Adhesive sheet and method for manufacturing semiconductor device

The adhesive sheet with a cured energy ray-curable component and nitrogen-containing polymer enhances adhesive strength and prevents residue and blistering, addressing issues in semiconductor manufacturing.

JP7568815B2Active Publication Date: 2024-10-16LINTEC CORP
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
JP2023186955
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-10
Filing Date
2023-10-31
Publication Date
2024-10-16
Estimated Expiration
2038-12-27

AI Technical Summary

Technical Problem

Adhesive sheets used in semiconductor manufacturing face issues with decreased adhesive strength upon exposure to ultraviolet rays, leading to easy peeling and adhesive residue, and blistering under high temperature or high temperature and reduced pressure conditions.

Method used

A pressure-sensitive adhesive sheet with a base material and adhesive layer containing a cured product of an energy ray-curable component, including a polymer component with nitrogen-containing functional groups and a polyfunctional energy ray-curable compound, which maintains adhesive strength and prevents blistering and residue.

Benefits of technology

The adhesive sheet maintains strong adhesion under high temperature conditions, reduces blistering and unintended peeling, and prevents adhesive residue, ensuring reliable semiconductor device manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568815000007
    Figure 0007568815000007
  • Figure 0007568815000008
    Figure 0007568815000008
  • Figure 0007568815000009
    Figure 0007568815000009
Patent Text Reader

Abstract

To provide an adhesive sheet that can improve adhesive strength when heated while preventing adhesive residues when peeled from an adherend, in order to reduce swelling under high-temperature conditions or combined high-temperature and low-pressure conditions, as well as to prevent unintended peeling from the adherend.SOLUTION: An adhesive sheet (10) for processing an electronic component has a base material (11) and an adhesive layer (12), and the adhesive layer (12) contains a cured material formed by curing an energy ray curable component.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet and a method for manufacturing a semiconductor device. [Background technology]

[0002] In the manufacturing process of semiconductor devices, adhesive sheets are used for the purpose of protecting semiconductor elements (such as semiconductor chips, etc.) etc. Various properties are required for the adhesive sheets used in the manufacturing process of semiconductor devices.

[0003] For example, Patent Document 1 describes a heat-resistant adhesive tape including a base layer and an adhesive layer provided on the base layer. Patent Document 1 describes that the adhesive layer of the heat-resistant adhesive tape is made of an ultraviolet-curable adhesive containing an ultraviolet-curable compound, and that the adhesive layer has an adhesive strength of 1 N / 19 mm width or less as measured in accordance with JIS Z0237 after irradiating the adhesive layer with ultraviolet light and further heating at 200° C. for 1 hour. Furthermore, Patent Document 2 describes an adhesive sheet having a substrate and an adhesive layer that contains an energy ray-curable adhesive formed on the substrate.

[0004] In recent years, there has also been a demand for adhesive sheets that, after undergoing a process involving high-temperature conditions, do not leave any adhesive residue on the adherend when the sheet is peeled off at room temperature, and that also have a small peeling force.

[0005] For example, Patent Document 3 describes a heat-resistant adhesive tape that is applied when resin-encapsulating a semiconductor chip mounted on a metal lead frame. The heat-resistant adhesive tape described in Patent Document 3 has at least a base layer and an active energy ray-curable adhesive layer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2012-46763 A [Patent Document 2] JP 2017-82104 A [Patent Document 3] JP 2010-73853 A Summary of the Invention [Problem to be solved by the invention]

[0007] The adhesive tapes and adhesive sheets (hereinafter collectively referred to as "adhesive sheets") described in Patent Documents 1 and 2 are configured so that the adhesive strength of the adhesive layer decreases when irradiated with ultraviolet light, allowing the adhesive sheets to be relatively easily peeled off from the adherend.

[0008] According to Patent Document 3, the heat-resistant adhesive tape described therein can be easily peeled off without leaving any adhesive residue when peeled off. Patent Document 3 also describes that the timing for curing the active energy ray curable adhesive layer is not particularly limited as long as it is after lamination and before the wire bonding process. The reason for this is that Patent Document 3 also describes that if the adhesive layer is cured before laminating it to the outer pad side of the lead frame, the effect of following the unevenness of the lead frame surface cannot be obtained, and the adhesive strength is reduced, making lamination difficult, and the adhesion to the lead frame is reduced, making it difficult to prevent leakage of the sealing resin.

[0009] However, when an adhesive tape containing an active energy ray-curable adhesive in the adhesive layer as described in Patent Documents 1, 2 and 3 is used in the manufacturing process of a semiconductor device, the adhesive tape may peel off from the adherend or blistering may occur in the high temperature environment of the sealing process. In addition, when a plasma treatment process is performed following the sealing process, defects such as blistering may occur between the adhesive tape and the adherend due to a temperature rise caused by heating or a process in which a temperature rise and a pressure reduction occur simultaneously.

[0010] The object of the present invention is to provide an adhesive sheet that can improve adhesive strength when heated while preventing adhesive residue when peeled off from an adherend, in order to reduce the occurrence of blistering and unintended peeling off from an adherend under high temperature, or high temperature and reduced pressure conditions. Another object of the present invention is to provide a method for manufacturing a semiconductor device using the pressure-sensitive adhesive sheet. [Means for solving the problem]

[0011] A pressure-sensitive adhesive sheet according to one embodiment of the present invention has a substrate and a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer including a cured product obtained by curing an energy ray-curable component.

[0012] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the pressure-sensitive adhesive layer further comprises a polymer component, and the polymer component comprises a structural unit derived from a monomer having a nitrogen-containing functional group, with the proviso that the nitrogen-containing functional group does not preferably contain an N-H bond.

[0013] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, it is preferable that the polymer component contains a structural unit derived from a functional group-containing monomer having a reactive functional group, and the reactive functional group is bonded to the main chain of the polymer component via three or more linearly bonded methylene groups.

[0014] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, it is preferable that the energy ray-curable component includes a polyfunctional energy ray-curable compound, and that the polyfunctional energy ray-curable compound has 2 to 5 polymerizable functional groups in one molecule.

[0015] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, it is preferable that the energy ray-curable component includes a polyfunctional energy ray-curable compound, the polyfunctional energy ray-curable compound has two or more polymerizable functional groups in one molecule, a methylene group is present in a linear chain between a first polymerizable functional group and a second polymerizable functional group arbitrarily selected from the two or more polymerizable functional groups contained in the polyfunctional energy ray-curable compound, and the number of methylene groups present in a linear chain between the first polymerizable functional group and the second polymerizable functional group is 4 or more.

[0016] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the number of methylene groups bonded in a linear chain between the first polymerizable functional group and the second polymerizable functional group is preferably 8 or more and 30 or less.

[0017] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the polyfunctional energy ray-curable compound preferably has a cyclic structure in the molecule.

[0018] In one embodiment of the pressure-sensitive adhesive sheet of the present invention, the pressure-sensitive adhesive layer has a breaking strength per unit cross-sectional area of ​​4.5 N / mm 2 More preferably, it is equal to or greater than this.

[0019] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the pressure-sensitive adhesive sheet preferably has an adhesive strength to polyimide at 100° C. of 0.04 N / 25 mm or more.

[0020] In one aspect of the pressure-sensitive adhesive sheet of the present invention, the pressure-sensitive adhesive sheet has an adhesive strength to polyimide of 0.06 N / 25 mm or more at 100° C., and the pressure-sensitive adhesive layer has a breaking strength per unit cross-sectional area of ​​4.5 N / mm 2 More preferably, it is equal to or greater than this.

[0021] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, it is preferable that the adhesive strength of the pressure-sensitive adhesive sheet to polyimide at 25° C. after heat treatment at 190° C. for 1.5 hours in a nitrogen atmosphere is 3 N / 25 mm or less.

[0022] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the pressure-sensitive adhesive layer preferably has a Young's modulus of 5 MPa or less.

[0023] The pressure-sensitive adhesive sheet according to one embodiment of the present invention is preferably used for fixing or protecting electronic components when the electronic components are processed.

[0024] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the electronic component is a semiconductor element, and the pressure-sensitive adhesive sheet is preferably used to fix the semiconductor element when encapsulating the semiconductor element.

[0025] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, it is preferable that an electronic component is attached directly to the pressure-sensitive adhesive layer.

[0026] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the polymer component is preferably crosslinked with a crosslinking agent.

[0027] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the polymer component is preferably a (meth)acrylic polymer.

[0028] In the pressure-sensitive adhesive sheet according to one aspect of the present invention, the nitrogen-containing functional group is preferably at least one selected from the group consisting of a tertiary amino group, an aminocarbonyl group, a cyano group, and a nitrogen-containing heterocyclic group.

[0029] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the monomer having a nitrogen-containing functional group is preferably at least one selected from the group consisting of heterocyclic vinyl compounds, (meth)acrylamide compounds, amino group-containing (meth)acrylic acid ester compounds, and (meth)acrylonitrile.

[0030] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the proportion of the structural units derived from the monomer having a nitrogen-containing functional group in the total mass of the polymer component is preferably 1 mass % or more and 20 mass % or less.

[0031] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the proportion of the cured product obtained by curing the energy ray-curable component in the total mass of the pressure-sensitive adhesive layer is preferably 5% by mass or more and 40% by mass or less.

[0032] A method for manufacturing a semiconductor device according to one embodiment of the present invention includes the steps of fixing a semiconductor element onto an adhesive sheet having an adhesive layer including a cured product formed by curing an energy ray-curable component, and encapsulating the semiconductor element with an encapsulant. Effect of the Invention

[0033] According to the present invention, it is possible to provide an adhesive sheet that can improve adhesive strength when heated and prevent adhesive residue when peeled off from an adherend, in order to reduce the occurrence of blistering and unintended peeling off from an adherend under high temperature, or high temperature and reduced pressure conditions. [Brief description of the drawings]

[0034] [Figure 1] 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a first embodiment. [Diagram 2] FIG. 4 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a second embodiment. [Diagram 3] FIG. 4 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Hereinafter, a pressure-sensitive adhesive sheet according to one embodiment of the present invention will be described with reference to the drawings.

[0036] In this specification, "adhesive residue" refers to the problem of residue being left on the adherend when the adhesive sheet is peeled off from the adherend due to components in the adhesive layer, regardless of whether the components are components blended into the adhesive layer or components that have penetrated into the adhesive layer after the adhesive layer is formed.

[0037] First Embodiment [Adhesive sheet] FIG. 1 shows a schematic cross-sectional view of a pressure-sensitive adhesive sheet 10 of the present embodiment.

[0038] The use mode of the adhesive sheet 10 is not particularly limited. One use mode of the adhesive sheet 10 is to use the adhesive sheet 10 as an adhesive sheet for processing electronic components. Another use mode of the adhesive sheet 10 is to use the adhesive sheet 10 to fix or protect electronic components. Another more specific use mode of the adhesive sheet 10 is to use the adhesive sheet 10 to fix a semiconductor element when sealing the semiconductor element on the adhesive sheet 10. Various members can be attached to the adhesive sheet 10. In this specification, a member that can be attached to the adhesive sheet 10 may be referred to as an adherend. Examples of the adherend include electronic components (such as semiconductor elements) and frame members. Adherends such as electronic components are preferably attached directly to the adhesive layer 12. The frame member can be used, for example, to prevent warping of the adhesive sheet 10 due to hardening and shrinkage of the sealing resin when sealing the semiconductor elements on the adhesive sheet 10 with a sealing resin. The frame member may remain in the semiconductor package obtained after sealing the semiconductor elements and may fulfill a predetermined function, or the semiconductor package may be obtained only from the portion excluding the frame member.

[0039] The adhesive sheet 10 of this embodiment has a substrate 11 and an adhesive layer 12. The adhesive layer 12 contains a cured product obtained by curing an energy ray-curable component. In this embodiment, a release sheet RL may be further laminated on the adhesive layer 12. When using the adhesive sheet 10, the release sheet RL is peeled off from the adhesive sheet 10.

[0040] The pressure-sensitive adhesive layer 12 preferably contains a polymer component (hereinafter also referred to as "polymer component (A)") and a cured product (hereinafter also referred to as "cured product (B)") obtained by curing an energy ray-curable component.

[0041] The pressure-sensitive adhesive layer 12 in one aspect of this embodiment includes a polymer component (hereinafter also referred to as "polymer component (AX)") containing a structural unit derived from a monomer having a nitrogen-containing functional group, and a cured product (hereinafter also referred to as "cured product (B)") obtained by curing an energy ray-curable component, where the nitrogen-containing functional group does not include an NH bond.

[0042] The substrate 11 has a first substrate surface 11a and a second substrate surface 11b opposite to the first substrate surface 11a. In the adhesive sheet 10 of this embodiment, an adhesive layer 12 is laminated on the first substrate surface 11a. An adherend such as a semiconductor element is attached to this adhesive layer 12. The adhesive layer 12 holds the adherend on the adhesive sheet 10 during the manufacturing process of the semiconductor device.

[0043] According to the adhesive sheet 10 of this embodiment, in order to reduce the occurrence of blistering and unintended peeling from the adherend under high temperature and reduced pressure conditions, it is possible to improve the adhesive strength when heated while preventing adhesive residue when peeled from the adherend (hereinafter also referred to as the "effect of this embodiment").

[0044] The reason why the effects of this embodiment are obtained is presumed to be as follows.

[0045] The adhesive layer 12 according to the present embodiment includes a cured product (B) obtained by curing the energy ray curable component. Therefore, even in a high-temperature environment, the adhesive layer 12 can sufficiently maintain the adhesive force to the adherend. As a result, the adhesive sheet 10 can fix the adherend to the adhesive sheet 10 without causing it to fall off. The high-temperature environment in this specification is not particularly limited, but examples thereof include a sealing process of a semiconductor element, a process of performing metal sputtering on an electronic component, and a process of cleaning an electronic component with hot water or the like. In this specification, the adherend to be attached to the adhesive sheet is not particularly limited, but when the adhesive sheet is used in the sealing process of a semiconductor element, examples of the material of the adherend include the silicon surface of the semiconductor element, or a polyimide film provided on the semiconductor element. When a frame member is used in sealing the semiconductor element, the frame member can also be an adherend of the adhesive sheet 10, and examples of the material include glass epoxy resin. In addition, examples of the adherend in applications of the adhesive sheet 10 other than the sealing process of the semiconductor element include glass wafers and the like.

