Connection structure for high-temperature superconducting wires, method for forming same, high-temperature superconducting wires, and high-temperature superconducting coils

By thickening the base material at the joint and using materials with specific thermal expansion coefficients, the connection structure addresses warping and peeling issues in superconducting wires, maintaining stability and performance in thermal cycles.

JP7568645B2Active Publication Date: 2024-10-16FURUKAWA ELECTRIC CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021562761
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-05
Filing Date
2020-12-04
Publication Date
2024-10-16
Estimated Expiration
2040-12-04

AI Technical Summary

Technical Problem

The existing methods for connecting superconducting wires with oxide superconducting layers on metal base materials face issues with warping and peeling due to thermal expansion coefficient differences, leading to a small contact area and separation at the joint.

Method used

The connection structure involves making the base material thicker at the joint portion than the non-joint portion, using materials with specific thermal expansion coefficients to suppress warping and peeling, and incorporating additional layers like metal and ceramic to enhance bonding and rigidity.

Benefits of technology

This configuration effectively prevents peeling of superconducting layers even with thermal deformation, ensuring stable superconducting properties and reducing warpage, suitable for applications like MRI and NMR magnetic coils.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568645000004
    Figure 0007568645000004
  • Figure 0007568645000005
    Figure 0007568645000005
  • Figure 0007568645000006
    Figure 0007568645000006
Patent Text Reader

Abstract

A structure for connecting high-temperature superconducting wire materials according to an embodiment comprises: a first superconducting wire material 3 and a second superconducting wire material 4, each of the two high-temperature superconducting wire materials comprising a band-shaped base material 1 made of metal or alloy, and an oxide superconducting layer 2 formed on an upper surface of the base material 1; and a joint portion 6 comprising a superconducting connection portion 5 formed between the first and second superconducting wire materials 3, 4 by joining the first and second superconducting wire materials 3, 4 together in a positional relationship such that the upper surfaces of the first and second superconducting layers 2, 2, which are the respective oxide superconducting layers of the first and second superconducting wire materials 3, 4, are opposed to each other. In the same base material 1 of the superconducting wire material 3 of at least one of the first and second superconducting wire materials 3, 4, a first portion 7 constituting the joint portion 6 is thicker than a second portion 8 that does not constitute the joint portion 6.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a connection structure for high-temperature superconducting wires, a method for forming the same, a high-temperature superconducting wire, and a high-temperature superconducting coil. [Background technology]

[0002] Superconducting wires (hereinafter, sometimes simply referred to as "superconducting wires") in which an oxide superconducting layer is formed on a metal substrate have low current loss and are therefore used, for example, as windings of magnetic coils in MRI (Magnetic Resonance Imaging) devices, NMR (Nuclear Magnetic Resonance) devices, etc. However, in such coils, it is necessary to connect the superconducting wires to each other to form a closed loop and pass a persistent current.

[0003] As a method for connecting superconducting wires, for example, Patent Document 1 proposes a method using the MOD method (coating pyrolysis method: Metal Organic Deposition method / metal organic deposition method). The connection of superconducting wires by this MOD method involves removing the protective layer at the connection end of two superconducting wires, applying an MOD liquid containing a metal constituting the oxide superconducting layer to the surface of the exposed oxide superconducting layer by spin coating or spray coating to form an MOD coating film, drying it, and then joining the MOD films of the two superconducting wires by contacting them with each other and heating them to the crystallization temperature of the oxide superconducting layer while applying pressure. For the MOD liquid, for example, an acetylacetonate-based MOD solution containing RE (rare earth elements such as Y (yttrium), Gd (gadolinium), Sm (samarium), and Ho (holmium)), Ba (barium), and Cu (copper) in a ratio of about 1:2:3 is used. This makes it possible to connect two superconducting wires with lower resistance than joining by soldering. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-235699 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when two superconducting wires each having an oxide superconducting layer formed on a metal substrate are joined in this manner, repeated changes in thermal expansion and contraction due to heat cycles and the like over time cause differences in the thermal expansion coefficients of the oxide superconducting layer and the metal substrate, and as a result, when viewed in a width-wise cross-section of the joint, the two joined superconducting wires are prone to warping deformation in which the joining (connection) surfaces of the oxide superconducting layers separate at the width ends.As a result, there is a problem in that the contact area of ​​the joint is reduced and the two oxide superconducting layers that form the joint are prone to peeling off.

[0006] The present invention has been made in consideration of the above problems, and aims to provide a connection structure for high-temperature superconducting wires, a method for forming the same, and a high-temperature superconducting wire and coil, which are capable of effectively suppressing peeling of the superconducting layers constituting the two superconducting wires forming the joint, even when repeated thermal deformation due to thermal expansion and thermal contraction caused by a heat cycle or the like occurs, by optimizing the substrate of at least one of the two superconducting wires having an oxide superconducting layer formed on a metal substrate. [Means for solving the problem]

[0007] The inventors have discovered that when joining first and second superconducting wires, each having an oxide superconducting layer formed on a metal substrate, to form a joint including a superconducting joint formed between the first and second superconducting wires, by making the substrate of at least one of the first and second superconducting wires such that the first portion forming the joint is thicker than the second portion not forming the joint, even if repeated thermal deformation due to thermal expansion and contraction caused by a heat cycle or the like occurs, warping deformation of the two superconducting wires forming the joint can be effectively suppressed and peeling of the superconducting layer at the superconducting joint can be effectively prevented, thereby completing the present invention.

