Method for producing carbon material granules

By preparing carbon black and nanotube particles to precise sizes and using specific granulators, the method addresses scattering issues in carbon material granule production, enabling efficient continuous granulation and improved properties.

WO2024228385A1PCT designated stage expired Publication Date: 2024-11-07DR GOO

Patent Information

Application Number
PCT/JP2024/016739
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2024-04-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing methods for producing carbon material granules are inefficient due to scattering issues during granulation, which complicates the continuous production process and poses safety concerns, limiting production efficiency.

Method used

The method involves preparing carbon black and carbon nanotube particles to specific sizes, using a solvent-soluble polymer binder, and employing an extrusion or shear crushing granulator to achieve continuous granulation, reducing scattering and improving mixing efficiency.

Benefits of technology

This approach enables the production of carbon material granules with enhanced conductivity and mechanical properties while allowing for continuous granulation, significantly improving production efficiency compared to batch methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016739_07112024_PF_FP_ABST
    Figure JP2024016739_07112024_PF_FP_ABST
Patent Text Reader

Abstract

A method for producing carbon material granules comprising: a step in which carbon black particles and carbon nanotube particles are pulverized so that the carbon black comes to have a particle diameter, as determined by the method described in JIS K-6219-4, of 500 μm or less and the carbon nanotubes come to have a particle diameter, as determined by the method described in JIS K-6219-4, of 500 μm or less, and are mixed to obtain a mixture; a step in which a solvent-soluble polymer is dissolved in a solvent to prepare a binder solution; a step in which the mixture is mixed with the binder solution to obtain a wet mixture; and a step in which the wet mixture is granulated to obtain carbon material granules.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing carbon material granules

[0001] The present invention relates to a method for producing carbon material granules.

[0002] Various studies have been conducted in recent years on imparting electrical conductivity or antistatic properties to resin compositions. For example, trays or carrier tapes molded from thermoplastic resins are known as packaging materials for electronic components using ICs or LSIs. However, typical resin molded products lack electrical conductivity and have high surface and volume resistivity. This can lead to problems such as insulation breakdown of electronic components due to static electricity or performance degradation due to dust adhesion. To prevent this, various types of materials have been added to solve the problem. In particular, many studies have been conducted on imparting antistatic properties or static electricity dissipation properties by blending carbon black (hereinafter sometimes referred to as CB) or carbon nanotubes (hereinafter sometimes referred to as CNT).

[0003] An example of a granulated mixture of CB and CNT is a method for producing carbon granules (see Patent Document 1), which includes a CNT dispersion step of dispersing CNTs with a particle size of 100 nm or less in water, a granulation step of mixing the CNT dispersion obtained in the CNT dispersion step with CB powder in a disperser and granulating the mixture, and a drying step of drying the carbon granules obtained in the granulation step. Another method for producing carbon granules (see Patent Document 2), which includes a step of dry-grinding and mixing carbon black granules and carbon nanotube granules to satisfy predetermined conditions to obtain a mixture, a step of dissolving a specific solvent-soluble polymer in a solvent to prepare a binder solution, and a step of adding a predetermined amount of the binder solution to the mixture, mixing, and granulating the mixture to obtain carbon granules. There is also a method for producing a carbon nanotube-blended aggregate (see Patent Document 3) that includes the following steps for producing a granulated product of CNTs alone: ​​(1) preparing an aqueous solution of a water-soluble polymer having a concentration of 0.005 to 3.0% by mass; (2) preparing a wet aggregate by impregnating carbon nanotubes with the aqueous solution of the water-soluble polymer in a ratio of 400 to 1,000 parts by mass per 100 parts by mass of carbon nanotubes; (3) shearing and crushing the wet aggregate to obtain a crushed aggregate; and (4) drying the crushed aggregate to obtain a carbon nanotube-blended aggregate containing the water-soluble polymer.

