxane structure. When the sealant is thermally cured, the polymer and the crosslinker react with each other, so that the sealant formed by thermal curing contains a polymer having both a cyclic polysiloxane structure and a linear polysiloxane structure.
[0012] The spacer can also be produced using a photosensitive resin composition. For example, a photosensitive resin composition containing a polysiloxane resin is applied and patterned by photolithography to obtain a spacer having a frame-shaped pattern.
[0013] As described above, the sealant (thermosetting resin composition) used to form the sealing portion and the photosensitive resin composition used to form the spacer each contain a polysiloxane resin. These resin compositions can also be provided as a resin composition set for a hollow semiconductor package. Effect of the Invention
[0014] The hollow semiconductor package of the present invention has high moisture permeability because the spacer and the sealing part contain polysiloxane resin. Therefore, even if moisture penetrates into the hollow structure, the moisture is easily dissipated to the outside via the spacer and the sealing agent, and the retention of moisture in the hollow structure can be suppressed. In addition, since the spacer and the sealing part are made of the same type of material, even if the humidity or temperature changes, the difference in the amount of dimensional change between the spacer and the sealing agent is small, so cracks and peeling are unlikely to occur at the bonding interface, and the package has excellent reliability. [Brief description of the drawings]
[0015] [Figure 1] 1 is a cross-sectional view showing an example of the configuration of a hollow semiconductor package. [Figure 2A] FIG. 2 is a plan view showing an example of a hollow cell substrate. [Figure 2B]FIG. 2B is a cross-sectional view taken along line II-II in FIG. 2A. [Diagram 3] 4A to 4C are cross-sectional views showing examples of the configurations of chip pieces and semiconductor chips obtained by dicing a hollow cell substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] 1 is a cross-sectional view showing an example of the configuration of a hollow semiconductor package. The hollow semiconductor package 100 includes a frame-shaped spacer 5 between a substrate 1 and a lid 3, and a hollow structure 6 is formed by the substrate 1, the lid 3, and the spacer 5. A semiconductor element 4 is disposed within this hollow structure 6. One end of a bonding wire 45 is connected to the semiconductor element 4. The other end of the bonding wire 45 is connected to an electrode (not shown) on the substrate 1.
[0017] The substrate 1 is a sensor substrate, and may be a semiconductor element substrate, a silicon wafer, a ceramic substrate, etc. The lid 3 may be made of a transparent material such as glass or transparent plastic. The semiconductor element 4 may be, for example, a solid-state imaging element such as a CMOS or CCD, a semiconductor laser element, etc.
[0018] A sealing portion 7 made of a sealant is formed on the outer surface of the spacer 5. The sealing portion 7 is provided so as to cover at least a joint portion 51 between the substrate 1 and the spacer 5 and a joint portion 53 between the lid 3 and the spacer 5. As shown in FIG. 1, the sealing portion 7 may cover the entire outer surface of the spacer 5.
[0019] Fig. 2A is a plan view of a hollow cell substrate used to fabricate a hollow semiconductor package. Fig. 2B is a cross-sectional view taken along line II-II in Fig. 2A. In this hollow cell substrate 300, a plurality of frame-shaped spacers 35 are arranged in a matrix on a transparent substrate 30 made of glass, plastic, or the like. For example, a frame-shaped spacer 5 is formed by applying a photosensitive resin composition onto the substrate 30 and patterning the composition by photolithography.
[0020] 2A and 2B, a chip piece 301 having a frame-shaped spacer 5 provided on a lid 3 is obtained as shown in Fig. 3. The spacer 5 of the chip piece 301 is pressed onto a semiconductor chip 101 having a semiconductor element 4 provided on a substrate 1, and the joint is sealed with a sealant to form the hollow semiconductor structure shown in Fig. 1. The sealant used in the sealing portion 7 is thermosetting, and after a composition is applied to the joint, it is cured by heating.
[0021] As described above, the spacer 5 is formed using a photosensitive resin composition, and the sealing portion 7 is formed using a thermosetting resin composition. In a preferred embodiment of the present invention, both the spacer 5 and the sealing portion 7 contain polysiloxane resin. Since both the spacer 5 and the sealing portion 7 contain polysiloxane resin, the distortion (e.g., coefficient of linear thermal expansion) caused by temperature change and the responsiveness to moisture (e.g., moisture permeability and water absorption rate) of the two are similar. Therefore, the reflow resistance is excellent, and even if the hollow semiconductor package is exposed to a high-humidity environment or a high-temperature environment, peeling or cracking between the spacer 5 and the sealing portion 7 is unlikely to occur. In addition, since polysiloxane resin has higher moisture permeability than general curable resins such as epoxy resin, moisture is unlikely to remain in the hollow structure 6. Therefore, deterioration of the semiconductor element due to moisture and dew condensation on the lid (transparent substrate) tend to be suppressed.
[0022] [Polysiloxane resin] The polysiloxane resin (polymer) contains a polysiloxane structure. The "polysiloxane structure" refers to a structural skeleton having siloxane units Si-O-Si. The polysiloxane structure may be a cyclic polysiloxane structure. The "cyclic polysiloxane structure" refers to a cyclic molecular structural skeleton having siloxane units (Si-O-Si) as ring components.
[0023] The polysiloxane polymer may contain a polysiloxane structure in the main chain or in the side chain. When the polymer contains a polysiloxane structure in the main chain, the heat resistance tends to be improved.
[0024] Typical examples of polysiloxane polymers include (-SiR 1 R 2 Examples of silicones include those having repeating units of R bonded to Si. 1 and R 2 is a monovalent organic group, for example, an alkyl group or a phenyl group. Typical examples of these silicones include methyl silicone having a repeating unit of (-Si(CH3)2-O-), phenyl methyl silicone having a repeating unit of (-Si(CH3)(C6H5)-O-), and phenyl silicone having a repeating unit of (-Si(C5H6)2-O-).
[0025] These silicone resins may be modified silicones having amino groups, epoxy groups, carboxy groups, carbinol groups, methacryl groups, mercapto groups, phenols, hydrogen atoms, etc., introduced at the terminals and / or side chains. The silicone resins may also be hydrogen silicones having hydrogen atoms (SiH groups) bonded to Si at the terminals and / or side chains. For example, a composition containing vinyl modified silicone and hydrogen silicone can be used as a thermosetting silicone resin composition because Si-C bonds are generated by hydrosilylation reaction between SiH groups and vinyl groups in the presence of a catalyst such as a platinum complex.
[0026] In one embodiment, the polysiloxane polymer is obtained by a hydrosilylation reaction between (α) a compound having at least two SiH groups (hydrosilyl groups) in one molecule and (β) a compound having at least two carbon-carbon double bonds (ethylenically unsaturated groups) reactive with SiH groups in one molecule. If either or both of (α) and (β) have a polysiloxane structure, a polymer having a polysiloxane structure is obtained by a hydrosilylation reaction between (α) and (β). By changing the types of (α) and (β), it is possible to prepare polymers having various functional groups.
[0027] (Compound (α): Polysiloxane compound having a SiH group) Compound (α) is a compound having a SiH group, and is preferably a polysiloxane compound having a hydrogen atom bonded to the Si atom of the polysiloxane structure. Specific examples of the polysiloxane compound (α) having at least two SiH groups in one molecule include a hydrosilyl group-containing polysiloxane having a linear structure, a polysiloxane having a hydrosilyl group at the molecular end, and a cyclic polysiloxane containing a hydrosilyl group. A polymer containing a cyclic polysiloxane structure tends to have excellent film-forming properties and heat resistance compared to a polymer containing only a chain polysiloxane structure.
