Communication cable and wire harness using the same
The communication cable with a crystalline polyolefin and thermoplastic elastomer sheath composition addresses plasticizer migration issues, maintaining flexibility and transmission quality under high temperatures, enhancing reliability and performance.
Patent Information
- Application Number
- JP2023200370
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2041-12-17
AI Technical Summary
Existing communication cables in automotive applications face issues with plasticizer migration leading to deterioration of insulating resins, reduced flexibility, and compromised transmission characteristics, especially under high-temperature conditions, necessitating a balance between flexibility and resistance to breakage.
A communication cable design featuring a sheath made of a resin composition comprising crystalline polyolefin and thermoplastic elastomer, with specific mass ratios and additives to control plasticizer migration, maintaining flexibility and transmission characteristics.
The solution provides a highly flexible communication cable with excellent communication properties that resist plasticizer transfer and transmission characteristic deterioration even under high-temperature conditions, ensuring reliable performance over time.
Smart Images

Figure 0007568821000007 
Figure 0007568821000008 
Figure 0007568821000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a communication cable and a wire harness using the same. [Background technology]
[0002] In two-core differential transmission cables used as communication cables for automobiles, such as cables used for Ethernet communication, strict control of characteristic impedance is required. Patent Document 1 discloses a communication cable in which an insulated electric wire is covered with a sheath made of polypropylene resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-188436 A Summary of the Invention [Problem to be solved by the invention]
[0004] Polyvinyl chloride resin (PVC) is often used as the insulation for general electric wires that are bundled around communication cables, and when exposed to high temperature conditions for a long period of time, the plasticizer contained in the PVC bleeds out and easily migrates to the sheath of the communication cable. Therefore, the plasticizer penetrates through the sheath of the communication cable and adsorbs to the additive that improves the heat resistance of the insulating resin that covers the wire core, accelerating the deterioration of the insulating resin and causing a decrease in the communication speed of the communication cable.
[0005] Therefore, it is generally known that the migration of the plasticizer is suppressed by using a highly crystalline material for the sheath material. However, such a resin composition tends to make the communication cable hard and less flexible. In vehicles, a communication cable having high flexibility and excellent communication characteristics is required in order to compactly bundle the insulated electric wires and arrange them in a narrow space.
[0006] On the other hand, there is a demand for communication cables that are less likely to break when subjected to tensile stresses applied when wiring harnesses are installed or when they are installed in vehicles. In the case of thin cables, the cable itself may break, or the cable may come loose from the connector. One solution to this problem is to use conductors with high breaking strength. However, this tends to make the cable stiff, so it is more effective to use a flexible sheath material.
[0007] The present invention has been made in view of the problems inherent in the conventional techniques, and an object of the present invention is to provide a communication cable that is highly flexible, has excellent communication characteristics, and is resistant to deterioration in transmission characteristics by suppressing migration of plasticizers from other components even in a high-temperature atmosphere for a long period of time, and a wire harness using the same. [Means for solving the problem]
[0008] A communication cable according to an embodiment of the present invention includes an insulated wire including a conductor and a coating layer made of an insulator that coats the conductor, and a sheath that coats the outer periphery of the insulated wire and is made of a resin composition containing crystalline polyolefin. The insulator contains polypropylene and a soft resin, and the polypropylene content relative to the total of the polypropylene and the soft resin is 51% by mass or more and 85% by mass or less, and contains 15 to 60 parts by mass of titanium oxide and 10 to 80 parts by mass of a brominated flame retardant relative to 100 parts by mass of the total of the polypropylene and the soft resin. The characteristic impedance of the communication cable is 100±10Ω.
[0009] A wire harness according to an aspect of the present invention includes the above-described communication cable and a polyvinyl chloride electric wire, and the communication cable and the polyvinyl chloride electric wire are bundled together. Effect of the Invention
[0010] According to the present invention, it is possible to provide a communication cable that is highly flexible, has excellent communication characteristics, and suppresses migration of plasticizers from other components even in a high-temperature atmosphere for a long period of time, thereby making it difficult for the transmission characteristics to deteriorate, and a wire harness using the same. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing an example of a communication cable (circular compressed conductor) according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing an example of a communication cable (circular conductor) according to an embodiment of the present invention. [Diagram 3] 1 is a schematic perspective view showing an example of a wire harness according to an embodiment of the present invention. [Figure 4] 1 is a schematic side view illustrating an example of a communication cable according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic side view showing an example of twisting of insulated electric wires according to the embodiment. [Figure 6] FIG. 1 is a schematic diagram showing a state in which a characteristic impedance and an insertion loss are measured using a vector network analyzer (VNA). [Figure 7] 4 is a graph showing the characteristic impedance of the communication cable according to the first embodiment. [Figure 8] 4 is a graph showing the characteristic impedance of the communication cable according to Comparative Example 1. [Figure 9] FIG. 2 is a schematic cross-sectional view showing a test sample. [Figure 10] 4 is a graph showing the relationship between frequency and insertion loss of the communication cable according to Example 1 before and after a plasticizer migration test. [Figure 11] 1 is a graph showing the relationship between frequency and insertion loss of the communication cable according to Comparative Example 1 before and after a plasticizer migration test. [Figure 12] FIG. 1 is a schematic diagram for explaining a method for measuring the flexibility of a communication cable. [Figure 13] 1 is a graph showing the relationship between the flexibility and DINP absorption amount of a communication cable and the tensile modulus of the sheath. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, a communication cable and a wire harness using the same according to an embodiment of the present invention will be described in detail with reference to the drawings. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.
[0013] [Communication cable] As shown in Figs. 1 and 2, a communication cable 100 includes an insulated electric wire 10 and a sheath 20 that covers the outer circumference of the insulated electric wire 10. The outer surface of the insulated electric wire 10 is directly covered with the sheath 20. The sheath 20 extends along the axial direction of the insulated electric wire 10. The thickness of the sheath 20 is not particularly limited, and may be, for example, 0.1 mm to 1 mm. In this embodiment, two insulated electric wires 10 form a twisted pair, but the number of insulated electric wires 10 may be at least one. In this embodiment, a gap may be provided between the insulated electric wire 10 and the sheath 20.
[0014] The sheath 20 contains a resin composition. As described above, the plasticizer added to polyvinyl chloride may bleed out to the surface of the material and migrate to the sheath 20 after long-term use. The dielectric tangent of the plasticizer is generally large, and the dielectric tangent of phthalic acid plasticizers and trimellitic acid plasticizers is particularly large. When the dielectric tangent is large, the insertion loss of the communication cable 100 increases, which hinders high-speed communication by the communication cable 100. Therefore, not only when the resin composition constituting the sheath 20 contains a plasticizer, but also when the plasticizer migrates, the dielectric properties of the sheath 20 may be deteriorated, which may hinder high-speed communication.
[0015] Thus, in a plasticizer migration test in which the communication cable 100 according to this embodiment and the polyvinyl chloride wire 110 were bundled and left in the air at 105°C for 3000 hours, the mass increase rate of the sheath 20 was less than 50 mass%. Since the mass increase rate of the sheath 20 is less than 50 mass%, migration of the plasticizer to the sheath 20 can be suppressed even when the communication cable 100 and the polyvinyl chloride wire 110 are bundled to form the wire harness 200 as shown in Fig. 3. Since the amount of plasticizer migrating to the sheath 20 is small, the transmission characteristics of the communication cable 100 are less likely to deteriorate.
