The insert's design with a controlled surface roughness and coating layer composition addresses the challenge of improving surface quality without compromising durability in cutting tools, achieving enhanced wear resistance and finish.
Patent Information
- Application Number
- JP2021058879
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Conventional cutting tools and inserts made of cemented carbide, cermet, or ceramics fail to improve finished surface quality without compromising durability.
The insert design features a rake surface, flank surface, and ridgeline portion with a cutting edge, where the third surface has an average arithmetic surface roughness of 0.20 μm or less, and a coating layer with specific residual stress and composition to enhance wear resistance and durability.
The insert improves finished surface quality of the workpiece while maintaining durability by reducing surface roughness and enhancing wear resistance through a specialized coating layer configuration.
Smart Images

Figure 0007568566000001 
Figure 0007568566000002 
Figure 0007568566000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an insert and a cutting tool. [Background technology]
[0002] 2. Description of the Related Art Inserts having a substrate made of, for example, cemented carbide, cermet, ceramics, or the like are known as tools used in cutting processes such as turning and milling (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-3284 A Summary of the Invention [Problem to be solved by the invention]
[0004] The above-mentioned conventional techniques have room for further improvement in terms of improving the quality of the finished surface of the workpiece without impairing durability.
[0005] The present disclosure has been made in consideration of the above, and aims to provide an insert and a cutting tool that can improve the finished surface quality of a workpiece without compromising durability. [Means for solving the problem]
[0006] According to one embodiment of the present disclosure, an insert has a first surface having a rake face, a second surface having a flank face, and a ridge portion located between the first surface and the second surface, and a cutting edge is located on at least a part of the ridge portion. The cutting edge has at least a part of a third surface, and when the average arithmetic surface roughness Ra of the third surface in a direction parallel to the ridge portion is Ra1, Ra1 is 0.20 μm or less.
[0007] A cutting tool according to one aspect of the present disclosure includes a rod-shaped holder having a pocket at an end thereof and an insert as described above positioned within the pocket. Effect of the Invention
[0008] According to the present disclosure, it is possible to improve the quality of the finished surface of a workpiece without compromising durability. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing an example of an insert according to an embodiment. [Diagram 2] FIG. 2 is a side cross-sectional view showing an example of an insert according to an embodiment. [Diagram 3] FIG. 3 is a schematic side view showing the configuration of a coating layer according to the embodiment. [Figure 4] FIG. 4 is a schematic plan view of the third coating layer as viewed in a direction perpendicular to the third surface. [Diagram 5] FIG. 5 is a schematic enlarged view of the V portion shown in FIG. [Figure 6] FIG. 6 is a schematic enlarged view of portion VI shown in FIG. [Figure 7] FIG. 7 is a front view showing an example of a cutting tool according to an embodiment. [Figure 8] FIG. 8 is a diagram showing the measurement results of the average arithmetic surface roughness Ra of the third surface. [Figure 9] FIG. 9 is a diagram showing the measurement results of the ten-point average surface roughness Rz of the third surface. [Figure 10] FIG. 10 is a graph showing the results of a wear resistance test on the inserts according to Example 1 and Comparative Examples 1, 3, and 4. [Figure 11] FIG. 11 is a graph showing the results of a fracture resistance test for the inserts according to Example 1 and Comparative Examples 1, 3, and 4. [Figure 12] FIG. 12 is a table showing the results of measuring the residual stress on the second coating layer of the inserts according to Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, a detailed description will be given of an embodiment (hereinafter, referred to as an "embodiment") for carrying out the insert and cutting tool according to the present disclosure with reference to the drawings. Note that the insert and cutting tool according to the present disclosure are not limited to this embodiment. In addition, each embodiment can be appropriately combined as long as the processing contents are not contradictory. In addition, the same parts in each of the following embodiments are given the same reference numerals, and duplicated explanations will be omitted.
[0011] In addition, in the embodiments described below, expressions such as "constant", "orthogonal", "vertical" and "parallel" may be used, but these expressions do not necessarily mean "constant", "orthogonal", "vertical" and "parallel" strictly. In other words, each of the above expressions allows for deviations due to, for example, manufacturing accuracy and installation accuracy.
[0012] <insert> Fig. 1 is a perspective view showing an example of an insert according to an embodiment. As shown in Fig. 1, the insert 1 according to the embodiment may have a tip body 2 and a cutting edge portion 3. The insert 1 according to the embodiment has, for example, a hexahedral shape in which the upper and lower surfaces (surfaces intersecting with the Z-axis shown in Fig. 1) are parallelogram shapes.
[0013] The insert 1 has a first surface 6 (here, an upper surface), a second surface 7 (here, a side surface) connected to the first surface 6, and a ridge portion 8 located between the first surface 6 and the second surface 7. The first surface 6 has a scooping surface that scoops up chips generated by cutting. In addition, the second surface 7 has a flank surface.