[0046] In addition, in a process involving heating or heating and decompression, gas generation due to moisture absorbed by the adhesive sheet 10 and other members during storage or manufacturing process may cause swelling (blisters) between the adhesive sheet and the adherend. The adhesive sheet 10 has high adhesive strength even at high temperatures or in a high temperature and decompression environment, so the occurrence of blisters and the like can be suppressed. In addition, since the adhesive layer 12 has sufficient cohesiveness, the adhesive sheet 10 can be peeled off and removed without generating residue on the adherend after a process involving heating or heating and decompression. In this specification, the process involving heating or heating and decompression is not particularly limited, but examples include, for example, a sealing process or a plasma treatment process following the sealing process. The adherend in a process involving heating or heating and decompression is not particularly limited, but examples include, for example, a semiconductor element, a frame member, or a glass wafer.

[0047] The residue remaining on the surface of the adherend after peeling off the adhesive sheet from the adherend is sometimes referred to as adhesive residue. For example, during the manufacturing process of a semiconductor device, when the adhesive sheet is peeled off from the encapsulation body after the encapsulation process is completed, the adhesive may be found to be attached to the conductive part of the semiconductor device (semiconductor element). For example, the conductive part may be a via part of the semiconductor device or a frame member, and the conductive part may be made of, for example, copper. According to the adhesive sheet of this embodiment, for example, even after being heated in the sealing process, it is possible to prevent the adhesive from adhering to the copper surface, and therefore it is possible to prevent glue from remaining on the conductive parts after the adhesive sheet is peeled off after the semiconductor device has been resin-sealed.

[0048] Unlike the polymer component (A), the cured product (B) is in an uncured (unreacted) state when it is a raw material for preparing the adhesive composition contained in the adhesive layer 12. The energy ray curable component in the cured product (B) reacts after the adhesive layer 12 is formed from the adhesive composition, synthesizing a polymer and curing it. Therefore, the cured product (B) is present continuously in the adhesive layer 12, and is different from organic fillers and the like that are present discontinuously. The pressure-sensitive adhesive layer 12 contains the cured material (B) present continuously in this manner, and thus the polymer component (A) is formed in the three-dimensional network structure of the cured material (B), and the polymer component (A) is crosslinked by the loose constraint of the network structure. This improves the cohesiveness of the pressure-sensitive adhesive layer at high temperatures, and is believed to improve the adhesive strength at high temperatures and prevent adhesive residue. In addition, the breaking strength of the pressure-sensitive adhesive layer 12 is improved.

[0049] When the pressure-sensitive adhesive layer 12 contains polymer component (AX) as one embodiment of polymer component (A), the significance of polymer component (AX) will be described. The polymer component (AX) contains a constituent unit derived from a monomer having a nitrogen-containing functional group. The nitrogen atom contained in the nitrogen-containing functional group is considered to be present as a polar group in the polymer component (AX). Due to the presence of this polar group (nitrogen-containing functional group), the polymer components (AX) in the pressure-sensitive adhesive layer 12 are considered to be more likely to interact with each other via the nitrogen-containing functional group, forming a pseudo-crosslinked structure in the pressure-sensitive adhesive layer 12. This makes it easier for the adhesive layer 12 to maintain its cohesive strength even when the adhesive sheet 10 is heated, and as a result, it is believed that adhesive residue is less likely to occur on the adherend when the adhesive sheet 10 is peeled off from the adherend after the sealing process. In addition, since the cohesive strength of the adhesive layer 12 is easily maintained during heating, it is believed that the adhesive strength during heating is also increased. In addition, the breaking strength of the adhesive layer also tends to increase.

[0050] Here, in one aspect of this embodiment, the nitrogen-containing functional group in the polymer component (AX) does not contain an NH bond for the following reason. Usually, when sealing a semiconductor element, an epoxy resin is often used as a sealant. Epoxy resins are prone to react with groups having an NH bond, such as amino groups. Therefore, in order to prevent the adhesive strength between the adhesive layer and the adherend from becoming too high when peeling the adhesive sheet from the adherend, making it difficult to peel the adhesive sheet from the adherend, or to prevent adhesive residue on the sealant, the NH bond is excluded from the nitrogen-containing functional group.

[0051] In one aspect of this embodiment, the adhesive layer 12 contains a polymer component (AX), and the polymer component (AX) contains a nitrogen-containing functional group. Therefore, the polarity of the adhesive layer as a whole is increased, the compatibility of the copolymer component (AX) and the energy ray curable component is further increased, and the three-dimensional network is easily interpenetrated. This is presumed to suppress the development of adhesive strength at high temperatures derived from the nitrogen-containing polar group and the generation of localized cured material (B) that may cause adhesive residue on the adherend. Therefore, it is considered that it becomes easier to achieve both the adhesive strength of the adhesive layer 12 during heating and the prevention of adhesive residue on the adherend.

[0052] From the above, the adhesive sheet 10 of this embodiment can improve the adhesive strength when heated, reduce the occurrence of blistering and unintended peeling from the adherend in processes involving heating or heating and decompression, and can also reduce adhesive residue on the adherend when the adhesive sheet 10 is peeled off after a process involving heating and decompression, for example.

[0053] In this embodiment, the cured product (B) is included in the adhesive layer 12 for the purpose of achieving at least the adhesive strength of the adhesive layer 12 during heating and the prevention of adhesive residue on the adherend, as described above. Therefore, in the case of the active energy ray curable adhesive component included simply for the purpose of reducing the adhesive strength of the adhesive layer as in Patent Documents 1, 2 and 3, when the polymer component (A) or the polymer component (AX) is crosslinked, the crosslinking of the polymer component (A) or the polymer component (AX) proceeds between the formation of the adhesive layer and the curing of the active energy ray curable adhesive at the time of use, whereas in this embodiment, the cured product (B) cures before the crosslinking of the polymer component (A) or the polymer component (AX) proceeds. Therefore, the three-dimensional network of the polymer component (A) or the polymer component (AX) and the cured product (B) is easily interpenetrated, and the above-mentioned effect of suppressing the occurrence of localized cured product (B) that may cause adhesive residue on the adherend is more easily obtained. Furthermore, from the viewpoint that the energy ray-curable component is already cured when the pressure-sensitive adhesive sheet is attached to the adherend, there is no problem caused by decomposition of the polymerization initiator during the sealing process, and there is also the advantage that the occurrence of adhesive residue on the adherend due to excessive anchoring effect caused by uncured energy ray-curable component is prevented.

[0054] The configuration of the adhesive sheet 10 of this embodiment will be described. In the following, reference numerals may be omitted.

[0055] (Adhesive layer) Polymer component (A) The pressure-sensitive adhesive layer preferably further contains a polymer component (A) in addition to the cured product (B). Polymer component (AX), which is one embodiment of polymer component (A), contains a structural unit derived from a monomer having a nitrogen-containing functional group, provided that the nitrogen-containing functional group does not contain an N-H bond. The polymer component (A) is a component formed by a polymerization reaction of a polymerizable compound. The polymer component (AX) is a component formed by a polymerization reaction of at least a monomer having a nitrogen-containing functional group as a polymerizable compound. The polymerization reaction here includes a polycondensation reaction.

[0056] In this specification, polymer component (AX) is one aspect included in the concept of polymer component (A). Therefore, even when polymer component (A) is simply referred to, polymer component (AX) is also included unless polymer component (AX) is explicitly excluded.

[0057] Unlike the energy ray-curable component, the polymer component (A) is a component that has already been polymerized in the state of a raw material for preparing the pressure-sensitive adhesive composition contained in the pressure-sensitive adhesive layer. By further including a polymer component in the pressure-sensitive adhesive layer, a structure is formed in which the polymer component penetrates into the three-dimensional network structure of the cured product of the energy ray-curable component, and the polymer component is in a crosslinked state due to loose constraint of the network structure, which makes it easier to achieve both the adhesiveness of the pressure-sensitive adhesive layer and the cohesiveness of the pressure-sensitive adhesive layer.

[0058] Type of polymer component (A) The type of polymer component (A) is selected in consideration of the type of energy ray curable component, the use of the adhesive layer, and the type of adherend to be attached to the adhesive layer. The type of polymer component (A) is preferably at least one compound selected from the group consisting of (meth)acrylic resins, polyester resins, polyurethane resins, acrylic urethane resins, silicone resins, rubber resins, phenoxy resins, and polystyrene resins, and is more preferably a (meth)acrylic resin. These polymer components (A) may be used alone or in combination of two or more.

[0059] From the viewpoint of realizing a state in which the polymer component (A) is loosely constrained by a structure in which it penetrates into the three-dimensional network structure of the cured product (B) rather than reacting with the above-mentioned energy ray curable component and directly bonding thereto, the pressure-sensitive adhesive layer preferably contains a non-energy ray curable polymer component that does not have energy ray curability as the polymer component (A). The content of the non-energy ray curable polymer component is preferably 60 mass% or more of the entire polymer component (A), more preferably 75 mass% or more, and even more preferably 90 mass% or more.

[0060] In this embodiment, the mass ratio of the polymer component (A) to the total mass of the pressure-sensitive adhesive layer is preferably 50 mass% or more and 90 mass% or less, and more preferably 65 mass% or more and 85 mass% or less, from the viewpoint of facilitating control of the adhesive strength when the pressure-sensitive adhesive sheet is heated and the cohesiveness of the pressure-sensitive adhesive layer.

[0061] When the type of the polymer component (A) is a (meth)acrylic resin, the polymer component (A) is preferably a (meth)acrylic polymer. If the polymer component (A) is a (meth)acrylic polymer, the compatibility with the energy ray curable component tends to be high, and the adhesive strength of the pressure-sensitive adhesive layer, particularly the adhesive strength during heating, becomes easy to control. However, when the polymer component (A) is a (meth)acrylic polymer, the polymer component (A) is more preferably an acrylic polymer from the viewpoints of being less susceptible to thermal decomposition and less susceptible to cohesive failure.

[0062] Hereinafter, the case where the polymer component (A) is a (meth)acrylic polymer will be described.

[0063] (Meth)acrylic polymers are (meth)acrylic acid alkyl esters (CH2=CR 1 COOR 2 (R 1 is hydrogen or a methyl group, R 2 It is preferable that the copolymer contains polymer units derived from a straight-chain, branched-chain or cyclic (alicyclic) alkyl group. 1 COOR2 ) is partly or entirely an alkyl group R 2 The alkyl group R is preferably a (meth)acrylic acid alkyl ester having 6 to 8 carbon atoms. 2 Examples of the (meth)acrylic acid alkyl ester having 6 to 8 carbon atoms include n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and n-octyl (meth)acrylate. 2 is preferably a linear or branched alkyl group. 2 From the viewpoints of improving the adhesiveness of the pressure-sensitive adhesive sheet immediately after attachment to the adherend and improving the releasability of the pressure-sensitive adhesive sheet from the adherend even after it has been heated, 2-ethylhexyl (meth)acrylate is more preferable, and 2-ethylhexyl acrylate is even more preferable.

[0064] Alkyl group R 2 (Meth)acrylic acid alkyl ester (CH2=CR 1 COOR 2 Examples of the acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. The (meth)acrylic acid alkyl esters may be used alone or in combination of two or more kinds. In this specification, "(meth)acrylic acid" is a notation used to represent both "acrylic acid" and "methacrylic acid", and the same applies to other similar terms.

[0065] From the viewpoint of being unlikely to undergo thermal decomposition and being unlikely to cause cohesive failure, it is preferable that the (meth)acrylic polymer is composed of a (meth)acrylic acid alkyl ester and a (meth)acrylic acid alkyl ester. 1 COOR 2 Where R 1 is hydrogen) is preferably 80 mass % or more, and more preferably 90 mass % or more.

[0066] The CH2=CR 1 COOR 2 The proportion of the mass of the polymer units derived therefrom is preferably 50 mass % or more. The (meth)acrylic acid alkyl ester (CH2=CR 1 COOR 2 The proportion of the mass of the polymer units derived from the (meth)acrylic acid alkyl ester (the above CH2=CR) is preferably 50 mass% or more, more preferably 60 mass% or more, and even more preferably 80 mass% or more. 1 COOR 2 From the viewpoint of improving the initial adhesion, the mass proportion of the polymer units derived from is preferably 96 mass % or less. In this embodiment, from the viewpoint of increasing the adhesiveness of the pressure-sensitive adhesive sheet immediately after it is applied to the adherend and increasing the peelability from the adherend even after the pressure-sensitive adhesive sheet is heated, the mass ratio of the polymer units derived from 2-ethylhexyl (meth)acrylate to the mass of the entire (meth)acrylic polymer is preferably 50% by mass or more. The mass ratio of the polymer units derived from 2-ethylhexyl (meth)acrylate to the mass of the entire (meth)acrylic polymer is more preferably 60% by mass or more, and even more preferably 80% by mass or more. The mass ratio of the polymer units derived from 2-ethylhexyl (meth)acrylate to the mass of the entire (meth)acrylic polymer is preferably 96% by mass or less.

[0067] When the (meth)acrylic polymer is a copolymer and the first copolymer unit in the (meth)acrylic copolymer is an alkyl (meth)acrylate ester, the type and number of copolymer units other than the alkyl (meth)acrylate ester in the acrylic copolymer (hereinafter referred to as "second copolymer units") are not particularly limited. In this case, in the polymer component (AX), the "second copolymer unit" is a structural unit derived from a monomer having a nitrogen-containing functional group. On the other hand, in the polymer component (A) that is not the polymer component (AX), for example, the second copolymer unit is preferably a functional group-containing monomer having a reactive functional group. When a crosslinking agent described later is used, the reactive functional group of the second copolymer unit is preferably a functional group that can react with the crosslinking agent. Examples of the reactive functional group include a carboxyl group, a hydroxyl group, an amino group, a substituted amino group, and an epoxy group.

[0068] In the case where the (meth)acrylic polymer in the polymer component (AX) is a copolymer, and the copolymer is composed of a (meth)acrylic acid alkyl ester ("first copolymer unit"), a constituent unit ("second copolymer unit") derived from a monomer having a nitrogen-containing functional group, and a copolymer unit other than the first copolymer unit and the second copolymer unit (hereinafter also referred to as "third copolymer unit"), the type and number of the third copolymer unit are not particularly limited. For example, as the third copolymer unit, a functional group-containing monomer having a reactive functional group is preferable. When a crosslinking agent described later is used, the reactive functional group of the third copolymer unit is preferably a functional group that can react with the crosslinking agent. Examples of the reactive functional group include a carboxyl group, a hydroxyl group, and a primary or secondary amino group. Among these, the reactive functional group is preferably a hydroxyl group. For the same reason as that the nitrogen-containing functional group does not contain an NH bond, it is preferable not to adopt a functional group-containing monomer having a primary or secondary amino group as the functional group-containing monomer having a reactive functional group.

[0069] In the present embodiment, from the viewpoint of extending the pot life of the raw material composition for forming the pressure-sensitive adhesive layer, it is also preferable that the (meth)acrylic copolymer does not contain a copolymer unit derived from a monomer having a carboxyl group. Alternatively, it is also preferable that the (meth)acrylic copolymer contains a copolymer unit derived from a monomer having a carboxyl group, and the mass ratio of the copolymer unit derived from the monomer having a carboxyl group to the mass of the entire (meth)acrylic copolymer is 1 mass% or less, and more preferably 0.05 mass% or more and 1 mass% or less.