[0008] That is, the gist of the present invention is as follows. (1) A connection structure for high-temperature superconducting wires comprising: a band-shaped substrate made of a metal or alloy; first and second superconducting wires which are two high-temperature superconducting wires having an oxide superconducting layer formed on the surface side of the substrate; and a joint including a superconducting joint formed between the first and second superconducting wires by joining the first and second superconducting wires together in a positional relationship in which the surfaces of the first and second superconducting layers which are the oxide superconducting layers of the first and second superconducting wires face each other, wherein the substrate of at least one of the first and second superconducting wires is such that, in the same substrate, a first portion constituting the joint is thicker than a second portion not constituting the joint. (2) A connection structure for high-temperature superconducting wires as described in (1) above, wherein the substrate of the at least one superconducting wire is composed of at least two substrates including a first substrate which is the substrate and a fragmentary second substrate located on the back side of the first substrate, in the first portion. (3) A connection structure for high-temperature superconducting wires according to (2) above, wherein the at least one superconducting wire satisfies the relationships α1>α3 and α2>α3, where α1 is the thermal expansion coefficient of the first substrate, α2 is the thermal expansion coefficient of the second substrate, and α3 is the thermal expansion coefficient of the oxide superconducting layer. (4) The thermal expansion coefficient α1 of the first base material is 10.5×10 -63. The connection structure for high-temperature superconducting wires according to any one of (1) to (3) above, wherein the .lambda. / K or more. (5) A connection structure for high-temperature superconducting wires according to any one of (2) to (4) above, further comprising a metal layer between the first base material and the second base material, the metal layer having a melting point higher than 800°C and being resistant to oxidation at high temperatures. (6) A connection structure for high temperature superconducting wires according to (5) above, wherein the metal layer is formed of at least one kind of noble metal or alloy selected from the group consisting of Ag, Au and Pt. (7) The connection structure for high temperature superconducting wires according to any one of (2) to (6) above, further comprising a ceramic layer on a rear surface of the second base material. (8) A connection structure for high-temperature superconducting wires according to any one of (1) to (7) above, wherein the substrate of at least one of the superconducting wires has a thickness of the first portion of 60 μm or more and 100 μm or less, and a thickness of the second portion of 30 μm or more and 55 μm or less. (9) A connection structure for high temperature superconducting wires according to any one of (1) to (8) above, wherein the oxide superconducting layers of the first and second superconducting wires each have a thickness of 0.5 μm or more. (10) A connection structure for high temperature superconducting wires according to any one of (1) to (9) above, wherein the oxide superconducting layers of the first and second superconducting wires are both made of a REBCO-based superconducting material. (11) A high-temperature superconducting wire having the connection structure according to any one of (1) to (10) above. (12) A high-temperature superconducting coil formed using the high-temperature superconducting wire according to (11) above. (13) A method for manufacturing a superconducting wire having a strip-shaped substrate made of a metal or alloy, an oxide superconducting layer formed on a surface side of the substrate, and a protective layer formed on the surface of the oxide superconducting layer, comprising: a coating film forming step of applying an organometallic solution containing a metal that forms a superconducting joint to a surface portion of the oxide superconducting layer exposed by peeling off a part of each protective layer of first and second superconducting wires, and drying the applied film; a pre-firing step of forming a pre-firing film by heating the applied film at a first temperature; and a positioning step of facing the surfaces of the pre-firing films of the first and second superconducting wires on which the pre-firing films have been formed. and a main sintering step of forming a joint that joins the first and second superconducting wires by contacting the first and second superconducting wires in a spaced relationship and heating them at a second temperature higher than the first temperature to form a superconducting joint between the first and second superconducting wires, wherein, at least before the main sintering step, a substrate of at least one of the first and second superconducting wires has a first portion that forms the joint and is thicker than a second portion that does not form the joint, within the same substrate. Effect of the Invention

[0009] According to the present invention, by effectively increasing the thickness of the metal substrate at the connection portion of the superconducting layer when connecting superconducting wires each having an oxide superconducting layer formed on a metal substrate, it is possible to provide a connection structure for high-temperature superconducting wires, a method for forming the same, a high-temperature superconducting wire, and a high-temperature superconducting coil, which are capable of suppressing peeling of the two superconducting layers forming the joint even when thermal deformation occurs due to repeated thermal expansion and contraction caused by a heat cycle or the like. [Brief description of the drawings]