[0014] The first surface 6 has a plurality of (four here) corners 61 when viewed in a plan view. The corners 61 are regions including the corners of the first surface 6. A cutting edge 11 is located on a ridge portion 8 of at least one of the plurality of corners 61. The insert 1 cuts the workpiece by bringing the cutting edge 11 into contact with the workpiece.
[0015] (Chip body 2) The tip body 2 is formed of, for example, a cemented carbide. The cemented carbide contains W (tungsten), specifically WC (tungsten carbide). The cemented carbide may also contain at least one of Ni (nickel) and Co (cobalt). The tip body 2 may also be formed of a cermet. The cermet contains, for example, Ti (titanium), specifically TiC (titanium carbide) or TiN (titanium nitride). The cermet may also contain Ni or Co.
[0016] A seat 4 for attaching a cutting edge portion 3 may be located in one of the locations of the tip body 2 that corresponds to a corner 61 of the insert 1. A through hole 5 that passes through the tip body 2 from top to bottom may be located in the center of the tip body 2. A screw 75 for attaching the insert 1 to a holder 70 described below is inserted into the through hole 5 (see FIG. 7).
[0017] (Cutting edge 3) The cutting edge portion 3 is attached to the seat surface 4 of the tip body 2, thereby being integrated with the tip body 2. The cutting edge portion 3 constitutes one of the multiple corner portions 61 of the insert 1. The cutting edge portion 3 also constitutes the first surface 6, the second surface 7, and a part of the ridge portion 8 described above. The cutting edge 11 is located on at least a part of the ridge portion 8 of the cutting edge portion 3.
[0018] The configuration of the cutting edge portion 3 will be described with reference to Fig. 2. Fig. 2 is a side cross-sectional view showing an example of the insert 1 according to the embodiment. As shown in Fig. 2, the cutting edge portion 3 has a base body 10. In addition, the cutting edge portion 3 may have a coating layer 20.
[0019] (Base 10) The substrate 10 may be a cemented carbide, a cermet, or a ceramic. It may also be a boron nitride sintered body containing a plurality of boron nitride particles. In the embodiment, the substrate 10 is a cubic boron nitride (cBN) sintered body and may contain a plurality of cubic boron nitride particles. The substrate 10 may have a bonding phase containing TiN, Al, Al2O3, or the like between the plurality of boron nitride particles. The plurality of boron nitride particles are firmly bonded by such a bonding phase. The substrate 10 does not necessarily have to have a bonding phase. In addition, although the substrate 10 is located at the cutting edge portion 3 in FIG. 1 and FIG. 2, the substrate 10 may be the tip body 2 and the cutting edge portion 3. In other words, for example, a rectangular substrate 10 may be used.
[0020] A third surface 9 continuous with the first surface 6 and the second surface 7 is located on at least a portion of the cutting edge 11. The third surface 9 is, for example, a C-surface (chamfered surface) obtained by cutting the corner between the first surface 6 and the second surface 7 obliquely and linearly. The third surface 9 may also be an R-surface (rounded surface) obtained by rounding the corner between the first surface 6 and the second surface 7.
[0021] A substrate 30 made of, for example, cemented carbide or cermet may be located on the lower surface of base 10. In this case, base 10 is joined to seating surface 4 of chip body 2 via substrate 30 and bonding material 40. Bonding material 40 is, for example, brazing material. In the portion of chip body 2 other than seating surface 4, base 10 may be joined to chip body 2 via bonding material 40.
[0022] (Coating layer 20) The coating layer 20 is applied to the base 10 for the purpose of improving the wear resistance, heat resistance, etc. of the cutting edge portion 3. In the example of Fig. 2, the coating layer 20 is located on both the tip body 2 and the base 10, but it is sufficient that the coating layer 20 is located at least on the base 10. When the coating layer 20 is located on the side surface of the base 10 corresponding to the second surface 7 of the cutting edge portion 3, the second surface 7 has high wear resistance and heat resistance.
[0023] Fig. 3 is a schematic side view showing the configuration of the coating layer according to the embodiment, and Fig. 4 is a schematic plan view showing the third coating layer 203 as viewed from a direction perpendicular to the third surface 9.
[0024] As shown in FIG. 3, the coating layer 20 has a first coating layer 201 located on the first surface 6, a second coating layer 202 located on the second surface 7, and a third coating layer 203 located on the third surface 9.
[0025] Here, when the average arithmetic surface roughness Ra in a direction D1 (see FIG. 4) parallel to the ridge line 8 on the third surface 9 is taken as Ra1, Ra1 may be 0.20 μm or less. The insert 1 having such a configuration can improve the finished surface quality of the workpiece without impairing durability.
[0026] Furthermore, when the average arithmetic surface roughness Ra in a direction D2 (see FIG. 4) perpendicular to the ridge line 8 on the third surface 9 is taken as Ra2, the difference between Ra1 and Ra2 may be 0.1 μm or less. With the insert 1 having such a configuration, the finished surface roughness of the workpiece can be reduced.