[0016] In a dielectric such as the resin composition of the sheath 20, the greater the values of the dielectric constant and the dielectric loss tangent, and the higher the frequency, the greater the attenuation of a high-frequency signal in the communication cable. In this embodiment, the mass increase rate of the sheath 20 in the plasticizer migration test is set to less than 50% by mass, thereby reducing the dielectric loss tangent and suppressing attenuation, thereby enabling communication in the high-frequency band. In the communication cable 100 of this embodiment, a preferable transmission speed is 1 Gbps or less. In addition, in this embodiment, since the mass increase rate of the sheath 20 is small, even when used in an environment such as a vehicle, deterioration of the communication quality of the communication cable 100, such as attenuation, can be suppressed for a long period of time. The mass increase rate of the sheath 20 is preferably less than 40% by mass, and more preferably less than 30% by mass. Since the value of the mass increase rate of the sheath 20 is preferably as small as possible, the lower limit of the mass increase rate of the sheath 20 may be 0% by mass or more. The mass increase rate of the sheath 20 can be adjusted by the composition of the resin composition as described later.
[0017] In order to achieve the above-mentioned mass increase rate of the sheath 20, it is effective to use a material with high crystallinity, such as homopolypropylene, in the resin composition of the sheath 20. However, the tensile modulus of such a sheath 20 is high, making it difficult to bend the communication cable 100, which may make it difficult to route the communication cable 100 in a narrow area.
[0018] Therefore, in this embodiment, the tensile modulus of the sheath 20 is 500 MPa or less. By setting the tensile modulus of the sheath 20 to 500 MPa or less, the communication cable 100 can be easily curved, which makes it easy to route the communication cable 100 in a narrow space. The tensile modulus of the sheath 20 can be adjusted by the composition of the resin composition as described below.
[0019] The tensile modulus can be measured in accordance with the provisions of JIS K7161-1 (Plastics - Determination of tensile properties - Part 1: General rules). Specifically, the sheath 20 is pulled at a tensile speed of 50 mm / min at a room temperature of 20° C., and the modulus can be calculated from the following calculation formula (1). E t =(σ2-σ1) / (ε2-ε1) (1) In the above formula, E t represents the tensile modulus of elasticity (Pa), σ1 represents the stress (Pa) at strain ε1 = 0.0005, and σ2 represents the stress (Pa) at strain ε2 = 0.0025.
[0020] The resin composition of the sheath 20 contains a crystalline polyolefin and a thermoplastic elastomer. The content of the crystalline polyolefin with respect to the total of the crystalline polyolefin and the thermoplastic elastomer is preferably 55% by mass or more and 70% by mass or less. When the content of the crystalline polyolefin is 55% by mass or more, the mass increase rate of the sheath 20 becomes smaller, the plasticizer is less likely to migrate to the sheath 20, and the communication reliability of the communication cable 100 can be maintained for a long period of time. When the content of the crystalline polyolefin is 70% by mass or less, the tensile modulus of the sheath 20 becomes smaller, and the workability of the installation of the communication cable 100 is improved. The content of the crystalline polyolefin is more preferably 65% by mass or more and 70% by mass or less.
[0021] The content of the thermoplastic elastomer relative to the total of the crystalline polyolefin and the thermoplastic elastomer is preferably 30% by mass or more and less than 45% by mass. When the content of the thermoplastic elastomer is 30% by mass or more, the tensile modulus of the sheath 20 becomes smaller, improving the workability of wiring the communication cable 100. When the content of the thermoplastic elastomer is less than 45% by mass, the mass increase rate of the sheath 20 becomes smaller, and the plasticizer is less likely to migrate to the sheath 20, making it possible to maintain the communication reliability of the communication cable 100 for a long period of time. The content of the thermoplastic elastomer is more preferably 30% by mass or more and less than 35% by mass.
[0022] The resin composition of the sheath 20 preferably has a dielectric constant of 6 or less. A communication cable mounted on an automobile must satisfy a specified characteristic impedance to enable high-speed communication. The characteristic impedance depends not only on the dielectric constant of the dielectric material such as the resin composition, but also on the structure of the communication cable. Lightweight and compact communication cables mounted on automobiles are required, but if the dielectric constant is large, it is necessary to increase the finished outer diameter of the insulated wire. If the resin composition has a dielectric constant of 6 or less, the characteristic impedance of the communication cable with a cross-sectional area of 0.13 sq (mm 2 This can be applied to communication cables with the thinnest conductors, i.e., 100±10Ω. It also satisfies the characteristic impedance standard of 100±10Ω required for communication cables. The dielectric constant can be measured at a frequency of 10GHz in an atmosphere of 30℃ by the cavity resonator method.
[0023] The relative dielectric constant can be appropriately adjusted by the content of the inorganic filler contained in the resin composition of the sheath 20, as described later. The relative dielectric constant of the resin composition of the sheath 20 is more preferably 2.5 or more and 4.0 or less. By setting the relative dielectric constant to 2.5 or more, the sheath 20 can be made to have a thickness that is easy to manufacture while satisfying the ISO21111-8 standard, and therefore the production efficiency of the communication cable 100 can be improved. In addition, by setting the relative dielectric constant of the resin composition to 4.0 or less, the sheath 20 can be made thin, and the outer diameter and weight of the communication cable 100 can be prevented from becoming too large. The relative dielectric constant of the resin composition is more preferably 3.0 or more and 3.5 or less.
[0024] The dielectric tangent of the resin composition of the sheath 20 is 5×10 -2 It is preferable that the dielectric loss tangent of the resin composition is 5×10 or less. -2 By keeping the dielectric tangent at 8.0×10 or less, it is possible to suppress an increase in the insertion loss of the communication cable 100. -3 It is preferable that the dielectric tangent value is smaller, so that the lower limit of the dielectric tangent is 0. The dielectric tangent can be measured by a cavity resonator method in an atmosphere at 30° C. at a frequency of 10 GHz.
[0025] The resin composition of the sheath 20 has a relative dielectric constant of 2.5 or more and 4.0 or less, and the dielectric tangent of the resin composition is 5×10 -2 The conductor 11 is 0.13sq (mm 2 The communication cable 100 as described above has a small diameter and good communication characteristics, and therefore can be suitably used in a vehicle as the communication cable 100 capable of high-speed communication.
[0026] (Crystalline polyolefin) Crystalline polyolefins are polymers of monomers containing olefins. The polyolefins may be olefin homopolymers or copolymers of olefins and monomers other than olefins (e.g., ethylene-vinyl acetate copolymer (EVA)). The olefin homopolymers may be polymers of one type of olefin or polymers of two or more types of olefins. The polyolefins may be modified with maleic acid or the like, or may not be modified.
[0027] The olefin may include α-olefins, β-olefins, and γ-olefins, etc. The α-olefin may include at least one monomer selected from the group consisting of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and 1-decene, etc.
[0028] The monomer other than the olefin may be a monomer having a carbon-carbon double bond. The monomer other than the olefin may include at least one of styrene and acrylate.
[0029] The crystalline polyolefin may be at least one selected from the group consisting of low density polyethylene (LDPE), linear low density polyethylene (LLDPE), high density polyethylene (HDPE), homopolypropylene (homoPP), random polypropylene (randomPP), block polypropylene (blockPP), ethylene-propylene-butene copolymer, and the like.
[0030] (Thermoplastic elastomer) The thermoplastic elastomer is a resin having a lower crystallinity than crystalline polyolefin. The thermoplastic elastomer may contain at least one elastomer selected from the group consisting of olefin-based thermoplastic elastomers (TPO), thermoplastic crosslinked rubbers (TPV), and styrene-based thermoplastic elastomers (TPS). The thermoplastic elastomer may be modified with maleic acid or the like, or may not be modified.
