Carbon black, slurry and lithium ion secondary battery
Carbon black with specific surface area and DBP/CDBP ratio optimization addresses conductivity and dispersion issues in lithium ion batteries, enhancing battery capacity and discharge performance.
Patent Information
- Application Number
- JP2022566979
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-04
- Filing Date
- 2021-12-02
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-02
AI Technical Summary
The aggregation of conductive agents like carbon black in lithium ion secondary battery electrodes leads to local conductivity issues, reducing discharge capacity and battery characteristics, especially when the blending ratio of conductive agents is decreased to increase active material content, resulting in higher viscosity and poor dispersion of the composite slurry.
Development of carbon black with a specific surface area of 150-400 m²/g, a DBP/CDBP ratio of 2.0 or less, and controlled ash and iron content, which allows for low viscosity slurry formation and improved dispersion, maintaining conductivity and preventing re-agglomeration.
The solution enables the production of lithium ion secondary batteries with enhanced capacity and discharge characteristics by ensuring uniform distribution of the conductive agent, reducing viscosity, and minimizing structural damage during slurry preparation.
Smart Images

Figure 0007568747000001 
Figure 0007568747000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon black, a slurry, and a lithium ion secondary battery. [Background technology]
[0002] Lithium-ion secondary batteries are widely used as power sources for small electronic devices such as smartphones and tablet computers. Lithium-ion secondary batteries are generally composed of electrodes, separators, and electrolyte. Electrodes are manufactured by coating and drying a composite slurry, in which active materials, conductive agents, binders, etc. are dispersed in a dispersion medium, on a metal plate for a current collector to form a composite layer.
[0003] The conductive agent may be, for example, carbon black (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-193986 A Summary of the Invention [Problem to be solved by the invention]
[0005] The role of the conductive agent is to form a conductive path within the electrode, so if the conductive agent aggregates within the electrode, localized areas of poor conductivity will appear, and the active material will not be used effectively, resulting in a decrease in discharge capacity and a deterioration in battery characteristics.
[0006] In recent years, there has been a demand for high capacity lithium ion secondary batteries, and there is a tendency to increase the mixing ratio of active material in the composite layer and decrease the mixing ratio of conductive agent and binder. If the mixing ratio of conductive agent decreases, it becomes difficult to form a conductive path in the electrode, and the battery characteristics deteriorate. Therefore, studies are being conducted to improve conductivity by using a conductive agent with a small particle size to increase the number of particles per unit mass, shorten the proximity distance between conductive agents in the electrode, and increase the contact points with the active material and the current collector. However, if the specific surface area increases with the reduction in particle size of the conductive agent, the viscosity of the composite slurry increases significantly, making it difficult to uniformly disperse the conductive agent.
[0007] Furthermore, when carbon black is used as a conductive agent, the structure of the carbon black affects the conductivity and slurry viscosity. Here, the carbon black structure refers to the structure in which the primary particles are connected. The carbon black structure develops into a complex entangled shape as the primary particles become smaller. When the structure develops, it is possible to efficiently form a conductive path within the electrode, but if the dispersion state is poor, this effect cannot be fully demonstrated.
[0008] In order to achieve high dispersion of the conductive agent and low viscosity of the composite slurry, methods such as dispersing by applying strong collision energy using equipment such as a high-pressure jet mill and extending the dispersion processing time have been considered, but these have problems such as impurities being mixed in due to wear of the equipment.Addition of a dispersant has also been considered, but there has been a problem that increasing the amount of dispersant added due to the small particle size of the conductive agent leads to a decrease in battery characteristics.
[0009] Therefore, an object of the present invention is to provide a novel carbon black that has a large specific surface area and is capable of forming a low-viscosity slurry, and to provide a slurry containing the carbon black and a lithium-ion secondary battery containing the carbon black. [Means for solving the problem]
[0010] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that in carbon black having a high specific surface area, the ratio of DBP absorption to compressed DBP absorption significantly affects the slurry viscosity.
[0011] That is, the present invention which solves the above problems is exemplified as follows. (1) Specific surface area is 150m 2 / g or more 400m 2 / g or less and having a ratio of DBP absorption (DBP) to compressed DBP absorption (CDBP) (DBP / CDBP) of 2.0 or less. (2) The carbon black according to (1), having a DBP absorption of 200 mL / 100 g or more and 350 mL / 100 g or less. (3) The carbon black according to (1) or (2), having an ash content of 0.02% by mass or less. (4) The carbon black according to any one of (1) to (3), having an iron content of less than 2,000 ppb by mass. (5) A slurry comprising the carbon black according to any one of (1) to (4) above and a dispersion medium. (6) Shear rate 10 s at 25°C -1 The slurry according to (5), having a viscosity of 200 mPa·s or more and 1200 mPa·s or less at 0.5° C. (7) A lithium ion secondary battery comprising a positive electrode, a negative electrode, and a separator, at least one of the positive electrode and the negative electrode containing the carbon black according to any one of (1) to (4). Effect of the Invention
[0012] The present invention provides a novel carbon black that has a large specific surface area and is capable of forming a low-viscosity slurry. The present invention also provides a slurry containing the carbon black, and a lithium-ion secondary battery containing the carbon black. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A preferred embodiment of the present invention will be described in detail below. The present invention is not limited to the embodiment described below. In this specification, unless otherwise specified, a numerical range indicated by "~" means a range "greater than or equal to" the numerical value on the left and "less than or equal to" the numerical value on the right. For example, "A~B" means A or more and B or less.