[0027] Furthermore, when the ten-point average surface roughness Rz of the third surface 9 in a direction D1 parallel to the ridge line portion 8 is defined as Rz1, Rz1 may be 1.5 μm or less. According to the insert 1 having such a configuration, it is possible to reduce the roughness of the finished surface of the workpiece.
[0028] In addition, when the ten-point average surface roughness Rz of the third surface 9 in a direction D2 perpendicular to the ridge line 8 is defined as Rz2, the difference between Rz1 and Rz2 may be 0.2 μm or less. With the insert 1 having such a configuration, the finished surface roughness of the workpiece can be reduced.
[0029] Furthermore, the second coating layer 202 located on the second surface 7 of the coating layer 20 may contain cubic crystal grains. For example, the cubic crystal grains contained in the second coating layer 202 may be AlTiN.
[0030] Of the residual stresses measured in the first coating layer 201 and the second coating layer 202 by a 2D method (a stress measurement method using an X-ray two-dimensional detector), the residual stress in the first coating layer 201 near the cutting edge 11 is designated as σ1, and the residual stress in the second coating layer 202 near the cutting edge 11 is designated as σ2.
[0031] For example, as shown in FIG. 3, the residual stress σ2 in the second coating layer 202 in the direction perpendicular to the first surface 6 11 and the residual stress σ2 in a direction parallel to the first surface 6 22 and are measured using the 2D method. 11 and σ 22 Similarly, for the first coating layer 201, the residual stress in the direction parallel to the first surface 6 and perpendicular to the ridge between the first surface 6 and the second surface 7 may be calculated as σ1. 22 Let σ1 22 The residual stress in the direction perpendicular to the 11 may be measured using a 2D method, and the average value of these may be calculated as σ1.
[0032] Both σ1 and σ2 may be compressive stresses. In general, a coated tool having a tensile stress as a residual stress in the coating layer is prone to cracking. In contrast, an insert 1 having both σ1 and σ2 as compressive stresses is less likely to crack. Therefore, the insert 1 having such a configuration has high durability.
[0033] The residual stress value of σ1 may be −1050 MPa or more and −750 MPa or less. The residual stress value of σ2 may be −1400 MPa or more and −1100 MPa or less. The insert 1 having such a configuration has even higher durability.
[0034] The thickness of the second coating layer 202 may be 0.5 μm or more and 5.0 μm or less. In the insert 1 having the above configuration, the coating layer 20 has high peel resistance and high impact resistance, so that the durability of the coating layer 20 is further increased.
[0035] (Specific configuration of covering layer 20) Next, a specific configuration of the coating layer 20 will be described with reference to Fig. 5. Fig. 5 is a schematic enlarged view of the V portion shown in Fig. 2.
[0036] As shown in FIG. 5, the coating layer 20 has at least a hard layer 21. The hard layer 21 may have one or more metal nitride layers. The hard layer 21 is a layer having superior wear resistance compared to the metal layer 22. The hard layer 21 may be a single layer. Alternatively, a plurality of metal nitride layers may be overlapped. Alternatively, the hard layer 21 may have a laminated portion 23 in which a plurality of metal nitride layers are laminated, and a third metal nitride layer 24 located on the laminated portion 23. The configuration of the hard layer 21 will be described later.
[0037] (metal layer 22) The coating layer 20 may also have a metal layer 22. The metal layer 22 may be located between the substrate 10 and the hard layer 21. Specifically, the metal layer 22 may be in contact with the substrate 10 on one surface and in contact with the hard layer 21 on the other surface.
[0038] The metal layer 22 has higher adhesion to the substrate 10 than the hard layer 21. Examples of metal elements having such properties include Zr, V, Cr, W, Al, Si, and Y. The metal layer 22 contains at least one of the above metal elements.
[0039] Note that simple elements of Ti, Zr, V, Cr, and Al are not used as the metal layer 22. These elements all have low melting points and low oxidation resistance, making them unsuitable for use in cutting tools. Also, simple elements of Hf, Nb, Ta, and Mo have low adhesion to the substrate 10. However, this does not apply to alloys containing Ti, Zr, V, Cr, Ta, Nb, Hf, and Al.
[0040] The metal layer 22 may be an Al-Cr alloy layer containing an Al-Cr alloy. Such a metal layer 22 has a particularly high adhesion to the substrate 10, and is therefore highly effective in improving the adhesion between the substrate 10 and the coating layer 20.
[0041] When the metal layer 22 is an Al-Cr alloy layer, the Al content in the metal layer 22 may be greater than the Cr content in the metal layer 22. For example, the composition ratio (atomic %) of Al to Cr in the metal layer 22 may be 70:30. With such a composition ratio, the adhesion between the substrate 10 and the metal layer 22 is higher.