[0028] The cyclic polysiloxane may have a polycyclic structure, and the polycyclic ring may have a polyhedral structure. In order to form a film having high heat resistance and mechanical strength, it is preferable to use a cyclic polysiloxane compound having at least two SiH groups in one molecule as the compound (α). The compound (α) preferably contains three or more SiH groups in one molecule. From the viewpoint of heat resistance and light resistance, it is preferable that the group present on the Si atom is either a hydrogen atom or a methyl group.
[0029] Examples of hydrosilyl group-containing polysiloxanes having a linear structure include copolymers of dimethylsiloxane units, methylhydrogensiloxane units, and terminal trimethylsiloxy units, copolymers of diphenylsiloxane units, methylhydrogensiloxane units, and terminal trimethylsiloxy units, copolymers of methylphenylsiloxane units, methylhydrogensiloxane units, and terminal trimethylsiloxy units, and polysiloxanes whose ends are blocked with dimethylhydrogensilyl groups.
[0030] Polysiloxanes having hydrosilyl groups at the molecular terminals include polysiloxanes whose terminals are blocked with dimethylhydrogensilyl groups, and polysiloxanes having a dimethylhydrogensiloxane unit (H(CH3)2SiO 1 / 2 units), and SiO2 units, SiO 3 / 2units and at least one siloxane unit selected from the group consisting of SiO units.
[0031] Examples of cyclic polysiloxane compounds include 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane, 1-propyl-3,5,7-trihydrogen-1,3,5,7-tetramethylcyclotetrasiloxane, 1,5-dihydrogen-3,7-dihexyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trihydrogen-1,3,5-trimethylcyclosiloxane, 1,3,5,7,9-pentahydrogen-1,3,5,7,9-pentamethylcyclosiloxane, and 1,3,5,7,9,11-hexahydrogen-1,3,5,7,9,11-hexamethylcyclosiloxane.
[0032] The compound (α) may be a cyclic polysiloxane having multiple rings. The multiple rings may have a polyhedral structure. The polysiloxane having a polyhedral skeleton preferably has 6 to 24 Si atoms constituting the polyhedral skeleton, more preferably 6 to 10 Si atoms. A specific example of the polysiloxane having a polyhedral skeleton is silsesquioxane. The cyclic polysiloxane may be a silylated silicic acid having a polyhedral skeleton.
[0033] (Compound (β): Compound containing an ethylenically unsaturated group) Compound (β) contains two or more carbon-carbon double bonds reactive with SiH groups in one molecule. Examples of the group containing a carbon-carbon double bond reactive with SiH groups (hereinafter, sometimes simply referred to as an "ethylenically unsaturated group" or an "alkenyl group") include a vinyl group, an allyl group, a methallyl group, an acryl group, a methacryl group, a 2-hydroxy-3-(allyloxy)propyl group, a 2-allylphenyl group, a 3-allylphenyl group, a 4-allylphenyl group, a 2-(allyloxy)phenyl group, a 3-(allyloxy)phenyl group, a 4-(allyloxy)phenyl group, a 2-(allyloxy)ethyl group, a 2,2-bis(allyloxymethyl)butyl group, a 3-allyloxy-2,2-bis(allyloxymethyl)propyl group, and a vinyl ether group.
[0034] Specific examples of the compound (β) having two or more alkenyl groups in one molecule include diallyl phthalate, triallyl trimellitate, diethylene glycol bisallyl carbonate, trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, pentaerythritol triallyl ether, pentaerythritol tetraallyl ether, 1,1,2,2-tetraallyloxyethane, diarylidene pentaerythritol, triallyl cyanurate, triallyl isocyanurate, diallyl monobenzyl isocyanurate, diallyl monomethyl isocyanurate, 1,2,4-trivinylcyclohexane, 1,4-butanediol divinyl ether, nonanediol divinyl ether, 1,4-cyclohexane dimethanol divinyl ether, triethylene glycol divinyl ether, trimethylolpropane trivinyl ether, pentaerythritol tetravinyl ether, ether, diallyl ether of bisphenol S, divinylbenzene, divinylbiphenyl, 1,3-diisopropenylbenzene, 1,4-diisopropenylbenzene, 1,3-bis(allyloxy)adamantane, 1,3-bis(vinyloxy)adamantane, 1,3,5-tris(allyloxy)adamantane, 1,3,5-tris(vinyloxy)adamantane, dicyclopentadiene, vinylcyclohexene, 1,5-hexadiene, 1,9-decadiene, diallyl ether, bisphenol A diallyl ether, 2,5-diallylphenol allyl ether, and oligomers thereof, 1,2-polybutadiene (1,2 ratio of 10 to 100%, preferably 1,2 ratio of 50 to 100%), allyl ether of novolak phenol, allylated polyphenylene oxide, and other conventionally known epoxy resins in which all of the glycidyl groups have been replaced with allyl groups. Furthermore, compounds in which the allyl group in the above-exemplified compounds is replaced with a (meth)acryloyl group (for example, polyfunctional (meth)acrylates) can also be suitably used as compound (β).
[0035] Compound (β) may be a polysiloxane compound having two or more alkenyl groups. Examples of linear polysiloxanes having two or more alkenyl groups include methyl silicone having dimethylvinylsilyl groups at both ends, phenyl silicone having dimethylvinylsilyl groups at both ends, phenyl methyl silicone having dimethylvinylsilyl groups at both ends, and silicones containing multiple methylvinylsiloxane units in the molecular chain.
[0036] Specific examples of the cyclic polysiloxane compound include 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1-propyl-3,5,7-trivinyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,5-divinyl-3,7-dihexyl-1,3,5,7-tetramethylcyclotetrasiloxane, 1,3,5-trivinyl-1,3,5-trimethylcyclosiloxane, 1,3,5,7,9-pentavinyl-1,3,5,7,9-pentamethylcyclosiloxane, and 1,3,5,7,9,11-hexavinyl-1,3,5,7,9,11-hexamethylcyclosiloxane.
[0037] The compound (β) may be a compound having an alkenyl group at the end and / or side chain of a polymer chain such as polyether, polyester, polyarylate, polycarbonate, polyolefin, polyacrylic acid ester, polyamide, polyimide, or phenol-formaldehyde.
[0038] (Other starting materials) In addition to the above-mentioned compound (α) and compound (β), a compound having only one functional group participating in the hydrosilylation reaction in one molecule may be used as a starting material for the hydrosilylation reaction. The functional group participating in the hydrosilylation reaction is a SiH group or an ethylenically unsaturated group. By using a compound having only one functional group participating in the hydrosilylation reaction, a specific functional group can be introduced at the end of a polymer.
[0039] A compound having a photopolymerizable functional group (photosensitive group) may be used as a starting material for the hydrosilylation reaction. Examples of the photopolymerizable functional group include cationic polymerizable functional groups and radical polymerizable functional groups. The term "cationically polymerizable functional group" refers to a functional group that undergoes polymerization and crosslinking by an acidic active substance generated from a photoacid generator when irradiated with active energy rays. Examples of active energy rays include visible light, ultraviolet light, infrared rays, X-rays, α rays, β rays, and γ rays. Examples of the cationic polymerizable functional group include an epoxy group, a vinyl ether group, an oxetane group, and an alkoxysilyl group. By introducing these photopolymerizable functional groups, a photosensitive polysiloxane polymer can be obtained. From the viewpoint of photosensitivity, an epoxy group is preferred as the cationic polymerizable functional group, and among the epoxy groups, an alicyclic epoxy group or a glycidyl group is preferred from the viewpoint of stability. In particular, an alicyclic epoxy group is preferred because of its excellent photocationic polymerizability.