[0010] [Figure 1] 1 is a perspective view that illustrates a schematic diagram of a connection structure of superconducting wires according to a first embodiment of the present invention; [Diagram 2] 4 is a cross-sectional view that illustrates a schematic diagram of a connection structure of superconducting wires according to a second embodiment of the present invention. FIG. [Diagram 3] 10 is a cross-sectional view that illustrates a schematic diagram of a connection structure of superconducting wires according to a third embodiment of the present invention. FIG. [Figure 4] 11 is a cross-sectional view that illustrates a schematic diagram of a connection structure of superconducting wires according to a fourth embodiment of the present invention. FIG. [Diagram 5] 5 is a flowchart of a method for forming a superconducting wire connection structure according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0012] [First embodiment] {Connection structure of high-temperature superconducting wire} FIG. 1 is a perspective view that illustrates a schematic connection structure of high-temperature superconducting wires (hereinafter sometimes simply referred to as "superconducting wires") according to the first embodiment. As shown in FIG. 1 , a connection structure A for superconducting wires according to the first embodiment includes two high-temperature superconducting wires, a first superconducting wire 3 (hereinafter sometimes simply referred to as "superconducting wire 3") and a second superconducting wire 4 (hereinafter sometimes simply referred to as "superconducting wire 4"), each of which has a band-shaped substrate 1, 1 made of a metal or an alloy, and superconducting layers 2, 2 made of oxide superconducting layers (hereinafter sometimes simply referred to as "superconducting layers") formed on the surface sides of the substrates 1, 1, respectively. The first and second superconducting wires 3, 4 are joined together in a positional relationship in which the surfaces of the superconducting layers 2, 2 face each other, and a joint 6 including a superconducting connection part 5 is formed between the first and second superconducting wires 3, 4, and the substrate 1 of at least one of the first superconducting wire 3 and the second superconducting wire 4 (referred to as the "first superconducting wire 3" in FIG. 1 ) is characterized in that, in the same substrate 1, a first portion 7 constituting the joint 6 is thicker than a second portion 8 not constituting the joint 6.

[0013] (base material) The substrate 1 is composed of a strip-shaped metal substrate or alloy substrate. Examples of materials for the substrate 1 include metals such as Co (cobalt), Cu (copper), Cr (chromium), Ni (nickel), Ti (titanium), Mo (molybdenum), Nb (niobium), Ta (tantalum), W (tungsten), Mn (manganese), Fe (iron), Ag (silver), and alloys thereof, which are excellent in strength and heat resistance. In particular, from the viewpoint of excellent corrosion resistance and heat resistance, it is preferable to use Ni-based alloys such as Hastelloy (registered trademark) and Inconel (registered trademark), or Fe-based alloys such as stainless steel, and it is more preferable to use Ni-Fe-Mo-based alloys such as Hastelloy (registered trademark). Table 1 shows the thermal expansion coefficients of Co, Cu, Cr, Ni, Ti, Mo, Nb, Ta, W, Mn, Fe, Ag, Hastelloy (registered trademark), Inconel (registered trademark), and stainless steel, which are examples of materials that can be used to form the first substrate 1 in the present invention.

[0014] [Table 1]

[0015] Among these metals or alloys, in the present invention, the first substrate 1 is made of a metal or alloy having a thermal expansion coefficient of 10.5×10 -6 It is preferable that the connecting structure B is made of a metal or alloy having a copper content of 1000 ppm or more, such as Co, Cu, Ni, Mn, Fe, Hastelloy (registered trademark), Inconel (registered trademark), or stainless steel. By making such a configuration, a connecting structure B having excellent corrosion resistance and heat resistance can be obtained.

[0016] (Superconducting layer) The superconducting layer 2 is an oxide superconducting layer, and is formed on the surface side of the substrate 1. The superconducting layer 2 is formed from an oxide superconducting layer whose transition temperature is higher than the boiling point of liquid nitrogen (-196°C: 77K), and in particular, is made of a REBCO-based superconducting material (REBa2Cu3O 7-δ As the REBCO-based oxide superconducting material, for example, REBa2Cu3O 7-δA superconducting layer such as (RE-based superconducting layer) is preferable. In addition, RE is a single rare earth element such as Y (yttrium), Nd (neodymium), Sm (samarium), Eu (europium), Gd (gadolinium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), Lu (lutetium), or a plurality of rare earth elements. In addition, δ is an oxygen non-stoichiometric amount, and is, for example, 0 or more and 1 or less, and is preferably closer to 0 in terms of a high superconducting transition temperature. In addition, if high-pressure oxygen annealing is performed using an apparatus such as an autoclave, the oxygen non-stoichiometric amount δ may be less than 0, that is, a negative value. In consideration of the balance between performance, mechanical strength, and productivity, the thickness of the superconducting layer 2 is preferably 0.1 to 10 μm, and more preferably 0.5 to 5 μm.

[0017] (joint part) The joint 6 has a superconducting joint 5 formed between the superconducting layer 2 of the first superconducting wire 3 and the superconducting layer 2 of the second superconducting wire 4, and the superconducting layer 2 of the first superconducting wire 3 and the superconducting layer 2 of the second superconducting wire 4, which are in contact with the superconducting joint 5, respectively. The superconducting joint 5 is preferably composed of the same superconducting layer composition as the superconducting layer 2, and can be formed using a composition (solution) containing raw materials necessary for forming a RE-based superconducting layer, in particular. As such a solution, for example, an acetylacetonate-based or naphthenate-based MOD solution containing RE (rare earth elements such as Y, Gd, Sm, and Ho), Ba, and Cu in a ratio of about 1:2:3 can be used. The MOD solution is applied to the surfaces of the first and second superconducting wires 3, 4 and dried to form a coating film, and then the coating films of these two superconducting wires are brought into contact with each other and pressed together while being heated to the crystallization temperature of the oxide superconducting layer (e.g., 760 to 800°C) and sintered to obtain a crystalline superconducting joint 5.