[0014] <Carbon black> The carbon black of this embodiment is 150 m 2 / g or more 400m 2 / g or less. This specific surface area is higher than that of carbon black, which has traditionally been used as a conductive agent in lithium-ion secondary batteries. Carbon black with such a high specific surface area is effective as a conductive agent because it has a high conductivity-imparting ability due to the percolation effect in the matrix.
[0015] The specific surface area is measured in accordance with JIS K6217-2:2017, Method A flow method (thermal conductivity measurement method).
[0016] The specific surface area of carbon black is 150m 2 When the specific surface area is less than 160 m / g, the number of contact points with the active material in the mixture layer is small, and sufficient electrical conductivity may not be exhibited. 2 / g or more, more preferably 180m 2 / g or more, more preferably 200m 2 That is, the specific surface area of the carbon black is, for example, 150 to 400 m 2 / g, 160-400m 2 / g, 180-400m 2 / g or 200~400m 2 / g. Also, the specific surface area of the carbon black may be 400 m 2When the specific surface area of carbon black exceeds 1 / g, it becomes extremely difficult to disperse the carbon black in the slurry, which may result in localized areas of poor electrical conductivity in the electrode and reduced battery performance. The specific surface area of carbon black can be increased by reducing the size of the primary particles, making the particles hollow, or making the particle surfaces porous.
[0017] In the carbon black of this embodiment, the ratio of DBP absorption (DBP) to compressed DBP absorption (CDBP) (DBP / CDBP) is 2.0 or less.
[0018] DBP absorption (DBP) is an index for evaluating the ability of carbon black to absorb dibutyl phthalate into the voids formed by the particle surface and structure. In this specification, DBP absorption refers to a value measured according to the method described in JIS K6221 Method B and converted into a value equivalent to JIS K6217-4:2008 by the following formula (a). DBP absorption amount = (A-10.974) / 0.7833 …(a) [In the formula, A represents the value of DBP absorption measured by the method described in JIS K6221.] In measuring DBP absorption (DBP), a strong external force is applied to break down carbon black agglomerates (secondary aggregations of the structure), and the surface area of the primary particles and the degree of structure development are evaluated.
[0019] Compressed DBP absorption (CDBP) is the DBP absorption measured after compressing carbon black in advance to destroy the structure, and is an index of the mechanical strength of the structure. It can be measured according to JIS K6217-4:2008, specifically, a sample is set in a hydraulic cylinder, compressed at 165 MPa for 1 second, removed, and sieved until the sample mass is 0.25 cm or less. This series of operations is repeated four times, and then the DBP absorption is measured to obtain the compressed DBP absorption (CDBP).
[0020] As a result of intensive research to solve the above problems, the present inventors have found that in carbon black having a high specific surface area, the ratio of DBP absorption to compressed DBP absorption (DBP / CDBP) has a large effect on the slurry viscosity. That is, the carbon black of the present embodiment can achieve a sufficiently low slurry viscosity while having a high specific surface area by having a ratio (DBP / CDBP) of 2.0 or less.
[0021] The shape and strength of the structure of carbon black varies greatly depending on factors such as the thermal history during synthesis (e.g., thermal history due to the thermal decomposition and combustion reaction of fuel oil, the thermal decomposition and combustion reaction of raw materials, rapid cooling and reaction cessation by a cooling medium, etc.), and the collision frequency of primary particles.
[0022] According to the findings of the present inventors, when comparing carbon blacks having the same specific surface area, carbon blacks having a ratio (DBP / CDBP) of 2.0 or less have a lower slurry viscosity than carbon blacks having a ratio (DBP / CDBP) of more than 2.0. Here, a low ratio (DBP / CDBP) means that the structure is less likely to be destroyed by an external force. The carbon black of this embodiment is less likely to have its structure destroyed by an external force during slurry preparation, so that less highly active surface is newly generated by the destruction, making it difficult for re-aggregation of carbon black to occur, resulting in a lower slurry viscosity.
[0023] In this embodiment, by making the ratio (DBP / CDBP) 2.0 or less, even if the carbon black has a small particle size, a large specific surface area, and a well-developed structure, it is possible to reduce uneven coating on the current collector caused by an increase in the viscosity of the composite slurry and uneven distribution of the material in the electrode. In addition, by improving the dispersion and contact state of the active material and the conductive agent in the electrode, it is possible to achieve a high capacity lithium-ion secondary battery while suppressing a local decrease in conductivity and a decrease in the discharge capacity of the battery.