[0070] Examples of monomers having a carboxyl group (hereinafter, sometimes referred to as "carboxyl group-containing monomers") include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. When using a carboxyl group-containing monomer, (meth)acrylic acid is preferred, and acrylic acid is more preferred, from the viewpoints of reactivity and copolymerizability among the carboxyl group-containing monomers. The carboxyl group-containing monomers may be used alone or in combination of two or more kinds.

[0071] In this embodiment, the (meth)acrylic copolymer preferably contains a copolymer unit derived from a monomer having a hydroxyl group. By including a copolymer unit derived from a monomer having a hydroxyl group in the (meth)acrylic copolymer, when a crosslinking agent described later is used, the crosslinking density with the hydroxyl group as the crosslinking point can be increased. As a result, the crosslinked structure of the (meth)acrylic copolymer can be effectively formed. From the viewpoint of enhancing such an effect, the mass ratio of the copolymer unit derived from the monomer having a hydroxyl group to the mass of the entire (meth)acrylic copolymer is preferably 3% by mass or more. The mass ratio of the copolymer unit derived from the monomer having a hydroxyl group to the mass of the entire (meth)acrylic copolymer is preferably 9.9% by mass or less.

[0072] Examples of monomers having a hydroxyl group (hereinafter, sometimes referred to as "hydroxyl group-containing monomers") include hydroxyl group-containing (meth)acrylic acid monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxyethyl-phthalic acid, and hydroxyl group-containing caprolactone-modified (meth)acrylate. Among the hydroxyl group-containing monomers, 2-hydroxyethyl (meth)acrylate is preferred from the viewpoint of the reactivity and copolymerizability of the hydroxyl group. In addition, from the viewpoint of appropriately adjusting the adhesive strength so that the adhesive strength at room temperature does not become too high after heating, for example, 4-hydroxybutyl (meth)acrylate is preferred. The hydroxyl group-containing monomers may be used alone or in combination of two or more.

[0073] Examples of acrylic esters having an epoxy group include glycidyl acrylate and glycidyl methacrylate.

[0074] The reactive functional group of the functional group-containing monomer having a reactive functional group is preferably bonded to the main chain of the polymer component (A) via three or more linearly bonded methylene groups. This increases the probability of association between the reactive functional group and the crosslinking agent, thereby increasing the crosslink density. In addition, the possibility that the reactive functional group remains after the formation of the adhesive layer is also reduced. As a result, the adhesive strength at room temperature after heating is reduced, making it easier to peel the adhesive sheet from the adherend. In the present invention, the methylene group does not include a methylidene group, and the methylene group may be substituted with one or more hydrogen atoms. In addition, the linear bond of the methylene group may be indirectly bonded via another group. For example, in a polymer component using 3-hydroxypropyl (meth)acrylate as a functional group-containing monomer, a hydroxy group as a reactive functional group is bonded to the main chain of the polymer component (A) via three linearly bonded methylene groups. In addition, in a polymer component using 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid as a functional group-containing monomer, a hydroxyl group as a reactive functional group is bonded to the main chain of the polymer component (A) via four linearly bonded methylene groups, and these methylene groups are indirectly bonded to phthalic acid via ester bonds. The reactive functional group of the functional group-containing monomer is preferably bonded to the main chain of the polymer component (A) via 10 or less linearly bonded methylene groups, and more preferably bonded to the main chain of the polymer component (A) via 6 or less linearly bonded methylene groups.

[0075] In the polymer component (A) that is not the polymer component (AX), examples of the second copolymer component in the acrylic copolymer include, in addition to the functional group-containing monomers described above, copolymer units derived from at least one monomer selected from the group consisting of an alkoxyalkyl group-containing (meth)acrylic acid ester, an aromatic ring-containing (meth)acrylic acid ester, vinyl acetate, and styrene.

[0076] Monomers with nitrogen-containing functional groups The monomer having a nitrogen-containing functional group is not particularly limited as long as it is a polymerizable compound having a nitrogen-containing functional group, but is preferably an ethylenically unsaturated monomer having a nitrogen-containing functional group. Examples of the nitrogen-containing functional group include a tertiary amino group (-NR 3 R 4 ), aminocarbonyl group (-(C=O)-NR 5 R 6 ), aminocarbonyloxy group (-O-(C=O)-NR 7 R 8 ), aminocarbonylamino group (-NR 9 -(C=O)-NR 10 R 10A ), a cyano group, a nitro group, and a nitrogen-containing heterocyclic group. 3 R 4 ), aminocarbonyl group (-(C=O)-NR 5 R 6 ), a cyano group, and a nitrogen-containing heterocyclic group. R 3 ~R 10 , and R 10A R each independently represents a substituent. Examples of the substituent include a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms) and a substituted or unsubstituted alkenyl group having 2 to 4 carbon atoms (preferably 2 to 3 carbon atoms). The alkyl group may be linear, branched, or cyclic. The alkenyl group may be linear, branched, or cyclic. 3 ~R 10 , and R 10A are the same or different from each other. In this specification, a numerical range expressed using "to" means a range that includes the numerical value before "to" as the lower limit and the numerical value after "to" as the upper limit.

[0077] Nitrogen-containing heterocyclic group is a group that removes one hydrogen atom from a nitrogen-containing heterocyclic compound. Examples of nitrogen-containing heterocyclic compounds include morpholine, carbazole, pyrrolidone, piperidine, quinoline, pyrrolidine, aziridine, pyridine, pyrimidine, pyrazine, imidazole, and phthalimide. As the nitrogen-containing heterocyclic compound that the nitrogen-containing heterocyclic group has, morpholine is preferred from the viewpoint of increasing the cohesiveness of the adhesive layer. The monomer (polymerizable compound) having a nitrogen-containing functional group may contain one or two or more of the nitrogen-containing functional groups listed above in one molecule.

[0078] The monomer having a nitrogen-containing functional group is preferably at least one selected from the group consisting of a heterocyclic vinyl compound, a (meth)acrylamide compound, an amino group-containing (meth)acrylic acid ester compound, and (meth)acrylonitrile, and more preferably a heterocyclic vinyl compound, provided that these compounds do not contain an NH bond. It is believed that the heterocyclic group contained in the heterocyclic vinyl compound is resistant to decomposition even when the pressure-sensitive adhesive sheet is heated, due to its structure (ring structure). Therefore, when the monomer having a nitrogen-containing functional group is a heterocyclic vinyl compound, it is believed that the cohesive strength of the pressure-sensitive adhesive layer is more easily maintained, and the effect of this embodiment is more pronounced. In this specification, (meth)acrylic means both acrylic and methacrylic, and (meth)acrylonitrile means both acrylonitrile and methacrylonitrile. The monomer having a nitrogen-containing functional group may be used alone or in combination of two or more kinds.

[0079] Examples of the heterocyclic vinyl compound include N-acryloylmorpholine, N-methacryloylmorpholine, N-vinyl-2-pyrrolidone, N-acryloylpyrrolidone, N-methacryloylpyrrolidone, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, N-methacryloylpyrrolidine, N-acryloylaziridine, N-methacryloylaziridine, aziridinylethyl acrylate, aziridinylethyl methacrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, and N-vinylphthalimide. Among these, from the viewpoint of exerting the effects of the present embodiment, the heterocyclic vinyl compound is preferably N-acryloylmorpholine, N-vinyl-2-pyrrolidone, N-acryloylpyrrolidone, N-acryloylpiperidine, N-acryloylpyrrolidine, N-acryloylaziridine, aziridinylethyl acrylate, 2-vinylpyridine, 4-vinylpyridine, 2-vinylpyrazine, 1-vinylimidazole, N-vinylcarbazole, or N-vinylphthalimide, and more preferably N-acryloylmorpholine.

[0080] An example of the (meth)acrylamide compound is a compound represented by the following general formula (1).

[0081] [ka]

[0082] In the general formula (1), R 11 R represents a hydrogen atom or a methyl group. 12 and R 13 each independently represents a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms (preferably 1 to 4 carbon atoms) or a substituted or unsubstituted alkenyl group having 2 to 4 carbon atoms (preferably 2 to 3 carbon atoms). The alkyl group may be linear, branched, or cyclic. The alkenyl group may be linear, branched, or cyclic. R 12 and R13 When the substituent has a substituent, each of the substituents independently represents a dialkylamino group (—NR 14 R 15 ), or a hydroxyl group. R 14 and R 15 each independently represents an unsubstituted alkyl group having 1 to 4 carbon atoms (preferably 1 to 3 carbon atoms).

[0083] Examples of (meth)acrylamide compounds include N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N-di-n-propylacrylamide, N,N-di-n-propylmethacrylamide, N,N-di-isopropylacrylamide, N,N-di-isopropylmethacrylamide, N,N-diallylacrylamide, N,N-di-allylmethacrylamide, N,N-di-n-butylacrylamide, N,N-di-n-butylmethacrylamide, N,N-ethylmethylacrylamide, and N,N-ethylmethylmethacrylamide.

[0084] Among these, from the viewpoint of exerting the effects of the present embodiment, the (meth)acrylamide compound is preferably N,N-dimethylacrylamide, N,N-diethylacrylamide, N,N-di-n-propylacrylamide, N,N-di-isopropylacrylamide, N,N-diallylacrylamide, N,N-di-n-butylacrylamide, or N,N-ethylmethylacrylamide, and more preferably N,N-dimethylacrylamide.

[0085] An example of the amino group-containing (meth)acrylic acid ester compound is a compound represented by the following general formula (2).

[0086] [ka]

[0087] In the general formula (2), R 16R represents a hydrogen atom or a methyl group. 17 and R 18 each independently represents a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms (preferably 1 to 2 carbon atoms). The alkyl group may be linear, branched, or cyclic (alicyclic). k is 1 or more and 4 or less, and preferably 1 or more and 3 or less.

[0088] Examples of amino group-containing (meth)acrylic acid ester compounds include N,N-dimethylaminoethyl acrylate, N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl acrylate, N,N-diethylaminoethyl methacrylate, N,N-dimethylaminopropyl acrylate, and N,N-dimethylaminopropyl methacrylate.

[0089] Among these, from the viewpoint of exerting the effects of the present embodiment, N,N-dimethylaminoethyl acrylate, N,N-diethylaminoethyl acrylate, and N,N-dimethylaminopropyl acrylate are preferred as the amino group-containing (meth)acrylic acid ester compound.

[0090] The proportion of the structural units derived from the monomer having a nitrogen-containing functional group in the total mass of the polymer component (A) is, from the viewpoint of realizing the effects of this embodiment, preferably from 1 mass% to 20 mass%, more preferably from 4.5 mass% to 18 mass%, and even more preferably from 9 mass% to 15 mass%. When the proportion of the constitutional unit derived from the monomer having a nitrogen-containing functional group is within this range, it becomes easier to adjust the adhesive strength of the pressure-sensitive adhesive sheet when heated and the cohesiveness of the pressure-sensitive adhesive layer.

[0091] When the acrylic copolymer contains a polymer component (AX), examples of the third copolymerization component of the polymer component (AX) include, in addition to the above-mentioned functional group-containing monomers, copolymer units derived from at least one monomer selected from the group consisting of an alkoxyalkyl group-containing (meth)acrylic acid ester, an aromatic ring-containing (meth)acrylic acid ester, vinyl acetate, and styrene.

[0092] Examples of the alkoxyalkyl group-containing (meth)acrylic acid ester include methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate. An example of the (meth)acrylic acid ester having an aromatic ring is phenyl (meth)acrylate. These monomers may be used alone or in combination of two or more kinds.

[0093] The weight average molecular weight (Mw) of the (meth)acrylic copolymer is preferably 50,000 to 2,000,000, more preferably 80,000 to 1,000,000, and even more preferably 100,000 to 400,000. If the weight average molecular weight Mw of the (meth)acrylic copolymer is 50,000 or more, the adhesive sheet can be easily peeled off without leaving any adhesive residue on the adherend. The smaller the weight average molecular weight Mw of the (meth)acrylic copolymer, the lower the adhesive strength of the adhesive sheet to polyimide at 25°C (room temperature) after heat treatment at 190°C for 1.5 hours in a nitrogen atmosphere tends to be. The weight average molecular weight (Mw) of the (meth)acrylic copolymer is a standard polystyrene equivalent value measured by gel permeation chromatography (GPC), and is specifically obtained by measuring under the following conditions. (Measurement conditions) GPC equipment: Tosoh Corporation, product name "HLC-8320" Measurement sample: 1% sample concentration in tetrahydrofuran solution Column: Two "TSK gel Super HM-H" columns and one "TSK gel Super H2000" column (both manufactured by Tosoh Corporation) connected in series Column temperature: 40°C Developing solvent: Tetrahydrofuran Flow rate: 0.60mL / min The weight average molecular weight (Mw) of the polymer component (A) can be measured in the same manner as the weight average molecular weight (Mw) of the (meth)acrylic copolymer.

[0094] The (meth)acrylic copolymer can be produced by using the various raw material monomers described above according to a conventionally known method.

[0095] The form of copolymerization of the (meth)acrylic copolymer is not particularly limited, and may be any of a block copolymer, a random copolymer, or a graft copolymer.

[0096] In this embodiment, the proportion of the mass of the polymer component in the total mass of the pressure-sensitive adhesive layer 12 is preferably 50 mass % or more and 90 mass % or less, and more preferably 65 mass % or more and 85 mass % or less. In this embodiment, the proportion of the mass of the acrylic copolymer in the total mass of the pressure-sensitive adhesive layer 12 is preferably 50% by mass or more and 90% by mass or less, and more preferably 65% ​​by mass or more and 85% by mass or less.

[0097] In this embodiment, the polymer component (A) is preferably crosslinked with a crosslinking agent. It is believed that the cohesive strength of the pressure-sensitive adhesive layer is further maintained by further crosslinking the polymer component (A) with a crosslinking agent, because the three-dimensional network structure formed from the polymer component (A) and the three-dimensional network structure of the cured product (B) form an interpenetrating network structure.

[0098] In the present embodiment, examples of the crosslinking agent for the (meth)acrylic copolymer include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, an aziridine-based crosslinking agent, a metal chelate-based crosslinking agent, an amine-based crosslinking agent, and an amino resin-based crosslinking agent, etc. These crosslinking agents may be used alone or in combination of two or more kinds.