[0004] JP 2017-201006 A Japanese Patent No. 7126666 A Japanese Patent No. 6714134 A

[0005] The methods for producing carbon material granules described in Patent Document 1 and Patent Document 2 produce carbon material granules that can reduce scattering and improve electrical conductivity and mechanical properties. These patent documents describe granulation methods using either continuous or batch processes. The continuous process uses a twin-screw pin mixer. This granulator introduces CB and CNT into the upstream section of a twin-screw rotating at 500 to 3,000 rpm, and then adds a binder solution through an inlet downstream, mixing the materials for granulation. However, CB and CNT fly off in a cloud from areas where the CB and CNT are not fully wetted with the binder solution, the base of the shaft rotating at high speed, and the carbon material inlet. This has proven undesirable for granulation using these raw materials from an environmental or human safety perspective. Therefore, these methods for producing carbon material granules use a batch process during the granulation process, leaving room for improvement in terms of production efficiency.

[0006] An object of the present invention is to provide a method for producing carbon material granules that allows continuous granulation and improves production efficiency.

[0007] That is, according to the present invention, there is provided the following method for producing carbon material granules. [1] A method for producing carbon material granules, comprising the steps of: pulverizing and mixing carbon black granules and carbon nanotube granules to obtain a mixture so that the particle size of the carbon black is 500 μm or less, as measured by the method described in JIS K-6219-4, and the particle size of the carbon nanotubes is 500 μm or less, as measured by the method described in JIS K-6219-4; dissolving a solvent-soluble polymer in a solvent to prepare a binder solution; mixing the mixture with the binder solution to obtain a wet mixture; and granulating the wet mixture to obtain carbon material granules. [2] The method for producing carbon material granules according to [1], wherein the pulverization is performed using at least one pulverizer selected from the group consisting of a jet mill, a vibrating ball mill, a roll crusher, and a hammer mill. [3] The method for producing a carbon material granule according to [1] or [2], wherein the solvent-soluble polymer is a water-soluble polymer, and the solvent is water. [4] The method for producing a carbon material granule according to any of [1] to [3], wherein a granulator is used to granulate the wet mixture, and the granulator is at least one selected from the group consisting of an extrusion granulator and a shear-crushing granulator.

[0008] According to the present invention, it is possible to provide a method for producing carbon material granules that is free from scattering during the granulation step, allows continuous granulation, and can improve production efficiency.

[0009] 1 is a SEM photograph of the carbon material granules obtained in the present embodiment, and a conceptual diagram thereof. FIG. 2 is a conceptual diagram of an extrusion granulator used in the present embodiment. FIG. 3 is a SEM photograph of the carbon material granules obtained in Example 5, Example 6, and Comparative Example 1.

[0010] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. Hereinafter, the carbon material granules may also be simply referred to as "granules".

[0011] [Method for Producing Carbon Material Granules] The method for producing granules according to this embodiment includes the following steps: a step of obtaining a mixture by pulverizing and mixing carbon black granules and carbon nanotube granules so that the particle size of the carbon black is 500 μm or less, as measured by the method described in JIS K-6219-4, and the particle size of the carbon nanotubes is 500 μm or less, as measured by the method described in JIS K-6219-4 (pulverizing and mixing step); a step of dissolving a solvent-soluble polymer in a solvent to prepare a binder solution (solution preparation step); a step of adding the binder solution while mixing the pulverized carbon black and carbon nanotubes to obtain a wet mixture (granulation precursor) (wet mixture preparation step); and a step of granulating the wet mixture to obtain carbon material granules (granule preparation step).