[0024] In the carbon black of the present embodiment, the ratio (DBP / CDBP) is preferably 1.9 or less, more preferably 1.8 or less, and even more preferably 1.7 or less, from the viewpoint of more significantly achieving the above-mentioned effects.
[0025] In the carbon black of this embodiment, if the ratio (DBP / CDBP) is too small, the mechanical strength of the structure is too high, or the structure has a shape that is difficult to destroy, so that the viscosity of the slurry may increase due to excessive development of agglomerates during slurry preparation. From the viewpoint of suppressing the excessive development of the agglomerates, the ratio (DBP / CDBP) is preferably 1.0 or more, more preferably 1.1 or more, even more preferably 1.2 or more, even more preferably 1.3 or more, and particularly preferably 1.4 or more. That is, the ratio (DBP / CDBP) may be, for example, 1.0 to 2.0, 1.0 to 1.9, 1.0 to 1.8, 1.0 to 1.7, 1.1 to 2.0, 1.1 to 1.9, 1.1 to 1.8, 1.1 to 1.7, 1.2 to 2.0, 1.2 to 1.9, 1.2 to 1.8, 1.2 to 1.7, 1.3 to 2.0, 1.3 to 1.9, 1.3 to 1.8, 1.3 to 1.7, 1.4 to 2.0, 1.4 to 1.9, 1.4 to 1.8, or 1.4 to 1.7.
[0026] The DBP absorption of the carbon black of this embodiment may be, for example, 180 mL / 100 g or more, preferably 190 mL / 100 g or more, more preferably 200 mL / 100 g or more. The DBP absorption of the carbon black of this embodiment is, for example, 370 mL / 100 g or less, more preferably 350 mL / 100 g or less. That is, the DBP absorption of the carbon black of this embodiment may be, for example, 180 to 370 mL / 100 g, 180 to 350 mL / 100 g, 190 to 370 mL / 100 g, 190 to 350 mL / 100 g, 200 to 370 mL / 100 g, or 200 to 350 mL / 100 g.
[0027] Carbon black with a well-developed structure has a large amount of DBP absorption due to the large number of necks formed by the fusion of primary particles and the large number of voids formed between particles. If the DBP absorption is too low, the structure may not be fully developed, resulting in low conductivity in the electrode. Also, the battery may not be able to buffer the volume change of the active material that accompanies the charge and discharge of a lithium-ion secondary battery, resulting in a decrease in battery characteristics such as cycle characteristics. If the DBP absorption is too high, the binder in the composite layer may be trapped in the carbon black structure, reducing adhesion to the active material and current collector, resulting in a decrease in battery characteristics.
[0028] The average primary particle size of the carbon black of this embodiment may be, for example, less than 35 nm, preferably less than 30 nm, and more preferably less than 25 nm. According to the findings of the present inventors, when two types of carbon black that satisfy the above-mentioned ratio (DBP / CDBP) are compared, which have the same specific surface area but different average primary particle size, the smaller particle size carbon black has a lower slurry viscosity. This is because the larger particle size carbon black has a higher specific surface area due to the porous surface, while the smaller particle size carbon black has a relatively smooth surface and achieves a high specific surface area by forming a complex structure, and the above-mentioned effect due to the structure strength represented by the ratio (DBP / CDBP) is more pronounced.
[0029] Conventionally, it was difficult to make a slurry of carbon black used as a conductive agent for lithium ion secondary batteries when the average primary particle diameter was small (for example, less than 30 nm). However, the carbon black of the present embodiment satisfies the above-mentioned ratio (DBP / CDBP), so that it can be made into a slurry even when the average primary particle diameter is small (for example, less than 30 nm). By making it possible to use carbon black with a small particle size in this way, high conductivity can be exhibited even if the blending ratio in the composite layer is low. The average primary particle diameter of carbon black may be, for example, 1 nm or more and less than 5 nm, or 10 nm or more. That is, the average primary particle diameter of carbon black may be, for example, 1 nm or more and less than 35 nm, 1 nm or more and less than 30 nm, 1 nm or more and less than 25 nm, 5 nm or more and less than 35 nm, 5 nm or more and less than 30 nm, 5 nm or more and less than 25 nm, 10 nm or more and less than 35 nm, 10 nm or more and less than 30 nm, or 10 nm or more and less than 25 nm.
[0030] The average primary particle size of carbon black can be determined by measuring the primary particle sizes of 100 or more carbon black particles randomly selected from a 50,000-times magnified image of a transmission electron microscope (TEM) and calculating the average value. Primary particles of carbon black have a small aspect ratio and are close to a sphere, but are not completely spherical. Therefore, in this embodiment, the maximum line segment connecting two outer peripheries of a primary particle in a TEM image is taken as the primary particle size of carbon black.