[0099] In the present embodiment, from the viewpoint of improving the heat resistance and adhesive strength of the (meth)acrylic adhesive composition, among these crosslinking agents, a crosslinking agent (isocyanate-based crosslinking agent) that is a compound having an isocyanate group is preferred. Examples of the isocyanate-based crosslinking agent include polyvalent isocyanate compounds such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and lysine isocyanate. The polyisocyanate compound may be a trimethylolpropane adduct type modified product of these compounds, a biuret type modified product obtained by reacting these compounds with water, or an isocyanurate type modified product having an isocyanurate ring.

[0100] In this embodiment, when the pressure-sensitive adhesive layer contains polymer component (A) crosslinked by a crosslinking agent, the blending ratio of polymer component (A) to crosslinking agent before crosslinking is preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 1 part by mass or more and 15 parts by mass or less, and even more preferably 5 parts by mass or more and 10 parts by mass or less, per 100 parts by mass. Even when a (meth)acrylic copolymer is used as the polymer component (A), the compounding ratio of the (meth)acrylic copolymer to the crosslinking agent before crosslinking is preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 1 part by mass or more and 15 parts by mass or less, and even more preferably 5 parts by mass or more and 10 parts by mass or less, per 100 parts by mass. It is preferable for the blending ratio of the polymer component (A) to the crosslinking agent before crosslinking to be within the above range, since this makes it easier to improve the adhesive strength of the adhesive sheet when heated.

[0101] In this embodiment, when the polymer component (A) is crosslinked by a crosslinking agent, the adhesive layer may contain the polymer component (A), the crosslinking agent, and a crosslinking accelerator. It is preferable to use a crosslinking accelerator appropriately selected according to the type of crosslinking agent. For example, when the (meth)acrylic copolymer is crosslinked by a polyisocyanate compound as a crosslinking agent, an organometallic compound-based crosslinking accelerator such as an organotin compound can be used.

[0102] It is also preferable that the pressure-sensitive adhesive layer 12 contains a crosslinked product obtained by crosslinking the above-mentioned (meth)acrylic copolymer with a crosslinking agent.

[0103] ·Cured product (B) The pressure-sensitive adhesive layer according to this embodiment contains a cured product of an energy ray-curable component (cured product (B)). The energy ray curable component includes an energy ray curable compound. The energy ray curable compound is a compound that is cured by irradiation with energy rays. The energy ray for curing the energy ray curable component is preferably at least one of ultraviolet rays (UV) and electron beams (EB), and more preferably ultraviolet rays.

[0104] The energy ray curable compound according to the present embodiment is not particularly limited and can be selected from conventionally known energy ray curable compounds. Examples of the energy ray curable compound include energy ray curable monomers, low molecular weight compounds, oligomers, and resins. The energy ray curable component may be a composition containing at least one selected from the group consisting of energy ray curable monomers, low molecular weight compounds, oligomers, and resins.

[0105] The energy ray curable component preferably contains at least one of a low molecular weight compound having a polymerizable functional group and an oligomer having a polymerizable functional group as the energy ray curable compound. When the energy ray curable component is a low molecular weight compound or oligomer having a polymerizable functional group, the crosslink density of the three-dimensional network structure in the cured product (B) is high. When the pressure-sensitive adhesive layer contains a cured product (B) of the energy ray curable component containing at least one of a low molecular weight compound having a polymerizable functional group and an oligomer having a polymerizable functional group, and a polymer component (A), the polymer component (A) easily penetrates into the three-dimensional network structure of the cured product, and the effect of improving the cohesive force of the pressure-sensitive adhesive layer is more easily obtained. The formula weight of the low molecular weight compound having a polymerizable functional group is usually 3,000 or less, and preferably 2,000 or less. The theoretical molecular weight of the oligomer having a polymerizable functional group is usually 10,000 or less, and preferably 8,000 or less.

[0106] The polymerizable functional group may be a functional group having a polymerizable carbon-carbon double bond. The polymerizable functional group is preferably, for example, any group selected from the group consisting of a (meth)acryloyl group, a vinyl group, and an allyl group.

[0107] From the viewpoint of improving the adhesive strength of the adhesive sheet to polyimide at 100°C, the number of polymerizable functional groups possessed by the energy ray curable compound contained in the energy ray curable component is preferably 2 to 6 in one molecule, more preferably 2 to 5 inclusive, even more preferably 2 to 3 inclusive, and particularly preferably 2 inclusive. Since the energy ray-curable component is a compound having two polymerizable functional groups in one molecule (bifunctional energy ray-curable compound), the cohesive strength of the adhesive layer is improved while the crosslinking density is kept low compared to a trifunctional or higher functional cured product (B), and the adhesive layer is able to better conform to minute irregularities on the surface of the adherend. In addition, the adhesive strength is easily improved in a heated environment in the sealing process, the flexibility of the adhesive is maintained, and the occurrence of adhesive residue is more easily suppressed. The heated environment in this embodiment is not particularly limited, but an example thereof is the sealing process. When the adhesive strength in a high-temperature environment is improved, when the adhesive sheet is placed in a high-temperature and vacuum environment, it becomes easier to prevent blisters from occurring at the interface between the adhesive sheet and the adherend due to gas generated from the adhesive sheet itself or from the member, and the adherend from peeling off from the adhesive sheet. The high-temperature environment in this embodiment is not particularly limited, but an example thereof is a process in which, after the sealing process, a plasma treatment is performed on the surface of the sealing material as a pretreatment for wiring while the adhesive sheet is still attached. Incidentally, by making the number of polymerizable functional groups in one molecule to be two or more, it becomes easier to form a three-dimensional network structure.

[0108] In one aspect of this embodiment, from the viewpoint of improving adhesive strength to an adherend such as polyimide (in one aspect of this embodiment, from the viewpoint of improving adhesive strength to polyimide in a high temperature or high temperature and reduced pressure environment), the energy ray curable compound is preferably a compound having a polymerizable functional group and a cyclic structure. The polymerizable functional group is as described above. The cyclic structure is more preferably at least one cyclic structure selected from the group consisting of an aromatic ring, a heterocyclic ring, and an aliphatic ring. It is also preferable that the energy ray curable compound is a compound having at least one cyclic structure of an aromatic ring and an aliphatic ring.

[0109] The breaking strength per unit cross-sectional area of ​​the adhesive layer containing the cured product (B) of the energy ray curable compound is 4.5 N / mm 2 It is preferable that the resistance is 5.0N / mm or more. 2 The method for measuring the breaking strength per unit cross-sectional area of ​​the pressure-sensitive adhesive layer is as described in the Examples below. In the case where the energy ray curable compound has two or more (preferably two) polymerizable functional groups in one molecule and has a cyclic structure, the breaking strength per unit cross-sectional area of ​​the pressure-sensitive adhesive layer containing the cured product of the energy ray curable compound is 4.5 N / mm 2 It is preferable that the resistance is 5.0N / mm or more. 2 More preferably, the breaking strength is equal to or more than that. By increasing the breaking strength in this way, the adhesive transfer prevention effect can be further improved. For example, in the case where the adhesive layer contains the polymer component (AX) and the energy ray curable compound in the cured product (B) is derived from a compound having a cyclic structure, even if the adhesive strength at 100°C is high, the adhesive transfer prevention effect can be further improved by increasing the breaking strength.

[0110] In one aspect of the present embodiment, the energy ray-curable compound is also preferably a compound having no cyclic structure and having a polymerizable functional group and a chain structure, and in this case, it is more preferable that the energy ray-curable compound is a polyfunctional energy ray-curable compound having no cyclic structure and having a chain structure.

[0111] In one aspect of this embodiment, a methylene group is present between a first polymerizable functional group and a second polymerizable functional group, which are arbitrarily selected from two or more polymerizable functional groups possessed by the multifunctional energy ray curable compound, and the number of methylene groups present in a linear chain between the first polymerizable functional group and the second polymerizable functional group (hereinafter also referred to as "functional group chain length") is preferably 4 or more, more preferably 6 or more. When the number of methylene groups present in a linear chain between the first polymerizable functional group and the second polymerizable functional group is 4 or more, the Young's modulus of the adhesive layer is reduced. As a result, even if the adhesive strength at room temperature after heating is low, the initial adhesion after the adhesive sheet is attached to the adherend is maintained. A method for determining the number of methylene groups present in a linear chain between the first polymerizable functional group and the second polymerizable functional group will be described using dipentaerythritol hexaacrylate as an example.

[0112] [ka]

[0113] In the case of dipentaerythritol hexaacrylate, two polymerizable functional groups are selected, and the number of methylene groups bonded in a linear chain between the first polymerizable functional group (acryloyl group) and the second polymerizable functional group (acryloyl group) is defined as the maximum number, which is 6. When there are three or more polymerizable functional groups in a molecule, such as dipentaerythritol hexaacrylate, the maximum number of the chain length between functional groups may be 4 or more. The chain length between functional groups is preferably 4 or more between all functional groups in the molecule. In the case of dipentaerythritol hexaacrylate, two hydrogen atoms are substituted with other groups in the linearly bonded methylene groups 2 and 5 in the above structural formula. In addition, for example, in tripropylene glycol diacrylate, some of the linearly bonded methylene groups have hydrogen atoms substituted with methyl groups, and these methylene groups are indirectly bonded via oxygen atoms.

[0114] In one aspect of this embodiment, a methylene group is present between a first polymerizable functional group and a second polymerizable functional group, which are arbitrarily selected from two or more polymerizable functional groups possessed by the multifunctional energy ray curable compound, and the number of methylene groups bonded in a linear chain between the first polymerizable functional group and the second polymerizable functional group is preferably 8 or more and 30 or less, more preferably 8 or more and 12 or less. By having the number of methylene groups bonded in a linear chain between the first polymerizable functional group and the second polymerizable functional group be 8 or more and 30 or less, the effect of preventing adhesive residue is further improved, and the effect of reducing the adhesive strength at room temperature after heating is also obtained. In this case, when there are three or more polymerizable functional groups in the molecule of the multifunctional energy ray curable compound, it is sufficient that the maximum number of inter-functional group chain lengths is within the above range, and it is preferable that the inter-functional group chain lengths are within the above range between all functional groups in the molecule.

[0115] Examples of the energy ray curable low molecular weight compound include polyfunctional (meth)acrylates. Examples of the energy ray curable oligomer include polyfunctional urethane (meth)acrylates, polyfunctional polyester (meth)acrylates, polyfunctional polyether (meth)acrylates, and polyfunctional silicone (meth)acrylates. These may be used alone or in combination of two or more. The term "polyfunctional" refers to the presence of two or more polymerizable functional groups in one molecule.

[0116] Among the polyfunctional (meth)acrylates, examples of (meth)acrylates having two (meth)acryloyl groups in one molecule include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, tripropylene glycol diacrylate, 1,9-nonanediol diacrylate, 1,10-decanediol diacrylate, neopentyl glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol #400 diacrylate (product name: APG-400), polypropylene glycol #700 diacrylate (product name: APG-700), hexanediol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, and propoxylated bisphenol A diacrylate. Among the polyfunctional (meth)acrylates, examples of (meth)acrylates having three (meth)acryloyl groups in one molecule include trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, and glycerol tri(meth)acrylate. Among the polyfunctional (meth)acrylates, examples of (meth)acrylates having four (meth)acryloyl groups in one molecule include pentaerythritol tetra(meth)acrylate. Among the polyfunctional (meth)acrylates, examples of (meth)acrylates having six (meth)acryloyl groups in one molecule include dipentaerythritol hexa(meth)acrylate. As the propoxylated bisphenol A diacrylate, for example, A-BPP (trade name) manufactured by Shin-Nakamura Chemical Co., Ltd. can be used. As the ε-caprolactone-modified tris-(2-acryloxyethyl) isocyanurate, for example, A-9300-1CL (trade name) manufactured by Shin-Nakamura Chemical Co., Ltd. can be used. The polyfunctional (meth)acrylates may be used alone or in combination of two or more kinds.

[0117] Among the polyfunctional (meth)acrylates, (meth)acrylates having 2 or more and 5 or less (meth)acryloyl groups in one molecule are preferred, (meth)acrylates having 2 or 3 are more preferred, and (meth)acrylates having 2 are even more preferred.

[0118] The energy ray-curable low molecular weight compound is preferably a (meth)acrylate having a cyclic structure, and more preferably a (meth)acrylate having at least one cyclic structure selected from the group consisting of an aromatic ring and an aliphatic ring.

[0119] The energy ray curable low molecular weight compound is preferably a polyfunctional (meth)acrylate having a cyclic structure. In the polyfunctional (meth)acrylate having a cyclic structure, the number of (meth)acryloyl groups is preferably 2 or more and 5 or less, more preferably 2 or 3, and even more preferably 2. In the polyfunctional (meth)acrylate having a cyclic structure, the cyclic structure is preferably at least one of an aromatic ring and an aliphatic ring.

[0120] When ultraviolet rays are used as the energy rays to be irradiated to the energy ray-curable component, the energy ray-curable component preferably further contains a photopolymerization initiator. By containing the photopolymerization initiator, the energy ray-curable component can be cured efficiently, and the polymerization curing time and the irradiation dose of the active energy rays can be reduced.

[0121] Examples of the photopolymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, Examples of the benzoic acid ester include dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tertiary-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1[4-(1-methylvinyl)phenyl]propanone], 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, and 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one. These may be used alone or in combination of two or more.

[0122] The photopolymerization initiator is preferably used in an amount of from 2 to 15 parts by mass, more preferably from 5 to 12 parts by mass, relative to 100 parts by mass of the energy ray-curable component.

[0123] The pressure-sensitive adhesive layer may contain other components within the range not impairing the effects of the present invention. Examples of other components that the pressure-sensitive adhesive layer may contain include at least one component selected from the group consisting of adhesive assistants, organic solvents, flame retardants, tackifiers, UV absorbers, light stabilizers, antioxidants, antistatic agents, preservatives, antifungal agents, plasticizers, antifoaming agents, colorants, fillers, and wettability adjusters.

[0124] In this embodiment, the proportion of the cured product (B) in the total mass of the pressure-sensitive adhesive layer is preferably from 5 mass % to 40 mass %, and more preferably from 10 mass % to 30 mass %.

[0125] The thickness of the adhesive layer is appropriately determined according to the application of the adhesive sheet. In this embodiment, the thickness of the adhesive layer is preferably 5 μm or more and 60 μm or less, and more preferably 10 μm or more and 50 μm or less. If the thickness of the adhesive layer is 5 μm or more, the adhesive layer can easily follow the unevenness of the adherend, and the occurrence of gaps can be prevented. The adherend having unevenness is not particularly limited, but an example is a chip circuit surface. Therefore, for example, there is no risk that the interlayer insulating material and the sealing resin enter the gaps of the unevenness of the circuit surface of the semiconductor chip, and the electrode pads for wiring connection on the chip circuit surface are blocked. If the thickness of the adhesive layer is 60 μm or less, the semiconductor chip is unlikely to sink into the adhesive layer, and a step between the semiconductor chip part and the resin part sealing the semiconductor chip is unlikely to occur. Therefore, there is no risk that the wiring will be broken due to the step during rewiring.