[0040] By using a compound having an alkenyl group and a cationic polymerizable functional group in one molecule as a starting material, the cationic polymerizable functional group can be introduced into the polymer. Specific examples of the compound having an alkenyl group and an epoxy group as a cationic polymerizable functional group in one molecule include vinylcyclohexene oxide, allyl glycidyl ether, diallyl monoglycidyl isocyanurate, and monoallyl diglycidyl isocyanurate.
[0041] The polysiloxane polymer used in the photosensitive resin composition is preferably alkali-soluble. By introducing an alkali-solubility imparting group into the polymer, alkali-solubility can be imparted. When the polymer has a photopolymerizable functional group and an alkali-soluble group, it is soluble in alkali before photocuring and becomes insoluble in alkali after photocuring, so that it can be used as a negative-type photosensitive resin. Examples of the alkali-solubility imparting group (acidic group) include a phenolic hydroxyl group, a carboxyl group, an N-substituted isocyanuric acid, and an N,N'-disubstituted isocyanuric acid.
[0042] An alkali-soluble polymer can be obtained by using a compound containing an acidic group and an alkenyl group and / or a SiH group as a starting material for the hydrosilylation reaction. For example, a siloxane polymer having an N-substituted isocyanuric acid can be obtained by using monoallyl isocyanurate as a starting material. Also, a siloxane polymer having an N,N'-disubstituted isocyanuric acid can be obtained by using diallyl isocyanurate, monoallyl monoglycidyl isocyanurate, monoallyl monomethyl isocyanurate, or the like as a starting material.
[0043] The polysiloxane polymer may be one that exhibits alkali solubility by eliminating a protecting group in the presence of an acid. A polymer that exhibits alkali solubility by eliminating a protecting group in the presence of an acid can be used as a positive-type photosensitive resin because the protecting group is eliminated (deprotected) by the reaction of an acid generated from a photoacid generator, increasing the alkali solubility.
[0044] Examples of the acidic group include a phenolic hydroxyl group, a carboxyl group, an N-substituted isocyanuric acid, and an N,N'-disubstituted isocyanuric acid. Examples of the protective group for the phenolic hydroxyl group include a tert-butoxycarbonyl group and a trialkylsilyl group. For example, the phenolic hydroxyl group can be protected by a tert-butoxycarbonyl group by a reaction using a Boc reagent. The alkyl group in the trialkylsilyl group as the protective group for the phenolic hydroxyl group is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group, from the viewpoint of ease of deprotection by an acid. The phenolic hydroxyl group can be protected by a trimethylsilyl group by a reaction using a silylating agent such as hexamethyldisilazane or trimethylchlorosilane. The acidic group (NH group) of the N-substituted isocyanuric acid and the N,N'-disubstituted isocyanuric acid can also be protected by the same protective group as the phenolic hydroxyl group. Examples of the protective group for the carboxylic acid include a tertiary alkyl ester and an acetal. Examples of the tertiary alkyl group in the tertiary alkyl ester of a carboxylic acid include a tert-butyl group, an adamantyl group, a tricyclodecyl group, and a norbornyl group.
[0045] By using a compound having a structure with a protecting group that is eliminated in the presence of an acid and containing an alkenyl group and / or a SiH group as a starting material for the hydrosilylation reaction, the protecting group is eliminated in the presence of an acid to give a polysiloxane polymer that exhibits alkali solubility.
[0046] (Hydrosilylation reaction) The order and method of the hydrosilylation reaction are not particularly limited. The hydrosilylation reaction may be carried out by charging all starting materials in one pot and carrying out polymerization, or by charging the raw materials in multiple batches and carrying out the reaction in multiple stages.
[0047] In the hydrosilylation reaction, the ratio B / A of the total amount A of alkenyl groups to the total amount B of SiH groups in the starting materials is preferably greater than 1. In the hydrosilylation reaction, the alkenyl groups and the SiH groups react at a ratio of 1:1. If B / A is greater than 1 and there is an excess of SiH groups relative to the alkenyl groups, a polysiloxane polymer having unreacted SiH groups is obtained. The unreacted SiH groups in the polymer can serve as crosslinking reaction sites in, for example, a thermosetting resin composition.
[0048] For the hydrosilylation reaction, a hydrosilylation catalyst such as chloroplatinic acid, platinum-olefin complex, or platinum-vinylsiloxane complex may be used. The hydrosilylation catalyst may be used in combination with a co-catalyst. The amount of the hydrosilylation catalyst to be added is not particularly limited, but is preferably 10 moles based on the total amount (number of moles) of alkenyl groups contained in the starting material. -8 ~10 -1 times, more preferably 10 -6 ~10 -2 It is double.
[0049] The temperature of the hydrosilylation reaction may be appropriately set, and is preferably 30 to 200° C., more preferably 50 to 150° C. The oxygen volume concentration in the gas phase in the hydrosilylation reaction is preferably 3% or less. From the viewpoint of promoting the hydrosilylation reaction by adding oxygen, the gas phase may contain about 0.1 to 3% by volume of oxygen.
[0050] A solvent may be used in the hydrosilylation reaction. Examples of the solvent include hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone and methyl ethyl ketone; and halogen solvents such as chloroform, methylene chloride, and 1,2-dichloroethane. Toluene, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and chloroform are preferred because they are easy to remove by distillation after the reaction. In the hydrosilylation reaction, a gelation inhibitor may be used as necessary.
[0051] [Resin composition] <Sealant> The sealing agent used to form the sealing portion has thermosetting properties. The thermosetting resin composition containing the polysiloxane resin is preferably one in which the polysiloxane resin is involved in thermosetting. For example, the polysiloxane polymer has thermosetting properties because Si-Si bonds are generated by reacting SiH groups with each other when heated.
[0052] The thermosetting resin composition preferably contains, in addition to the polysiloxane polymer, a compound (crosslinking agent) having a functional group capable of bonding with the polysiloxane polymer to introduce a crosslinked structure. For example, when the polysiloxane polymer contains a SiH group, by containing a compound having multiple ethylenically unsaturated groups as a crosslinking agent, thermosetting (crosslinking) proceeds by hydrosilylation reaction between the SiH group of the polymer and the ethylenically unsaturated group of the crosslinking agent. As a specific example of the compound having two or more ethylenically unsaturated groups in one molecule, the same compound as the compound (β) exemplified above can be used.
[0053] The crosslinking agent may or may not have a polysiloxane structure. As the crosslinking agent, a compound having a polysiloxane structure and a compound not having a polysiloxane structure may be used in combination.
[0054] The polymer obtained after the thermosetting resin composition (sealant) is thermally cured preferably has a cyclic polysiloxane structure. If either or both of the polysiloxane polymer and the crosslinking agent contain a cyclic polysiloxane structure, the polymer obtained after curing contains a cyclic polysiloxane structure. In particular, it is preferable that the polysiloxane polymer contains a cyclic polysiloxane structure. When the polymer contains a cyclic polysiloxane structure, the applicability of the composition is improved, and the outflow of the sealant when forming a sealing portion with the sealant tends to be suppressed.