[0042] The metal layer 22 may contain components other than the above metal elements (Zr, V, Cr, W, Al, Si, Y). However, from the viewpoint of adhesion to the substrate 10, the metal layer 22 may contain at least 95 atomic % or more of the above metal elements in total. More preferably, the metal layer 22 may contain at least 98 atomic % or more of the above metal elements in total. For example, when the metal layer 22 is an Al-Cr alloy layer, the metal layer 22 may contain at least Al and Cr in total of 95 atomic % or more. Furthermore, the metal layer 22 may contain at least Al and Cr in total of 98 atomic % or more. The ratio of the metal components in the metal layer 22 can be identified by, for example, analysis using EDS (energy dispersive X-ray spectrometry).
[0043] Moreover, since Ti has poor wettability with the base 10 according to the embodiment, it is preferable that the metal layer 22 contains as little Ti as possible from the viewpoint of improving adhesion with the base 10. Specifically, the Ti content in the metal layer 22 may be 15 atomic % or less.
[0044] In this way, in the insert 1 according to the embodiment, the metal layer 22, which has higher wettability with the substrate 10 than the hard layer 21, is provided between the substrate 10 and the hard layer 21, thereby improving the adhesion between the substrate 10 and the coating layer 20. Since the metal layer 22 also has high adhesion with the hard layer 21, the hard layer 21 is unlikely to peel off from the metal layer 22.
[0045] Moreover, cBN used as the base 10 is an insulator. As an insulator, cBN has room for improvement in adhesion with a film formed by a PVD (physical vapor deposition) method. In contrast, in the insert 1 according to the embodiment, by providing a conductive metal layer 22 on the surface of the base 10, adhesion between the hard layer 21 formed by PVD and the metal layer 22 is high.
[0046] (hard layer 21) Next, the configuration of the hard layer 21 will be described with reference to Fig. 6. Fig. 6 is a schematic enlarged view of a portion VI shown in Fig. 5.
[0047] As shown in FIG. 6, the hard layer 21 has a laminated portion 23 located on the metal layer 22, and a third metal nitride layer 24 located on the laminated portion 23.
[0048] The laminated portion 23 has a plurality of first metal nitride layers 23a and a plurality of second metal nitride layers 23b. The laminated portion 23 has a configuration in which the first metal nitride layers 23a and the second metal nitride layers 23b are alternately laminated.
[0049] The thickness of each of the first metal nitride layer 23a and the second metal nitride layer 23b may be 50 nm or less. By forming the first metal nitride layer 23a and the second metal nitride layer 23b thin in this manner, the residual stress of the first metal nitride layer 23a and the second metal nitride layer 23b is small. As a result, for example, peeling or cracking of the first metal nitride layer 23a and the second metal nitride layer 23b is less likely to occur, and the durability of the coating layer 20 is high.
[0050] The first metal nitride layer 23a is a layer in contact with the metal layer 22, and the second metal nitride layer 23b is formed on the first metal nitride layer 23a.
[0051] The first metal nitride layer 23a and the second metal nitride layer 23b may contain the metal contained in the metal layer 22.
[0052] For example, suppose that metal layer 22 contains two types of metals (herein referred to as a "first metal" and a "second metal"). In this case, first metal nitride layer 23a contains nitrides of the first metal and a third metal. The third metal is a metal not contained in metal layer 22. In addition, second metal nitride layer 23b contains nitrides of the first metal and the second metal.
[0053] For example, in the embodiment, the metal layer 22 may contain Al and Cr. In this case, the first metal nitride layer 23a may contain Al. Specifically, the first metal nitride layer 23a may be an AlTiN layer containing AlTiN, which is a nitride of Al and Ti. Also, the second metal nitride layer 23b may be an AlCrN layer containing AlCrN, which is a nitride of Al and Cr.
[0054] In this manner, by positioning the first metal nitride layer 23a containing the metal contained in the metal layer 22 on the metal layer 22, the adhesion between the metal layer 22 and the hard layer 21 is high. This makes it difficult for the hard layer 21 to peel off from the metal layer 22, and therefore the durability of the coating layer 20 is high.
[0055] The first metal nitride layer 23a, i.e., the AlTiN layer, has excellent adhesion to the metal layer 22, for example, in wear resistance. The second metal nitride layer 23b, i.e., the AlCrN layer, has excellent heat resistance and oxidation resistance, for example. In this way, the coating layer 20 includes the first metal nitride layer 23a and the second metal nitride layer 23b, which have different compositions, and thus the characteristics of the hard layer 21, such as wear resistance and heat resistance, can be controlled. This can extend the tool life of the insert 1. For example, in the hard layer 21 according to the embodiment, mechanical properties, such as adhesion to the metal layer 22 and wear resistance, can be improved while maintaining the excellent heat resistance of AlCrN.
[0056] The laminated portion 23 may be formed by, for example, an arc ion plating method (AIP method). The AIP method is a method in which a target metal (here, an AlTi target and an AlCr target) is evaporated by using an arc discharge in a vacuum atmosphere, and then combined with N2 gas to form a metal nitride (here, AlTiN and AlCrN). The metal layer 22 may also be formed by the AIP method.