[0018] (Relationship between the thickness of the first part and the second part) In this embodiment, the substrate 1 of at least one of the first superconducting wire 3 and the second superconducting wire 4 (referred to as "first superconducting wire 3" in FIG. 1) is configured such that the first portion 7 constituting the joint 6 is made thicker than the second portion 8 of the substrate 1 not constituting the joint 6, thereby increasing the rigidity of the first portion 7 and reducing the deformation of the entire joint including the first portion 7 during heating and subsequent cooling for forming the connection structure A of the superconducting wires of the first embodiment. In the present invention, the effective thickness of the first portion 7 is made thicker than the effective thickness of the second portion 8 in this manner, thereby reducing the thermal deformation of the first portion 7 during heating and cooling by heat treatment, thereby reducing the deformation of the first portion 7, the superconducting layer 2, and the joint 6, and thereby suppressing warping of the connection structure A of the superconducting wires. In the substrate 1 of the first superconducting wire 3, which is at least one of the superconducting wires, the thickness of the first portion 7 is preferably 60 μm to 100 μm and the thickness of the second portion 8 is preferably 30 μm to 55 μm, and the thickness of the first portion 7 is more preferably 70 μm to 150 μm and the thickness of the second portion 8 is 30 μm to 50 μm. With this configuration, even if the heating and subsequent cooling for forming the connection structure A are repeated a relatively large number of times, the rigidity of the first portion 7, the deformation amount of the entire joint including the first portion 7, and the high-temperature superconducting wire can be appropriately harmonised to improve the effect of suppressing warpage of the connection structure A. Although an example in which the first portion 7 is formed only on the first superconducting wire 3 has been described here as the connection structure A for superconducting wires according to the first embodiment, as shown in Fig. 1, the connection structure A is not limited to this example, and for example, the first portion 7 may be formed on both the first superconducting wire 3 and the second superconducting wire 4, and the first portions 7, 7 may be configured to have a substantially symmetrical positional relationship with each other. With this configuration, the effect of suppressing warping of the connection structure A for superconducting wires according to the first embodiment can be further improved.

[0019] [Second embodiment] Next, a superconducting wire connection structure B according to a second embodiment of the present invention will be described. In the second to fourth embodiments described below, the description of the parts that overlap with the first embodiment will be omitted, and only the parts that differ from the first embodiment will be described. In addition, the same reference numerals will be used for the components of the superconducting wire connection structure that are the same as those in the first embodiment.

[0020] 2 is a cross-sectional view showing a schematic diagram of a connection structure B of a superconducting wire according to the second embodiment. In the connection structure A of the first embodiment, the effective thickness of the first portion 7 constituting the joint 6 is made thicker than the effective thickness of the second portion 8 not constituting the joint 6, whereas in the connection structure B of the second embodiment, the effective thickness of the first portion 70 constituting the joint 60 is made thicker than the effective thickness of the second portion 8 not constituting the joint 60 by disposing a fragmentary second substrate 9 on the back surface side of the first substrate 1a opposite to the surface on which the superconducting layer 2 is located. In other words, connection structure B is configured by applying a first superconducting wire 30 (hereinafter sometimes simply referred to as "superconducting wire 30") having a first portion 70 with a fragmentary second substrate 9 arranged on the back side of first substrate 1a instead of the first superconducting wire 3 constituting connection structure A, and by including a second superconducting wire 40 (hereinafter sometimes simply referred to as "superconducting wire 40") arranged opposite superconducting wire 30, having first substrate 1a and a superconducting layer 2 arranged on the front side of first substrate 1a, and forming a joint 60 via superconducting connection portion 5 by opposing the superconducting layer 2 to the superconducting layer 2 of superconducting wire 30.

[0021] In this embodiment, a first portion 70 of a superconducting wire 30 includes a fragmentary second substrate 9 located on the back side of a first substrate 1a, so that the thickness of the first portion 70 is greater than the thickness of the second portion 8 by the thickness of the second substrate 9. According to this embodiment, the second substrate 9 is appropriately selected from materials having various thermal expansion coefficients, so that the degree of the warping effect of a connection structure B for high-temperature superconducting wires can be set to a desired degree.

[0022] (Fragmentary second substrate) In order to further enhance the effect of suppressing warping of the connection structure B of the superconducting wire, it is preferable that the second substrate 9 is configured to satisfy the relationships α1>α3 and α2>α3, where α1 is the thermal expansion coefficient of the first substrate 1a, α2 is the thermal expansion coefficient of the second substrate 9, and α3 is the thermal expansion coefficient of the superconducting layer 2. With this configuration, the amount of deformation of the first portion 70 is smaller than that of the second portion 8 during heating and cooling when forming the connection structure B of the superconducting wire of the second embodiment, and warping of the connection structure B of the superconducting wire of the second embodiment can be more effectively suppressed. 2, an example in which the second base material 9 is formed only on the first portion 70 of the superconducting wire 30 has been described, but the connection structure B is not limited to this example, and for example, the second base material 9 may be formed on both the superconducting wire 30 and the superconducting wire 40, and the first portions 70, 70 may be configured to have a substantially symmetrical positional relationship with each other. With this configuration, the effect of suppressing warping of the connection structure B for superconducting wires of the second embodiment can be further improved.

[0023] When the first base material 1a is made of Hastelloy C276 (registered trademark), Inconel 600 (registered trademark), or stainless steel (SUS304) as exemplified in the first embodiment, the thermal expansion coefficients of these materials are 11.2×10 -6 / K(25~100℃), 11.5~13.3×10 -6 / K(20~1000℃), 17.3×10 -6 / K (0 to 100° C.). Therefore, as a material for the fragmentary second base material 9 that satisfies the above relationship (1), for example, Ti (thermal expansion coefficient: 8.4×10 -6 / K(20℃)), Pt(8.8×10 -6 / K (25° C.) Alternatively, the second base material 9 may be made of the same material as the first base material 1a.