[0031] The olefin-based thermoplastic elastomer (TPO) is a mixture of polyolefin and rubber, and the mixed rubber has no or almost no crosslinking points. The polyolefin may be any of those mentioned above. Examples of the rubber used in the olefin-based thermoplastic elastomer (TPO) include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), ethylene-propylene rubber (EPM), and ethylene-propylene-diene rubber (EPDM).
[0032] An example of an olefin-based thermoplastic elastomer is "Prime TPO (registered trademark)" available from Prime Polymer Co., Ltd.
[0033] The crosslinked thermoplastic rubber is a mixture of polyolefin and rubber, and the mixed rubber is crosslinked by dynamic vulcanization. The rubber used in the above-mentioned olefin-based thermoplastic elastomer can be used. The crosslinked thermoplastic rubber has the characteristic of being difficult to expand due to plasticizers of highly crystalline resins such as ethylene and homopolypropylene, and also has flexibility like rubber.
[0034] Examples of the crosslinked thermoplastic rubber include "THERMORUN (registered trademark)" available from Mitsubishi Chemical Corporation, "MILASTOMER (registered trademark)" available from Mitsui Chemicals, Inc., "EXCELINK (registered trademark)" available from JSR Corporation, "ESPOLEX (registered trademark) TPE series" available from Sumitomo Chemical Co., Ltd., and "SANTOPRENE (registered trademark)" available from ExxonMobil Corporation.
[0035] The styrene-based thermoplastic elastomer (TPS) may be a block copolymer or random copolymer having an aromatic vinyl polymer block (hard segment) and a diene polymer block (soft segment). The monomer constituting the aromatic vinyl polymer may be styrene, α-substituted styrene such as α-methylstyrene, α-ethylstyrene, α-methyl-p-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, ethylstyrene, 2,4,6-trimethylstyrene, ot-butylstyrene, pt-butylstyrene, etc. The diene polymer block may be a copolymer of at least one of butadiene and isoprene, or a partially hydrogenated copolymer.
[0036] The styrenic thermoplastic elastomer (TPS) may be at least one block copolymer selected from the group consisting of polystyrene-polybutadiene-polystyrene (SBS), polystyrene-polyisoprene-polystyrene (SIS), polystyrene-polyisobutylene-polystyrene (SIBS), polystyrene-poly(ethylene-butylene)-polystyrene (SEBS), polystyrene-poly(ethylene-butylene)-crystalline polyolefin (SEBC), and polystyrene-poly(ethylene-propylene)-polystyrene (SEPS).
[0037] Examples of styrene-based thermoplastic elastomers include "TEFABLOCK (registered trademark)" available from Mitsubishi Chemical Corporation, "ESPOLEX (registered trademark) SB Series" available from Sumitomo Chemical Co., Ltd., "SEPTON (registered trademark)" available from Kuraray Co., Ltd., "DYNARON (registered trademark)" available from JSR Corporation, and "HYBRA (registered trademark)" available from Kuraray Co., Ltd.
[0038] In addition to the crystalline polyolefin and the thermoplastic elastomer, various additives may be blended in appropriate amounts to the extent that the effects of this embodiment are not impaired in the resin composition of the sheath 20. Examples of additives include flame retardants, inorganic fillers, flame retardant assistants, antioxidants, processing assistants, crosslinking agents, metal deactivators (copper inhibitors), anti-aging agents, fillers, reinforcing agents, UV absorbers, stabilizers, plasticizers, pigments, dyes, colorants, antistatic agents, foaming agents, etc.
[0039] (Flame retardant) The flame retardant improves the flame retardancy of the sheath 20. By improving the flame retardancy of the sheath 20, even if a fire breaks out in a vehicle, the sheath 20 can suppress the spread of fire. Therefore, it is not necessarily required to impart flame retardancy to the coating layer 12 of the insulated wire 10. However, from the viewpoint of improving the flame retardancy, it is preferable to add a flame retardant to the coating layer 12 as well.
[0040] The flame retardant may be, for example, at least one of an organic flame retardant and an inorganic flame retardant. As the organic flame retardant, for example, a halogen-based flame retardant such as a bromine-based flame retardant and a chlorine-based flame retardant, and a phosphorus-based flame retardant such as a phosphate ester, a condensed phosphate ester, a cyclic phosphorus compound, and red phosphorus can be used. As the inorganic flame retardant, at least one metal hydroxide selected from the group consisting of aluminum hydroxide, magnesium hydroxide, and calcium hydroxide can be used. These flame retardants may be used alone or in combination. The flame retardant may include, for example, an organic flame retardant and an inorganic flame retardant.
[0041] The content of the flame retardant in the resin composition of the sheath 20 is preferably 5 parts by mass to 200 parts by mass, and more preferably 50 parts by mass to 160 parts by mass, per 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By setting the content of the flame retardant in the above range, it is possible to satisfactorily improve the flame retardancy while maintaining the mechanical properties of the resin composition.
[0042] The organic flame retardant preferably contains at least a halogen-based flame retardant. The halogen-based flame retardant can capture hydroxyl radicals that promote the combustion of the resin composition of the sheath 20 and suppress the combustion of the resin composition. The halogen-based flame retardant may be, for example, a compound in which at least one halogen is substituted on an organic compound. Examples of the halogen-based flame retardant include a fluorine-based flame retardant, a chlorine-based flame retardant, a bromine-based flame retardant, and an iodine-based flame retardant. The halogen-based flame retardant is preferably a bromine-based flame retardant.
[0043] Brominated flame retardants include, for example, 1,2-bis(bromophenyl)ethane, 1,2-bis(pentabromophenyl)ethane, hexabromobenzene, ethylene bis-dibromonorbornane dicarboximide, ethylene bis-tetrabromophthalimide, tetrabromobisphenol S, tris(2,3-dibromopropyl-1)isocyanurate, hexabromocyclododecane (HBCD), octabromophenyl ether, tetrabromobisphenol A (TBA), TBA epoxy oligomer or polymer, TBA-bis(2,3-dibromopropyl ether), decabromodiphenyl oxide, polydibromophenylene oxide, bis(tribromophenoxy)ethane, ethylene bis-pentabromobenzene, dibromophenyl ether, tetra ... Bromoethyl-dibromocyclohexane, dibromoneopentyl glycol, tribromophenol, tribromophenol allyl ether, tetradecabromodiphenoxybenzene, 2,2-bis(4-hydroxy-3,5-dibromophenyl)propane, 2,2-bis(4-hydroxyethoxy-3,5-dibromophenyl)propane, pentabromophenol, pentabromotoluene, pentabromodiphenyl oxide, hexabromodiphenyl ether, octabromodiphenyl ether, decabromodiphenyl ether, octabromodiphenyl oxide, dibromoneopentyl glycol tetracarbonate, bis(tribromophenyl)fumaramide, N-methylhexabromophenylamine, etc. The flame retardant preferably contains 1,2-bis(pentabromophenyl)ethane and tetrabromobisphenol A. Such flame retardants have a low relative dielectric constant, and therefore can impart flame retardancy while suppressing the increase in viscosity and relative dielectric constant of the resin composition.
[0044] The content of the halogen-based flame retardant contained in the resin composition of the sheath 20 is preferably 5 parts by mass to 40 parts by mass, more preferably 10 parts by mass to 30 parts by mass, relative to 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By making the content of the halogen-based flame retardant 10 parts by mass or more, the flame retardancy of the resin composition can be improved. In addition, by making the content of the halogen-based flame retardant 30 parts by mass or less, it is possible to maintain the mechanical properties while not using more flame retardant than necessary, thereby reducing the production cost of the resin composition.