[0057] The third metal nitride layer 24 may be located on the laminated portion 23. Specifically, the third metal nitride layer 24 contacts the second metal nitride layer 23b of the laminated portion 23. The third metal nitride layer 24 is, for example, a metal nitride layer containing Ti and Al (AlTiN layer) like the first metal nitride layer 23a.
[0058] The thickness of the third metal nitride layer 24 may be thicker than the thicknesses of the first metal nitride layer 23a and the second metal nitride layer 23b. Specifically, when the thicknesses of the first metal nitride layer 23a and the second metal nitride layer 23b are 50 nm or less as described above, the thickness of the third metal nitride layer 24 may be 1 μm or more. For example, the thickness of the third metal nitride layer 24 may be 1.2 μm.
[0059] Thereby, for example, when the friction coefficient of the third metal nitride layer 24 is low, the adhesion resistance of the insert 1 can be improved. Also, for example, when the hardness of the third metal nitride layer 24 is high, the wear resistance of the insert 1 can be improved. Also, for example, when the oxidation onset temperature of the third metal nitride layer 24 is high, the oxidation resistance of the insert 1 can be improved.
[0060] Furthermore, the thickness of third metal nitride layer 24 may be thicker than the thickness of laminated portion 23. Specifically, in the embodiment, when the thickness of laminated portion 23 is 0.5 μm or less, the thickness of third metal nitride layer 24 may be 1 μm or more. For example, when the thickness of laminated portion 23 is 0.3 μm, the thickness of third metal nitride layer 24 may be 1.2 μm. In this way, by making third metal nitride layer 24 thicker than laminated portion 23, the effect of improving the above-mentioned adhesion resistance, wear resistance, etc. is further enhanced.
[0061] The thickness of metal layer 22 may be, for example, not less than 0.1 μm and less than 0.6 μm. That is, metal layer 22 may be thicker than each of first metal nitride layer 23a and second metal nitride layer 23b, and thinner than stacked portion 23.
[0062] <Cutting tools> Next, the configuration of a cutting tool including the above-mentioned insert 1 will be described with reference to Fig. 7. Fig. 7 is a front view showing an example of a cutting tool according to an embodiment.
[0063] As shown in FIG. 7, a cutting tool 100 according to the embodiment has an insert 1 and a holder 70 for fixing the insert 1.
[0064] The holder 70 is a rod-shaped member extending from a first end (the upper end in FIG. 7) to a second end (the lower end in FIG. 7). The holder 70 is made of, for example, steel or cast iron. Of these materials, it is particularly preferable to use steel, which has high toughness.
[0065] The holder 70 has a pocket 73 at the end on the first end side. The pocket 73 is a portion where the insert 1 is attached, and has a seating surface that intersects with the rotation direction of the workpiece and a constraint side surface that is inclined relative to the seating surface. The seating surface is provided with a screw hole into which a screw 75, which will be described later, is screwed.
[0066] The insert 1 is positioned in a pocket 73 of the holder 70, and is attached to the holder 70 by a screw 75. That is, the screw 75 is inserted into the through hole 5 of the insert 1, and the tip of the screw 75 is inserted into a screw hole formed in the seating surface of the pocket 73 to screw the threaded portions together. In this way, the insert 1 is attached to the holder 70 such that the cutting edge portion 3 protrudes outward from the holder 70.
[0067] In the embodiment, a cutting tool used for so-called turning is exemplified. Examples of turning include inner diameter machining, outer diameter machining, and grooving. The cutting tool is not limited to the one used for turning. For example, the insert 1 may be used in a cutting tool used for milling.
[0068] For example, cutting of a workpiece includes (1) a step of rotating the workpiece, (2) a step of bringing the cutting edge 11 of the insert 1 into contact with the rotating workpiece to cut the workpiece, and (3) a step of separating the insert 1 from the workpiece. Representative examples of the material of the workpiece include carbon steel, alloy steel, stainless steel, cast iron, and non-ferrous metals.
[0069] (Example) Next, an example of a manufacturing method of the insert 1 will be described. Here, an example of a manufacturing method in the case where the substrate 10 is made of cBN will be described. First, TiN raw material powder of 72 volume % to 82 volume %, Al raw material powder of 13 volume % to 23 volume %, and Al2O3 raw material powder of 1 volume % to 11 volume % are prepared. Then, an organic solvent is added to each of the prepared raw material powders. As the organic solvent, alcohols such as acetone and isopropyl alcohol (IPA) can be used. Then, the mixture is pulverized and mixed in a ball mill for 20 hours to 24 hours. After pulverization and mixing, the solvent is evaporated to obtain a first mixed powder.