[0126] Adhesion to polyimide at 100℃ The adhesive strength of the pressure-sensitive adhesive sheet to polyimide at 100° C. is preferably 0.04 N / 25 mm or more, more preferably 0.05 N / 25 mm or more, and even more preferably 0.08 N / 25 mm or more. Adhesive sheets with an adhesive strength of 0.04 [N / 25 mm] or more maintain their adhesive strength when heated and are therefore suitable for processing. Therefore, by using an adhesive sheet with a hardness of 0.04 [N / 25 mm] or more, it is possible to prevent the adhesive sheet from peeling off from an adherend such as a semiconductor element. Furthermore, it is also possible to prevent the adherend from shifting (misalignment) from the position where it is attached to the adhesive sheet. Even when processing such as plasma treatment is performed at high temperature or in a high temperature and reduced pressure environment with the adhesive sheet attached to a semiconductor element sealed with a sealing resin (sealed body), swelling (blistering) between the adhesive sheet and the sealed body and peeling off from the sealed body are unlikely to occur. The adhesive strength of the adhesive sheet to polyimide at 100° C. is preferably 1 N / 25 mm or less, and more preferably 0.5 N / 25 mm or less.

[0127] The adhesive strength of the adhesive sheet to polyimide at 25°C (room temperature) after heat treatment at 190°C for 1.5 hours in a nitrogen atmosphere is preferably 3N / 25mm or less, more preferably 2.5N / 25mm or less. If the adhesive strength is 3N / 25mm or less, the adhesive sheet can be easily peeled off and removed after processing of electronic components.

[0128] The Young's modulus of the pressure-sensitive adhesive layer is preferably 5 MPa or less, and more preferably 4 MPa or less. When the pressure-sensitive adhesive layer has such a Young's modulus, the adhesiveness when the pressure-sensitive adhesive sheet is attached to an electronic component is improved, and the pressure-sensitive adhesive sheet can be prevented from peeling off before the start of subsequent processing.

[0129] The adhesive strength of the adhesive sheet to polyimide at 100°C is 0.06 N / 25 mm or more, and the breaking strength per unit cross-sectional area of ​​the adhesive layer is 4.5 N / mm 2 By satisfying such adhesive strength and breaking strength, the adhesive transfer prevention effect can be improved.

[0130] (base material) The substrate is a member that supports the pressure-sensitive adhesive layer. As the substrate, for example, a sheet material such as a synthetic resin film can be used. As the synthetic resin film, for example, a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a polymethylpentene film, a polyvinyl chloride film, a vinyl chloride copolymer film, a polyethylene terephthalate film, a polyethylene naphthalate film, a polybutylene terephthalate film, a polyurethane film, an ethylene-vinyl acetate copolymer film, an ionomer resin film, an ethylene-(meth)acrylic acid copolymer film, an ethylene-(meth)acrylic acid ester copolymer film, a polystyrene film, a polycarbonate film, and a polyimide film can be mentioned. As the substrate, further, a crosslinked film and a laminated film of these can be mentioned.

[0131] The substrate preferably contains a polyester resin, and more preferably is made of a material mainly composed of a polyester resin. In this specification, a material mainly composed of a polyester resin means that the mass ratio of the polyester resin to the mass of the entire material constituting the substrate is 50 mass% or more. The polyester resin is preferably any resin selected from the group consisting of, for example, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate resin, polybutylene naphthalate resin, and copolymer resins of these resins, and more preferably polyethylene terephthalate resin. The substrate is preferably a polyethylene terephthalate film or a polyethylene naphthalate film, and more preferably a polyethylene terephthalate film.

[0132] When the energy ray-curable component is cured by irradiating the energy ray from the substrate side, the substrate is preferably made of a material that transmits the energy ray. When ultraviolet light is used as the energy ray, the substrate is preferably made of a material that transmits ultraviolet light.

[0133] The lower limit of the storage modulus of the base material at 100 °C is 1 × 10 from the viewpoint of dimensional stability during processing. 7 Pa or more, and 1×10 8 The upper limit of the storage modulus of the substrate at 100° C. is 1×10 Pa or more from the viewpoint of processability. 12 It is preferable that the pressure is 0.1 Pa or less. In this specification, the storage modulus of the substrate at 100°C is the tensile modulus measured at a frequency of 1 Hz using a viscoelasticity measuring device. The substrate to be measured is cut to a width of 5 mm and a length of 20 mm, and the storage viscoelasticity at 100°C is measured using a viscoelasticity measuring device (DMAQ800, manufactured by TA Instruments) at a frequency of 1 Hz in tension mode.

[0134] In order to enhance the adhesion between the substrate and the pressure-sensitive adhesive layer, the first substrate surface may be subjected to at least one surface treatment such as a primer treatment, a corona treatment, or a plasma treatment.

[0135] The thickness of the substrate is preferably 10 μm or more and 500 μm or less, more preferably 15 μm or more and 300 μm or less, and even more preferably 20 μm or more and 250 μm or less.

[0136] (Release sheet) The release sheet is not particularly limited. For example, from the viewpoint of ease of handling, the release sheet preferably comprises a release substrate and a release agent layer formed by applying a release agent onto the release substrate. In addition, the release sheet may comprise a release agent layer on only one side of the release substrate, or may comprise a release agent layer on both sides of the release substrate. In the case where the energy ray-curable component is cured by irradiating the release sheet with energy rays from the release sheet side after lamination, the release sheet is preferably formed of a material that transmits energy rays. In the case where ultraviolet rays are used as the energy rays, the release sheet is preferably formed of a material that transmits ultraviolet rays.

[0137] Examples of the release substrate include a paper substrate, a laminated paper obtained by laminating a thermoplastic resin such as polyethylene on the paper substrate, and a plastic film. Examples of the paper substrate include glassine paper, coated paper, and cast-coated paper. Examples of the plastic film include a polyester film (e.g., polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate), and a polyolefin film (e.g., polypropylene and polyethylene). Examples of the release agent include olefin resins, rubber elastomers (e.g., butadiene resins, isoprene resins, etc.), long-chain alkyl resins, alkyd resins, fluorine resins, and silicone resins, etc. When the pressure-sensitive adhesive layer is made of a silicone pressure-sensitive adhesive composition, the release agent is preferably a non-silicone release agent.

[0138] The thickness of the release sheet is not particularly limited, and is usually from 20 μm to 200 μm, preferably from 25 μm to 150 μm. The thickness of the release agent layer is not particularly limited. When the release agent layer is formed by applying a solution containing a release agent, the thickness of the release agent layer is preferably 0.01 μm or more and 2.0 μm or less, and more preferably 0.03 μm or more and 1.0 μm or less. When a plastic film is used as the release substrate, the thickness of the plastic film is preferably 3 μm or more and 50 μm or less, and more preferably 5 μm or more and 40 μm or less.

[0139] (Method of manufacturing pressure-sensitive adhesive sheet) The method for producing the pressure-sensitive adhesive sheet is not particularly limited. When the pressure-sensitive adhesive layer is formed by a coating method, it is preferable to prepare and use a coating liquid (pressure-sensitive adhesive liquid for coating) by diluting the pressure-sensitive adhesive composition with an organic solvent. The pressure-sensitive adhesive composition contains at least an energy ray-curable component and a polymer component (A). The pressure-sensitive adhesive composition may further contain at least one component selected from the group consisting of a crosslinking agent, a crosslinking accelerator, and other components. Examples of organic solvents include aromatic solvents, aliphatic solvents, ester solvents, ketone solvents, and alcohol solvents. Examples of aromatic solvents include benzene, toluene, and xylene. Examples of aliphatic solvents include normal hexane and normal heptane. Examples of ester solvents include ethyl acetate and butyl acetate. Examples of ketone solvents include methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and cyclopentanone. Examples of alcohol solvents include isopropyl alcohol and methanol.

[0140] For example, the pressure-sensitive adhesive sheet is manufactured through the following steps. First, a pressure-sensitive adhesive composition is applied onto the first substrate surface of a substrate to form a coating film. Next, the coating film is dried, and then irradiated with energy rays to cure the energy ray curable component and form a cured product, thereby forming a pressure-sensitive adhesive layer. After that, a release sheet is attached to cover the pressure-sensitive adhesive layer. Another method for producing a pressure-sensitive adhesive sheet is to produce the sheet through the following steps. First, a pressure-sensitive adhesive composition is applied onto a release sheet to form a coating film. Next, the coating film is dried, and a first substrate surface of a substrate is bonded to the coating film. Next, an energy ray is irradiated onto the coating film through the release sheet to cure the energy ray-curable component and form a cured product, thereby forming a pressure-sensitive adhesive layer. Another method for producing a pressure-sensitive adhesive sheet includes coating a pressure-sensitive adhesive composition on a first substrate surface of a substrate to form a coating film. Next, the coating film is dried, and a release sheet is attached to the coating film to cover the coating film. Thereafter, energy rays are irradiated from at least one of the substrate side and the release sheet side to cure the energy ray-curable component in the coating film to form a cured product, thereby forming a pressure-sensitive adhesive layer.

[0141] The method for applying the coating liquid is not particularly limited, and examples of the application method include spin coating, spray coating, bar coating, knife coating, roll knife coating, roll coating, blade coating, die coating, and gravure coating. In order to prevent the organic solvent and low boiling point components from remaining in the pressure-sensitive adhesive layer, it is preferable to heat and dry the coating film after applying the coating liquid to the substrate or release sheet. When a crosslinking agent is blended in the adhesive composition, it is preferable to heat the coating film in order to promote the crosslinking reaction and improve the cohesive force. The energy ray may be irradiated before or after heating to promote the crosslinking reaction, but it is preferable to irradiate the energy ray after heating. It is considered that when the adhesive composition is heated to dry the coating film and promote the crosslinking reaction of the adhesive composition, the reaction of all functional groups involved in the crosslinking is not completed by heating, and the remaining functional groups react gradually during the storage of the adhesive sheet thereafter, and the crosslinking of the adhesive composition progresses further. Therefore, it is considered that after the coating film is heated, a structure in which the polymer component (A) is constrained in the three-dimensional network structure of the cured product (B) is formed by irradiation with energy rays, and the crosslinking of the polymer component (A) progresses further, and a state in which the crosslinked structures of the cured product (B) and the polymer component (A) penetrate each other is formed.

[0142] (Using adhesive sheets) The pressure-sensitive adhesive sheet is used as a pressure-sensitive adhesive sheet for processing electronic components. Another use of the pressure-sensitive adhesive sheet is to fix or protect electronic components. As an example of fixing or protecting electronic components, the pressure-sensitive adhesive sheet is used when sealing a semiconductor element. The pressure-sensitive adhesive sheet of the present embodiment is used after the energy ray-curable component in the pressure-sensitive adhesive composition is cured to form a cured product. The adhesive sheet is preferably used when sealing a semiconductor element that is attached to an adhesive sheet, not when mounted on a metal lead frame. Specifically, the adhesive sheet is preferably used when sealing a semiconductor element that is attached to an adhesive layer, not when mounted on a metal lead frame. That is, the adhesive sheet is preferably used in a state where the semiconductor element is directly attached to the adhesive sheet. The adhesive sheet of the present invention is unlikely to cause blistering between the adhesive sheet and the encapsulant or peeling from the encapsulant, even when a process is performed at high temperature or in a high temperature and reduced pressure environment. Examples of packaging a semiconductor element without using a metal lead frame include a panel level package (PLP) and a WLP. The adhesive sheet is preferably used in a process having the steps of adhering a frame member having a plurality of openings formed therein to the adhesive sheet, adhering a semiconductor chip to the adhesive layer exposed at the opening of the frame member, covering the semiconductor chip with an encapsulating resin, and thermally curing the encapsulating resin. The material of the sealing resin is not particularly limited, and may be a thermosetting resin or an energy ray curable resin that is cured by energy rays such as ultraviolet rays. When the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet of the present embodiment contains the polymer component (AX), the polymer component (AX) has a "nitrogen-containing functional group not containing an N-H bond", and therefore an epoxy-based resin can be suitably used as the material for the sealing resin. When the sealing resin is made of an epoxy resin, no reaction occurs between the epoxy resin and a group having an N-H bond when the adhesive sheet is peeled off from the adherend, so that the adhesive sheet can be peeled off relatively easily from the adherend and adhesive residue on the adherend can be further reduced. After the step of thermally curing the sealing resin, a processing step such as plasma treatment may be performed as a step performed at high temperature or in a high temperature and reduced pressure environment. Other than the process of thermally curing the sealing resin and the plasma treatment process, processes that are performed at high temperature or in a high temperature and reduced pressure environment include a process of sputtering metal or the like onto the electronic components, and a process of cleaning the electronic components with hot water or the like.

[0143] An intermediate layer may be provided between the substrate and the pressure-sensitive adhesive layer. It is preferable that the intermediate layer has a function according to a desired purpose. Examples of the intermediate layer include an oligomer sealing layer, a primer layer, and an antistatic layer, which will be described later. For example, by providing an intermediate layer, it is possible to improve at least one of the adhesion between the substrate and the pressure-sensitive adhesive layer, the inhibition of oligomer precipitation on the substrate surface, and antistatic properties.

[0144] In addition, a functional layer may be provided on the surface of the substrate on the side where the pressure-sensitive adhesive layer is not provided. Examples of the functional layer include an oligomer sealing layer and an antistatic layer, which will be described later. For example, by providing an intermediate layer, it is possible to improve at least one of the following: suppression of oligomer precipitation on the substrate surface and antistatic properties.

[0145] Second Embodiment The pressure-sensitive adhesive sheet according to the second embodiment differs from the pressure-sensitive adhesive sheet according to the first embodiment in that it includes an oligomer sealing layer between the substrate and the pressure-sensitive adhesive layer. Since the pressure-sensitive adhesive sheet according to the second embodiment is otherwise similar to the pressure-sensitive adhesive sheet according to the first embodiment, the description thereof will be omitted or simplified. Hereinafter, the reference numerals may be omitted.