[0055] The polymer after the thermosetting resin composition (sealant) is thermally cured preferably has a chain polysiloxane structure. By including a chain polysiloxane structure, the moisture permeability of the sealant (sealing portion) is improved, and the retention of moisture in the hollow structure tends to be suppressed. In addition, by including a chain polysiloxane structure, the reflow resistance in a moisture-absorbing state is improved, and the occurrence of peeling and cracks at the bonding interface tends to be suppressed. As a crosslinking agent having a chain polysiloxane structure, for example, a chain polysiloxane in which both ends are vinyl-modified (for example, a silicone oil modified with vinyl at both ends) is used. The silicone oil modified with vinyl at both ends is available from companies such as Shin-Etsu Chemical Co., Ltd., Dow, and Constell Chemical.
[0056] From the viewpoint of achieving both the applicability and durability of the sealant, the polymer after the sealant is thermally cured preferably contains both a cyclic polysiloxane structure and a chain polysiloxane structure. For example, the thermosetting resin composition constituting the sealant contains a polymer containing a cyclic polysiloxane structure and a crosslinking agent containing a chain polysiloxane structure, so that the polymer after the sealant is thermally cured contains both a cyclic polysiloxane structure and a chain polysiloxane structure.
[0057] The resin composition exhibiting thermosetting properties due to a hydrosilylation reaction preferably contains a hydrosilylation catalyst. As the hydrosilylation catalyst, the above-mentioned catalysts are preferable. As the thermosetting resin composition constituting the sealant, a commercially available product may be used.
[0058] <Resin composition for spacers> The resin material used to form the spacer is a photosensitive resin composition containing a polysiloxane resin. The photosensitivity of the photosensitive resin composition may be positive or negative. By using the photosensitive resin composition, a spacer having a frame-shaped pattern as shown in Figures 2A and 2B can be formed by applying the resin composition in a film form on a substrate and then patterning it by photolithography.
[0059] (Negative Photosensitive Resin Composition) The negative photosensitive resin composition contains a polysiloxane polymer exhibiting alkali solubility. As described above, the polymer used in the negative photosensitive resin composition contains an alkali-soluble group and further contains a photopolymerizable functional group.
[0060] The negative photosensitive resin composition may further contain a crosslinking agent. For example, when the polysiloxane polymer has cationic polymerizability, if a compound having two or more alkenyl groups in one molecule is used as a crosslinking agent, the polymer and the crosslinking agent react with each other by exposure to light, and the crosslinking agent hardens, making the composition insoluble in alkali. As a crosslinking agent having photocationic polymerizability, a compound having two or more alicyclic epoxy groups in one molecule is preferable. Specific examples of a compound having two or more alicyclic epoxy groups in one molecule include 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexanecarboxylate (Daicel's "Celloxide 2021P"), ε-caprolactone-modified 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate (Daicel's "Celloxide 2081"), bis(3,4-epoxycyclohexylmethyl)adipate, and the like. A compound having two or more alicyclic epoxy groups in one molecule may contain a chain siloxane structure such as the compound of formula S1 below, or may contain a cyclic siloxane structure such as the compound of formula S2 below.
[0061] [ka]
[0062] (Positive-type photosensitive resin composition) The positive photosensitive resin composition contains a polysiloxane polymer that exhibits alkali solubility by elimination of a protective group in the presence of an acid. The polysiloxane polymer may further have thermosetting properties. The positive photosensitive resin composition may contain a thermosetting crosslinking agent. For example, when the polysiloxane polymer contains a SiH group, if a compound having two or more ethylenically unsaturated groups in one molecule is contained in the photosensitive resin composition as a crosslinking agent, a crosslinked structure is introduced by a hydrosilylation reaction with the polysiloxane polymer. As a specific example of the compound having two or more ethylenically unsaturated groups in one molecule, the same compound as the compound (β) exemplified above can be used.
[0063] (Photoacid generator) The photosensitive resin composition used to form the spacer may contain a photoacid generator. When the photoacid generator is irradiated with active energy rays such as ultraviolet rays, an acid is generated. In a cationic polymerizable composition (e.g., a negative photosensitive resin composition), the photoacid generator acts as a polymerization initiator, and curing by cationic polymerization proceeds. In a positive photosensitive resin composition, the action of the acid generated from the photoacid generator causes the protective group bonded to the alkali-solubility-imparting group (acidic group) to be released, thereby increasing the alkali solubility.
[0064] The photoacid generator contained in the photosensitive resin composition is not particularly limited as long as it generates a Lewis acid upon exposure to light. Specific examples of the photoacid generator include ionic photoacid generators such as sulfonium salts, iodonium salts, ammonium salts, and other onium salts; and nonionic photoacid generators such as imide sulfonates, oxime sulfonates, and sulfonyl diazomethanes.
[0065] The content of the photoacid generator in the photosensitive resin composition is preferably 0.1 to 20 parts by weight, more preferably 0.1 to 15 parts by weight, and further preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the resin content of the composition.
[0066] (sensitizer) The photosensitive resin composition may contain a sensitizer. By using the sensitizer, the exposure sensitivity during patterning is improved. Examples of the sensitizer include naphthalene-based compounds, anthracene-based compounds, and thioxanthone-based compounds, and among them, anthracene-based sensitizers are preferred because of their excellent photosensitizing effect. Specific examples of anthracene-based sensitizers include anthracene, 2-ethyl-9,10-dimethoxyanthracene, 9,10-dimethylanthracene, 9,10-dibutoxyanthracene (DBA), 9,10-dipropoxyanthracene, 9,10-diethoxyanthracene, 9,10-bis(octanoyloxy)anthracene, 1,4-dimethoxyanthracene, 9-methylanthracene, 2-ethylanthracene, 2-tert-butylanthracene, 2,6-di-tert-butylanthracene, and 9,10-diphenyl-2,6-di-tert-butylanthracene.
[0067] The content of the sensitizer in the composition is not particularly limited and may be appropriately adjusted within a range in which the sensitizing effect can be exhibited. From the viewpoint of the balance between curability and physical properties, the content is preferably 0.01 to 20 parts by weight, more preferably 0.1 to 15 parts by weight, and even more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the resin content of the composition.
[0068] <Other components of the resin composition> The thermosetting resin composition constituting the sealant and the photosensitive resin composition used to form the spacer may contain resin components, solvents, additives, etc. other than those described above.
[0069] (thermosetting resin) The resin composition may contain a polymerizable compound (thermosetting resin) that does not show reactivity with the above-mentioned polysiloxane polymer and can be thermoset alone or by reacting with other compounds. Examples of the thermosetting resin include epoxy resin, oxetane resin, isocyanate resin, blocked isocyanate resin, bismaleimide resin, bisallylnadimide resin, acrylic resin, allyl cured resin, unsaturated polyester resin, etc. The thermosetting resin may be a side chain reactive group type thermosetting polymer having a reactive group such as an allyl group, a vinyl group, an alkoxysilyl group, or a hydrosilyl group on the side chain or end of the polymer chain.
[0070] (thermoplastic resin) The resin composition may contain resin components and additives other than those mentioned above. For example, the resin composition may contain various thermoplastic resins for the purpose of property modification, etc. Examples of the thermoplastic resin include acrylic resins, polycarbonate resins, cycloolefin resins, olefin-maleimide resins, polyester resins, polyethersulfone resins, polyarylate resins, polyvinyl acetal resins, polyethylene resins, polypropylene resins, polystyrene resins, polyamide resins, silicone resins, fluororesins, natural rubber, EPDM and other rubber-like resins. The thermoplastic resin may have a crosslinkable group such as an epoxy group, an amino group, a radically polymerizable unsaturated group, a carboxy group, an isocyanate group, a hydroxy group, and an alkoxysilyl group.