[0012] (Crushing and Mixing Process) In the crushing and mixing process, the CB granules and the CNT granules are crushed to a specific particle size or less and then mixed to obtain a mixture. The order of crushing and mixing is not particularly limited. (1) The CB granules and the CNT granules may be dry crushed separately and then mixed, or (2) the CB granules and the CNT granules may be mixed and then crushed. Crushing methods include dry crushing and wet crushing, and are used depending on the purpose. In this embodiment, dry crushing is preferred, but in the case of dry crushing, the crusher used varies depending on the desired particle size or particle size distribution. For example, (1) when medium crushing (1 mm to several tens of μm) is the goal, a roll crusher, impeller mill, cutter mill, or ring mill is used. A Henschel mixer or a Loedige mixer, which are commonly used as mixers or granulators, can also be used. On the other hand, for the purpose of (2) fine pulverization (tens of μm to several μm), jet mills, roller mills, pin mills, planetary mills, etc. are used. Among pulverizer manufacturers, jet mill-type pulverizers include Seishin Enterprise Co., Ltd., Aisin Nano Technologies Co., Ltd., and Earth Technica Co., Ltd. Manufacturers of pin mills include Makino Sangyo Co., Ltd., Nishimura Machinery Works, Ltd., and Hosokawa Micron Co., Ltd. Manufacturers of impeller mills include Seishin Enterprise Co., Ltd. and Earth Technica Co., Ltd. Manufacturers of sanitary rotary type crushers include Aishin Sangyo Co., Ltd. and Tokuju Kosakusho Co., Ltd. Among these, the sanitary type crusher manufactured by Aishin Sangyo Co., Ltd., and the Randle Mill (RM-1N type) manufactured by Tokuju Kosakusho Co., Ltd., are capable of directly inserting materials from a raw material hopper into a mixer or twin-screw extruder while crushing them in a sealed state. On the other hand, the CB and CNT may be mixed by a method in which the pulverized product is charged into a mixer granulator such as a Henschel mixer or a Loedige mixer, and then mixed while water in which a polymer is dissolved is added. Alternatively, the CB and CNT may be directly charged into a mixer granulator such as a Henschel mixer without pulverization, and pulverized in the granulator by high-speed stirring without adding water in which a polymer is dissolved, and then water in which a polymer is dissolved is added to produce a wet mixture that serves as a granulation precursor.As mentioned above, most brands of CB and CNT are shipped in a granulated form for reasons such as workability, reduced transportation costs, and scattering prevention. Generally, CB granules are manufactured with diameters ranging from 0.25 mm to 2 mm, while CNTs come in a variety of shapes and sizes. Currently, CNTs manufactured by LG Chemicals, the world's largest producer of MWCNTs, are button-cell-shaped with a diameter of 7 mm and a height of 2 mm, and each granule weighs approximately 0.0198 g. On the other hand, a 1 mm diameter CB (DC3501 manufactured by OCI Corporation, Korea) weighs approximately 0.0002 g, making the weight ratio between the two approximately 100 times. For example, when CB and CNT are mixed in a ratio of 70 g to 30 g, the number of CB and CNT granules is (70 g) / (0.0002 g / particle) = 350,000 CB particles and (30 g) / (0.0198 g / particle) = 1,515 CNT particles. Since the particle ratio of the two is approximately 231 to 1, it can be easily inferred that the two will not be uniformly mixed by simply mixing them. Patent Document 3 outlines the process of adding water containing a water-soluble polymer to CNT in a screw conveyor, then producing aggregates in a shear crusher, followed by drying. More specifically, the amount of polymer added to the CNT is 0.005 to 3% by mass, and the amount of aqueous solution is 400 to 1,000 parts by mass per 100 parts by mass of CNT. Furthermore, the CNT supply rate to the screw conveyor is 0.25 to 1.0 kg / min, with a residence time of 1 to 3 minutes. Furthermore, it is stated that a rotary cutter mill or a multistage rotary cutter mill is preferred as a shear crushing device. Even if CB and CNT are supplied to the screw conveyor described in Patent Document 3 and rotated while adding water, the screw conveyor is a device that transports objects by rotating blades at a low speed, and therefore has little ability to mix two or more types of carbon. In particular, as mentioned above, it can be said that it is difficult to uniformly mix granulated CB and CNT using a screw conveyor. In contrast, the method for producing granulated material according to this embodiment allows for uniform mixing of CB and CNT (see Figure 1).