[0045] The content of the inorganic flame retardant contained in the resin composition of the sheath 20 is preferably 30 parts by mass to 200 parts by mass, and more preferably 40 parts by mass to 150 parts by mass, relative to 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By making the content of the inorganic flame retardant 40 parts by mass or more, it is possible to prevent the relative dielectric constant of the resin composition from becoming too low. By making the content of the inorganic flame retardant 150 parts by mass or less, it is possible to prevent the relative dielectric constant from becoming too high. In addition, by making the content of the inorganic flame retardant 150 parts by mass or less, the viscosity of the resin composition is reduced, and therefore the processability of the resin composition can be improved.
[0046] The inorganic flame retardant preferably contains at least a metal hydroxide. Metal hydroxides are widely used as flame retardants and are relatively cheaper than bromine-based flame retardants. In addition, metal hydroxides have a higher dielectric constant than general polyolefin-based resins, and therefore act as a dielectric constant adjuster. Therefore, the resin composition of the sheath 20 of this embodiment preferably contains a metal hydroxide in addition to a halogen-based flame retardant. As the metal hydroxide, one or more metal compounds having a hydroxyl group or crystal water, such as magnesium hydroxide (Mg(OH)2), aluminum hydroxide (Al(OH)3), calcium hydroxide (Ca(OH)2), basic magnesium carbonate (mMgCO3·Mg(OH)2·nH2O), hydrated aluminum silicate (aluminum silicate hydrate, Al2O3·3SiO2·nH2O), and hydrated magnesium silicate (magnesium silicate pentahydrate, Mg2SiO8·5H2O), can be used. Among these, magnesium hydroxide is particularly preferable as the metal hydroxide.
[0047] The resin composition of the sheath 20 preferably further contains 40 to 150 parts by mass of a metal hydroxide relative to 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By making the content of the metal hydroxide 40 parts by mass or more, it is possible to prevent the relative dielectric constant of the resin composition from becoming too low, and the flame retardancy can also be improved. By making the content of the metal hydroxide 150 parts by mass or less, it is possible to prevent the relative dielectric constant from becoming too high, and it is also possible to improve the flexibility of the resin composition. In addition, by making the content of the metal hydroxide 150 parts by mass or less, the viscosity of the resin composition is reduced, and therefore the processability of the resin composition can be improved. The resin composition may further contain 80 parts by mass or more of a metal hydroxide, or may further contain 100 parts by mass or less of a metal hydroxide, relative to 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer.
[0048] When the viscosity of the resin composition of the sheath 20 is high, the extrusion processability of the resin composition can be improved by reducing the content of the inorganic flame retardant and increasing the content of the organic flame retardant. When the flame retardant contains an organic flame retardant and an inorganic flame retardant, the ratio of the inorganic flame retardant to the organic flame retardant may be, for example, 0.75 to 40, or may be 1 to 10.
[0049] (Inorganic filler) In order to adjust the dielectric constant of the resin composition of the sheath 20, the resin composition may contain an inorganic filler. The inorganic filler may contain the inorganic flame retardant described above. The inorganic filler may be, for example, the above-mentioned metal hydroxides, metal oxides such as aluminum oxide, and titanium oxide, and titanate compounds such as barium titanate and strontium titanate.
[0050] The content of the inorganic filler contained in the resin composition of the sheath 20 is preferably 30 parts by mass to 200 parts by mass, and more preferably 40 parts by mass to 150 parts by mass, relative to 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By making the content of the inorganic filler 30 parts by mass or more, it is possible to prevent the relative dielectric constant of the resin composition from becoming too low. By making the content of the inorganic filler 150 parts by mass or less, it is possible to prevent the relative dielectric constant from becoming too high.
[0051] (Flame retardant assistant) The flame retardant assistant improves the flame retardancy of the resin composition of the sheath 20 together with the flame retardant. The flame retardant assistant may be, for example, antimony trioxide. The antimony trioxide can improve the flame retardancy of the resin composition by using it in combination with a halogen-based flame retardant. The content of the flame retardant assistant in the resin composition is preferably 0.1 to 30 parts by mass, and more preferably 1 to 15 parts by mass, relative to 100 parts by mass of the total of the polyolefin and the thermoplastic elastomer.
[0052] (Antioxidants) The antioxidant suppresses, for example, oxidation of the resin composition of the sheath 20. As the antioxidant, known antioxidants used for thermoplastic resins, etc., such as radical chain inhibitors such as phenol-based antioxidants, hindered phenol-based antioxidants, and amine-based antioxidants, peroxide decomposers such as phosphorus-based antioxidants and sulfur-based antioxidants, and metal deactivators such as hydrazine-based antioxidants and amine-based antioxidants, can be used. The antioxidants may be used alone or in combination.
[0053] The amount of antioxidant added may be adjusted taking into consideration the antioxidant effect and problems caused by bleed-out. The content of the antioxidant contained in the resin composition of the sheath 20 is preferably 0.5 parts by mass to 10 parts by mass per 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer. By making the content of the antioxidant 0.5 parts by mass or more, it is possible to improve heat resistance. In addition, by making the content of the antioxidant 10 parts by mass or less, it is possible to reduce bleed-out.
[0054] (Processing aids) The processing aid is added to prevent resin generated during extrusion and to maintain the shape of the extrusion product. The processing aid may contain at least one of a metal soap and a polymer lubricant. The content of the processing aid contained in the resin composition of the sheath 20 is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the total of the crystalline polyolefin and the thermoplastic elastomer.
[0055] The resin composition of the sheath 20 may further contain 40 to 150 parts by mass of a metal hydroxide and 10 to 30 parts by mass of a halogen-based flame retardant, relative to 100 parts by mass of the crystalline polyolefin and the thermoplastic elastomer in total. The relative dielectric constant of the resin composition is 6 or less, and the dielectric loss tangent of the resin composition is 5×10 -2By forming sheath 20 from such a resin composition, it is possible to provide communication cable 100 that has higher flexibility, is superior in communication characteristics, and is resistant to deterioration in transmission characteristics by suppressing migration of plasticizers from other components even in a high-temperature atmosphere for a long period of time.
[0056] The communication cable 100 can be formed by a known method, for example, a general extrusion molding method. Specifically, the sheath 20 can be formed by bundling one or more insulated electric wires 10 together and then extruding the material of the sheath 20 onto the outer surface of the insulated electric wire 10 to cover it.
[0057] (Insulated Wire) As shown in Figs. 1 and 2, the insulated wire 10 includes a conductor 11 and a coating layer 12 made of an insulator that coats the conductor 11. The conductor 11 may be composed of only one strand, or may be a bunched stranded wire made by bundling a plurality of strands. The conductor 11 may be composed of only one twisted wire, or may be a composite twisted wire made by bundling a plurality of bunched twisted wires. The conductor 11 may be a circular compressed conductor as shown in Fig. 1, or may be a circular conductor as shown in Fig. 2. The material constituting the conductor 11 is not particularly limited, but is preferably at least one conductive metal material selected from the group consisting of copper, copper alloys, aluminum, aluminum alloys, and the like.
[0058] Conductor 11 has a tensile strength of 400 MPa or more. By making conductor 11 have a tensile strength of 400 MPa or more, communication cable 100 is less likely to break due to tensile stress applied when wiring the wire harness or installing it in a vehicle. The tensile strength can be measured in accordance with the provisions of JIS Z2241 (Method of tensile test for metallic materials).