[0146] (Oligomer sealing layer) The oligomer sealing layer is provided between the substrate and the pressure-sensitive adhesive layer. The oligomer sealing layer is a layer for sealing oligomers originating from the substrate in the substrate. The oligomer sealing layer preferably prevents the oligomers from penetrating into the pressure-sensitive adhesive layer even under high temperature conditions, for example, from 180°C to 200°C. 2 shows a cross-sectional view of an adhesive sheet 10A according to a second embodiment. The adhesive sheet 10A has an oligomer sealing layer 13. Pressure-sensitive adhesive sheet 10A has, in this order, substrate 11, oligomer sealing layer 13, and pressure-sensitive adhesive layer 12. In pressure-sensitive adhesive sheet 10A, oligomer sealing layer 13 is laminated on first substrate surface 11a. The pressure-sensitive adhesive layer 12 contains a polymer component (A) and a cured product (B). The adhesive sheet 10A of the second embodiment has an oligomer sealing layer 13 between the substrate 11 and the adhesive layer 12, so that even when the adhesive sheet 10A is heated, migration of oligomers to the interface between the adhesive layer 12 and the adherend can be suppressed. Therefore, according to the pressure-sensitive adhesive sheet 10A of the second embodiment, the adhesive strength when heated can be further improved, and adhesive residue when peeled off from an adherend can be further prevented.

[0147] -Oligomer sealing layer thickness The thickness of the oligomer sealing layer is preferably 50 nm or more and 500 nm or less, and more preferably 80 nm or more and 300 nm or less. When the thickness of the oligomer sealing layer is 50 nm or more, it is possible to effectively prevent the oligomer contained in the base material from penetrating into the pressure-sensitive adhesive layer. If the thickness of the oligomer sealing layer is 500 nm or less, for example, the pressure-sensitive adhesive sheet can be easily wound up into a roll around a core material. Examples of the material for the core material include paper, plastic, and metal.

[0148] The material of the oligomer sealing layer is not particularly limited as long as it can prevent the oligomer in the base material from penetrating into the pressure-sensitive adhesive layer 12 . For example, the oligomer sealing layer is preferably a cured film obtained by curing a composition for oligomer sealing layer. The composition for oligomer sealing layer preferably contains at least one selected from the group consisting of (A) an epoxy compound, (B) a polyester compound, and (C) a polyfunctional amino compound, more preferably contains (A) an epoxy compound and (C) a polyfunctional amino compound, and further preferably contains (A) an epoxy compound, (B) a polyester compound, and (C) a polyfunctional amino compound. The oligomer sealing layer composition may further contain (D) an acid catalyst to promote the curing reaction.

[0149] (A) Epoxy compound The (A) epoxy compound is preferably a bisphenol A type epoxy compound. Examples of the bisphenol A type epoxy compound include bisphenol A diglycidyl ether.

[0150] (B) Polyester compound The polyester compound (B) is not particularly limited, and can be appropriately selected from known polyester compounds. Specific examples of the polyester compound include a resin obtained by a condensation reaction between a polyhydric alcohol and a polybasic acid, such as a non-convertible polyester compound which is a condensate of a dibasic acid and a dihydric alcohol, or a compound modified with a non-drying oil fatty acid, and a convertible polyester compound which is a condensate of a dibasic acid and a trihydric or higher alcohol.

[0151] As the polyhydric alcohol and polybasic acid used as raw materials for the polyester compound (B), known polyhydric alcohols and polybasic acids can be appropriately selected and used.

[0152] (C) Polyfunctional amino compounds As the (C) polyfunctional amino compound, for example, a melamine compound, a urea compound, a benzoguanamine compound, and a diamine can be used. Examples of melamine compounds include hexamethoxymethylmelamine, methylated melamine compounds, and butylated melamine compounds. Examples of the urea compound include a methylated urea compound and a butylated urea compound. Benzoguanamine compounds include, for example, methylated benzoguanamine compounds and butylated benzoguanamine compounds. Examples of diamines include ethylenediamine, tetramethylenediamine, hexamethylenediamine, N,N'-diphenylethylenediamine, and p-xylylenediamine. From the viewpoint of curability, the polyfunctional amino compound (C) is preferably hexamethoxymethylmelamine.

[0153] ·(D) Acidic catalyst Examples of the acid catalyst (D) include hydrochloric acid and p-toluenesulfonic acid.

[0154] ·Cured film In this embodiment, the oligomer sealing layer is preferably a cured film obtained by curing a composition for oligomer sealing layer containing (A) a bisphenol A type epoxy compound, (B) a polyester compound, and (C) a polyfunctional amino compound in a blending ratio of (A) 50% to 80% by mass, (B) 5% to 30% by mass, and (C) 10% to 40% by mass, respectively. When (D) an acid catalyst is blended in the composition for oligomer sealing layer, the content of component (D) is preferably 1% to 5% by mass. A cured coating obtained by curing a composition for oligomer sealing layer having a blending ratio within the above-mentioned range can improve the effect of the oligomer sealing layer in preventing the penetration of oligomers into pressure-sensitive adhesive layer 12.

[0155] (Method for manufacturing the pressure-sensitive adhesive sheet according to the second embodiment) The pressure-sensitive adhesive sheet of the second embodiment is produced, for example, through the following steps. First, the composition for forming an oligomer sealing layer is applied onto the first substrate surface of the substrate to form a coating film. Next, the coating film is heated and cured to form a cured film that will become the oligomer sealing layer. The heat curing conditions are, for example, 120°C or higher and 170°C or lower, and 5 seconds or higher and 5 minutes or lower. Next, a pressure-sensitive adhesive layer is formed on the oligomer sealing layer formed on the first substrate surface of the substrate in the same manner as described in the first embodiment.

[0156] <Third embodiment> The pressure-sensitive adhesive sheet according to the third embodiment differs from the pressure-sensitive adhesive sheet according to the second embodiment in that it has oligomer sealing layers on both sides of the substrate, and is otherwise similar to the second embodiment, and therefore description thereof will be omitted or simplified. FIG. 3 shows a cross-sectional view of an example of a pressure-sensitive adhesive sheet 10B according to the third embodiment. The adhesive sheet 10B has, in this order, an oligomer sealing layer 13B formed on the second substrate surface 11b of the substrate 11, the substrate 11, an oligomer sealing layer 13A formed on the first substrate surface 11a of the substrate 11, and an adhesive layer 12. The pressure-sensitive adhesive sheet 10B of the third embodiment has oligomer sealing layers 13A, 13B on both sides of the substrate 11, and therefore, in addition to the effect of the second embodiment, it is possible to suppress the oligomers precipitated on the second substrate surface 11b from adhering to and contaminating members and devices other than the adherend. For example, when manufacturing a semiconductor device, it is possible to suppress the contamination of a plate-like member that comes into contact with the pressure-sensitive adhesive sheet in a hot press process.

[0157] (Method for manufacturing pressure-sensitive adhesive sheet according to the third embodiment) The adhesive sheet of the third embodiment is produced by forming a coating film made of the oligomer sealing layer forming composition on the first substrate surface and the second substrate surface of a substrate in the adhesive sheet producing method of the second embodiment.

[0158] [Modifications of the embodiment] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention are included in the present invention. In the following description, the same reference numerals are used to designate the same components as those described in the above-described embodiment, and the description thereof will be omitted or simplified.

[0159] The PSA sheet may be a piece of sheet, or may be provided in a state where a plurality of PSA sheets are laminated together, in which case, for example, the PSA layer may be covered by the substrate of another PSA sheet to be laminated. The pressure-sensitive adhesive sheet may be a strip-shaped sheet or may be provided in a rolled-up state. The rolled-up pressure-sensitive adhesive sheet can be used by being unwound from the roll and cut to a desired size. The pressure-sensitive adhesive sheet may be provided in a state in which it is cut to a desired size in advance and supported on a strip-shaped release sheet. The oligomer sealing layer may be provided only on the second substrate surface of the substrate. An adhesive layer may be provided directly on the second substrate surface of the substrate, or via an oligomer sealing layer or the like. The adhesive layer is used when attaching a pressure-sensitive adhesive sheet to a support substrate or the like with the adhesive layer, and fixing electronic components on the adhesive layer of the pressure-sensitive adhesive sheet. The adhesive used in the adhesive layer may be the same type as the adhesive in the adhesive layer, or may be a different type. EXAMPLES

[0160] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0161] [Evaluation method] The pressure-sensitive adhesive sheets were evaluated according to the methods described below. The results are shown in Tables 1, 2 and 3.

[0162] (Evaluation of blister occurrence under high temperature and vacuum conditions) A glass epoxy substrate (Hitachi Chemical Co., Ltd., "MCL-E-679FG" (product name), 100 mm x 100 mm x 0.4 mm) was polished using an abrasive of #800. After polishing, the adhesive sheets prepared in the Examples and Comparative Examples were attached to the entire polished surface of the glass epoxy substrate. A roll laminator was used to attach the adhesive sheets. The adhesive sheet was attached to a glass epoxy substrate and then vacuum laminated at 100°C using a heating vacuum laminator (Nikko Materials Co., Ltd., "V130" (product name)) to prepare a measurement sample. After vacuum lamination, the measurement sample was immersed in hot water at 85°C for 30 minutes. After immersion, the measurement sample was removed from the hot water and the water droplets on the surface of the measurement sample were wiped off. After wiping, the measurement sample was placed in a heated vacuum dryer at 25°C. Thereafter, the pressure inside the heating vacuum dryer was reduced (less than 0.005 MPa), and the measurement sample was heated to a set temperature of 130°C. The temperature rise rate was 5°C / min. The occurrence of blisters was visually confirmed until the temperature inside the heating vacuum dryer rose from 25°C to 130°C. Rating A: No blisters were observed. Judgment B: Area of ​​adherend 10cm 2 Blisters occurred over an area of ​​less than 50% of the surface. Judgment C: Area of ​​adherend 10cm 2 Blisters occurred over 50% or more of the surface area.

[0163] (Initial adhesion test) The surface of a glass epoxy substrate (Hitachi Chemical Co., Ltd., "MCL-E-679FG" (product name), 100 mm x 100 mm x 0.4 mm) was polished using a #800 abrasive. After polishing, the adhesive sheets prepared in the Examples and Comparative Examples were attached to the entire polished surface of the glass epoxy substrate. The adhesive sheets were attached by moving a 2 kg roll back and forth once. After leaving it to stand for 30 minutes in a standard environment (23°C 50% RH), the adhesive strength was measured in the same standard environment. The measurement conditions were as follows: Equipment: Shimadzu tensile testing machine AG-X plus 10kN ·Peel angle: 180° ·Peel speed: 300mm / min When the adhesive strength was 0.08N / 25mm or more, it was rated A, and when it was less than 0.08N / 25mm, it was rated B.

[0164] (Adhesion to polyimide at 100℃) A polyimide film (Kapton 200H (trade name), manufactured by Toray DuPont Co., Ltd.) was attached to an aluminum plate (150 mm x 70 mm, thickness 1 mm) using a double-sided tape (TL-450S-16 (trade name), manufactured by Lintec Corporation). The adhesive strength of the adhesive sheet was measured for the polyimide film by changing the measurement temperature, with reference to JIS Z 0237 (2000). The adhesive sheets prepared in the examples and comparative examples were attached to the polyimide film to prepare a measurement sample, which was placed in an environment of 23°C and 50% relative humidity for 30 minutes, and then placed in an environment of 100°C for 3 minutes, and then a tensile test was performed in an environment of 100°C. In addition, adhesive sheets with an adhesive strength of 0.04 [N / 25 mm] or more are judged to have sufficient adhesive strength and to be sheets that exhibit good process suitability. The measurement conditions were as follows: Equipment: Tensile testing machine with thermostatic chamber ("Tensilon" (product name) manufactured by Orientec Co., Ltd.) · Peeling angle: 180° · Peeling speed: 300mm / min In this specification, polyimide may be abbreviated as PI.

[0165] (Adhesive strength to polyimide at room temperature after heating) As in the case of the adhesive strength to polyimide at 100° C., the adhesive sheets produced in the Examples and Comparative Examples were attached to the above-mentioned polyimide film to produce measurement samples, which were then heated in a nitrogen environment. The heating conditions were as follows: Equipment: MOTOYAMA MS-3642 ·N2 flow rate: 1.5L / min (N2 purity: 99.995% (volume)) Actual temperature: 190°C Time: 1.5 hours After that, it was left to stand in a standard environment (23°C, 50% RH) for more than 6 hours, and then the adhesive sheet was peeled off from the measurement sample in the same standard environment at a peel angle of 180° and a peel speed of 300 mm / min.

[0166] (Young's modulus of adhesive layer) In the examples and comparative examples, instead of laminating the dried coating film of the adhesive solution for application to a substrate with an oligomer sealing layer, the coating film was laminated to the surface of a release film "SP-PET381031" (product name) manufactured by Lintec, which has a release layer, to prepare a single-layer adhesive layer without a substrate. Four of these adhesive layers were laminated so that the sample had a thickness of 200 μm. A tensile test was performed under the following conditions using this laminate of only the adhesive layer as a sample, and the change in stress relative to the change in strain was graphed from the measurement results of strain and stress. The Young's modulus of the adhesive was measured from the initial slope of the change in stress relative to the change in strain. Equipment: Shimadzu tensile testing machine AG-X plus 10kN · Test sample size: Measurement area length 50mm x width 15mm · Tensile test speed: 200mm / min

[0167] (Breaking strength per unit cross-sectional area of ​​adhesive layer) A tensile test was carried out in the same manner as in measuring the Young's modulus of the adhesive layer, and the maximum force at which break occurred (breaking strength) was divided by the initial cross-sectional area of ​​the sample to calculate the breaking strength per unit area.

[0168] (First residue evaluation (first adhesive residue evaluation)) The copper foil was polished in advance with an abrasive of #800 to form polishing scratches along one direction on the surface of the copper foil (arithmetic mean roughness after polishing Ra = 0.2 ± 0.1 μm). The pressure-sensitive adhesive sheets prepared in the examples and comparative examples were attached to the surface of the copper foil on which the polishing scratches had been formed. Here, only for the pressure-sensitive adhesive sheets of Comparative Examples 1-3, a high-pressure mercury lamp manufactured by Eye Graphics was used as the ultraviolet irradiation device, and an illuminance of 200 mW / cm was used. 2 , cumulative light intensity 200mJ / cm 2 The copper foil was irradiated with ultraviolet light under the following conditions. The adhesive sheet attached to the copper foil was then heated at 100°C for 30 minutes, then at 180°C for 30 minutes, and then at 190°C for 60 minutes. After heating, the adhesive sheet was peeled off at room temperature at a speed of 3 mm / min. The adhesive sheet was peeled off in a direction perpendicular to the polishing scratches. After the adhesive sheet was peeled off, the surface of the copper foil was observed with a digital microscope to evaluate the adhesive residue. The following criteria were used to evaluate the adhesive residue. Rating A: No glue residue was left behind. Grade B: Glue remained in some areas. C rating: Glue residue remained over the entire surface.