[0071] (solvent) The resin composition may contain a solvent. The solvent may be any solvent capable of dissolving the polysiloxane polymer and other components, and specifically includes hydrocarbon solvents such as benzene, toluene, hexane, and heptane; ether solvents such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and diethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol solvents such as propylene glycol-1-monomethyl ether-2-acetate (PGMEA), diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, and ethylene glycol diethyl ether; and halogen-based solvents such as chloroform, methylene chloride, and 1,2-dichloroethane. From the viewpoint of film formation stability, propylene glycol-1-monomethyl ether-2-acetate and diethylene glycol dimethyl ether are preferred. The amount of the solvent used may be appropriately set. When the polymer is in a liquid state, a solvent may not be used.
[0072] (Additives) The photosensitive composition may contain a filler or a colorant. Examples of the filler include silica-based fillers (quartz, fume silica, precipitated silica, silicic anhydride, fused silica, crystalline silica, and ultrafine amorphous silica), silicon nitride, silver powder, alumina, aluminum hydroxide, titanium oxide, glass fiber, carbon fiber, mica, carbon black, graphite, diatomaceous earth, white clay, clay, talc, calcium carbonate, magnesium carbonate, barium sulfate, and inorganic balloons. Examples of the colorant include organic pigments, inorganic pigments, and dyes.
[0073] In addition to the above, the resin composition may contain an adhesion improver, a coupling agent such as a silane coupling agent, a deterioration inhibitor, a hydrosilylation reaction inhibitor, a polymerization inhibitor, a polymerization catalyst (crosslinking accelerator), a release agent, a flame retardant, a flame retardant auxiliary, a surfactant, an antifoaming agent, an emulsifier, a leveling agent, an anti-repellent agent, an ion trapping agent, a thixotropy imparting agent, a tackifier, a storage stability improver, a light stabilizer, a thickener, a plasticizer, a reactive diluent, an antioxidant, a heat stabilizer, an electrical conductivity imparting agent, an antistatic agent, a radiation shielding agent, a nucleating agent, a phosphorus-based peroxide decomposer, a lubricant, a metal deactivator, a thermal conductivity imparting agent, and a physical property adjusting agent.
[0074] <Resin composition set> The sealant (thermosetting resin composition) used to form the sealing portion and the spacer resin composition (photosensitive resin composition) used to form the spacer are both resin compositions containing a polysiloxane polymer. These resin compositions can also be provided as a resin composition set for hollow semiconductor packages.
[0075] [Spacer formation] A photosensitive resin composition for spacers is applied onto the substrate 30 and heated to form a resin film. The method for applying the composition is not particularly limited as long as it allows uniform application, and general coating methods such as spin coating, slit coating, and screen coating can be used. The thickness of the resin film can be adjusted according to the height of the spacers (height of the hollow structure), and is, for example, 1 to 200 μm, and preferably 10 to 150 μm.
[0076] The resin film formed on the substrate is exposed and developed to pattern the resin film, forming a frame-shaped spacer. Before exposure, heating (pre-baking) may be performed to remove the solvent, etc. The heating temperature may be appropriately set, and is preferably 50 to 150°C.
[0077] The light source for exposure may be selected according to the wavelength sensitivity of the photoacid generator and sensitizer contained in the photosensitive resin composition. Usually, a light source having a wavelength in the range of 200 to 450 nm (e.g., a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a high-power metal halide lamp, a xenon lamp, a carbon arc lamp, or a light-emitting diode) is used. The exposure dose is not particularly limited, and is, for example, 1 to 10,000 mJ / cm. 2 About 10 to 4000 mJ / cm 2 For the purpose of accelerating the photoreaction, post-exposure baking by heating may be performed after the photoirradiation and before the development.
[0078] In the pattern exposure, a general photomask can be used. In the case of a negative photosensitive resin composition, a pattern mask having openings formed therein is used so that the portions where the spacers 5 are to be formed are selectively exposed. In the case of a positive photosensitive resin composition, a pattern mask capable of selectively blocking the portions where the spacers 5 are to be formed is used.
[0079] The exposed resin film is contacted with an alkaline developer by immersion or spraying to dissolve and remove the resin film, thereby performing patterning. In a negative photosensitive resin composition, the exposed portion is photocured and no longer shows alkaline solubility, so that the film in the non-exposed portion is selectively removed by alkaline development. In a positive photosensitive resin composition, the action of the acid generated by light irradiation of the photoacid generator increases the alkaline solubility, so that the film in the exposed portion is selectively removed.
[0080] The alkaline developer may be any commonly used one without any particular limitations. Specific examples of the alkaline developer include organic alkaline aqueous solutions such as tetramethylammonium hydroxide (TMAH) aqueous solution and choline aqueous solution, and inorganic alkaline aqueous solutions such as potassium hydroxide aqueous solution, sodium hydroxide aqueous solution, potassium carbonate aqueous solution, sodium carbonate aqueous solution and lithium carbonate aqueous solution. The alkaline concentration of the developer is preferably 0.01 to 25% by weight, more preferably 0.1 to 10% by weight, and even more preferably 0.3 to 5% by weight. The developer may contain a surfactant or the like for the purpose of adjusting the dissolution rate.
[0081] The line width of the spacer 5 is, for example, 1 to 2000 μm. From the viewpoint of achieving both ensuring the strength of the spacer and miniaturization of the semiconductor package, the line width of the spacer 5 is preferably 10 to 1000 μm, more preferably 50 to 700 μm, and may be 70 to 500 μm or 100 to 300 μm. The pattern shape of the mask used during exposure may be adjusted so that the line width of the portion that remains without being dissolved in alkali during development falls within the above range.
[0082] The substrate provided with a plurality of frame-shaped spacers 5 is divided into individual pieces by dicing or the like to obtain chip pieces 301 provided with frame-shaped spacers 5. The substrate may be divided into individual pieces after forming a hollow structure in which a semiconductor element is disposed.
[0083] [Formation of hollow structure] A hollow structure 6 is formed by the substrate 1, the lid 3 and the frame-shaped spacer 5, by pressing the spacer 5 of the chip piece onto a chip 101 having a semiconductor element 4 mounted on a substrate 1 such as a silicon substrate. An adhesive layer may be provided between the spacer 5 and the substrate 1. Since the spacer 5 containing the polysiloxane resin has adhesive properties, the spacer 5 can be fixed onto the substrate 1 by pressing, even without providing a separate adhesive.
[0084] The conditions for compression bonding are not particularly limited, but the temperature is about 30° C. to 300° C., preferably 60° C. to 250° C., and more preferably 80° C. to 250° C. The pressure applied to the bonding surfaces during compression bonding is about 0.1 to 20 MPa, and preferably 0.2 to 10 MPa.
[0085] When the resin composition constituting the spacer 5 has thermosetting properties, it is preferable to thermally cure (post-bake) the resin composition by heating during or after thermocompression bonding. By thermally curing the resin composition, the adhesion between the spacer 5 and the substrate 1, and between the spacer 5 and the lid 3 is further improved. The spacer may be post-baked after or when the sealing portion is formed.