[0059] The outer diameter of the conductor 11 is not particularly limited, but is preferably 0.435 mm or more, and more preferably 0.440 mm or more. By setting the diameter of the conductor 11 as described above, the resistance of the conductor 11 can be reduced. Furthermore, the diameter of the conductor 11 is not particularly limited, but is preferably 0.465 mm or less, and more preferably 0.460 mm or less. By setting the outer diameter of the conductor 11 as described above, the insulated wire 10 can be easily routed even in a narrow and short path.
[0060] The cross-sectional area of the conductor 11 is 0.22 mm 2 The cross-sectional area of the conductor 11 is preferably 0.22 mm 2 By making the above-mentioned, it is possible to easily arrange the insulated wire 10 even in a narrow and short path. The conductor 11 has a diameter of 0.13 sq (mm 2 ) conductor.
[0061] When the insulated wire 10 forms a twisted pair as shown in FIG. 4, the strength of the conductor can be calculated by the following formula (2). Conductor strength (N) = tensile strength (MPa) x cross-sectional area of conductor (mm 2 )×2 (2)
[0062] Considering the aspect of quality reliability, the strength of the conductor 11 is preferably 100 N or more. According to the above calculation formula (2), the tensile strength of the conductor 11 is 400 MPa, and the cross-sectional area of the conductor 11 is 0.13 sq (mm 2 ) then the value is 104N.
[0063] The thickness of the coating layer 12 is not particularly limited, but is preferably 0.15 mm or more, and more preferably 0.18 mm or more. By making the coating layer 12 have the above thickness, the conductor 11 can be effectively protected. Furthermore, the thickness of the coating layer 12 is not particularly limited, but is preferably 0.32 mm or less. By making the coating layer 12 have the above thickness, the insulated wire 10 can be easily routed even in a narrow path.
[0064] When the insulated wire 10 forms a twisted pair as shown in FIG. 4, the characteristic impedance can be calculated by the following formula (1).
[0065]
number
[0066] In the above formula (1), Z0 is the characteristic impedance (Ω), ε e represents the effective relative dielectric constant, k1 represents the conductor outer diameter factor, and D represents the distance (mm) between the centers of the conductors 11, and d represents the diameter (mm) of the conductors 11, as shown in FIG.
[0067] According to the above formula (1), for example, in order to achieve a characteristic impedance of 100 Ω required for a communication cable, the conductor 11 must be 0.13 sq (mm 2 ) conductor, the thickness of the coating layer 12 is 0.20 mm. 2 ) the thickness of the coating layer 12 is 0.26 mm. That is, if the surface area of the conductor 11 is large, the coating layer needs to be thicker.
[0068] The insulator constituting the covering layer 12 contains polypropylene and a soft resin. From the viewpoints of the flexibility of the communication cable and the workability of installing the communication cable, the content of polypropylene in the total of the polypropylene and the soft resin is preferably 51% by mass or more and 85% by mass or less.
[0069] The polypropylene may be at least one selected from the group consisting of homopolypropylene (homoPP), random polypropylene (randomPP), block polypropylene (blockPP), and the like.
[0070] The content of the soft resin in the total of polypropylene and the soft resin is preferably 15% by mass or more and less than 49% by mass, from the viewpoints of the flexibility of the communication cable and the workability of installing the communication cable 100.
[0071] The soft resin may contain any of the above crystalline polyolefins except polypropylene, or may contain any of the above thermoplastic elastomers.
[0072] The dielectric constant of the insulator constituting the coating layer 12 is preferably 2.25 or more and 3.5 or less. By setting the dielectric constant to 2.25 or more, the insulated wire 10 can be made to have a thickness that is easy to manufacture while still satisfying the ISO21111-8 standard, and therefore the production efficiency of the communication cable 100 can be improved. In addition, by setting the dielectric constant of the insulator to 3.5 or less, the 0.13 sq (mm 2 The dielectric constant can also be applied to a communication cable having the thinnest conductor of 100 mm diameter. Furthermore, by setting the dielectric constant of the insulator to 3.5 or less, it is possible to prevent the outer diameter and weight of the communication cable 100 from becoming too large. The dielectric constant can be measured by a cavity resonator method in an atmosphere at 30° C. at a frequency of 10 GHz.
[0073] The insulator constituting the coating layer 12 can be made of polypropylene and soft resin, as well as various additives contained in the resin composition of the sheath 20 described above in appropriate amounts, within the range that does not interfere with the effects of this embodiment, but from the viewpoint of communication characteristics, it is preferable that it does not contain a plasticizer.
[0074] In order to adjust the dielectric constant of the coating layer 12, the insulator constituting the coating layer 12 preferably contains titanium oxide as an inorganic filler. The insulator preferably contains 15 to 60 parts by mass of titanium oxide per 100 parts by mass of polypropylene and soft resin in total. By making the content of titanium oxide 15 parts by mass or more, it is possible to prevent the relative dielectric constant of the insulator from becoming too low. By making the content of titanium oxide 60 parts by mass or less, it is possible to prevent the relative dielectric constant of the insulator from becoming too high.
[0075] More preferably, the insulator constituting the coating layer 12 contains 10 to 80 parts by mass of a brominated flame retardant per 100 parts by mass of the polypropylene and the soft resin in total. By making the content of the brominated flame retardant 10 parts by mass or more, the flame retardancy of the insulator can be improved. Furthermore, by making the content of the brominated flame retardant 80 parts by mass or less, it is possible to maintain the mechanical properties while not using more flame retardant than necessary, thereby reducing the manufacturing cost of the insulator.
[0076] The insulator constituting the coating layer 12 preferably contains 0.1 to 30 parts by mass of a flame retardant assistant, and more preferably 1 to 15 parts by mass of a flame retardant assistant, per 100 parts by mass of the polypropylene and the soft resin in total. The flame retardant assistant may be, for example, antimony trioxide. Antimony trioxide can improve the flame retardancy of the insulator by using it in combination with a bromine-based flame retardant.
[0077] The insulator constituting the coating layer 12 preferably contains less than 45 parts by mass of magnesium hydroxide per 100 parts by mass of the total of polypropylene and soft resin. By making the content of magnesium hydroxide less than 45 parts by mass, it is possible to prevent the relative dielectric constant from becoming too high and also to improve the flexibility of the insulator.
[0078] The insulator constituting the coating layer 12 preferably contains 0.5 to 10 parts by mass of an antioxidant per 100 parts by mass of the polypropylene and the soft resin in total. For example, the antioxidant used in the resin composition of the sheath 20 can be used. The antioxidant may be used alone or in combination of two or more kinds.
[0079] The insulator constituting the coating layer 12 preferably contains 0.01 to 10 parts by mass, and more preferably 0.1 to 5 parts by mass, of a processing aid relative to 100 parts by mass of the polypropylene and soft resin in total. For example, the processing aid used in the resin composition of the sheath 20 can be used as the processing aid.
[0080] The insulator constituting the coating layer 12 preferably contains 0.5 to 10 parts by mass of a metal deactivator (copper inhibitor) per 100 parts by mass of the polypropylene and soft resin combined. By using a metal deactivator in the insulator, the metal ions are chelated, captured, and stabilized, thereby preventing oxidation deterioration of the resin in the insulator. As the metal deactivator, an oxalic acid compound, an amide compound such as salicylic acid, or a hydrazide compound can be used. In addition, since the metal deactivator itself does not have a stabilizing effect, it is preferable to use it in combination with an antioxidant such as a phenolic antioxidant in order to impart thermal stability.