[0169] (Second residue evaluation (second adhesive residue evaluation)) A polyimide film (Kapton 200H (product name), manufactured by Toray DuPont Co., Ltd.) was attached to the mirror surface of a silicon mirror wafer (diameter 6 inches, thickness 0.68 mm) using double-sided tape (TL-450S-16 (product name), manufactured by Lintec Corporation). Thereafter, circular marks of 200 μmφ were engraved at 3 mm intervals on the surface of the polyimide film using a laser marker (CSM300M manufactured by EO TECHNICS) (laser wavelength 512 nm, output 1.0 W, scanning speed 300 mm / s). In order to perform the evaluation under conditions that tend to cause adhesive residue, the above marks were engraved on the surface of the polyimide film by laser ablation to form projections and recesses, as described above. The pressure-sensitive adhesive sheets prepared in the Examples and Comparative Examples were laminated onto the processed surface of the polyimide film using the weight of a 2 kg roller in accordance with JIS Z0237 (2000), and then heat-laminated on top of that to prepare a measurement sample. The heat lamination conditions were as follows: Equipment: Vacuum laminator V-130, manufactured by Nikko Materials Co., Ltd. ·Heating temperature: 100℃ ·Vacuum standby: 60sec Diaphragm pressure: 0.3MPa

[0170] The measurement sample was then heated in a nitrogen environment. The heating conditions were as follows: Equipment: MOTOYAMA MS-3642 ·N2 flow rate: 1.5L / min (N2 purity: 99.995% (volume)) Actual temperature: 190℃ Time: 1.5hr

[0171] After that, the sample was left to stand in a standard environment (23°C, 50% RH) for 6 hours or more, and then the adhesive sheet was peeled off from the measurement sample at a peel angle of 180° and a peel speed of 300 mm / min. After the adhesive sheet was peeled off, the surface of the polyimide film was observed with an SEM (scanning electron microscope, observation magnification 3000 times), and the adhesive residue was evaluated based on the state of residue generation. The judgment criteria for the evaluation of adhesive residue were as follows. -Judgment criteria- Grade A: No residue was found. Grade B: Residue was present and the size of the residue was less than 5 μm. C rating: Residue was present and the size of the residue was 5 μm or more and less than 10 μm. D: Residue was present and the size of the residue was 10 μm or more.

[0172] [Preparation of Adhesive Sheet] [Example 1-1] (1-1) Preparation of oligomer sealant solution for application The following (A) bisphenol A type epoxy compound, (B) polyester compound, (C) polyfunctional amino compound, and (D) acid catalyst were mixed and thoroughly stirred to prepare an oligomer sealant solution for coating (oligomer sealing layer composition) according to Example 1-1. (A) Bisphenol A epoxy compound "EPICLON H-360" (product name) manufactured by DIC, solid content concentration: 40% by mass, mass average molecular weight: 25000 (B) Polyester compound "Vylon GK680" (product name) manufactured by Toyobo Co., Ltd., number average molecular weight: 6000, glass transition temperature: 10°C (C) Polyfunctional amino compound Hexamethoxymethylmelamine, Cymel 303 (product name) manufactured by Japan Cytec Industries Co., Ltd. (D) Acidic catalyst Methanol solution of p-toluenesulfonic acid (solid content: 50% by mass) Specifically, 19.0 parts by mass of the above (B) polyester compound diluted in toluene (solid content concentration: 30% by mass) and 11.4 parts by mass of the above (C) hexamethoxymethylmelamine were added to 100 parts by mass of the above (A) bisphenol A type epoxy compound, and further diluted with a mixed solvent of toluene / methyl ethyl ketone = 50% by mass / 50% by mass to prepare a solution with a solid content concentration of 3% by mass. The prepared solution was stirred, and 2.9 parts by mass of (D) p-toluenesulfonic acid in methanol solution (solid content concentration: 50% by mass) was added to the stirred solution to obtain an oligomer sealant solution for application. Note that all parts by mass are calculated as solid content.

[0173] (1-2) Preparation of oligomer sealing layer (preparation of substrate with oligomer sealing layer) The prepared oligomer sealant solution for application was uniformly applied to one side of an annealed biaxially stretched polyethylene terephthalate film (Teijin Film Solutions Co., Ltd., "Teijin Tetron G2A" (product name), thickness 25 μm) by the Mayer bar coating method. The coated film was passed through the inside of an oven, and the coating film was heat-cured to form an oligomer sealing layer with a thickness of 150 nm, to obtain a substrate with an oligomer sealing layer. The hot air blowing conditions in the oven were a temperature of 150°C and a wind speed of 8 m / min. The processing speed in the oven was adjusted so that the coated film passed through the inside of the oven in 20 seconds.

[0174] (1-3) Preparation of adhesive composition The following materials (polymer (polymer component), crosslinking agent, low molecular weight compound having a polymerizable functional group, photopolymerization initiator, and dilution solvent) were mixed and thoroughly stirred to prepare a pressure-sensitive adhesive liquid for application according to Example 1-1. Polymer: acrylic ester copolymer, 100 parts by weight (solids) The acrylic acid ester copolymer was prepared by copolymerizing 92.8% by mass of 2-ethylhexyl acrylate, 7.0% by mass of 2-hydroxyethyl acrylate, and 0.2% by mass of acrylic acid. Crosslinking agent: Aliphatic isocyanate containing hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd.; Coronate HX), 7.4 parts by mass (solid content) Low molecular weight compound having a polymerizable functional group: Tricyclodecane dimethanol diacrylate [A-DCP, manufactured by Shin-Nakamura Chemical Co., Ltd.] 23.3 parts by mass (solid content) Photopolymerization initiator: 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one [IGM Resin; Omnirad 127] 4.1 parts by mass (solid content) Dilution solvent: Ethyl acetate was used, and the solids concentration of the adhesive solution for application was adjusted to 30 mass %.

[0175] (1-4) Preparation of adhesive layer The prepared adhesive solution for application was applied to the release layer side of a release film (manufactured by Lintec Corporation; SP-PET382150) made of a 38 μm thick transparent polyethylene terephthalate film with a silicone-based release layer, using a knife coater. The coating of the adhesive solution for application on the release film was then heated at 90° C. for 90 seconds, and then heated at 115° C. for 90 seconds to dry the coating. Thereafter, the coating was bonded to the surface of the substrate with an oligomer sealing layer obtained by the above-mentioned procedure, on which the oligomer sealing layer was provided. The coating was then irradiated with ultraviolet light using a high-pressure mercury lamp manufactured by Eye Graphics Corporation, with an illuminance of 200 mW / cm. 2 , cumulative light intensity 200mJ / cm 2 An adhesive layer having a thickness of 50 μm was produced by irradiating the release film side with ultraviolet light under the conditions of: In this way, an adhesive sheet according to Example 1-1 was obtained.

[0176] [Example 1-2] The adhesive sheet of Example 1-2 was obtained in the same manner as Example 1-1, except that 23.3 parts by mass (solid content) of 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPEF) was used instead of 23.3 parts by mass (solid content) of tricyclodecane dimethanol diacrylate.

[0177] [Examples 1-3] The adhesive sheet of Example 1-3 was obtained in the same manner as Example 1-1, except that 23.3 parts by mass (solid content) of propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP) was used instead of 23.3 parts by mass (solid content) of tricyclodecane dimethanol diacrylate.

[0178] [Examples 1-4] The adhesive sheet of Example 1-4 was obtained in the same manner as Example 1-1, except that 23.3 parts by mass (solid content) of dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-DPH) (chain length between functional groups: 6) was used instead of 23.3 parts by mass (solid content) of tricyclodecane dimethanol diacrylate.

[0179] [Examples 1-5] An adhesive sheet of Example 1-5 was obtained in the same manner as in Example 1-1, except that 23.3 parts by mass (solid content) of ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-9300-1CL) was used instead of 23.3 parts by mass (solid content) of tricyclodecane dimethanol diacrylate.

[0180] [Comparative Example 1-1] In preparing the adhesive composition, the following materials (polymer, adhesive assistant, crosslinking agent, and dilution solvent) were blended, and in preparing the adhesive layer, the step of irradiating with ultraviolet light was omitted, but otherwise the adhesive sheet of Comparative Example 1-1 was obtained in the same manner as in Example 1-1. Polymer: acrylic ester copolymer, 100 parts by weight (solids) The acrylic acid ester copolymer was prepared by copolymerizing 92.8% by mass of 2-ethylhexyl acrylate, 7.0% by mass of 2-hydroxyethyl acrylate, and 0.2% by mass of acrylic acid. Adhesive aid: Hydrogenated polybutadiene with hydroxyl groups at both ends (GI-1000, manufactured by Nippon Soda Co., Ltd.), 12.5 parts by weight (solid content) Crosslinking agent: Aliphatic isocyanate containing hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd.; Coronate HX), 8.75 parts by mass (solid content) Dilution solvent: Methyl ethyl ketone was used, and the solids concentration of the adhesive solution for application was adjusted to 30 mass %.

[0181] [Comparative Example 1-2] An adhesive sheet of Comparative Example 1-2 was obtained in the same manner as in Comparative Example 1-1, except that no adhesive assistant was added in preparing the adhesive composition.

[0182] [Comparative Example 1-3] A pressure-sensitive adhesive sheet of Comparative Example 1-3 was obtained in the same manner as in Example 1-1, except that the step of irradiating with ultraviolet light was omitted. In addition, when evaluating the first residue, the evaluation was performed after irradiating with ultraviolet light under the above-mentioned conditions.

[0183] [Table 1]

[0184] [Test and evaluation results] As a result of the blister test, Examples 1-1, 1-2, and 1-3 did not develop blisters and were rated A, Examples 1-4 and 1-5 were rated B, Comparative Examples 1-1 and 1-2 were rated C, and Comparative Example 1-3 was rated B. By curing the ultraviolet-curable component to form a cured product before application to the adherend, the adhesive layer containing the cured product had improved adhesive strength and was found to have an effect of suppressing blister generation. Examples 1-1, 1-2, and 1-3, which used an ultraviolet-curable component having two polymerizable functional groups in one molecule, had a higher effect of suppressing blisters. As a result of the first residue evaluation, Examples 1-1, 1-2, 1-3, 1-4, and 1-5 were rated A, with no adhesive residue. Comparative Example 1-1 was rated B, with some adhesive residue, and Comparative Examples 1-2 and 1-3 were rated C, with adhesive residue over the entire surface. These results confirmed that no adhesive residue was left behind even when the adhesive sheets of Examples 1-1, 1-2, 1-3, 1-4 and 1-5 were used in the sealing process, and further that the adhesive sheets of Examples 1-1, 1-2 and 1-3 were less likely to peel off even in processes where blisters are likely to occur, such as plasma processes.

[0185] [Example 2-1] (2-1) Preparation of oligomer sealant solution for application An oligomeric sealant liquid for coating according to Example 2-1 was prepared in the same manner as in the preparation of the oligomeric sealant liquid for coating according to Example 1-1.

[0186] (2-2) Preparation of oligomer sealing layer (preparation of substrate with oligomer sealing layer) An annealed biaxially oriented polyethylene terephthalate film ("Teijin Tetron G2A" (product name), thickness 25 μm, manufactured by Teijin Film Solutions Co., Ltd.) was prepared as a substrate. Hereinafter, the annealed biaxially oriented polyethylene terephthalate film is also simply referred to as "PET film." The prepared oligomer sealant liquid for application was uniformly applied to one side of the "PET film" by the Mayer bar coating method. The "PET film" after application of the oligomer sealant liquid for application was passed through the inside of an oven, and the coating film was heat cured to form an oligomer sealing layer with a thickness of 150 nm on one side of the PET film. Next, an oligomer sealing layer with a thickness of 150 nm was formed in the same manner on the other surface of the "PET film", to obtain a substrate with oligomer sealing layers on both sides. The hot air blowing conditions in the oven were a temperature of 150°C and a wind speed of 8 m / min. The processing speed in the oven was adjusted to a speed at which the "PET film" after application passed through the inside of the oven in 20 seconds.

[0187] (2-3) Preparation of adhesive composition The following materials (polymer (polymer component (A)), crosslinking agent, low molecular weight compound having a polymerizable functional group, photopolymerization initiator, and dilution solvent) were mixed and thoroughly stirred to prepare a pressure-sensitive adhesive liquid for application according to Example 2-1. Polymer: acrylic ester copolymer (polymer component (A)), 100 parts by weight (solid content) The acrylic acid ester copolymer was prepared by copolymerizing 80.8 mass% of 2-ethylhexyl acrylate, 12.0 mass% of acryloylmorpholine (a monomer having a nitrogen-containing functional group), 7.0 mass% of 2-hydroxyethyl acrylate, and 0.2 mass% of acrylic acid to prepare a polymer with a weight average molecular weight of 440,000. Crosslinking agent: Aliphatic isocyanate containing hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd.; Coronate HX), 7.4 parts by mass (solid content) Low molecular weight compound having a polymerizable functional group: Propoxylated bisphenol A diacrylate [A-BPP-3, manufactured by Shin-Nakamura Chemical Co., Ltd.] 23.3 parts by mass (solid content) Photopolymerization initiator: 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one [IGM Resin; Omnirad 127] 4.1 parts by mass (solid content) Dilution solvent: Ethyl acetate was used, and the solids concentration of the adhesive solution for application was adjusted to 30 mass %.

[0188] (2-4) Preparation of adhesive layer The prepared adhesive solution for application was applied to the release layer side of a release film (manufactured by Lintec Corporation; SP-PET382150) made of a 38 μm thick transparent polyethylene terephthalate film with a silicone-based release layer, using a knife coater. The coating of the adhesive solution for application on the release film was then heated at 90° C. for 90 seconds, and then heated at 115° C. for 90 seconds to dry the coating. Thereafter, the coating was bonded to one side of the substrate with an oligomer sealing layer obtained by the above-mentioned procedure, on which the oligomer sealing layer was provided. The coating was then irradiated with ultraviolet light using a high-pressure mercury lamp manufactured by Eye Graphics Corporation, with an illuminance of 200 mW / cm. 2 , cumulative light intensity 200mJ / cm 2 An adhesive layer having a thickness of 50 μm was produced by irradiating the adhesive sheet of Example 2-1 with ultraviolet light from the release film side under the conditions of:

[0189] [Example 2-2] The adhesive sheet of Example 2-2 was obtained in the same manner as in Example 2-1, except that the acrylic acid ester copolymer used as polymer component (A) was prepared by copolymerizing 86.8 mass% of 2-ethylhexyl acrylate, 6.0 mass% of acryloylmorpholine, 7.0 mass% of 2-hydroxyethyl acrylate, and 0.2 mass% of acrylic acid to prepare a polymer having a weight average molecular weight of 510,000.

[0190] [Example 2-3] The adhesive sheet of Example 2-3 was obtained in the same manner as in Example 2-1, except that the acrylic acid ester copolymer used as polymer component (A) was prepared by copolymerizing 89.8 mass% of 2-ethylhexyl acrylate, 3.0 mass% of acryloylmorpholine, 7.0 mass% of 2-hydroxyethyl acrylate, and 0.2 mass% of acrylic acid to prepare a polymer having a weight average molecular weight of 520,000.