[0013] (Measuring particle size of crushed products) The particle size distribution of CNT and CB is measured according to JIS K-6219-4, "Method for determining the size distribution of granulated particles." The measuring device is a classification method that uses stacked mesh sieves, and depending on the method of vibration, there are sonic vibration, low-tap, and electromagnetic types. Manufacturers of sonic vibration types include Hatsuratsu Co., Ltd. and Seishin Enterprise Co., Ltd. Manufacturers of low-tap sieves include the two companies mentioned above, as well as CMT Co., Ltd. and AS ONE Corporation. Manufacturers of electromagnetic shaking sieving machines include Tsutsui Rikagakuhin Co., Ltd. Taking the low-tap type manufactured by CMT Co., Ltd. as an example, a specific measurement method involves setting four to six stacked 200 mm mesh sieves on the low-tap. The mesh types are usually a combination of 10 mesh (opening 1000 μm), 30 mesh (500 μm), 60 mesh (250 μm), and 100 mesh (150 μm), but 86 mesh (2000 μm) and 149 mesh (100 μm) may also be added for measurement. For the measurement, a tray is attached to the bottom, 100 g of granulated product is placed on the top mesh sieve, the lid is attached, and the sieve is shaken for 1 minute under conditions of a shaking speed of 290 rpm, an amplitude of 28 mm, and a hitting rate of 156 t.p.m. The granulated product clogging the top and mesh openings of each sieve is scraped off, their weights are measured, and the particle size distribution is calculated. The mesh opening value of the mesh with the smallest opening among all the meshes is the particle size of the pulverized product. The preferred particle size after pulverization, when measured using a rotary tap classification method, is preferably 10 μm to 500 μm for both CB and CNT, and more preferably 25 μm to 250 μm. If the particle size exceeds 500 μm, the number of agglomerates increases, resulting in poor dispersibility and poor uniform mixing of CB and CNT. Furthermore, processing to reduce the particle size to less than 10 μm is not easy due to industrial-scale production, and even if processing is possible, it requires a long time and is not practical. Furthermore, this processing cuts the CNT fibers, which reduces conductivity, making it undesirable. Furthermore, when CB and CNT are blended and then pulverized, the particle size is preferably the same as that of the CNT.

[0014] Examples of CB include those obtained by thermal decomposition methods such as thermal methods or acetylene cracking methods, incomplete combustion methods such as oil furnace methods, and those obtained by heavy oil gasification processes such as the Texas method, the Fazer method, or the Shell method. These may be used alone or in combination of two or more. Specific examples include the #4000 and #5000 series manufactured by Tokai Carbon Co., Ltd., the #3000 series manufactured by Mitsubishi Chemical Corporation, FX, HS, and Denka Black manufactured by Denka Co., Ltd., the Conductex series manufactured by Birla Carbon Corporation, the Vulcan series or LITX series manufactured by Cabot Corporation, the ENSACO series and Super P-Li series manufactured by Imerys GC, and Printex L manufactured by Orion Engineer Carbons.

[0015] The fiber diameter of CNT is 0.3 nm, which is feasible with current technology, but may be thinner than 0.3 nm. Furthermore, as the fiber diameter increases beyond 50 nm, electrical or mechanical properties tend to decrease, and as the fiber diameter increases beyond 100 nm, the CNT tends to lose its superiority over CB or carbon nanofibers. Furthermore, from the viewpoint of efficiently forming a three-dimensional network with the CNT in the granulated product according to this embodiment, the CNT fiber diameter is preferably 3 nm or more and 50 nm or less, even more preferably 5 nm or more and 40 nm or less, and particularly preferably 10 nm or more and 30 nm or less. The fiber length of CNT is related to conductivity, mechanical properties, or dispersibility. The fiber length of CNT is preferably 0.1 μm or more and 2000 μm or less, and more preferably 1 μm or more and 1000 μm or less. As the fiber length decreases, conductivity or mechanical properties tend to be less readily exhibited. On the other hand, as the fiber length increases, the entanglement of the fibers becomes stronger, resulting in an increase in poorly dispersed agglomerates and an increase in fiber breakage during kneading and dispersion, which is undesirable. The aspect ratio of CNT is, for example, 10 to 10,000. Furthermore, a structure in which hexagonal mesh graphite sheets are cylindrically shaped is preferably used as the CNT. The CNT may be either single-walled or multi-walled, and can be selected depending on the final purpose. Furthermore, there are no limitations on the manufacturing method of CNT. Examples of manufacturing methods for CNT include the pyrolysis method in which a carbon-containing gas is brought into contact with a catalyst, the arc discharge method in which an arc discharge is generated between carbon rods, the laser evaporation method in which a laser is irradiated onto a carbon target, the CVD method in which a carbon source gas is reacted at high temperature in the presence of metal fine particles, and the HiPco method in which carbon monoxide is decomposed under high pressure. Furthermore, CNT may be doped with metal atoms.