[0031] The ash content of the carbon black of this embodiment may be, for example, 0.05% by mass or less, preferably 0.03% by mass or less, and more preferably 0.02% by mass or less. The ash content can be measured according to JIS K1469:2003, and can be reduced, for example, by classifying the carbon black with a device such as a dry cyclone.
[0032] The iron content of the carbon black of this embodiment may be, for example, less than 2500 ppb by mass, preferably less than 2300 ppb by mass, and more preferably less than 2000 ppb by mass. The iron content can be reduced, for example, by contacting the carbon black with a magnet.
[0033] The iron content of carbon black can be measured by high-frequency inductively coupled plasma mass spectrometry after pretreatment by acid decomposition according to JIS K0116:2014. Specifically, it can be measured by the following method. First, 1 g of carbon black is precisely weighed into a quartz beaker and heated at 800°C for 3 hours in an electric furnace in an air atmosphere. Next, 10 mL of mixed acid (70% by mass hydrochloric acid, 30% by mass nitric acid) and 10 mL or more of ultrapure water are added to the residue and heated and dissolved at 200°C for 1 hour on a hot plate. After cooling, the solution is diluted and adjusted to 25 mL with ultrapure water and measured with a high-frequency inductively coupled plasma mass spectrometry device (Agilent 8800, manufactured by Agilent).
[0034] When the carbon black of the present embodiment has a low ash and iron content, it is possible to more significantly suppress the inclusion of foreign matter such as metals and ceramics due to damage to equipment during the kneading process. It is also possible to suppress a decrease in electrical conductivity in the electrode due to the inclusion of ash, insulating foreign matter, etc. Therefore, the carbon black of the present embodiment, which has a low ash and iron content, can be suitably used in lithium ion secondary batteries, which require high safety.
[0035] The method for producing carbon black in this embodiment is not particularly limited, and for example, a raw material such as a hydrocarbon is supplied from a nozzle installed upstream of a reactor, carbon black is produced by a pyrolysis reaction and / or a combustion reaction, and carbon black is collected by a bag filter directly connected to the downstream of the reactor.
[0036] The raw material used is not particularly limited, and gaseous hydrocarbons such as acetylene, methane, ethane, propane, ethylene, propylene, and butadiene, and oily hydrocarbons such as toluene, benzene, xylene, gasoline, kerosene, light oil, and heavy oil can be used. Among them, it is preferable to use acetylene, which has a small amount of impurities. Since acetylene has a larger heat of decomposition than other raw materials and can raise the temperature inside the reactor, the nucleation of carbon black becomes dominant over particle growth by addition reaction, and the primary particle size of carbon black can be reduced. Furthermore, the present inventors have conducted extensive research to control the structure strength of carbon black and have found that it is effective to use multiple raw materials and to heat the raw materials before supplying them to the reactor. In the conventional manufacturing method, carbon black produced through the high temperature part of the reactor and carbon black produced through the low temperature part were mixed, and the characteristics were widely varied. However, by using multiple raw materials, the temperature in the reactor becomes uniform, and the reaction history of the pyrolysis and combustion is also uniform, so the strength of the carbon black structure becomes uniform and destruction from weak parts is reduced. In addition, it is considered that the mixing of multiple raw materials is promoted by heating the raw materials, and a more uniform temperature field can be formed. It is preferable to mix multiple raw materials before supplying them to the reactor. When oily hydrocarbons are used, it is preferable to gasify them by heating and supply them. The heating method is not particularly limited, and for example, a tank or a transport pipe can be heated by heat exchange with a heat medium.
[0037] In addition, it is preferable to supply oxygen, hydrogen, nitrogen, steam, etc. to the reactor in addition to the raw material that serves as the carbon source. These gases other than the raw material promote gas agitation in the reactor and increase the frequency of collision and fusion between primary particles of carbon black generated from the raw material, so the structure of carbon black tends to develop and the DBP absorption amount tends to increase by using a gas other than the raw material. It is preferable to use oxygen as the gas other than the raw material. When oxygen is used, a part of the raw material is burned, the temperature in the reactor increases, and carbon black with a small particle size and a high specific surface area is easily obtained. Multiple gases can also be used as the gas other than the raw material. The supply point of the gas other than the raw material is preferably the upstream part of the reactor, and it is preferable to supply it from a nozzle different from the raw material. This makes it possible to efficiently agitate the raw material supplied from the upstream part, making it easier to develop the structure.
[0038] In conventional carbon black production, a cooling medium such as water may be introduced from the downstream of the reactor to stop the thermal decomposition and combustion reaction of the raw material. However, this has no effect on the development of the structure, and there is a risk that a sudden change in temperature will increase the variation in structure strength, resulting in a low ratio (DBP / CDBP). Therefore, in this embodiment, it is preferable not to introduce a cooling medium from the downstream of the reactor.
[0039] <Slurry> The slurry of the present embodiment contains the carbon black of the present embodiment and a dispersion medium.