[0024] (metal layer) The superconducting wire 30 preferably has a metal layer 10 formed between the first base 1a and the second base 9 as a layer for bonding the first base 1a and the second base 9. The metal layer 10 is preferably made of a metal having a melting point higher than 800°C and a property of being difficult to oxidize at high temperatures. With this configuration, the metal layer 10 increases the adhesion and bonding strength between the first base 1a and the second base 9, and the connection structure B of the superconducting wire having heat resistance to the heat treatment temperature (760 to 800°C) when forming the superconducting connection part 5 by the above-mentioned MOD method is obtained. The metal layer 10 having such properties is preferably made of at least one precious metal or alloy selected from the group of Ag, Au, and Pt. If the metal layer 10 is made of at least one precious metal or alloy selected from the group of Ag, Au, and Pt, the metal layer 10 having the above-mentioned excellent bonding property and heat resistance can be formed relatively easily.

[0025] The superconducting wires 30, 40 preferably further have a protective layer 11 covering the entire surface of the superconducting layer 2 except for the superconducting joint 5. With this configuration, the surfaces of the superconducting layers 2, 2 can be effectively protected without being exposed. The protective layer 11 is preferably a metal or alloy layer containing at least one of Ag, Au, and Cu, and is more preferably a metal layer of Ag. The thickness of the protective layer 11 is preferably 1 to 50 μm, and more preferably 1.5 to 5 μm. When the protective layer 11 is formed on the surfaces of the superconducting layers 2, 2, the surfaces of the superconducting layers 2, 2 can be effectively protected without being exposed.

[0026] [Third embodiment] Next, a superconducting wire connection structure C according to a third embodiment of the present invention will be described. 3 is a cross-sectional view showing a connection structure C according to the third embodiment. The first portion 7 of the connection structure A according to the first embodiment and the first portion 70 of the connection structure B according to the second embodiment are made of only a metal material, whereas in the connection structure C according to the third embodiment, a portion of the first superconducting wire 31 (hereinafter, sometimes simply referred to as "superconducting wire 31") constituting the joint 61 is made of the superconducting layer 2, the first base material 1a, the metal layer 10, the second base material 9, the ceramic layer 20, and the protective layer 11 in this order. Note that the connection structure C here is made up of the first superconducting wire 31, the second superconducting wire 40, and the joint 61 formed between the first and second superconducting wires 31, 40.

[0027] (Ceramic layer disposed on the surface of the fragmentary second substrate facing the first substrate) The ceramic layer 20 is disposed on the back surface of the second substrate 9, which is opposite to the front surface on which the metal layer 10 is located, thereby making the amount of thermal deformation of the first portion 71 after heat treatment smaller than the amounts of thermal deformation of the first portion 7 of connection structure A and the first portion 70 of connection structure B after heat treatment, thereby further improving the warpage reduction effect. That is, since ceramic materials generally have a smaller thermal expansion coefficient than metal materials, connection structure C in which the ceramic layer 20 is formed on the back surface side of the second substrate 9 has the effect of reducing the amount of thermal deformation after heat treatment in the MOD method or the like. 3, an example has been described in which second base material 9 having ceramic layer 20 is formed only on first portion 71 of superconducting wire 31, but connection structure C is not limited to this example, and for example, second base material 9 may be formed on both superconducting wire 31 and superconducting wire 40, with first portions 71, 71 being configured to have a substantially symmetrical positional relationship. With this configuration, the effect of suppressing warping of connection structure C for superconducting wire of the third embodiment can be further improved. There is no particular limitation on the ceramic material applicable to the ceramic layer used in the present invention. In the present invention, it is particularly preferable to configure the ceramic layer 20 from the same material as the superconducting layer 2. Table 2 shows the thermal expansion coefficients of the ceramic material configuring the superconducting layer 2 and other major ceramic materials.

[0028] [Table 2]

[0029] [Fourth embodiment] Next, a superconducting wire connection structure D according to a fourth embodiment of the present invention will be described. FIG. 4 is a cross-sectional view that illustrates a connection structure D according to the fourth embodiment. In the connection structures A, B and C of the first to third embodiments, the first portion 7, 70, 71 is formed only on the back side of one of the first and second superconducting wires included in each connection structure, thereby making the effective thickness of each of the first portions 7, 70, 71 constituting the respective joints 6, 60, 61 thicker, whereas in the connection structure D of the fourth embodiment, fragmentary second base materials 9, 9 are formed, via metal layers 10, 10, respectively, on the back side of each of the first base materials 1a, 1a constituting the joints 62 of both the first and second superconducting wires 30, 41, thereby forming first portions 72, 72 and second portions 8, 8 in each of the first superconducting wire 30 and the second superconducting wire 41, and making the effective thickness of each of the first portions 72 thicker than the effective thickness of the second portions 8, thereby reducing warping of the connection structure for high-temperature superconducting wires. That is, in the connection structure D, instead of the second superconducting wire 40 of the connection structure B, the second superconducting wire 41 has a configuration in which fragmentary second base materials 9, 9 are formed on the back side of each of the first base materials 1a, 1a constituting the joint 62, with metal layers 10, 10 interposed therebetween. Note that the connection structure D here is configured to include the first superconducting wire 30, the second superconducting wire 41, and the joint 62 formed between the first and second superconducting wires 30, 41.