[0070] Next, cBN powder having an average particle size of 2.5 μm to 4.5 μm and cBN powder having an average particle size of 0.5 μm to 1.5 μm are mixed in a volume ratio of 8 to 9:1 to 2.0. An organic solvent is then added. As the organic solvent, alcohols such as acetone and IPA can be used. The mixture is then pulverized and mixed in a ball mill for 20 to 24 hours. After pulverization and mixing, the solvent is evaporated to obtain a second mixed powder.
[0071] Next, the obtained first mixed powder and second mixed powder are mixed in a volume ratio of 68 to 78:22 to 32. An organic solvent and an organic binder are added to the mixed powder. As the organic solvent, alcohols such as acetone and IPA can be used. As the organic binder, paraffin, acrylic resin, etc. can be used. Then, the mixture is pulverized and mixed in a ball mill for 20 to 24 hours, and the organic solvent is evaporated to obtain a third mixed powder. In addition, a dispersant may be added in the process using the ball mill as necessary.
[0072] The third mixed powder is then molded into a desired shape to obtain a molded body. For molding, known methods such as uniaxial pressing and cold isostatic pressing (CIP) can be used. The molded body is heated to a desired temperature within a range of 300°C to 600°C to evaporate and remove the organic binder.
[0073] Next, the compact is placed in an ultra-high pressure heating device and heated at 1200°C to 1500°C for 15 minutes to 30 minutes under a pressure of 4 GPa to 6 GPa. This produces a cubic boron nitride sintered body according to the embodiment. The resulting cubic boron nitride sintered body is then attached to the seat of a tip body made of cemented carbide via a bonding material.
[0074] Next, a coating layer 20 is formed on the surface of the chip by physical vapor deposition (PVD). After that, the coating layer 20 is treated with AeroWrap (registered trademark) under the conditions shown below to produce inserts according to Example 1 and Comparative Examples 3 to 5. In addition, an insert in which the coating layer 20 was not treated with AeroWrap (registered trademark) was used as Comparative Example 1, and a commercially available insert was used as Comparative Example 2.
[0075] <AeroWrap (registered trademark) treatment conditions> Equipment: AeroWrap (registered trademark) manufactured by Yamashita Works Media: Multicone Media diameter: 0.1~0.5mm Wing inverter frequency: 40Hz Spray time: 0 seconds (no treatment, Comparative Example 1), 5 seconds (Comparative Example 2), 10 seconds (Example 1), 15 seconds (Comparative Example 3) Wet / Dry: Wet
[0076] The media is sprayed by the rotation of the blades, whose rotation speed is controlled by an inverter to 40Hz (40 rotations per second).
[0077] The surface roughness of the third surface 9 was measured for the inserts according to Example 1 and Comparative Examples 1 to 5. For example, a shape analysis laser microscope VK-X1000 manufactured by KEYENCE Corporation was used for the surface roughness measurement. As specific measurement conditions, when the third surface 9 was observed from a direction perpendicular to the third surface 9, an area surrounded by 750 μm in a direction parallel to the first surface 6 and 300 μm in a direction perpendicular to the first surface 6 was scanned with a red semiconductor laser having a wavelength of 661 nm. Then, five roughness curves were extracted in the direction parallel to the first surface 6 at a measurement distance of 0.4 mm in the center of the third surface 9 within the measurement area, and the roughness curves of the five measured points were synthesized to obtain one roughness curve. The arithmetic surface roughness (Ra) and ten-point surface roughness (Rz) were measured from the obtained one roughness curve.
[0078] Fig. 8 is a diagram showing the measurement results of the average arithmetic surface roughness Ra of the third surface 9. Fig. 8 shows the average arithmetic surface roughness Ra1 in a direction D1 parallel to the ridge line 8 on the third surface 9 and the average arithmetic surface roughness Ra2 in a direction D2 perpendicular to the ridge line 8 on the third surface 9 for Example 1 and Comparative Examples 1 to 5.
[0079] As shown in FIG. 8, the average arithmetic surface roughness Ra1 of the inserts according to Comparative Examples 1 to 4 was greater than 0.20 μm, whereas the average arithmetic surface roughness Ra1 of the inserts according to Example 1 and Comparative Example 5 was 0.20 μm or less.
[0080] In the insert according to Example 1, the difference between the average arithmetic surface roughness Ra1 and the average arithmetic surface roughness Ra2 was 0.1 μm or less. Specifically, Ra1 was larger than Ra2, and the difference (Ra1-Ra2) was 0.01 μm or more and 0.025 μm or less.
[0081] Fig. 9 is a diagram showing the measurement results of the ten-point average surface roughness Rz of the third surface 9. Fig. 9 shows the ten-point average surface roughness Rz1 in a direction D1 parallel to the ridge line 8 of the third surface 9 and the ten-point average surface roughness Rz2 in a direction D2 perpendicular to the ridge line 8 of the third surface 9 for Example 1 and Comparative Examples 1 to 5.
[0082] As shown in FIG. 9, the ten-point average surface roughness Rz1 of the inserts according to Comparative Examples 1 to 5 was greater than 1.5 μm, whereas the ten-point average surface roughness Rz1 of the insert according to Example 1 was 1.5 μm or less.