[0016] In the granulated product according to this embodiment, the amount of CNT is preferably 5% by mass or more and 40% by mass or less, and more preferably 10% by mass or more and 35% by mass or less, relative to the total amount of CB and CNT (100% by mass). When the amount of CNT is equal to or less than the upper limit, the dispersibility of the CNT can be improved. When the amount of CNT is equal to or greater than the lower limit, the conductivity can be further improved. In this embodiment, after mixing the CB and CNT, grinding the CB and CNT is an essential step before the series of steps of mixing the CB and CNT with a solvent-soluble polymer and granulating them. Recently, most commercially available CNTs are in the form of granules for purposes such as preventing scattering, reducing transportation costs, and improving workability during processing. As a result, CNTs, which were difficult to disperse even in powder form, are becoming even more difficult to disperse. Furthermore, among furnace-type CBs, those known as conductive CBs are almost entirely provided as granules, which are significantly more difficult to disperse than powdered CBs. After studying various methods for improving this dispersibility, we discovered that pulverization improves dispersibility. Furthermore, we found that pulverizing both CB and CNT also improves the mixing of the two materials. The pulverization method involves applying energy to a material as a force such as "compression," "impact," "friction," or "shear," which generates stress in the material, causing it to deform and break down, resulting in a finer particle size. There are two pulverization methods: dry and wet. In this embodiment, it is preferable to use materials processed by the dry method.

[0017] (Solution Preparation Step) In the solution preparation step, a solvent-soluble polymer is dissolved in a solvent to prepare a binder solution. Any solvent-soluble polymer can be used as long as it is soluble in water, organic solvents, and mixtures thereof. Examples of solvent-soluble polymers include polymeric surfactants and high molecular weight polymers. Examples of surfactants include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants. These surfactants may be used alone or in combination of two or more. Examples of high molecular weight polymers include ether-based polymers (e.g., polyethylene glycol (polyethylene oxide) and polypropylene glycol), vinyl-based polymers (e.g., polyvinyl alcohol, polyvinyl acetate, and polyvinylpyrrolidone), acrylamide-based polymers (e.g., polyacrylamide), amine-based polymers (e.g., polyethyleneimine and polybutyleneimine), cellulose-based polymers (e.g., methylcellulose, ethylcellulose, carboxymethylcellulose, hydroxyethylcellulose, and hydroxypropylmethylcellulose), and starch-based polymers (e.g., oxidized starch and gelatin). These may be used alone or in combination of two or more. Among these, from the viewpoint of reducing scattering or improving dispersibility, it is more preferable to use a glycol-based polymer, and it is particularly preferable to use polyethylene oxide.

[0018] The solvent may be water, an organic solvent, or a mixture thereof, with water being the most preferred. Furthermore, when water is used as the solvent, the solvent-soluble polymer is a water-soluble polymer. The concentration of the solvent-soluble polymer in the binder solvent is preferably 1% by mass or more and 10% by mass or less, more preferably 2% by mass or more and 5% by mass or less. When the concentration of the solvent-soluble polymer is above the lower limit, the solvent-soluble polymer can coat the carbon material more efficiently. On the other hand, when the concentration of the solvent-soluble polymer exceeds the upper limit, the solvent-soluble polymer does not sufficiently penetrate the carbon material, reducing its effectiveness in expelling air present on the surface or in pores that is detrimental to conductive performance, which tends to result in reduced conductivity. Adding the solvent-soluble polymer at as low a concentration as possible facilitates penetration of the solvent-soluble polymer into the voids of the carbon material, enabling a uniform coating of the entire carbon material. Furthermore, adding a surfactant to the binder solution can facilitate penetration of the binder solution into the carbon material.

[0019] (Wet Mixture Preparation Step) In the mixture preparation step, the mixture obtained in the grinding and mixing step is mixed with the binder solution obtained in the solution preparation step to obtain a wet mixture. Here, the amount of binder solution is preferably adjusted depending on the amount of solvent-soluble polymer. That is, the amount of solvent-soluble polymer is preferably 0.01 parts by mass or more and 15 parts by mass or less, more preferably 0.1 parts by mass or more and 12 parts by mass or less, and particularly preferably 2 parts by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the total amount of carbon black and carbon nanotubes.

[0020] In this embodiment, a shearing treatment for shearing the CB and CNT may be performed during or after the wet mixture preparation step. However, in this embodiment, the CB and CNT are sufficiently pulverized in the aforementioned pulverization and mixing step, so this shearing treatment is not necessarily required.