[0030] By configuring in this manner, it is possible to obtain connection structure D in which the warping reduction effect is further improved compared to the first to third embodiments due to the synergistic effect of increasing the effective thickness of both first portion 72 of first superconducting wire 30 and first portion 72 of second superconducting wire 41. As explained in the third embodiment, if ceramic layers 20, 20 are formed on the back sides of the two first portions 72, 72 constituting the joint, respectively, the effect of reducing the warpage can be further improved. In this case, if the ceramic layer 20 is formed from the same material as the superconducting layer 2, the effect of reducing the warpage can be further improved. Furthermore, protective layers 11, 11 similar to those in the third embodiment can be formed on the ceramic layers 20, 20, respectively.

[0031] (High-temperature superconducting wire having a joint structure of high-temperature superconducting wire) The connection structure of the high-temperature superconducting wire of the above-mentioned embodiment is suitable for application to various high-temperature superconducting wires in which it is necessary to suppress peeling of the two superconducting layers forming the joint even when repeated thermal expansion and contraction occurs due to a heat cycle or the like, such as the windings of magnetic coils for MRI, NMR, etc.

[0032] (Method of forming a connection structure for high-temperature superconducting wires) A method for forming the connection structures A, B, C, and D of the high-temperature superconducting wire of this embodiment will be described. Here, a method for forming the connection structure B (FIG. 2) will be described, but the methods for forming the connection structures A, C, and D are basically the same. As shown in FIG. 5, first, a first and a second superconducting wire 30, 40 are prepared, which are two superconducting wires having a band-shaped base material 1 made of a metal or an alloy, an oxide superconducting layer 2 formed on the surface side of the base material 1, and a protective layer 11 formed on the surface of the oxide superconducting layer 2. Among them, at least one of the first and second superconducting wires 30, 40 is prepared such that the base material 1 has a first portion 70 constituting the joint 60 formed thicker than the second portion 8 not constituting the joint 60, or the first portion 70 constituting the joint 60 is thicker than the second portion 8 not constituting the joint 60 (superconducting wire preparation step S1). Next, a part of the protective layer 11, 11 of each of the first and second superconducting wires 30, 40 prepared in step S1 is peeled off and removed to expose the oxide superconducting layers 2, 2 (protective layer removing step S2). Subsequently, an organometallic solution containing a metal forming the superconducting joint 5 is applied to the surface portion of the oxide superconducting layers 2, 2 exposed in step S2 and dried to form a coating film (organometallic solution coating forming step S3). Thereafter, the coating film formed in step S3 is heated to a first temperature (preferably 450 to 550°C) to remove the organic matter in the coating film and form a pre-fired film (pre-fired film forming step S4). Next, the first and second superconducting wires 30, 40 having the pre-sintered films formed in step S4 are brought into contact with each other in a mutually opposed positional relationship and heated at a second temperature (preferably 760 to 820°C) higher than the first temperature to form a superconducting joint 5 between the first and second superconducting wires 30, 40, and a main sintering step is performed to form a joint 60 by the first and second superconducting wires 30, 40 and the superconducting joint 5 (main sintering joint formation step S5). By performing steps S1 to S5 in this manner in order, a connection structure for high-temperature superconducting wires can be formed that can effectively suppress peeling of the superconducting layers constituting the two superconducting wires forming the joint, even if thermal deformation occurs due to repeated thermal expansion and thermal contraction caused by a heat cycle or the like. Additionally, in this embodiment, after step S5, a heat treatment may be performed in an oxygen atmosphere to further perform an oxygen replenishment heat treatment for replenishing oxygen to oxygen-deficient portions of the film constituting the bonding portion. EXAMPLES

[0033] Next, in order to further clarify the effects of the present invention, examples and comparative examples will be described, but the present invention is not limited to these examples.

[0034] <Preparation of test material> First, a high-temperature superconducting wire (hereinafter sometimes simply referred to as "superconducting wire") was prepared by sequentially forming a 1.6 μm-thick superconducting layer 2 made of GdBCO and a 2 μm-thick protective layer 11 made of Ag on the front surface of a 50 μm-thick, 6 m-wide Hastelloy (registered trademark) substrate 1, and forming a 2 μm-thick metal layer 10 made of Ag on the back surface (see FIG. 2). Next, a MOD solution was applied to the removed portion of the protective layer 11 to form a MOD coating film, and then the organic solvent in the MOD coating film was evaporated at 500° C. in a mixed gas atmosphere of nitrogen and oxygen to produce a superconducting wire with a MOD pre-fired film formed on the front surface side, which was used as a test material.

[0035] Example 1 A Hastelloy (registered trademark) substrate 9 (hereinafter, sometimes referred to as a "Hastelloy (registered trademark) dummy substrate 9") having a thickness of 50 μm, a length of 20 mm, and a width of 6 mm was arranged on the back side of the test material opposite to the front side of the MOD pre-fired film, and another test material was prepared without the Hastelloy (registered trademark) dummy substrate 9. Next, these test materials were arranged so that the front sides of the MOD pre-fired films faced each other, and then main firing was performed under conditions of a mixed gas atmosphere of argon gas and oxygen gas, a heating temperature of 800° C., and a pressure of 100 MPa, and the MOD pre-fired film was crystallized to form a joint 60 consisting of a crystallized MOD layer, and two superconducting wires 30, 40 were joined together. In this way, a superconducting wire connection structure B was produced in which, in one of the two superconducting wires 30, 40, the first portion 70 constituting the joint 60 was thicker than the second portion 8 not constituting the joint, and this was designated Example 1 (see Figure 2).