[0086] [Formation of sealing part] A sealant (thermosetting resin composition) is applied so as to cover the joint portion 51 between the substrate 1 and the spacer 5 and the joint portion 53 between the lid 3 and the spacer 5, and then thermally cured to form the sealing portion 7. The heating temperature during thermal curing may be set according to the composition of the sealant and is, for example, 50 to 300°C, preferably 100 to 250°C, and more preferably 120 to 200°C.
[0087] The glass transition temperature of the sealing portion 7 (sealant after thermal curing) is preferably 30 to 150°C, more preferably 35 to 100°C. If the glass transition temperature of the sealing portion is excessively high, the stress relaxation effect of the sealant is low due to the high elastic modulus at high temperatures, and peeling or cracks may occur at the interface when a heating test or a thermal cycle test is performed. On the other hand, if the glass transition temperature of the sealing portion is excessively low, the sealant is likely to flow when heated, resulting in a decrease in adhesion and causing contamination due to the sealant protruding from the application area.
[0088] The product WD of the moisture permeability W and the thickness D of the sealing part 7 is preferably 0.05 to 0.6 g / m 24h. The moisture permeability W and the thickness D are inversely proportional to each other, and the product WD of the moisture permeability and the thickness is almost constant for sheet-like objects made of the same material. WD is an index that indicates the ease (movement speed) of moisture movement in a material, and the larger the WD, the faster the moisture movement speed in the sealing part 7 and the easier it is to permeate moisture. If the WD is within the above range, the sealing part 7 has appropriate moisture permeability, so that the retention of moisture in the hollow structure 6 can be suppressed. If the WD is excessively large, the amount of moisture that penetrates into the hollow structure 6 in a high humidity environment increases, which may cause deterioration of the semiconductor element or peeling at the bonding interface.
[0089] The moisture permeability of the sealing portion 7 is measured using a measurement sample in which the sealant (thermosetting resin composition) constituting the sealing portion 7 is molded into a sheet having a thickness of 0.5 mm. A moisture permeability test is carried out for 5 hours in an environment of a temperature of 80°C and a relative humidity of 85%, and the moisture permeability (g / m) is calculated from the amount of moisture that permeates the measurement sample. 2 5h) and multiplying this value by 24 / 5 gives the 24-hour moisture permeability W (g / m 2 24h) is calculated. The moisture permeability W and the thickness D of the sample are calculated as 5×10 -4 The WD is calculated from the product of this and m. The WD value of the sealing portion is more preferably 0.07 to 0.5 g / m·24h, further preferably 0.1 to 0.4 g / m·24h, and may be 0.12 to 0.35 g / m·24h.
[0090] In a resin composition containing a polysiloxane polymer, when the polymer contains a cyclic siloxane structure, the glass transition temperature tends to be high and the moisture permeability tends to be low. When the polymer contains both a cyclic polysiloxane structure and a chain polysiloxane structure, the glass transition temperature tends to be high and the moisture permeability tends to be low as the ratio of the cyclic polysiloxane structure increases.
[0091] [Fabrication of hollow semiconductor packages] As described above, a frame-shaped spacer 7 is placed between a semiconductor chip having a semiconductor element 4 provided on a substrate 1 and a lid 3, and the sides of the spacer 7 are sealed to form a hollow semiconductor package 100 having a semiconductor element within a hollow structure 6.
[0092] In the above embodiment, the spacer 5 is formed using a photosensitive resin composition containing a polysiloxane resin, but the spacer 5 may be formed by screen printing or the like of a resin composition containing a polysiloxane resin. In the above embodiment, the cell substrate 300 having a plurality of frame-shaped spacers 5 formed on one glass substrate 30 is diced to form a chip piece having one spacer 5 provided on the lid 3 made of glass, but one spacer 5 may be formed on the lid 3. Also, instead of forming a spacer on the lid 3 (transparent substrate), a frame-shaped spacer may be formed on the sensor substrate 1 (e.g., a silicon substrate). When forming a spacer on a sensor substrate, a plurality of frame-shaped spacers may be formed on one substrate and then diced to form a semiconductor chip, or a spacer may be formed on the substrate after dicing.
[0093] 2A illustrates the spacer 5 having a square shape in plan view, the shape of the frame-shaped spacer is not particularly limited, and may be a quadrangle such as a rectangle, a rhombus, or a parallelogram, a polygon such as a triangle, a pentagon, or a hexagon, or may be a circle or an ellipse. The spacer may have a polygonal shape with rounded corners, for example, a square with rounded corners or a rectangle with rounded corners. By having rounded corners of the polygon, even if a dimensional change occurs due to humidity or temperature change, the concentration of stress at the corners is mitigated, and cracks and peeling at the sealing portion and the bonding interface tend to be suppressed. EXAMPLES
[0094] The present invention will be described in more detail below based on examples, but the present invention is not limited to the following examples.
[0095] [Synthesis of polyorganosiloxane compounds] <Synthesis Example 1> 1459g of tetraethoxysilane was added to 1803g of 48% choline aqueous solution (aqueous solution of trimethyl-2-hydroxyethylammonium hydroxide) and stirred vigorously at room temperature for 2 hours. When the reaction system became heated and a homogeneous solution was formed, the stirring was slowed down and the reaction was continued for another 12 hours. Next, 1400mL of methanol was added to the solid matter formed in the reaction system to make a homogeneous solution.
[0096] 1149g of dimethylvinylchlorosilane and 830g of trimethylsilyl chloride were dissolved in 1400mL of hexane, and the above solution was slowly added dropwise while vigorously stirring. After completion of the addition, the mixture was reacted for 1 hour, and then the organic layer was extracted and concentrated to obtain a solid. The resulting solid was washed by vigorously stirring in methanol, and then filtered to obtain 760g of a cage polysiloxane compound, tetrakis(vinyldimethylsiloxy)tetrakis(trimethylsiloxy)octasilsesquioxane (Fw=1175.8), as a white solid.
[0097] 30.0 g of the above-mentioned cage polysiloxane compound was dissolved in 123.0 g of toluene, and 31.5 g of methyldiphenylvinylsilane and 1.46 μL of a xylene solution of platinum vinylsiloxane complex (Pt-VTSC-3X manufactured by Umicore Precious Metals Japan, platinum content 3 wt%) were added. This solution was slowly dropped into a solution of 224.6 g of 1,3,5,7-tetrahydrogen-1,3,5,7-tetramethylcyclotetrasiloxane (hereinafter referred to as "TMCTS") and 24.6 g of toluene, and reacted at 105 ° C. for 2 hours. After the reaction was completed, 2.8 μL of ethynylcyclohexanol and 0.65 μL of dimethyl maleate were added, and the toluene and unreacted components were distilled off to obtain 80.8 g of liquid polyorganosiloxane compound 1 (hydrosilyl valence 1.8 mol / kg).
[0098] <Synthesis Example 2> 626 g of TMCTS and 602 g of toluene were mixed uniformly and stirred under a nitrogen atmosphere at 105° C. A mixture of 90 g of triallyl isocyanurate, 90 g of toluene, and 0.1 g of a xylene solution of platinum vinylsiloxane complex was added dropwise to this solution over 40 minutes, and the mixture was allowed to react at 105° C. for 4 hours. Unreacted components and toluene were distilled off under reduced pressure to obtain 310 g of liquid polyorganosiloxane compound 2 (hydrosilyl valence 8.60 mol / kg).