[0021] (Granulated Product Preparation Process) In the granulated product preparation process, the wet mixture obtained in the wet mixture preparation process is granulated to obtain carbon material granules. Granulating the wet mixture enables continuous granulation and improves the production efficiency of the granulated product. Examples of granulators used here include extrusion granulators and shear crushing granulators. Among these, from the perspective of production efficiency, the use of an extrusion granulator (see Figure 2, which is a model of the interior of an extrusion granulator) is particularly preferred. As shown in Figure 2, the extrusion granulator comprises a screw case 1, a screw 2, an extractor blade 3, a screen 4, and a screen holder 5. The mainstream of extrusion granulators is a screw-type extrusion granulator, and there are single-screw and twin-screw types. Furthermore, extrusion granulators are broadly classified into two types: front extruders and side extruders, depending on the installation position of the extrusion screen die. In the case of a single-screw type, the screen die is almost always attached to the front end of the granulation chamber. On the other hand, twin-screw extrusion machines often have screen dies attached to both sides of the granulation chamber. Comparing the features of single-screw and twin-screw extrusion machines, the single-screw extrusion machine generates stronger extrusion pressure, allowing for relatively large particle sizes and high hardness. Twin-screw extrusion machines excel at small particle sizes and produce weaker particles, but are superior in production efficiency. Examples of screw-type extrusion granulators and their manufacturers include Dalton's Pelletter Double EXD or Fineluzer EXR, Okawara Manufacturing's Granumaster, and Hosokawa Micron's Extrude Mix EM. Examples of shear-crushing granulators include Fuji Yakuhin Kikai's Speed ​​Mill HM series and Nippon Pneumatic Mfg. Co., Ltd.'s Chopper Mill.

[0022] After the granule preparation step, a step of drying the carbon material granules (drying step) may be carried out as needed. Vacuum drying, hot air drying, etc. can be used for drying. As the hot air dryer, a vibration / fluidized air dryer, a fluidized air dryer, a box dryer, a dryer-type dryer, etc. can be used. On the other hand, as the vacuum (reduced pressure) dryer, a vacuum tray dryer, a reduced pressure outer mixer dryer, a box dryer, etc. can be used.

[0023] The drying temperature is preferably a temperature at which the solvent-soluble polymer does not deteriorate, and therefore there is an optimum temperature or a maximum temperature depending on the type of solvent-soluble polymer, but generally, the temperature is preferably from 40° C. to 200° C., more preferably from 50° C. to 150° C., and particularly preferably from 60° C. to 100° C. The drying time varies depending on the drying temperature, but is usually from 1 hour to 20 hours, and preferably from 2 hours to 10 hours.

[0024] [Effects of the Present Embodiment] The present embodiment can achieve the following effects. (1) It is possible to produce a carbon material granule that can reduce scattering and improve electrical conductivity and mechanical properties. (2) As described above, the present embodiment enables continuous granulation. Therefore, compared with conventional methods for producing granules that perform granulation in a batch system, production efficiency can be improved.

[0025] [Modifications of the Embodiments] The present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of achieving the object of the present invention are included in the present invention. For example, in the above-described embodiment, the grinding and mixing process is performed continuously, but this is not limited to this. For example, the CB granules may be purchased from a supplier and pre-ground, and used. Furthermore, the CNT granules may be purchased from a supplier and pre-ground, and used.

[0026] The present invention will be specifically described below based on examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by mass unless otherwise specified.

[0027] The following describes the methods for measuring physical properties used in the examples and the samples used in the examples. (1) Ash Content (ASH) The miscibility of CB and CNT was determined by the ash content present in both CB and CNT. Ash content was measured by weighing 2.0 g of CB or CNT, placing it in a porcelain crucible, and completely incinerating it in an electric furnace set at 750°C. The remaining amount was then weighed. The ash content was expressed as a percentage by dividing the remaining amount by the initial sample amount. (2) Resin Dispersibility To evaluate resin dispersibility, a resin composition was prepared by blending 1% of the sample with polycarbonate resin (Teijin Ltd., Panlite 1-1225WP) using a Labo Plastomill at 210°C and 150 rpm for 4 minutes. This was then melt-pressed to prepare flakes. These flakes were then evaluated by observing them under a microscope. Resin dispersibility was rated in the order of "AA," "A," "B," and "C." "AA" indicates the best resin dispersibility. "B" is a practical level. (3) Scatterability Scatterability was measured using SKY-2 manufactured by Shibata Scientific Co., Ltd., and the sample was placed from the bottom into an airflow of 10 L / min. The amount of scattering was calculated from the weight adsorbed on a filter paper placed at the outlet of the device. This method is a measurement method adopted by the Japan Industrial Accident Prevention Association.