[0036] Example 2 Two specimens were prepared by disposing the Hastelloy (registered trademark) dummy substrate 9 on the back side opposite to the front side of the MOD pre-sintered film. Next, the front sides of the MOD pre-sintered films were disposed facing each other, and then main sintering was performed under a mixed gas atmosphere of argon gas and oxygen gas at a heating temperature of 800° C. and a pressure of 100 MPa to crystallize the MOD pre-sintered film, thereby forming a joint 62 made of a crystallized MOD layer to join two superconducting wires 30 and 41. In this way, a superconducting wire connection structure D was produced in which the first parts 72, 72 constituting the joint 62 were thicker than the second parts 8, 8 not constituting the joint 62 in the two superconducting wires 30 and 41, and this was designated as Example 2 (see FIG. 4 ).

[0037] Example 3 Two carbon steel substrates 9 (hereinafter sometimes referred to as "carbon steel dummy substrates 9") having a thickness of 50 μm, a length of 20 mm, and a width of 6 mm were prepared on the back side of the test material opposite to the front side of the MOD pre-sintered film. Next, the front sides of the MOD pre-sintered films were arranged facing each other, and then main sintering was performed under a mixed gas atmosphere of argon gas and oxygen gas at a heating temperature of 800° C. and a pressure of 100 MPa to crystallize the MOD pre-sintered film, thereby forming a joint 62 made of a crystallized MOD layer to join two superconducting wires 30, 41. In this way, a superconducting wire connection structure D was produced in which the first parts 72, 72 constituting the joint 62 were thicker than the second parts 8, 8 not constituting the joint 62 in the two superconducting wires 30, 41, and this was designated as Example 3 (see FIG. 4).

[0038] Example 4 Two test pieces were prepared by placing the back side of the test piece, which was 50 μm thick, 20 mm long, and 6 mm wide, facing each other on the back side opposite to the front side of the MOD pre-sintered film of the test piece. Next, the front sides of the MOD pre-sintered films of the test pieces were placed facing each other, and then main sintering was performed under a mixed gas atmosphere of argon gas and oxygen gas at a heating temperature of 800° C. and a pressure of 100 MPa to crystallize the MOD pre-sintered film, thereby forming a joint made of a crystallized MOD layer to join two superconducting wires. In this way, a connection structure of superconducting wires was produced in which the part of the superconducting wire that constitutes the joint is thicker than the part of the superconducting wire that does not constitute the joint, and this was designated as Example 4 (not shown).

[0039] (Comparative Example) Two of the above test materials were prepared, and the MOD pre-sintered films of these were placed opposite each other and sintered in a mixed gas atmosphere of argon gas and oxygen gas at a heating temperature of 800°C and a pressure of 100 MPa to crystallize the MOD pre-sintered film and form a joint made of a crystallized MOD layer. In this way, a superconducting wire connection structure was produced in which the part of the superconducting wire constituting the joint and the part of the superconducting wire not constituting the joint had the same thickness in both of the above two superconducting wires, and this was used as a comparative example.

[0040] <Evaluation> In order to confirm the warpage reducing effect of Examples 1 to 4 and Comparative Example 1, the following tests were carried out to investigate and evaluate the degree of peelability. The results are shown in Table 3.

[0041] [Table 3]

[0042] From the results shown in Table 3, in all of Examples 1 to 4, the Hastelloy (registered trademark) substrate, the carbon steel substrate, or the superconducting wire is disposed on the superconducting wire that constitutes the joint, so that the portion of the superconducting wire that constitutes the joint is thicker than the portion of the superconducting wire that does not constitute the joint. Therefore, compared to the comparative example in which the portion of the superconducting wire that constitutes the joint and the portion of the superconducting wire that does not constitute the joint have the same thickness, the proportion of "no peeling" is significantly higher, and the proportions of "partial peeling" and "peeling" are lower, and it is clear that the effect of reducing warping is improved. In particular, in the connection structure in which the substrate made of the same material as the superconducting wire is disposed on the superconducting wire that constitutes both joints of the two superconducting wires included in the connection structure for the superconducting wire, the evaluation result of "no peeling" is obtained for all samples, and the effect of reducing warping is significantly improved. In addition, connection structures in which the superconducting wire constituting the connection part is provided with a metal other than the Hastelloy (registered trademark) substrate or the carbon steel substrate, such as various stainless steel substrates or various Inconel (registered trademark) substrates, or a substrate containing a ceramic material other than the superconducting wire, such as Al2O3, were also evaluated.Compared to the comparative examples, the proportion of "no peeling" was significantly higher and the proportions of "partial peeling" and "peeling" were lower, confirming an improvement in the effect of reducing warping.

[0043] As described above, when the high-temperature superconducting wire connection structure of the present invention is applied to high-temperature superconducting wire or a high-temperature superconducting coil formed using this high-temperature superconducting wire, even if repeated thermal deformation due to thermal expansion and contraction caused by a heat cycle or the like occurs, peeling of the superconducting layers constituting the two superconducting wires forming the joint can be effectively suppressed, and stable superconducting characteristics can be exhibited.