[0081] 5, the twist pitch 151 of two insulated wires 10 forming a twisted pair is preferably 15 to 45 times the outer diameter of the insulated wire 10, and more preferably 15 to 40 times the outer diameter of the insulated wire 10. By setting the twist pitch 151 to 15 times or more, the stress applied to the center side of the twist is not too large, and it is possible to prevent the insulator constituting the coating layer 12 from being crushed and the characteristic impedance from being disturbed. Furthermore, by setting the twist pitch 151 to 45 times or less, the twist pitch 151 is stable, and it is possible to prevent deterioration of the mode conversion characteristics related to the emission or resistance of electrical noise.
[0082] 5, the twist pitch 151 is one revolution of the insulated electric wire 10 spirally around the twist center 152, and means the length in the longitudinal direction of the insulated electric wire 10. The outer diameter of the insulated electric wire 10 means the diameter of a circle of a cross section of the insulated electric wire 10 perpendicular to the longitudinal direction.
[0083] Furthermore, it is preferable that the difference in length between the two insulated wires 10 be 3 mm or less per meter. By making the difference in length 3 mm or less per meter, it is possible to prevent deterioration of the mode conversion characteristics related to the emission or resistance to electrical noise.
[0084] The insulated wire 10 can be formed by a known method, for example, a general extrusion molding method. Specifically, the covering layer 12 can be formed by extruding a material for the covering layer 12 onto the outer surface of the conductor 11, which is made of one or more strands.
[0085] As described above, the communication cable 100 has a tensile strength of 400 MPa or more and a cross-sectional area of 0.22 mm 2 The communication cable 100 includes an insulated wire 10 including a conductor 11 having a thickness of 100 mm or less and a coating layer 12 made of an insulator that coats the conductor 11. The communication cable 100 further includes a sheath 20 that coats the outer periphery of the insulated wire 10 and is made of a resin composition containing crystalline polyolefin. The sheath 20 has a tensile modulus of 500 MPa or less, and in a plasticizer migration test in which the communication cable 100 and a polyvinyl chloride wire 110 are bundled and left in air at 105°C for 3000 hours, the mass increase rate of the sheath 20 is less than 50 mass%. The communication cable 100 has a characteristic impedance of 100±10Ω. Therefore, it is possible to provide a communication cable 100 that has higher flexibility, is more excellent in communication characteristics, and is less susceptible to deterioration in transmission characteristics by suppressing migration of plasticizers from other members even in a high-temperature atmosphere for a long period of time.
[0086] [Wire harness] As shown in Fig. 3, the wire harness 200 according to the present embodiment includes a communication cable 100 and a polyvinyl chloride electric wire 110, and the communication cable 100 and the polyvinyl chloride electric wire 110 are bundled together. The communication cable 100 and the polyvinyl chloride electric wire 110 are electrically connected to a connector 120. Since the above-mentioned sheath 20 is resistant to migration of a plasticizer, even if the insulation of the polyvinyl chloride electric wire 110 contains a plasticizer, migration of the plasticizer to the sheath 20 and the coating layer 12 of the insulated electric wire 10 can be suppressed. Therefore, the wire harness 200 can bundle the communication cable 100 and the polyvinyl chloride electric wire 110, which is inexpensive and highly flexible.
[0087] The polyvinyl chloride electric wire 110 may have a conductor and a coating layer. The conductor of the polyvinyl chloride electric wire 110 may have the same shape and material as the conductor 11 of the insulated electric wire 10 described above. The coating layer of the polyvinyl chloride electric wire 110 may have the same shape as the coating layer 12 of the insulated electric wire 10 described above. The coating layer of the polyvinyl chloride electric wire 110 may contain a plasticizer in addition to polyvinyl chloride. As the plasticizer, a known plasticizer that is added to polyvinyl chloride may be used. The plasticizer may be at least one selected from the group consisting of trimellitic acid-based plasticizers, aliphatic dibasic acid-based plasticizers, epoxy-based plasticizers, phthalic acid-based plasticizers, pyromellitic acid ester-based plasticizers, phosphate ester-based plasticizers, and ether ester-based plasticizers.
[0088] The phthalate plasticizer may be at least one phthalate ester selected from the group consisting of di-2-ethylhexyl phthalate (DEHP), di-n-octyl phthalate (DNOP), diisononyl phthalate (DINP), dinonyl phthalate (DNP), diisodecyl phthalate (DIDP), and ditridecyl phthalate.
[0089] The trimellitic acid-based plasticizer may be, for example, at least one trimellitic acid ester selected from the group consisting of trioctyl trimellitate (TOTM) and triisodecyl trimellitate. EXAMPLES
[0090] The present embodiment will be described in more detail below with reference to examples and comparative examples, but the present embodiment is not limited to these examples.
[0091] The conductor for Example 1 was manufactured as follows. First, pure copper was solid-solution strengthened by adding 0.3% by mass of tin using a continuous casting machine, and then work hardening was performed by applying processing strain by wire drawing, and wire drawing was performed to a wire diameter of 0.168±0.03 mm. Seven of the obtained wires were then twisted at a twist pitch of 16 mm and compression molded to form a circular compressed conductor. The obtained conductor had a cross-sectional area of 0.13 mm. 2 , the outer diameter was 0.46 mm.
[0092] The copper alloy conductor thus obtained was evaluated for tensile strength and elongation at break according to JIS Z2241. The distance between marks was 250 mm, and the pulling speed was 50 mm / min. As a result of the evaluation, the tensile strength was 760 MPa, and the elongation at break was 3%.
[0093] On the other hand, in Comparative Example 1, the conductor was prepared as follows. In Comparative Example 1, a copper alloy conductor was prepared in the same manner as in Example 1, except that compression molding was not performed and a circular conductor was used. 2 The outer diameter was 0.48 mm. Furthermore, when evaluated in the same manner as in Example 1, the conductor had a tensile strength of 790 MPa and a breaking elongation of 3%.
[0094] For the insulators constituting the coating layers of Example 1 and Comparative Example 1, the above-mentioned preparation raw materials were mixed according to the blending ratio (parts by mass) of the resin composition shown in Table 1, and kneaded in a batch-type or continuous kneader to prepare resin pellets. The resin pellets were then fed into an extruder in which the copper alloy conductor of Example 1 or Comparative Example 1 was set, and coated with a coating layer by extrusion molding, to produce two insulated wires specified in ISO21111-8.
[0095] Next, a twisted pair was formed with a twist pitch of 30 mm for the insulated wires of Example 1 and Comparative Example 1. Thereafter, the insulated wires were covered with a sheath having a blending amount (parts by mass) of the resin composition shown in Table 2 by extrusion molding in the same manner as in the production method of the insulated wire, and a communication cable was produced so that no gap was generated between the sheath and the insulated wire. The thickness of the covering layer, the finished outer diameter of the insulated wire, the thickness of the sheath, and the finished outer diameter of the communication cable are as shown in Table 3. The twist pitch of the insulated wire was 35 times the outer diameter of the insulated wire in the case of Example 1, and 33 times the outer diameter of the insulated wire in the case of Comparative Example 1.