[0040] If the viscosity of the slurry is too high, strong shear is applied during kneading with the active material, which may destroy the structure of the carbon black, resulting in a decrease in conductivity, or may cause contamination with foreign matter due to wear of the device. On the other hand, if the viscosity of the slurry is too low, the carbon black may be more likely to settle in the slurry, making it difficult to maintain uniformity. In this embodiment, the viscosity of the slurry can be reduced due to the use of the above-mentioned carbon black, so that the destruction of the structure of the carbon black is significantly suppressed, excellent conductivity-imparting ability can be maintained, and contamination with foreign matter due to wear of the equipment is significantly suppressed. That is, in this embodiment, the compounding ratio of the active material in the mixture layer can be increased without impairing the viscosity characteristics and conductivity of the slurry, and a high capacity of the lithium ion secondary battery can be achieved.
[0041] In order to obtain the above effects more significantly, the viscosity of the slurry (25°C, shear rate 10 s -1 ) is preferably 100 mPa·s or more, more preferably 200 mPa·s or more. This suppresses the settling of the carbon black and improves the uniformity of the slurry. From the viewpoint of obtaining the above-mentioned effect more significantly, the slurry viscosity (at 25°C and a shear rate of 10 s -1 ) is preferably 1500 mPa·s or less, more preferably 1200 mPa·s or less. That is, the viscosity of the slurry (at 25°C and a shear rate of 10 s -1 ) may be, for example, 100 to 1500 Pa·s, 100 to 1200 Pa·s, 200 to 1500 Pa·s, or 200 to 1200 Pa·s.
[0042] The dispersion medium is not particularly limited, and for example, N-methyl-2-pyrrolidone, ethanol, ethyl acetate, etc. can be used.
[0043] The slurry of the present embodiment may further contain other carbon black, graphite, carbon nanotubes, carbon nanofibers, and the like, as long as the electrical conductivity imparting ability and dispersibility of the carbon black of the present embodiment are not impaired.
[0044] The slurry of the present embodiment may further contain an active material and additives such as a dispersant.
[0045] In the slurry of this embodiment, the content of the carbon black of this embodiment may be, for example, 0.5% by mass or more, and preferably 1% by mass or more. In addition, in the slurry of this embodiment, the content of the carbon black of this embodiment may be, for example, 50% by mass or less, and preferably 20% by mass or less. That is, in the slurry of this embodiment, the content of the carbon black of this embodiment may be, for example, 0.5 to 50% by mass, 0.5 to 20% by mass, 1 to 50% by mass, or 1 to 20% by mass.
[0046] The method for producing the slurry of the present embodiment is not particularly limited, and the slurry can be produced by kneading the components using, for example, a general device such as a mixer, a kneader, a disperser, a mill, or an automatic orbital rotating device.
[0047] The slurry of the present embodiment can be suitably used as an electrode forming slurry for forming an electrode of a lithium ion secondary battery. The electrode forming slurry may be a positive electrode forming slurry or a negative electrode forming slurry.
[0048] When the slurry of the present embodiment is an electrode-forming slurry, the slurry of the present embodiment may contain an active material, a conductive agent, and a dispersion medium, and in this case, the slurry contains the carbon black of the present embodiment as the conductive agent.
[0049] The content of the conductive agent in the electrode-forming slurry may be, for example, 0.01% by mass or more, preferably 0.05% by mass or more, and more preferably 0.08% by mass or more. The content of the conductive agent in the electrode-forming slurry may be, for example, 20% by mass or less, preferably 15% by mass or less, and more preferably 10% by mass or less. That is, the content of the conductive agent in the electrode-forming slurry may be, for example, 0.01 to 20% by mass, 0.01 to 15% by mass, 0.01 to 10% by mass, 0.05 to 20% by mass, 0.05 to 15% by mass, 0.05 to 10% by mass, 0.08 to 20% by mass, 0.08 to 15% by mass, or 0.08 to 10% by mass.
[0050] The electrode-forming slurry may further contain a conductive agent other than carbon black, such as graphite, carbon nanotubes, and carbon nanofibers.
[0051] In the electrode-forming slurry, the proportion of carbon black in the conductive agent may be, for example, 50% by mass or more, preferably 70% by mass or more, more preferably 90% by mass or more, and may be 100% by mass.
[0052] The active material is not particularly limited, and known active materials used in lithium ion secondary batteries can be used without particular limitation. Examples of the positive electrode active material include lithium cobalt oxide, lithium nickel oxide, lithium manganate, lithium nickel-manganese-cobalt oxide, and lithium iron phosphate. Examples of the negative electrode active material include carbonaceous materials such as natural graphite, artificial graphite, graphite, activated carbon, coke, needle coke, fluid coke, mesophase microbeads, carbon fiber, and pyrolytic carbon.