[0028] (Samples used in Examples, etc.) The CB is DC3501, a conductive CB manufactured by OCI. This CB is a granulated product, with a particle size of approximately 0.5 mm to 1.5 mm. The CNT is BT1003M manufactured by LG Chemical. This granulated product is formed into a shape with a diameter of 7 mm and a thickness of 2 mm using a tablet machine. The binder polymer is PEO (polyethylene oxide). The PEO has a molecular weight of 100,000 to 200,000 and is available under the trade name "Alcox R-150" manufactured by Meisei Chemical Industry Co., Ltd.

[0029] [Test Example 1] By changing the pulverizer and pulverization conditions as follows, pulverized products with different particle sizes were produced, and the uniform mixing of CB and CNT and the resin dispersibility when blended into the resin were evaluated. (Pulverization Condition 1) CB and CNT were pulverized separately using a Henschel mixer (FM-20 manufactured by Nippon Coke Engineering Co., Ltd.) and stirred at 1000 rpm for 5 minutes. (Pulverization Condition 2) CB and CNT were pulverized separately using a cutter mill (U-210) manufactured by Nishimura Machinery Works, Ltd. (Pulverization Condition 3) CB and CNT were pulverized separately using a jet mill (single track jet mill FS-4) manufactured by Seishin Enterprise Co., Ltd. (Pulverization Condition 4) Neither CB nor CNT was pulverized. The pulverized particle sizes of the pulverized products pulverized under the above pulverization conditions are shown in Table 1. Next, these pulverized materials were placed in a Henschel mixer in a ratio of 70% CB and 30% CNT, and after stirring at 500 rpm for 1 minute, approximately 10 g samples were taken from four locations in the tank and the ash content was measured. Furthermore, the samples collected from the four locations were mixed and the resin dispersibility was examined. The results are shown in Tables 1 and 2.

[0030]

[0031]

[0032] Example 1: CB (DC3501) and CNT (BT1003M) were placed in a Henschel mixer in a ratio of 7:3 and milled at 1000 rpm for 5 minutes. Next, a binder solution containing a binder polymer equivalent to 10% of the total amount of CB and CNT was added over 3 minutes using a Henschel mixer set at 500 rpm to obtain a wet mixture. The water content of the wet mixture was 80%. Next, the wet mixture was granulated using an EXD-100 twin-screw horizontal extrusion granulator manufactured by Dalton to obtain a carbon material granule. The obtained carbon material granule was dried in a vacuum dryer set at 80°C.

[0033] Example 2 A carbon material granule was obtained in the same manner as in Example 1, except that the amount of polymer added was 5% based on the total amount of CB and CNT.

[0034] Example 3 A carbon material granule was obtained in the same manner as in Example 1, except that the amount of polymer added was 2% based on the total amount of CB and CNT.

[0035] Example 4 A carbon material granule was obtained in the same manner as in Example 1, except that the amount of polymer added was 0.1% relative to the total amount of CB and CNT.

[0036] [Evaluation of Polymer Adhesion Amount and Scatterability] The scattering amounts of the carbon material granules obtained in Examples 1 to 4 and CB (DC3501) were measured. The scattering properties of K-Nanos 100P, a non-granulated powdered CNT from Kumho Corporation, were also measured. The results are shown in Table 3. Here, it was found that the CNT (BT1003M) from LG Chemical Corporation, which has been used in the examples, has large formed particles and must be crushed to measure scattering properties. Since true data cannot be obtained when crushed, it was excluded from the estimation this time.

[0037]

[0038] As is clear from the results shown in Table 3, it was found that carbon material granules with a small amount of scattering were obtained in Examples 1 to 4, which used a binder solution. Furthermore, even when the polymer amount was 0.1%, as in Example 4, the amount of scattering was significantly smaller than that of K-Nanos 100P or DC3501. This is thought to be because, as can be seen from the SEM photograph and conceptual diagram shown in Figure 1, the granules according to the present invention have CB and CNTs conveniently entangled in the micron-order range.