[0044] Although the embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments, and includes all aspects encompassed by the technical idea of ​​the present invention and the scope of the claims, and various modifications can be made within the scope of the present invention. [Explanation of symbols]

[0045] 1, 1a base material, first base material 2. Oxide superconducting layer 3, 30, 31 First superconducting wire 4, 40, 41 Second superconducting wire 5 Superconducting joint 6, 60, 61, 62 joints 7, 70, 71, 72 Part 1 8 Part 2 9 Base material, 2nd base material 10 metal layer 11 Protective layer 20 Ceramic Layer A Connection structure of the first embodiment B. Connection structure of second embodiment C. Third embodiment of connection structure D Fourth embodiment of connection structure

Claims

1. A band-shaped substrate made of a metal or alloy, and An oxide superconducting layer formed on the surface side of the substrate A first superconducting wire and a second superconducting wire are two high-temperature superconducting wires having the following characteristics: a joint including a superconducting joint formed between the first and second superconducting wires by joining the first and second superconducting wires together in a positional relationship in which surfaces of the first and second superconducting layers, which are the oxide superconducting layers of the first and second superconducting wires, face each other; A connection structure for high-temperature superconducting wires comprising: a first portion of a substrate of at least one of the first and second superconducting wires that constitutes the joint is thicker than a second portion of the substrate that does not constitute the joint; the substrate of the at least one superconducting wire is configured such that the first portion is composed of at least two substrates including a first substrate which is the substrate and a fragmentary second substrate located on a back surface side of the first substrate; The connection structure of a high temperature superconducting wire, further comprising a ceramic layer on a rear surface of the second substrate.

2. In the at least one superconducting wire, when the thermal expansion coefficient of the first substrate is α1, the thermal expansion coefficient of the second substrate is α2, and the thermal expansion coefficient of the oxide superconducting layer is α3, 2. The connection structure of high temperature superconducting wires according to claim 1, wherein the relationships α1>α3 and α2>α3 are satisfied.

3. The thermal expansion coefficient α1 of the first base material is 10.5×10 -6 3. The connection structure for high-temperature superconducting wires according to claim 1, wherein the temperature is 0.15 to 1.5° C. / K or more.

4. The connection structure of high-temperature superconducting wires according to any one of claims 1 to 3, further comprising a metal layer between the first substrate and the second substrate, the metal layer having a melting point higher than 800°C and being resistant to high-temperature oxidation.

5. 5. The connection structure of high temperature superconducting wires according to claim 4, wherein the metal layer is formed of at least one kind of noble metal or alloy selected from the group consisting of Ag, Au and Pt.

6. The connection structure of high temperature superconducting wires according to any one of claims 1 to 5, wherein the substrate of at least one of the superconducting wires has a thickness of the first portion of 60 μm or more and 100 μm or less, and a thickness of the second portion of 30 μm or more and 55 μm or less.

7. 7. The connection structure for high temperature superconducting wires according to claim 1, wherein the oxide superconducting layers of the first and second superconducting wires each have a thickness of 0.1 μm or more.

8. 8. The connection structure of high temperature superconducting wires according to claim 1, wherein the oxide superconducting layers of the first and second superconducting wires are both made of a REBCO-based superconducting material.

9. A high-temperature superconducting wire having the connection structure according to any one of claims 1 to 8.

10. A high-temperature superconducting coil formed by using the high-temperature superconducting wire according to claim 9.

11. a coating film forming step of applying an organometallic solution containing a metal that forms a superconducting joint to a surface portion of the oxide superconducting layer exposed by peeling off a part of each protective layer of a first and a second superconducting wire, the first and second superconducting wires having a band-shaped substrate made of a metal or an alloy, an oxide superconducting layer formed on a surface side of the substrate, and a protective layer formed on the surface of the oxide superconducting layer, and drying the solution to form a coating film; a pre-baking step of heating the coating film at a first temperature to form a pre-baked film; a firing step of contacting surfaces of the pre-fired films of the first and second superconducting wires on which the pre-fired films have been formed in a positional relationship opposite to each other and heating the wires at a second temperature higher than the first temperature to form a superconducting joint between the first and second superconducting wires, and forming a joint that joins the first and second superconducting wires by the superconducting joint; A method for forming a connection structure of high-temperature superconducting wires, comprising: At least before the firing step, a base material of at least one of the first and second superconducting wires is such that a first portion constituting the joint is thicker than a second portion not constituting the joint in the same base material, the substrate of the at least one superconducting wire is configured such that the first portion is composed of at least two substrates including a first substrate which is the substrate and a fragmentary second substrate located on a back surface side of the first substrate; The method for forming a connection structure of high temperature superconducting wires, wherein the connection structure further comprises a ceramic layer on a rear surface of the second substrate.

Citation Information

Patent Citations

  • Joint method of high temperature superconducting thin film wire and high temperature superconducting thin film wire

    JP2013235699A

  • Connection structure and connection method of oxide superconductive wire material, and oxide superconductive wire material using the connection structure

    JP2014130730A

  • Connection structure body for oxide superconducting wire material and method for manufacturing same

    WO2017038826A1

  • Connecting structure

    WO2018181561A1