[0191] [Example 2-4] The adhesive sheet of Example 2-4 was obtained in the same manner as in Example 2-1, except that the acrylic acid ester copolymer used as polymer component (A) was prepared by copolymerizing 80.8 mass% of 2-ethylhexyl acrylate, 12.0 mass% of N,N-dimethylacrylamide (monomer having a nitrogen-containing functional group) as a monomer having a nitrogen-containing functional group, 7.0 mass% of 2-hydroxyethyl acrylate, and 0.2 mass% of acrylic acid to prepare a polymer having a weight average molecular weight of 500,000.

[0192] [Example 2-5] The adhesive sheet of Example 2-5 was obtained in the same manner as in Example 2-1, except that the acrylic acid ester copolymer was prepared by copolymerizing 92.8% by mass of 2-ethylhexyl acrylate, 7.0% by mass of 2-hydroxyethyl acrylate, and 0.2% by mass of acrylic acid to prepare a polymer with a weight average molecular weight of 1,050,000. The acrylic acid ester copolymer itself was the same as the acrylic acid ester copolymer of Example 1-3.

[0193] [Comparative Example 2-2] In preparing the adhesive composition, the following materials (polymer, adhesive assistant, crosslinking agent, and dilution solvent) were blended, and in preparing the adhesive layer, the step of irradiating with ultraviolet light was omitted, but otherwise the adhesive sheet of Comparative Example 2-2 was obtained in the same manner as in Example 2-1. Polymer: acrylic ester copolymer, 100 parts by weight (solids) The acrylic acid ester copolymer was prepared by copolymerizing 92.8% by mass of 2-ethylhexyl acrylate, 7.0% by mass of 2-hydroxyethyl acrylate, and 0.2% by mass of acrylic acid to prepare a polymer having a weight average molecular weight of 1,050,000. Adhesive aid: Hydrogenated polybutadiene with hydroxyl groups at both ends (GI-1000, manufactured by Nippon Soda Co., Ltd.), 12.5 parts by weight (solid content) Crosslinking agent: Aliphatic isocyanate containing hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd.; Coronate HX), 8.75 parts by mass (solid content) Dilution solvent: Methyl ethyl ketone was used, and the solids concentration of the adhesive solution for application was adjusted to 30 mass %. The acrylic ester copolymer itself is the same as the acrylic ester copolymer according to Comparative Example 1-1.

[0194] [Table 2]

[0195] (Explanation of Table 2) "ACMO" stands for acryloylmorpholine. "DMAA" stands for N,N-dimethylacrylamide. · "PI" stands for polyimide.

[0196] [Evaluation Results] The pressure-sensitive adhesive sheets of Examples 2-1, 2-2, 2-3 and 2-4 were more favorable in the second residue evaluation than the pressure-sensitive adhesive sheet of Comparative Example 2-2. In addition, since the adhesive sheet of Example 2-5 has the same structure as that of Example 1-3, the first residue evaluation was good compared to Comparative Example 2-2 (the structure of the adhesive layer itself is the same as that of Comparative Example 1-1) as shown in Table 1, but the second residue evaluation resulted in a rating of D for both. The pressure-sensitive adhesive sheets of Examples 2-1, 2-2, 2-3, and 2-4 had an adhesive strength to polyimide of 0.04 [N / 25 mm] or more at 100° C. That is, the pressure-sensitive adhesive sheets of Examples 2-1, 2-2, 2-3, and 2-4 had sufficient adhesive strength and were sheets that showed good process suitability. According to the adhesive sheet of this embodiment, the adhesive layer contains the polymer component (A) and the cured product (B), which improves the adhesive strength when heated and prevents adhesive residue when peeled off from the adherend.

[0197] [Preparation of Adhesive Sheet] [Example 3-1] (3-1) Preparation of oligomer sealant solution for application An oligomeric sealant liquid for coating according to Example 3-1 was prepared in the same manner as in the preparation of the oligomeric sealant liquid for coating according to Example 1-1.

[0198] (3-2) Preparation of oligomer sealing layer (preparation of substrate with oligomer sealing layer) A substrate with an oligomer sealing layer according to Example 3-1 was prepared in the same manner as in the preparation of the substrate with an oligomer sealing layer according to Example 2-1.

[0199] (3-3) Preparation of adhesive composition The following materials (polymer (polymer component), crosslinking agent, low molecular weight compound having a polymerizable functional group, photopolymerization initiator, and dilution solvent) were mixed and thoroughly stirred to prepare a pressure-sensitive adhesive liquid for application according to Example 3-1. The acrylic acid ester copolymer was prepared by copolymerizing 80.8 mass% of 2-ethylhexyl acrylate, 12.0 mass% of acryloylmorpholine (a monomer having a nitrogen-containing functional group), 7.0 mass% of 4-hydroxybutyl acrylate, and 0.2 mass% of acrylic acid to prepare a polymer with a weight average molecular weight of 120,000. Crosslinking agent: Aliphatic isocyanate containing hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd.; Coronate HX), 7.4 parts by mass (solid content) Low molecular weight compound having a polymerizable functional group: Propoxylated bisphenol A diacrylate [A-BPP-3, manufactured by Shin-Nakamura Chemical Co., Ltd.] 23.3 parts by mass (solid content) Photopolymerization initiator: 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one [IGM Resin; Omnirad 127] 4.1 parts by mass (solid content) Dilution solvent: Ethyl acetate was used, and the solids concentration of the adhesive solution for application was adjusted to 30 mass %.

[0200] (3-4) Preparation of adhesive layer The adhesive layer of Example 3-1 was prepared in the same manner as in Example 2-1, except that the adhesive liquid for application in "(2-4) Preparation of adhesive layer" of Example 2-1 was changed to the adhesive liquid for application of Example 3-1.

[0201] [Example 3-2] An adhesive sheet of Example 3-2 was obtained in the same manner as in Example 3-1, except that the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) in Example 3-1 was changed to 1,6-hexanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-HD-N) (chain length between functional groups: 4).

[0202] [Example 3-3] An adhesive sheet of Example 3-3 was obtained in the same manner as in Example 3-1, except that the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) in Example 3-1 was changed to tripropylene glycol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; APG-200) (chain length between functional groups: 6).

[0203] [Example 3-4] An adhesive sheet of Example 3-4 was obtained in the same manner as in Example 3-1, except that the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) in Example 3-1 was changed to 1,9-nonanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-NOD-N) (chain length between functional groups: 9).

[0204] [Examples 3-5] An adhesive sheet of Example 3-5 was obtained in the same manner as in Example 3-1, except that the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) in Example 3-1 was changed to 1,10-decanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-DOD-N) (chain length between functional groups: 10).

[0205] [Examples 3-6] The acrylic acid ester copolymer in Example 3-1 was changed to that in Example 2-5, and further, the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) was changed to 1,10-decanediol diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-DOD-N) (chain length between functional groups: 10), but the adhesive sheet of Example 3-6 was obtained in the same manner as in Example 3-1.

[0206] [Examples 3-7] The adhesive sheet of Example 3-7 was obtained in the same manner as in Example 3-1, except that the acrylic acid ester copolymer in Example 3-1 was changed to that in Example 2-5, and further, the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) was changed to polypropylene glycol #400 diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; APG-400) (chain length between functional groups: 14).

[0207] [Examples 3-8] The acrylic acid ester copolymer in Example 3-1 was changed to that in Example 2-5, and further, the propoxylated bisphenol A diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; A-BPP-3) was changed to polypropylene glycol (#700) diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd.; APG-700) (number of carbon atoms in the chain portion between functional groups: 24), except that the adhesive sheet of Example 3-8 was obtained in the same manner as in Example 3-1.

[0208] Table 3 shows the evaluation results of the pressure-sensitive adhesive sheets according to Examples 3-1 to 3-8. In order to evaluate the pressure-sensitive adhesive sheets of Examples 3-1 to 3-8, the evaluation results of the pressure-sensitive adhesive sheets of Examples 1-3, 2-1, and Comparative Example 1-1 used as comparison targets are also included in Table 3.

[0209] [Table 3]

[0210] [Evaluation Results] The pressure-sensitive adhesive sheets according to Examples 3-1 to 3-8 exhibited better results in the second adhesive residue evaluation than Comparative Example 1-1.

[0211] The pressure-sensitive adhesive sheets according to Examples 3-1 to 3-5 were able to improve the releasability. After heating, Example 2-1, which used HEA as the functional group-containing monomer, had a slightly high adhesive strength to polyimide at room temperature, whereas the pressure-sensitive adhesive sheets according to Examples 3-1 to 3-5, which used 4-HBA as the functional group-containing monomer, showed a moderate adhesive strength to polyimide at room temperature and improved releasability.

[0212] Comparing the pressure-sensitive adhesive sheets of Example 3-1 and Examples 3-2 to 3-6, the pressure-sensitive adhesive sheets of Examples 3-2 to 3-6 were superior in initial adhesion. In Example 3-1, an energy ray curable compound having a cyclic structure was used as the energy ray curable compound. In Examples 3-2 to 3-6, an energy ray curable compound having a specific chain structure was used, and the initial adhesion was improved. This is considered to be because the Young's modulus was reduced and the initial adhesion was improved by using an energy ray curable compound having a specific chain structure instead of a cyclic structure.

[0213] Although the pressure-sensitive adhesive sheets according to Examples 3-6 to 3-8 did not contain ACMO as a structural unit of the polymer component, the use of an energy ray-curable compound having a predetermined chain structure improved the adhesive transfer prevention effect.

[0214] Comparing Examples 1-3, 2-1, and 3-1, the results of the first adhesive residue evaluation were all rated A. However, the results of the second adhesive residue evaluation, which is conducted under stricter conditions, were rated D for Example 1-3, and A for Examples 2-1 and 3-1, which used ACMO having a nitrogen-containing functional group as the monomer of the polymer component. [Explanation of symbols]

[0215] 10, 10A, 10B...adhesive sheet, 11...substrate, 11a...first substrate surface, 11b...second substrate surface, 12...adhesive layer, 13, 13A, 13B...oligomer sealing layer, RL...release sheet.

Claims

1. The adhesive layer includes a substrate and a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes a cured product obtained by curing an energy ray-curable component and a polymer component, the polymer component is at least one selected from the group consisting of a (meth)acrylic resin, a polyester resin, a polyurethane resin, an acrylic urethane resin, a silicone resin, a rubber resin, and a polystyrene resin; The polymer component comprises constitutional units derived from a monomer having a nitrogen-containing functional group, provided that the nitrogen-containing functional group does not contain an N-H bond, or the polymer component includes a structural unit derived from a functional group-containing monomer having a reactive functional group, and the reactive functional group is bonded to a main chain of the polymer component via three or more methylene groups bonded in a linear chain; Adhesive sheet for processing electronic parts.

2. The pressure-sensitive adhesive sheet according to claim 1 , The pressure-sensitive adhesive sheet, wherein the polymer component is a (meth)acrylic resin.

3. The pressure-sensitive adhesive sheet according to claim 1 or 2, the energy ray-curable component contains a multifunctional energy ray-curable compound, The polyfunctional energy ray curable compound has 2 to 5 polymerizable functional groups in one molecule. Adhesive sheet.

4. The pressure-sensitive adhesive sheet according to claim 1 or 2, the energy ray-curable component contains a multifunctional energy ray-curable compound, The polyfunctional energy ray-curable compound has two or more polymerizable functional groups in one molecule, a methylene group is present in a linear chain between a first polymerizable functional group and a second polymerizable functional group, the first polymerizable functional group and the second polymerizable functional group being selected from two or more polymerizable functional groups contained in the multifunctional energy ray-curable compound; the number of methylene groups bonded in a linear chain between the first polymerizable functional group and the second polymerizable functional group is 8 or more and 30 or less; Adhesive sheet.

5. The pressure-sensitive adhesive sheet according to claim 3 or 4, The polyfunctional energy ray-curable compound has a cyclic structure in a molecule, the polymer component includes a structural unit derived from a functional group-containing monomer having a reactive functional group, and the reactive functional group is bonded to a main chain of the polymer component via three or more methylene groups bonded in a linear chain; Adhesive sheet.

6. The pressure-sensitive adhesive sheet according to any one of claims 1 to 5, The pressure-sensitive adhesive sheet has an adhesive strength to polyimide of 0.04 N / 25 mm or more at 100°C.

7. The pressure-sensitive adhesive sheet according to claim 6 , The adhesive strength of the pressure-sensitive adhesive sheet to polyimide at 100° C. is 0.06 N / 25 mm or more, The pressure-sensitive adhesive layer has a breaking strength per unit cross-sectional area of ​​4.5 N / mm 2 That's all. Adhesive sheet.

8. The pressure-sensitive adhesive sheet according to any one of claims 1 to 7, the adhesive strength of the pressure-sensitive adhesive sheet to polyimide at 25° C. after heat treatment at 190° C. for 1.5 hours in a nitrogen atmosphere is 3 N / 25 mm or less; Adhesive sheet.

9. The pressure-sensitive adhesive sheet according to any one of claims 1 to 8, The Young's modulus of the pressure-sensitive adhesive layer is 5 MPa or less. Adhesive sheet.

10. The pressure-sensitive adhesive sheet according to any one of claims 1 to 9, Used to fix or protect electronic components when processing the electronic components; Adhesive sheet.

11. The pressure-sensitive adhesive sheet according to claim 1 , The pressure-sensitive adhesive sheet, wherein the nitrogen-containing functional group is at least one selected from the group consisting of a tertiary amino group, an aminocarbonyl group, a cyano group, and a nitrogen-containing heterocyclic group.

12. The pressure-sensitive adhesive sheet according to claim 1 , the monomer having a nitrogen-containing functional group is at least one selected from the group consisting of heterocyclic vinyl compounds, (meth)acrylamide compounds, amino group-containing (meth)acrylic acid ester compounds, and (meth)acrylonitrile.

13. A step of fixing a semiconductor element on the pressure-sensitive adhesive sheet according to any one of claims 1 to 12; and sealing the semiconductor element with a sealing material.

Citation Information

Patent Citations

  • Heat-resistant adhesive tape for manufacturing semiconductor device, and method for manufacturing semiconductor device

    JP2010073853A

  • Adhesive composition and adhesive sheet

    JP2010229367A

  • Heat-resistant pressure-sensitive adhesive tape

    JP2012046763A

  • Dicing die-bonding film, manufacturing method of dicing die-bonding film, and manufacturing method of semiconductor device

    JP2012069586A

  • Pressure-sensitive adhesive tape for electronic part production

    JP2013040276A