[0099] <Synthesis Example 3> 500g of TMCTS and 1800g of toluene were mixed uniformly and stirred under a nitrogen atmosphere at 105°C. A mixture of 180g of triallyl isocyanurate, 300g of allyl glycidyl ether, 350g of toluene, and 0.1g of a xylene solution of platinum vinyl siloxane complex was added dropwise to this solution over 40 minutes, and the mixture was reacted at 105°C for 4 hours. Unreacted components and toluene were distilled off under reduced pressure to obtain 700g of liquid polyorganosiloxane compound 3 (hydrosilyl valence 3.5mol / kg).
[0100] <Synthesis Example 4> 44 g of TMCTS and 88 g of toluene were mixed uniformly and stirred under a nitrogen atmosphere at 105° C. To this solution, a mixture of 14.5 g of diallyl monomethyl isocyanurate, 20 g of diallyl isocyanurate, 132 g of dioxane, and 0.03 g of a xylene solution of platinum vinyl siloxane complex was added dropwise over 40 minutes. 1 After confirming the disappearance of the allyl group by H-NMR, a mixed liquid of 31 g of toluene and 31 g of vinylcyclohexene oxide was added dropwise. 1 The disappearance of the vinyl group was confirmed by H-NMR, and the reaction was terminated by cooling. Toluene and dioxane were distilled off under reduced pressure, and then propylene glycol-1-monomethyl ether-2-acetate was added to obtain a solution of polyorganosiloxane compound 4 (concentration 75% by weight).
[0101] <Synthesis Example 5> 20 g of TMCTS and 40 g of toluene were mixed uniformly and stirred under a nitrogen atmosphere at 105° C. To this solution, a mixture of 12.2 g of diallyl monoglycidyl isocyanurate, 15.6 g of monoallyl isocyanurate, 100 g of dioxane, and 0.03 g of a xylene solution of platinum vinylsiloxane complex was added dropwise over 40 minutes. 1 After confirming the disappearance of the allyl group by H-NMR, a mixed liquid of 15 g of toluene and 12 g of vinylcyclohexene oxide was added dropwise. 1 The disappearance of the vinyl group was confirmed by H-NMR, and the reaction was terminated by cooling. Toluene and dioxane were distilled off under reduced pressure, and then propylene glycol-1-monomethyl ether-2-acetate was added to obtain a solution of polyorganosiloxane compound 5 (concentration 75% by weight).
[0102] [Preparation of sealant] The components were blended in the weight ratios shown in Table 1 and mixed with stirring to prepare sealant compositions (thermosetting resin compositions) 1 to 12. The both-terminally vinyl-modified siloxane A used in compositions 1 to 3 was a both-terminally vinyl-modified polymethylphenylsiloxane (manufactured by Constur Chemical). The both-end vinyl-modified siloxane B used in composition 4 was 1,5-divinyl-1,1,5,5-tetramethyl-3,3-diphenyltrisiloxane. The Pt catalyst solution used in compositions 1 to 8 was a xylene solution of platinum vinylsiloxane complex ("Pt-VTSC-3X" manufactured by Umicore Precious Metals Japan, platinum content 3% by weight). The silicone composition of Compositions 9 and 10 was a two-liquid type methylsilicone elastomer (Dow's "DOWSIL JCR6140"), and 50 parts by weight each of Agent A and Agent B were used. The epoxy composition of the sealant compositions 11 and 12 is a one-liquid type epoxy resin composition containing an alicyclic epoxy resin and an acid anhydride as main components ("EH1600G2" manufactured by Inabata & Co., Ltd.). The silica particles used in Compositions 7, 10, and 12 were fused spherical silica ("SF650" manufactured by Tatsumori).
[0103] [Evaluation of the physical properties of sealants] <Moisture permeability> The sealant composition was poured into a mold prepared by sandwiching a 0.5 mm thick silicone rubber spacer between two glass substrates, and the sealant was cured by heating at 150°C for 3 hours to prepare a 0.5 mm thick evaluation sample.
[0104] A jig was made by fixing a 5 cm square frame-shaped polyisobutylene rubber sheet (3 mm thick, with a 3 cm square cut out in the center) to the surface of a 5 cm square glass plate, and 1 g of calcium chloride (for moisture measurement) was filled into the frame. The above-mentioned evaluation sample was fixed on top of the jig to obtain a test specimen.
[0105] The test specimen was left to stand in a thermohygrostat at a temperature of 80°C and a relative humidity of 85% for 5 hours, and the total weight of the test specimen was measured before and after the test. The moisture permeability after 5 hours was calculated according to the following formula. Moisture permeability (g / m 2 ·5h) = {(total weight of specimen after test (g)) - (total weight of specimen before moisture permeability test (g))} / 9 × 10 -4 (m 2 ) In addition, the polyisobutylene rubber used in the test specimen was found to have a moisture permeability of 0 g / m 2 -Confirmed to be 5h.
[0106] The moisture permeability (g / m2) of the 0.5 mm thick sample measured above for 5 hours 2 The product of the 24-hour moisture permeability W and thickness D, WD (g / m 24h), was calculated from the measured moisture permeability W and thickness D.
[0107] <Glass transition temperature> A 2 mm thick evaluation sample was prepared by pouring the sealant composition into a mold prepared by sandwiching a 2 mm thick silicone rubber spacer between two glass substrates and curing the sealant by heating at 150°C for 3 hours. The dynamic viscoelasticity of this sample was measured under the following conditions using a dynamic viscoelasticity measuring device (UBM "Reogel E4000"), and the temperature at which the loss tangent was maximized was determined as the glass transition temperature (Tg). Test mode: Tensile Measurement temperature: room temperature ~ 200℃ Heating rate: 4℃ / min Distortion: 4μm Frequency: 10Hz Chuck distance: 25mm
[0108] The formulations and evaluation results of sealant compositions 1 to 12 are shown in Table 1. Note that sealant compositions 9 and 10 did not show a maximum in loss tangent at temperatures above room temperature, and therefore the glass transition temperatures were determined to be below room temperature (RT).
[0109] [Table 1]
[0110] [Preparation of Photosensitive Resin Composition for Spacers] Photosensitive resin compositions for spacers 21 to 25 were prepared by mixing and stirring the components in the weight ratios shown in Table 2. The values shown in Table 2 are the weight ratios of solids (non-volatile contents) other than the organic solvent.
[0111] Epoxy compound 1 in Table 2 is ε-caprolactone-modified 3′,4′-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (manufactured by Daicel under the name “Celloxide 2081”), and epoxy compound 2 is 3,4-epoxycyclohexylmethyl-3′,4′-epoxycyclohexanecarboxylate (manufactured by Daicel under the name “Celloxide 2021P”).
[0112] The photoacid generator in Table 2 is a sulfonium salt-based photoacid generator "CPI-310FG" manufactured by San-Apro. The phenolic resin used in Composition 25 was polyparavinylphenol (Marukalinker M manufactured by Maruzen Petrochemicals), the photoradical polymerization initiator was Omnirad 184 manufactured by IGM Resins, the sensitizer was 9,10-dibutoxyanthracene, and the solvent was propylene glycol monomethyl ether acetate.
[0113] [Table 2]
[0114] [Example 1] The photosensitive resin composition 21 prepared above was spin-coated onto a 0.4 mm thick glass substrate to a film thickness of 80 μm, and heated on a hot plate at 120° C. for 10 minutes. Further, using a high-pressure mercury lamp, the composition was irradiated with an integrated light dose of 1500 mJ / cm through a negative photomask having rectangular frame-shaped openings measuring 6.23 mm in the horizontal direction, 5.18 mm in the vertical direction, and 0.39 mm in line width arranged in a matrix pattern. 2 Thereafter, the substrate was immersed in an alkaline developer (a 2.38% aqueous solution of tetramethylammonium hydroxide) for 300 seconds, rinsed with water for 30 seconds, and the moisture on the surface was removed with compressed air to obtain a cell pattern substrate in which frame-shaped spacers were arranged in a matrix on the glass substrate.