[0039] [Examples 5, 6, and Comparative Example 1] (Example 5) Carbon material granules were produced using a Dalton Co., Ltd. double EXD-60 pelletizer. Specifically, the CB to CNT ratio was set to 7:3, and the mixture was pulverized at 1,000 rpm for 5 minutes. Then, 325 parts by mass of a binder solution containing a binder polymer was added to 100 parts by mass of the total amount of CB and CNT. This was then granulated using a twin-screw horizontal extrusion granulator (screen die opening: 1.2 mm). The output rate of the carbon material granules was approximately 100 kg / hour in wet terms. (Comparative Example 1) Patent Document 2 primarily uses a batch-type granulator. As batch-type granulators, Hensel mixer-type and Loedige mixer-type granulators are preferred, with Loedige mixers being particularly preferred. To compare the productivity of Example 5 with that of Patent Document 2, carbon material granules were produced under the following conditions. "Productivity of the Loedige Mixer" CB and CNT were added to a Loedige Mixer M-130 (internal volume 130 L) manufactured by Chuo Kiko Co., Ltd. in a ratio of 7:3 and pulverized at 1000 rpm for 5 minutes. A predetermined amount of binder solution was then added over 20 minutes, and granulation and sizing were carried out over another 20 minutes. As a result, 8.6 kg of carbon material granules were obtained in 40 minutes. This corresponds to 12.9 kg per hour on a dry basis. (Example 6) "Productivity of the Extrusion Granulator" Carbon material granules were granulated in the same manner as in Example 5, except that a Pelletizer Double EXD-100 manufactured by Dalton Co., Ltd. (with an installation area not significantly different from that of the Loedige Mixer M-130) was used. With this granulator, the output varied depending on the screen hole diameter. With a screen die with a 2.0 mm diameter opening, the output was 290 kg / hour in a wet state and 113 kg / hour on a dry basis. This was found to be about 8.8 times the production volume of the Lödige mixer described above. SEM photographs of the carbon material granules obtained in Examples 5, 6, and Comparative Example 1 are shown in Figure 3. As shown in Figure 3, it can be seen that good carbon material granules were obtained in all of the examples.

[0040] 1...Screw case, 2...Screw, 3...Extract blade, 4...Screen, 5...Screen holder.

Claims

1. A method for producing a carbon material granule, comprising the steps of: pulverizing and mixing carbon black granules and carbon nanotube granules to obtain a mixture, so that the particle size of the carbon black is 500 μm or less, as measured by the method specified in JIS K-6219-4, and the particle size of the carbon nanotubes is 500 μm or less, as measured by the method specified in JIS K-6219-4, and the particle size of the carbon nanotubes is 500 μm or less, as measured by the method specified in JIS K-6219-4, respectively; dissolving a solvent-soluble polymer in a solvent to prepare a binder solution; mixing the mixture with the binder solution to obtain a wet mixture; and granulating the wet mixture to obtain a carbon material granule.

2. The method for producing a carbon material granule according to claim 1, wherein the pulverization is carried out by at least one pulverizer selected from the group consisting of a jet mill, a vibrating ball mill, a roll crusher and a hammer mill.

3. The method for producing a carbon material granule according to claim 1 or 2, wherein the solvent-soluble polymer is a water-soluble polymer, and the solvent is water.

4. A method for producing a carbon material granule as defined in claim 1 or 2, wherein a granulator is used to granulate the wet mixture, and the granulator is at least one selected from the group consisting of an extrusion granulator and a shear crushing granulator.

Citation Information

Patent Citations

  • Liquid formulations, particularly masterbatches of carbon-based conductive fillers for lithium-ion batteries.

    JP2013522439A

  • Method for producing granule of carbon having different bulk density and granule of carbon obtained by the same

    JP2017201006A

  • Production method of carbon nanotube mixture aggregate

    JP2021031514A

  • Carbon material granules, method for producing carbon material granules, and conductive resin composition

    JP7126666B1

Cited By

  • Low-dust environment-friendly carbon black particle granulation device and method

    CN121103235A

  • Method for producing carbon-material granules

    WO2026163270A1