[0083] In the insert according to Example 1, the difference between the ten-point average surface roughness Rz1 and the ten-point average surface roughness Rz2 was 0.2 μm or less. Specifically, Rz1 was larger than Rz2, and the difference (Rz1-Rz2) was 0.1 μm or more and 0.20 μm or less.
[0084] Further, for the inserts according to Example 1 and Comparative Examples 1, 3, and 4, a wear resistance test and a fracture resistance test were carried out under the following conditions.
[0085] <Fracture resistance test> Material: SCr420 Cutting speed: 160m / min Feed: 0.2mm / rev Depth of cut: 0.2 mm Cutting condition: Dry Evaluation method: Number of impacts until breakage
[0086] Fig. 10 is a graph showing the results of a wear resistance test for the inserts according to Example 1 and Comparative Examples 1, 3, and 4. Fig. 11 is a graph showing the results of a fracture resistance test for the inserts according to Example 1 and Comparative Examples 1, 3, and 4.
[0087] As shown in Figs. 10 and 11, the insert according to Example 1 has the same wear resistance and chipping resistance as the insert according to Comparative Example 1, i.e., the insert not subjected to Aero Wrap (registered trademark) treatment. It is also found that the inserts according to Comparative Examples 3 and 4 have the same wear resistance and chipping resistance as the insert not subjected to Aero Wrap (registered trademark) treatment. Note that the insert according to Comparative Example 5, i.e., the insert irradiated with the media for 30 seconds in the Aero Wrap (registered trademark) treatment, had the same chipping resistance as the insert according to Comparative Example 1, but the wear resistance was worse.
[0088] The reason why the wear resistance of the insert according to Comparative Example 5 was deteriorated is believed to be that the thickness of the coating layer located at the corner of the boundary between the second and third surfaces became too thin by setting the media irradiation time to 30 seconds. In contrast, the insert according to Example 1 had good wear resistance because the thickness of the coating layer located at the corner of the boundary between the second and third surfaces was prevented from becoming thin by limiting the media irradiation time to 10 seconds.
[0089] Further, the surface roughness of the finished surface of the workpiece used in the above-mentioned wear resistance test was measured. <Measurement conditions> Measurement equipment: Olympus LEXT OLS4000 Measurement length: 4.0mm Cutoff value: 0.8mm Scanning speed: 0.6mm / sec
[0090] The workpiece cut using the insert according to Example 1 had a smaller finished surface roughness than the workpiece cut using the insert according to Comparative Example 1. In addition, the workpiece cut using the insert according to Example 1 also had a smaller finished surface roughness than the workpiece cut using the insert according to Comparative Example 3 and the workpiece cut using the insert according to Comparative Example 4.
[0091] For the inserts according to Example 1 and Comparative Example 1, the residual stress of the second coating layer was measured under the following conditions. The residual stress measurement of the first coating layer was performed at a position 0.8 mm away from the cutting edge of the cutting edge toward the center of the insert. The second coating layer was measured at a position 1.3 mm away from the cutting edge of the cutting edge in a direction parallel to the first surface and 0.5 mm away from the cutting edge in a direction perpendicular to the first surface. The residual stress value was determined by averaging the residual stress values of the first coating layer in two mutually perpendicular directions, and the residual stress values of the second coating layer in directions parallel and perpendicular to the first surface, which were respectively designated as σ1 and σ2.
[0092] <Conditions for residual stress measurement> Equipment: Bruker Japan D8 Discover Plus IμS Source: CuKα Collimator diameter: 0.3 mm Measured diffraction line: TiAlN (311) surface, 2θ = 75.5° Measurement method: 2D method
[0093] Fig. 12 is a table showing the results of measuring the residual stress on the second coating layer of the inserts according to Example 1 and Comparative Example 1. Fig. 12 also shows the results of measuring the surface roughness of the third surface of the inserts according to Example 1 and Comparative Examples 1 to 3, along with the results of measuring the residual stress on the second coating layer of the inserts according to Example 1 and Comparative Example 1. The results of measuring the surface roughness are similar to those shown in Figs. 8 and 9.
[0094] 12, in the insert according to Example 1, σ1 was a compressive stress of -1050 MPa or more and -750 MPa or less, and σ2 was a compressive stress of -1400 MPa or more and -1100 MPa or less. In contrast, σ2 of the insert according to Comparative Example 1 was outside the range of -1400 MPa or more and -1100 MPa or less.
[0095] <Other embodiments> In the above-described embodiment, the insert 1 has been described in which the base 10 made of boron nitride particles or the like is attached to the tip body 2 made of cemented carbide or the like, and these are coated with the coating layer 20. However, the insert according to the present disclosure is not limited to this, and may be, for example, a hexahedral base whose upper and lower surfaces are parallelogram-shaped, and the entire base is made of a cubic boron nitride sintered body, with a coating layer formed on top of such a base.