[0096] [Table 1]
[0097] [Table 2]
[0098] [Table 3]
[0099] [resin] Block polypropylene (block PP): Made by Prime Polymer Co., Ltd. Product name: Prime Polypro (registered trademark) E150GK Low-density polyethylene (LDPE): manufactured by Dow Mitsui Polychemicals Co., Ltd. Product name: Mirason (registered trademark) 3530 Polypropylene (PP) / EVA (60wt% / 40wt%) mixture Cross-linked polyethylene Thermoplastic rubber crosslinked body: JSR Corporation Product name: EXCELINK (registered trademark) 1200B Maleic anhydride modified polystyrene-poly(ethylene-butylene)-polystyrene (modified SEBS): manufactured by Asahi Kasei Corporation, product name: Tuftec (registered trademark) M1943
[0100] [Flame retardant] (metal hydroxide) Magnesium hydroxide (Mg(OH)2): Konoshima Chemical Co., Ltd. Product name: YG-O (halogen-based flame retardant) Brominated flame retardant (1,2-bis(pentabromophenyl)ethane): manufactured by Albemarle Corporation; Trade name: SAYTEX (registered trademark) 8010
[0101] [Flame retardant synergist] Antimony trioxide (Sb2O3): manufactured by Nihon Seiko Co., Ltd. Product name: PATOX (registered trademark) M
[0102] [Antioxidants] Phenolic antioxidant: ADEKA Corporation, product name: Adeka STAB (registered trademark) AO-20 Hindered phenol antioxidant: BASF Ltd., product name: Irganox (registered trademark) 1010 Hindered phenol antioxidant: BASF Ltd. Product name: Irganox 1076 Phosphorus-based antioxidant: BASF Ltd. Product name: Irgafos (registered trademark) 168
[0103] [Processing aids] Metal soap: Katsuta Chemical Industry Co., Ltd. Product name: EMS-6P Acrylic polymer lubricant: Mitsubishi Chemical Corporation, product name: Metablen (registered trademark) P-1050 [Inorganic filler] Titanium oxide: Ishihara Sangyo Kaisha, Ltd. Product name: Typaque (registered trademark) CR-63 [Metal deactivator] Salicylic acid amide compound: ADEKA Corporation, product name: Adeka STAB (registered trademark) CDA-1
[0104] [evaluation] (characteristic impedance) The characteristic impedance of the communication cables according to Example 1 and Comparative Example 1 prepared as described above was measured using a vector network analyzer (VNA) (E5071C manufactured by Keysight Technologies) 500, as shown in FIG. 6. A test sample having a length of 10 m was prepared for the communication cables according to Example 1 and Comparative Example 1. A plate of dielectric (foam material) 502 having a relative dielectric constant of 1.4 or less was placed on a metal plate 501, and a test sample was placed on the plate. The test samples were placed 30 mm or more apart from each other and 30 mm or more inward from the edge of the metal plate 501. The test sample was then connected to a measurement board matched to 100 Ω, and a square wave with a rise time of 700 ps was applied to measure the characteristic impedance.
[0105] Fig. 7 is a graph showing the characteristic impedance of the communication cable according to Example 1. Fig. 8 is a graph showing the characteristic impedance of the communication cable according to Comparative Example 1. It can be seen that the characteristic impedance of both Example 1 and Comparative Example 1 is within the range of the standard value (100±10Ω).
[0106] As shown in Fig. 9, the communication cable 300 was formed so that a gap was generated between the outer surfaces of the two insulated electric wires 210 and the sheath 220. Other conditions were the same as those in the manufacturing method of the communication cables of Example 1 and Comparative Example 1. The insulated electric wires 210 had a cross-sectional area of 0.13 mm 2 The conductor 201 is covered with a covering layer 202. On the other hand, the polyvinyl chloride electric wire 310 includes a plurality of conductors 301 and a covering layer 302 that covers the periphery of the conductors 301. The covering layer 302 includes polyvinyl chloride and a plasticizer.
[0107] 9, six polyvinyl chloride electric wires 310 were arranged so as to surround the periphery of the communication cable 300 according to Example 1 or Comparative Example 1 at the center. Then, a polyvinyl chloride tape 320 was wound around the periphery of the polyvinyl chloride electric wires 310 to prepare a test sample 400.
[0108] (Plasticizer migration test) A plasticizer migration test was carried out to examine the effect on communication cable 300 of migration of plasticizer added to polyvinyl chloride wire 310 to sheath 220. Test samples 400 according to Example 1 and Comparative Example 1 prepared as described above were each heated to 105°C in an oven for 3000 hours, and then removed from the oven and left at room temperature for a while.
[0109] (insertion loss) The influence of the plasticizer migration test on the insertion loss of the communication cable 300 was investigated. As shown in Fig. 6, the insertion loss of the communication cable 300 according to Example 1 and Comparative Example 1 was measured before and after the plasticizer migration test using a VNA under conditions of a measurement frequency of 300 kHz to 1000 MHz and a measurement bandwidth of 100 Hz.
[0110] FIG. 10 is a graph showing the insertion loss before and after the plasticizer migration test in the communication cable according to Example 1. FIG. 11 is a graph showing the insertion loss before and after the plasticizer migration test in the communication cable according to Comparative Example 1. As shown in FIG. 10 and FIG. 11, before the plasticizer migration test (initial period), both Example 1 and Comparative Example 1 exceed the standard value of the insertion loss, but as the frequency increases, the insertion loss decreases. After the plasticizer migration test, as the frequency increases, the insertion loss decreases more significantly than at the initial period. However, the communication cable according to Example 1 has a suppressed decrease in insertion loss compared to the communication cable according to Comparative Example 1, satisfies the standard value, and is considered to have sufficient communication characteristics. On the other hand, the communication cable according to Comparative Example 1 does not satisfy the standard value, and when used for a long time under high temperature such as in a vehicle, the communication characteristics in the high frequency range may decrease, and the desired insertion loss may not be fully satisfied.
[0111] (Dielectric properties) Table 4 shows the results of measuring the dielectric constant and dielectric loss tangent of the resin composition of the sheath before and after the plasticizer migration test. Table 4 also shows the results of measuring the dielectric constant and dielectric loss tangent of the insulator constituting the coating layer before (initial) the plasticizer migration test. Specifically, for the test samples before and after the plasticizer migration test, the communication cable was cut out perpendicularly to the longitudinal direction to a length of 150 mm, and the conductor and coating layer were removed from the cut cable to prepare a sample of only the sheath. The dielectric constant and dielectric loss tangent of the test sample were measured by a cavity resonator method using a dielectric constant measuring device (ADMS01Nc manufactured by AET Corporation). The dielectric constant and dielectric loss tangent were measured at a frequency of 10 GHz in an atmosphere of 30°C. As shown in Table 4, in both Example 1 and Comparative Example 1, the dielectric constant and dielectric loss tangent of the resin composition of the sheath after the plasticizer migration test tended to increase compared to before (initial) the plasticizer migration test.
[0112] [Table 4]
[0113] (Mass increase rate) The state of migration of the plasticizer added to the polyvinyl chloride wire into the sheath was confirmed for the communication cables according to Example 1 and Comparative Example 1. Table 4 shows the results of measuring the mass of the sheath before and after the plasticizer migration test, and the rate of increase in the mass of the sheath after the plasticizer migration test.
[0114] To calculate the mass increase rate, the sheath was removed from the communication cable manufactured as described above and immersed in a container filled with DINP. After immersing the sheath in an oven at 105°C for 3000 hours, the sheath was removed from the container and the DINP adhering to the surface of the sheath was wiped off. The mass of the sheath was measured before and after immersion in DINP, and the mass increase rate was calculated as follows. DINP manufactured by J-Plus Corporation was used.
[0115] The mass gain rate can be calculated using the following formula (3). Mass increase rate (mass%) = ((mass after immersion) / (mass before immersion)-1) x 100 (3)
[0116] As shown in Table 4, it is understood that the mass increase rate of the sheath after the plasticizer migration test is significantly higher in Comparative Example 1 than in Example 1. Therefore, it is understood that the plasticizer added to the polyvinyl chloride wire of the communication cable according to Comparative Example 1 is likely to migrate to the sheath when used for a long time under high temperature conditions such as in a vehicle.