[0053] The electrode forming slurry may further contain a binder. The binder is not particularly limited, and any known binder used in lithium ion secondary batteries can be used without particular limitation. Examples of binders include polyethylene, nitrile rubber, polybutadiene, butyl rubber, polystyrene, styrene-butadiene rubber, polysulfide rubber, nitrocellulose, carboxymethylcellulose, polyvinyl alcohol, tetrafluoroethylene resin, polyvinylidene fluoride, and polychloroprene fluoride.
[0054] The method for forming an electrode using the electrode-forming slurry is not particularly limited. For example, the electrode-forming slurry can be applied onto a current collector and dried to form an electrode including a current collector and a mixture layer.
[0055] The current collector is not particularly limited, and may be, for example, a metal foil of gold, silver, copper, platinum, aluminum, iron, nickel, chromium, manganese, lead, tungsten, titanium, or an alloy mainly composed of these metals. For example, aluminum foil is preferably used as the positive electrode current collector, and copper foil is preferably used as the negative electrode current collector.
[0056] <Lithium-ion secondary battery> The lithium ion secondary battery of this embodiment includes a positive electrode, a negative electrode, and a separator. In addition, at least one of the positive electrode and the negative electrode of the lithium ion secondary battery of this embodiment contains the carbon black of this embodiment. In the lithium ion secondary battery of this embodiment, at least one of the positive electrode and the negative electrode may be formed from the above-mentioned electrode forming slurry, and at least one of the positive electrode and the negative electrode may include a composite layer formed on a current collector by the above-mentioned electrode forming slurry.
[0057] The lithium ion secondary battery of this embodiment has a high capacity because of the use of the carbon black of this embodiment, and can be produced with good productivity by using the above-mentioned electrode forming slurry.
[0058] In the lithium ion secondary battery of the present embodiment, the positive electrode preferably contains the carbon black of the present embodiment. In addition, in the lithium ion secondary battery of the present embodiment, the positive electrode is preferably formed from the above-mentioned electrode-forming slurry, and more preferably includes a composite layer formed on a current collector by the above-mentioned electrode-forming slurry.
[0059] In the lithium ion secondary battery of this embodiment, the configuration other than the electrode containing the carbon black of this embodiment may be the same as that of a known lithium ion secondary battery.
[0060] The separator is not particularly limited, and any separator known as a separator for lithium ion secondary batteries can be used without particular limitation. Examples of the separator include synthetic resins such as polyethylene and polypropylene. The separator is preferably a porous film because it has good electrolyte retention.
[0061] The lithium ion secondary battery of this embodiment may include an electrode group in which a positive electrode and a negative electrode are stacked or wound with a separator interposed therebetween.
[0062] In the lithium ion secondary battery of the present embodiment, the positive electrode, the negative electrode, and the separator may be immersed in the electrolyte.
[0063] The electrolyte is not particularly limited, and may be, for example, a non-aqueous electrolyte containing a lithium salt. Examples of the non-aqueous solvent in the non-aqueous electrolyte containing a lithium salt include ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, methyl ethyl carbonate, etc. Examples of the lithium salt that can be dissolved in the non-aqueous solvent include lithium hexafluorophosphate, lithium borotetrafluoride, and lithium trifluoromethanesulfonate, etc.
[0064] The lithium ion secondary battery of this embodiment may use an ion conductive polymer or the like as an electrolyte.
[0065] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments.
[0066] For example, one aspect of the present invention is a method for producing a ferroelectric material having a specific surface area of 150 m 2 / g or more 400m 2 The evaluation method may include a measuring step of determining a ratio (DBP / CDBP) of DBP absorption (DBP) to compressed DBP absorption (CDBP), and an evaluation step of evaluating the carbon black based on the ratio (DBP / CDBP).
[0067] The evaluation step may be a selection step of selecting carbon black having a ratio (DBP / CDBP) of 2.0 or less. In this case, the evaluation method can also be said to be a method of selecting carbon black. EXAMPLES
[0068] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0069] Example 1 <Manufacture of Carbon Black> The raw material, acetylene, was pumped at 12 Nm from a nozzle installed upstream of the carbon black reactor (furnace length 6 m, furnace diameter 0.65 m). 3 / h, toluene at 32 kg / h, and oxygen at 20 Nm3 as a non-raw gas. 3 / h to produce carbon black, which was then collected in a bag filter installed downstream of the reactor. The carbon black was then passed through a dry cyclone device and a magnet for removing iron, before being collected in a tank. Note that acetylene, toluene, and oxygen were heated to 115°C before being supplied to the reactor. The following physical properties were measured for the carbon black obtained. The evaluation results are shown in Table 1.