[0096] In the above embodiment, an example was shown in which the shape of the upper and lower surfaces of the insert 1 is a parallelogram, but the shape of the upper and lower surfaces of the insert 1 may be a rhombus, a square, etc. In addition, the shape of the upper and lower surfaces of the insert 1 may be a triangle, a pentagon, a hexagon, etc.
[0097] The shape of the insert 1 may be a positive type or a negative type. The positive type is a type in which the side surface is inclined with respect to a central axis passing through the center of the upper surface and the center of the lower surface of the insert 1, and the negative type is a type in which the side surface is parallel to the central axis.
[0098] In the above-described embodiment, an example in which the substrate 10 contains particles of cubic boron nitride (cBN) has been described. The substrate disclosed in the present application may contain particles of hexagonal boron nitride (hBN), rhombohedral boron nitride (rBN), wurtzite boron nitride (wBN), or the like. The substrate 10 is not limited to boron nitride, and may be, for example, a cemented carbide or a cermet. The cemented carbide contains W (tungsten), specifically WC (tungsten carbide). The cemented carbide may contain Ni (nickel) or Co (cobalt). The cermet contains, for example, Ti (titanium), specifically TiC (titanium carbide) or TiN (titanium nitride). The cermet may contain Ni or Co.
[0099] In the above embodiment, the insert 1 has been described as being used for cutting processing, but the insert according to the present application can also be applied to tools other than cutting tools, such as excavation tools and blades.
[0100] Further advantages and modifications may readily occur to those skilled in the art. Thus, the invention in its broader aspects is not limited to the specific details and representative embodiments shown and described above. Accordingly, various modifications may be made without departing from the spirit or scope of the general inventive concept as defined by the appended claims and equivalents thereof. [Explanation of symbols]
[0101] 1 Insert 2 Chip body 3 Cutting edge 4 Seat 5 Through hole 6 Front page 7 Side 2 8 Ridge 9 Page 3 10 Base 11 Cutting edge 20 Covering layer 21 Hard layer 22 Metal layer 23 Laminated section 23a First metal nitride layer 23b Second metal nitride layer 24 Third metal nitride layer 100 cutting tools 201 1st coating layer 202 Second coating layer 203 Third coating layer
Claims
1. A substrate made of any one of cemented carbide, cermet, boron nitride sintered body, and ceramics; a coating layer overlying the substrate; and The substrate is a first surface having a rake face; a second surface having a flank; a ridge portion located between the first surface and the second surface; a cutting edge located at least partly on the ridge line portion; and The cutting edge has a third surface at least in part, When the average arithmetic surface roughness Ra of the third surface in a direction parallel to the ridge line portion is defined as Ra1, the Ra1 is 0.20 μm or less, When the average arithmetic surface roughness Ra of the third surface in a direction perpendicular to the ridge line portion is defined as Ra2, the difference between Ra1 and Ra2 is 0.1 μm or less, and the coating layer includes a first coating layer located on the first surface and a second coating layer located on the second surface, The residual stress measured by the 2D method in the vicinity of the cutting edge of the first coating layer is defined as σ1, When the residual stress measured by the 2D method in the vicinity of the cutting edge of the second coating layer is σ2, The σ1 is the residual stress σ1 in the first coating layer in a direction parallel to the first surface and perpendicular to the ridge line portion. 22 and the σ1 22 Residual stress σ1 in the direction perpendicular to the direction of 11 is the average value of The σ2 is the residual stress σ2 in the second coating layer in a direction perpendicular to the first surface. 11 and residual stress σ2 in a direction parallel to the first surface. 22 is the average value of The σ1 is −1050 MPa or more and −750 MPa or less, The insert, wherein the σ2 is −1400 MPa or more and −1100 MPa or less.
2. 2. The insert according to claim 1, wherein, when a ten-point average surface roughness Rz of the third surface in a direction parallel to the ridge line portion is defined as Rz1, the Rz1 is 1.5 μm or less.
3. 3. The insert according to claim 2, wherein when the ten-point average surface roughness Rz of the third surface in a direction perpendicular to the ridge line portion is Rz2, the difference between Rz1 and Rz2 is 0.2 μm or less.
4. The coating layer is a hard layer; a metal layer other than a simple substance of Ti, Zr, V, Cr, Ta, Nb, Hf, or Al, located between the substrate and the hard layer; The insert according to any one of claims 1 to 3, comprising:
5. 5. The insert according to claim 4, wherein the metal layer contains at least one element selected from the group consisting of Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, and Y.
6. a rod-shaped holder having a pocket at an end; and an insert according to any one of claims 1 to 5 located in the pocket.
Citation Information
Patent Citations
Hard layer coated member
JP1995216561A
Throw away tip
JP2000326110A
Polycrystalline hard sintered cutting tool
JP2001212703A
Hard coating ultrahigh temperature high pressure sintered material