[0117] From these results, it is believed that the decrease in insertion loss is due to the plasticizer contained in the coating layer of the polyvinyl chloride wire. Therefore, we proceeded with the development of a sheath that is resistant to plasticizer migration, and in the communication cable of Example 1, the plasticizer is resistant to migration, and the decrease in insertion loss was also suppressed.
[0118] (tensile modulus) The sheaths were stripped from the communication cables according to Example 1 and Comparative Example 1 produced as described above. The stripped sheaths were pulled at a pulling speed of 50 mm / min at a room temperature of 20° C. in accordance with the provisions of JIS K7161-1. The tensile modulus of elasticity of the sheath was calculated from the stress at 0.00005 and the stress at 0.0025.
[0119] As shown in Table 4, the tensile modulus of the sheath before the plasticizer migration test (initial stage) was 500 MPa or less in both Example 1 and Comparative Example 1, which shows that the workability in wiring the communication cable is excellent.
[0120] It is found that the communication cable according to Example 1 has a sheath with a tensile modulus and a mass increase rate below a predetermined value, is more flexible, and can suppress migration of plasticizer from other members even in a high-temperature atmosphere for a long period of time. On the other hand, the communication cable according to Comparative Example 1 has a sheath with a tensile modulus below a predetermined value, but has a mass increase rate that is not below a predetermined value, and therefore is considered unable to suppress migration of plasticizer from other members in a high-temperature atmosphere for a long period of time.
[0121] In Comparative Example 2, the conductor was prepared as follows. In Comparative Example 2, a copper alloy conductor was prepared in the same manner as in Example 1. The cross-sectional area of the conductor was 0.13 mm 2 The outer diameter was 0.48 mm. Furthermore, when evaluated in the same manner as in Example 1, the conductor had a tensile strength of 750 MPa and a breaking elongation of 3%.
[0122] The conductor of Comparative Example 2 was covered with an olefin-based resin coating layer by extrusion molding to produce two insulated wires specified in ISO21111-8. Then, the wires were covered with an olefin-based resin sheath by extrusion molding to produce a communication cable. The thickness of the coating layer, the finished outer diameter of the insulated wire, the thickness of the sheath, and the finished outer diameter of the communication cable are as shown in Table 3.
[0123] (Flexibility of communication cables) The communication cables according to Example 1, Comparative Example 1, and Comparative Example 2 prepared as described above were cut perpendicular to the longitudinal direction of the communication cables to a length of 100 mm to prepare test samples. Next, as shown in FIG. 12, both ends of a test sample 600 having a length L of 100 mm were placed on a support stand 601. Then, a load was applied from above to the center of the test sample 600 at a speed of 100 mm / min, and the maximum load until the electric wire fell was measured using a force gauge. The target range of flexibility of the communication cable was evaluated as a force gauge value of 2.0 N or less.
[0124] (DINP absorption amount) The sheaths were stripped from the communication cables according to Example 1, Comparative Example 1, and Comparative Example 2 produced as described above, and immersed in a container filled with DINP (manufactured by J-Plus Corporation). After immersing the sheaths in an oven at 100°C for 72 hours, the sheaths were removed from the container, and the DINP adhering to the surface of the sheaths was wiped off. The masses of the sheaths before and after immersion in DINP were measured, and the DINP absorption amount was calculated as follows. The target range for the DINP absorption amount of the sheath was evaluated to be 20 mass% or less.
[0125] The amount of DINP absorbed can be calculated using the following formula (4). DINP absorption amount (mass%) = (mass of sheath after immersion - mass of sheath before immersion) / mass of sheath before immersion × 100 (4)
[0126] 13 and Table 5 show the relationship between the flexibility of the communication cable and the DINP absorption amount of the sheath relative to the tensile modulus of the sheath for the communication cables of Example 1, Comparative Example 1, and Comparative Example 2. The communication cable of Example 1 has a sheath tensile modulus of 500 MPa or less, a communication cable flexibility of 2.0 N or less, and a DINP absorption amount of 20 mass % or less. Thus, a communication cable with excellent flexibility and low plasticizer absorption amount was obtained.
[0127] [Table 5]
[0128] On the other hand, the communication cable of Comparative Example 1 has a sheath with a tensile modulus of 500 MPa or less and a communication cable with a flexibility of 2.0 N or less, but the DINP absorption amount is greater than 20 mass%, so it is considered to have excellent flexibility but a high amount of plasticizer absorption. Also, the communication cable of Comparative Example 2 has a DINP absorption amount of 20 mass% or less, but the sheath with a tensile modulus of 500 MPa or more and a communication cable with a flexibility of greater than 2.0 N, so it is considered to have low plasticizer absorption but poor flexibility and workability for installation.
[0129] Generally, hard materials have high crystallinity of resin, so that the amount of plasticizer absorbed is low. On the other hand, soft materials have low crystallinity or contain soft components, so that the amount of plasticizer absorbed is high. The communication cable of Example 1 can reduce the amount of plasticizer absorbed while increasing flexibility. From the above, the communication cable of Example 1 is a communication cable that has high flexibility, excellent communication characteristics, and is resistant to deterioration of transmission characteristics by suppressing the migration of plasticizer from other components even in a high-temperature atmosphere for a long period of time. Note that DINP used in the evaluation of the amount of plasticizer absorbed is a typical plasticizer, and it is considered that the same tendency is observed for plasticizers used in other polyvinyl chlorides.
[0130] Although the present embodiment has been described above with reference to examples, the present embodiment is not limited to these examples, and various modifications are possible within the scope of the present embodiment. [Explanation of symbols]
[0131] 10 Insulated wire 11 Conductor 12 Covering layer 20 Sheath 100 Communication Cable 110 Polyvinyl chloride wire 200 Wire Harness
Claims
1. An insulated wire including a conductor and a coating layer covering the conductor and made of an insulator; a sheath covering an outer periphery of the insulated wire and made of a resin composition containing a crystalline polyolefin; Equipped with The insulator contains polypropylene and a soft resin, a content of the polypropylene with respect to a total of the polypropylene and the soft resin is 51% by mass or more and 85% by mass or less, and contains 15 to 60 parts by mass of titanium oxide and 10 to 80 parts by mass of a brominated flame retardant with respect to 100 parts by mass of the total of the polypropylene and the soft resin, A communication cable having a characteristic impedance of 100±10 Ω.
2. 2. The communication cable according to claim 1, wherein the resin composition contains the crystalline polyolefin and a thermoplastic elastomer, and the content of the crystalline polyolefin relative to the total of the crystalline polyolefin and the thermoplastic elastomer is 55% by mass or more and 70% by mass or less.
3. 3. The communication cable according to claim 2, wherein the resin composition contains 40 parts by mass to 150 parts by mass of a metal hydroxide and 10 parts by mass to 30 parts by mass of a halogen-based flame retardant, relative to a total of 100 parts by mass of the crystalline polyolefin and the thermoplastic elastomer.
4. The communication cable according to any one of claims 1 to 3, wherein the insulator has a relative dielectric constant of 2.25 or more and 3.5 or less.
5. 5. The communication cable according to claim 1, wherein a twist pitch of the insulated wires is 15 times or more and 45 times or less the outer diameter of the insulated wires.
6. A communication cable according to any one of claims 1 to 5; Polyvinyl chloride wire; Equipped with The communication cable and the polyvinyl chloride electric wire are bundled together to form a wire harness.
Citation Information
Patent Citations
Communication wire
JP2017188436A
Communication cable and wire harness
JP2021044237A
Communication cable, and wire harness
WO2021200146A1