[0070] (1) Specific surface area Measurements were taken according to JIS K6217-2:2017, Method A flow method (thermal conductivity measurement method). (2) DBP absorption: The value measured according to the method described in JIS K6221, Method B was converted to a value equivalent to JIS K6217-4:2008 using the above formula (a). (3) Compressed DBP absorption (CDBP): Samples were prepared according to JIS K6217-4:2008 Appendix A (method of preparing compressed samples, using compression apparatus type I) and measured according to JIS K6217-4:2008. (4) Average primary particle diameter: The primary particle diameters of 100 or more randomly selected carbon black particles were measured from a 50,000-times magnified image taken with a transmission electron microscope, and the average value was calculated. (5) Ash content: Measured in accordance with JIS K1469:2003. (6) Iron content: The iron content was measured by high-frequency inductively coupled plasma mass spectrometry after pretreatment by acid decomposition in accordance with JIS K0116:2014.
[0071] <Preparation of slurry> 3 parts by mass of carbon black and 97 parts by mass of N-methyl-2-pyrrolidone (Kanto Chemical Co., Ltd.) as a dispersion medium were kneaded for 30 minutes at 2000 rpm in a planetary centrifugal mixer (Thinky Corporation's "Awatori Rentaro ARV-310") to prepare a carbon black slurry. The viscosity of this slurry at 25°C was evaluated using a viscoelasticity measuring device (Anton Paar's "MCR102", using a cone plate with a diameter of 30 mm and an angle of 3°, and a gap of 1 mm). The shear rate was 0.01 s -1 From 100s -1 The shear rate was changed to 10 s -1 The viscosity was measured at 100° C. The measurement results are shown in Table 2.
[0072] <Battery Construction> Carbon black slurry 40 parts by mass (carbon black 1.2 parts by mass, N-methyl-2-pyrrolidone 38.8 parts by mass), LiNi as a positive electrode active material 0.5 Mn 0.3 Co 0.296.8 parts by mass of O2 ("TX10" manufactured by Umicore), 2 parts by mass of polyvinylidene fluoride ("HSV900" manufactured by Arkema) as a binder, 0.1 parts by mass of polyvinyl alcohol ("B05" manufactured by Denka) as a dispersant, and 10 parts by mass of N-methyl-2-pyrrolidone (manufactured by Kanto Chemical Co., Ltd.) as a dispersion medium were kneaded for 10 minutes at a rotation-revolution type mixer ("Awatori Rentaro ARV-310" manufactured by Thinky Corporation) rotation speed of 2000 rpm to prepare a positive electrode forming composite material slurry. The obtained positive electrode forming composite material slurry was applied to an aluminum foil (manufactured by UACJ) having a thickness of 15 μm with an applicator and pre-dried at 105 ° C for 1 hour. Next, it was pressed with a roll press machine at a linear pressure of 200 kg / cm, and the sum of the thicknesses of the aluminum foil and the coating film was adjusted to 80 μm. In order to remove volatile components, the positive electrode was prepared by vacuum drying at 170°C for 3 hours.
[0073] 97 parts by mass of artificial graphite (Hitachi Chemical Co., Ltd. "MAG-D") as a negative electrode active material, 2 parts by mass of styrene butadiene rubber (Nippon Zeon Co., Ltd. "BM-400B") as a binder, and 1 part by mass of carboxymethyl cellulose (Daicel Co., Ltd. "D2200") as a dispersant were weighed, and pure water was added and mixed using a rotating and revolving mixer (Thinky Corporation, Awatori Rentaro ARV-310) to prepare a negative electrode forming composite slurry. The obtained negative electrode forming composite slurry was applied to a copper foil (UACJ Corporation) with a thickness of 10 μm with an applicator and pre-dried at 60 ° C for 1 hour. Next, it was pressed with a roll press machine at a linear pressure of 100 kg / cm, and the sum of the thickness of the copper foil and the coating film was adjusted to 40 μm. In order to completely remove moisture, it was vacuum dried at 120 ° C for 3 hours to prepare a negative electrode.
[0074] The positive electrode was processed to 40 × 40 mm, and the negative electrode was processed to 44 × 44 mm, and a polyolefin microporous membrane was placed between the two electrodes as a separator to prepare a battery. The electrolyte used was a solution in which ethylene carbonate (manufactured by Aldrich) / dimethyl carbonate (manufactured by Aldrich) was mixed in a volume ratio of 1 / 1 and 1 mol / L of lithium hexafluorophosphate (manufactured by Stella Chemifa Corporation) was dissolved.
[0075] As a battery discharge test, the prepared battery was charged at 25°C at a constant current and constant voltage of 4.35V and limited to 0.2C, and then discharged to 3.0V at a constant current of 0.2C. Next, the discharge current was changed to 0.2C, 0.5C, 1C, 2C, and 3C, and the discharge capacity for each discharge current was measured. The capacity retention rate at 3C discharge relative to 0.2C discharge was calculated and evaluated as the discharge rate characteristic. In addition, the prepared battery was charged at 25°C at a constant current and constant voltage of 4.35V and limited to 1C, and then discharged to 3.0V at a constant current of 1C. Next, the above charge and discharge were repeated 500 cycles, and the discharge capacity was measured. The capacity retention rate at 500 cycles discharge relative to 1 cycle discharge was calculated and evaluated as the cycle characteristic. The measurement results are shown in Table 2.