[0115] The cell pattern substrate obtained above was cut into individual pieces using a dicing device. The individualized cell spacers were placed on a silicon wafer cut into 1 cm squares so that they were in contact with each other, and the pieces were pressed against each other on a hot plate at 120°C with a load of 800 g. The sample after pressing was heated in an oven at 200°C for 2 hours to post-bake (thermally cure) the photosensitive resin composition.
[0116] Thereafter, the sample was placed on a hot plate at 60° C., and the sealant composition 1 was applied so as to fill the gap between the glass substrate and the silicon wafer, and the sample was heated in an oven at 150° C. for 3 hours to cure the sealant.
[0117] [Examples 2 to 13, Comparative Examples 1 to 3] Samples having a hollow structure were produced in the same manner as in Example 1, except that the types of photosensitive resin compositions used to form the sealant and spacers were changed as shown in Table 3.
[0118] [evaluation] <Sealant application> The sealed portions of the samples prepared in the examples and comparative examples were visually inspected, and a rating of B was given if the sealant had flowed out onto the glass surface or outside the silicon chip, and a rating of A was given if the sealant had not flowed out.
[0119] <Moisture absorption reflow test> The samples prepared in the examples and comparative examples were left to stand in a thermo-hygrostat at 85°C and 85% relative humidity for 7 hours to absorb moisture, and then heated in a reflow furnace at 260°C for 1 minute three times. The samples after reflow were observed under a microscope to evaluate the presence or absence of peeling or cracks in the sealant. For each example and comparative example, evaluation was performed on 10 samples, and samples with 2 or less peeling or cracks were rated as "A", samples with 3 to 7 peeling or cracks were rated as "B", and samples with 8 or more peeling or cracks were rated as "C".
[0120] Table 3 shows the combinations of compositions used in the examples and comparative examples, as well as the evaluation results of the application properties of the sealant and the moisture absorption reflow test.
[0121] [Table 3]
[0122] In both Comparative Example 1 and Comparative Example 2, in which a sealant made of an epoxy resin composition was used, cracks or peeling occurred in the sealing portion in many samples after the moisture absorption reflow test. In Comparative Example 3, in which a polysiloxane-based sealant composition 1 was used and a phenolic resin-based photosensitive resin composition 25 was used as the spacer, cracks or peeling occurred in the sealing portion in many samples after the moisture absorption reflow test.
[0123] In all of Examples 1 to 13, in which a composition containing a polysiloxane polymer was used as both the sealant and the spacer material, the occurrence of peeling and cracks after the moisture absorption reflow test was suppressed compared to the comparative example.
[0124] In Examples 1 to 8 and 11 to 13, which used sealant compositions 1 to 8 containing cyclic polysiloxanes (compounds 1 to 3), there was no overflow of the sealant, and the coatability of the sealant was better than in Examples 9 and 10, which used compositions 9 and 10.
[0125] In Examples 1 to 4, 8 to 13, which used sealants 1 to 4, 8 to 10 containing a chain polysiloxane structure, the moisture absorption reflow resistance was further improved compared to Examples 5 and 6, which used sealants 5 and 6 containing only a cyclic polysiloxane structure and not a chain polysiloxane structure. Since sealants 1 to 4, 8 to 10 contain a chain siloxane structure, they have higher moisture permeability than sealants 5 and 6, and moisture in the hollow structure is easily released to the outside of the hollow structure during reflow, which is thought to have suppressed cracks and peeling in the sealing portion.
[0126] Sealant 7, in which 150 parts by weight of filler (silica particles) was added to 100 parts by weight of resin, had the same resin composition as sealant 4, but the inclusion of the filler reduced the moisture permeability of the sealant (see Table 1). In Example 7, which used sealant 7, the moisture absorption reflow resistance was reduced compared to Example 4, and it is believed that the moisture permeability of the sealant is involved in the reliability of the sealing part. [Explanation of symbols]
[0127] 100 Hollow Semiconductor Package 1 Board 3 Lid 4. Semiconductor elements 45 Bonding Wire 5 Spacer 6 Hollow structure 7 Sealing part 30 Substrate 300 Hollow cell substrate 101 Semiconductor Chip 301 Chip Piece
Claims
1. substrate; Lid; a frame-shaped spacer disposed between the substrate and the lid; a semiconductor element disposed within a hollow structure formed by the substrate, the lid, and the spacer; and a sealing portion that seals a joint portion between the substrate and the spacer and a joint portion between the lid and the spacer; A hollow semiconductor package comprising: the spacer comprises a polysiloxane resin; the sealing portion includes a polysiloxane resin, The lid and the spacer are in direct contact with each other. Hollow semiconductor package.
2. 2. The hollow semiconductor package according to claim 1, wherein the sealing portion is made of a cured product of a thermosetting resin composition containing a polysiloxane resin.
3. 3. The hollow semiconductor package according to claim 1, wherein the polysiloxane resin of the sealing portion includes a cyclic polysiloxane structure.
4. 3. The hollow semiconductor package according to claim 1, wherein the polysiloxane resin of the sealing portion contains a cyclic polysiloxane structure and a chain polysiloxane structure.
5. 5. The hollow semiconductor package according to claim 1, wherein the sealing portion has a product of moisture permeability and thickness of 0.05 to 0.6 g / m·24 h.
6. 6. The hollow semiconductor package according to claim 1, wherein the sealing portion has a glass transition temperature of 30 to 150°C.
7. A method for producing a hollow semiconductor package according to any one of claims 1 to 6, comprising the steps of: The sealing portion is formed by thermally curing a thermosetting resin composition containing a polysiloxane resin. A method for manufacturing a hollow semiconductor package.
8. 8. The method for producing a hollow semiconductor package according to claim 7, wherein the thermosetting resin composition comprises a polysiloxane polymer having two or more SiH groups in one molecule and a crosslinking agent having two or more alkenyl groups in one molecule.
9. The method for manufacturing a hollow semiconductor package according to claim 8 , wherein the polysiloxane polymer comprises a cyclic polysiloxane structure.
10. The method for producing a hollow semiconductor package according to claim 8 or 9, wherein the crosslinking agent contains a chain polysiloxane structure.
11. The method for producing a hollow semiconductor package according to any one of claims 7 to 10, wherein the spacer is formed by applying a photosensitive resin composition containing a polysiloxane resin and patterning the composition by photolithography.
12. A resin composition set for forming a hollow semiconductor package according to any one of claims 1 to 6, comprising: the resin composition set includes a spacer resin composition used for producing the spacer and a sealant used for producing the sealing portion, the spacer resin composition is a photosensitive resin composition containing a polysiloxane polymer, The sealant is a thermosetting resin composition containing a polysiloxane polymer. A resin composition set for hollow semiconductor packages.
Citation Information
Patent Citations
Semiconductor device
JP2002124589A
METHOD FOR PRODUCING CYCLIC SILOXANE SKELETON-CONTAINING COMPOUND HAVING SiH GROUP
JP2005139123A
Device apparatus
JP2005285864A
Leadless hollow package and its manufacturing method
JP2007035779A
Shape-retainable curable composition
JP2007138098A