[0076] (Examples 2 to 4) Oxygen supply: 21Nm 3 / h (Example 2), 22 Nm 3 / h (Example 3) or 24 Nm 3 / h (Example 4), carbon black was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0077] Example 5 The temperature of toluene was changed to 100°C, and the amount of oxygen supplied was increased to 21 Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0078] Example 6 The temperature of acetylene was changed to 85°C, the temperature of toluene was changed to 100°C, and the amount of oxygen was increased to 21 Nm 3Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0079] Example 7 The temperature of acetylene was changed to 85°C, the temperature of toluene was changed to 85°C, and the oxygen supply was increased to 21 Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0080] Example 8 Acetylene supply volume 11Nm 3 / h, toluene supply rate of 30 kg / h, oxygen supply rate of 19 Nm 3 / h, respectively, carbon black was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0081] Example 9 Acetylene supply volume is 13Nm 3 / h, toluene supply rate 35kg / h, oxygen supply rate 26Nm 3 / h, respectively, carbon black was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0082] Example 10 12Nm instead of acetylene 3 / h ethylene was heated to 115°C and supplied, and the amount of oxygen supplied was 22 Nm 3Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0083] Example 11 Instead of toluene, 32 kg / h of benzene was heated to 115°C and supplied, and the amount of oxygen supplied was 21 Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0084] Comparative Example 1 21Nm instead of oxygen 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that 100 / h of hydrogen was heated to 115°C and supplied. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0085] Comparative Example 2 Acetylene supply volume 11Nm 3 / h, toluene supply rate 30kg / h, oxygen supply rate 24Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0086] Example 12 The carbon black obtained in Comparative Example 1 was subjected to an oxidation treatment in an electric furnace heated to 720°C to obtain carbon black. The obtained carbon black was evaluated in the same manner as in Example 1. The results are shown in Table 1. In addition, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0087] (Example 13) Oxygen supply: 21Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the flow rate was changed to 100 / h and the classification conditions of the dry cyclone device were changed to adjust the ash content. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0088] Example 14 Oxygen supply: 21Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the heating rate was changed to 100 / h and the magnetic flux density conditions of the iron-removing magnet were changed to adjust the iron content. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0089] Comparative Example 3 Acetylene supply volume 38Nm 3 / h, toluene was not supplied, and the oxygen supply was changed to 10 Nm 3 Carbon black was produced and evaluated in the same manner as in Example 1, except that the carbon black was changed to 0.1% by weight per 1000 g / h. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0090] Comparative Example 4 Oxygen supply: 22Nm 3 / h, and the temperatures when acetylene was supplied, when toluene was supplied, and when oxygen was supplied were all changed to 25° C. Carbon black was produced and evaluated in the same manner as in Example 1. The results are shown in Table 1. Furthermore, using the obtained carbon black, a slurry and a battery were prepared and evaluated in the same manner as in Example 1. The results are shown in Table 2.
[0091] [Table 1]
[0092] [Table 2]
[0093] As shown in Table 1, when the carbon black of the examples was used, excellent slurry viscosity characteristics and excellent battery characteristics were achieved, and it was confirmed that the carbon black of the present invention can be used to produce high-performance lithium-ion secondary batteries with good productivity. [Industrial Applicability]
[0094] The carbon black of the present invention can be suitably used in slurries for lithium ion secondary battery electrodes and in lithium ion secondary batteries.
Claims
1. Specific surface area is 150m 2 / g or more 400m 2 / g or less, DBP absorption is 180 mL / 100 g or more; a ratio of DBP absorption (DBP) to compressed DBP absorption (CDBP) (DBP / CDBP) of 1.4 or greater and 2.0 or less; Carbon black having an average primary particle size of less than 25 nm.
2. 2. The carbon black according to claim 1, which has a DBP absorption of 200 mL / 100 g or more and 350 mL / 100 g or less.
3. 3. The carbon black according to claim 1 or 2, having an ash content of 0.02 mass% or less.
4. The carbon black according to any one of claims 1 to 3, having an iron content of less than 2,000 ppb by mass.
5. A slurry comprising the carbon black according to any one of claims 1 to 4 and a dispersion medium.
6. Shear rate 10 s at 25°C -1 The slurry according to claim 5, having a viscosity of 200 mPa·s or more and 1200 mPa·s or less at 0.5° C.
7. A positive electrode, a negative electrode, and a separator are provided, A lithium ion secondary battery, wherein at least one of the positive electrode and the negative electrode contains the carbon black according to any one of claims 1 to 4.
Citation Information
Patent Citations
Improved performance carbon black
JP1994500138A
High-structure carbon black and method for producing the same
JP2002121422A
Conductive thermoplastic resin composition and IC tray
JP2006213767A
Carbon black dispersion and use thereof
JP2014193986A
Carbon black
JP2014221889A