Method for recovering rare earth elements
By controlling pH during leaching and employing solid-liquid separation and extraction processes, the method effectively recovers high-purity rare earth elements from steel slag, addressing separation challenges and reducing radioactive waste.
Patent Information
- Application Number
- JP2021006598
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-19
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-01-19
AI Technical Summary
Existing methods for recovering rare earth elements from steel slag face challenges in separating main component elements and radioactive elements, leading to potential environmental issues due to the concentration of naturally occurring radioactive elements.
A method involving leaching rare earth elements from steel slag with controlled pH adjustment, followed by solid-liquid separation and extraction processes, including solid phase and solvent extraction, to achieve high purity recovery while minimizing radioactive element concentration.
The method enables efficient separation and recovery of highly pure rare earth elements with controlled separation ratios, reducing the burden of subsequent purification processes and minimizing radioactive waste production.
Smart Images

Figure 0007568925000003 
Figure 0007568925000004 
Figure 0007568925000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering rare earth elements, and more particularly to a method for recovering rare earth elements from blast furnace slag, steelmaking slag, or electric furnace slag. [Background technology]
[0002] Rare earth elements are used as additives to a wide variety of materials, including hydrogen storage alloys, secondary battery raw materials, optical glass, rare earth magnets, phosphors, abrasives, and aluminum, and are a group of elements with high industrial value. However, rare earth element ores are unevenly distributed and highly valuable, so there is a problem that the supply is small worldwide and prices fluctuate greatly due to changes in social conditions. Therefore, establishing a method to steadily supply rare earth elements in large quantities is important for industrial development.
[0003] Incidentally, the production volume of steel accounts for the majority of the total metal production, and the production volume of steel slag, which is produced as a by-product, is also very large. For example, in Japan, more than 100 million tons of crude steel is produced annually, and as by-products, about 23 million tons of blast furnace slag, about 12 million tons of steelmaking slag, and about 3 million tons of electric furnace slag are produced annually. The raw materials for steel slag, such as iron ore, coal, limestone, and iron scrap, contain trace amounts of rare earth elements, which are incorporated into the steel slag after the steelmaking process.
[0004] Patent Document 1 discloses a method for recovering rare earth elements from steel slag by magnetic separation and wet refining. The method for leaching rare earth elements described in Patent Document 1 uses salt water, a chelating agent, 0.1 mol / L hydrochloric acid or nitric acid, etc. Patent Document 2 discloses a method for recovering rare earth elements, which comprises dissolving rare earth elements, radioactive materials, iron, aluminum and other metals from tin slag with inorganic acid to obtain a leachate, adding an oxidizing agent and a neutralizing agent to the leachate to precipitate radioactive materials and separate them from rare earth elements, filtering the liquid, adding an oxidizing agent and a neutralizing agent to the filtrate to precipitate iron and separate it from rare earth elements, filtering the liquid, adjusting the pH of the filtrate, adding an organic solvent to extract rare earth elements into the organic solvent, mixing the resulting extract with inorganic acid to perform a stripping step to strip rare earth metals, and then adding oxalic acid to the stripping liquid from which rare earth metals have been stripped to produce an oxalic acid precipitate containing rare earth elements. The method of Patent Document 2 involves acid leaching of the elements to be recovered and impurities, followed by separation of impurities in an oxidation / neutralization step and a solvent extraction step. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2018-530673 [Patent Document 2] JP 2012-224943 A Summary of the Invention [Problem to be solved by the invention]
[0006] The main components of steel slag are silicon (Si), iron (Fe), aluminum (Al), magnesium (Mg), calcium (Ca), etc. It is necessary to develop a process that can separate these main component elements from rare earth elements and recover the rare earth elements.
[0007] In addition, common ores, not limited to steel slag, contain extremely small amounts of naturally radioactive elements such as thorium (Th) and uranium (U). The amount of naturally radioactive elements contained in steel slag is as small as that of natural ores, so it does not cause environmental problems. However, since the chemical properties of thorium and uranium are similar to those of rare earth elements, refining rare earth elements can produce concentrated naturally radioactive elements as by-products, which can cause environmental problems. Therefore, in order to recover rare earth elements from steel slag, it is necessary to develop a process that does not produce concentrated naturally radioactive elements, or to strictly manage by-products that contain naturally radioactive elements.
[0008] The present invention aims to provide a method for recovering rare earth elements in steel slag, which makes it possible to easily control the separation ratio between the rare earth elements and the main component elements and / or radioactive elements of the steel slag. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the leaching rate of rare earth elements and main component elements and / or radioactive elements can be controlled by leaching rare earth elements contained in steel slag with acid while controlling the pH. They have found that it is possible to use this to leach rare earth elements at a predetermined leaching rate and to remove main component elements and / or radioactive elements in the leaching process, and have completed the present invention. Furthermore, they have found that high-purity rare earth elements can be recovered by subjecting the rare earth element-containing leachate obtained in the above leaching process to an extraction process consisting of one or both of a solid-phase extraction process and a solvent extraction process, separating the rare earth elements from the main components of the steel slag, such as iron, aluminum, magnesium, calcium, and silicon, to prepare a rare earth element concentrated solution, and adding a precipitant to this to prepare a precipitate of the rare earth elements in a precipitation process, which is then roasted to obtain oxides of the rare earth elements. That is, the present invention includes the following aspects.
[0010] (1) A method for recovering rare earth elements from steel slag produced by a steelmaking process, comprising the steps of: The pH of the leachate obtained by contacting the iron and steel slag with acid The best final pH is between 1.5 and 5.0 a leaching step of adjusting the content of the rare earth element in the leachate to obtain a rare earth element-containing leachate; A solid-liquid separation step of separating solids from the rare earth element-containing leachate. and, A step of treating the rare earth element-containing leachate after the solid-liquid separation step by solid-phase extraction or by both solvent extraction and solid-phase extraction to obtain a rare earth element-enriched solution. A method for recovering rare earth elements comprising: (2 ) before The final pH is selected from the range of 3.0 to 5.0. R, (1 ) The method for recovering rare earth elements described herein. (3) 2. The method for recovering rare earth elements according to claim 1, wherein the acid is nitric acid and the final pH is selected from the range of 2.5 to 5.0. (4) 2. The method for recovering rare earth elements according to claim 1, wherein the acid is hydrochloric acid and the final pH is selected from the range of 3.0 to 4.5. (5) The method for recovering rare earth elements according to (1), wherein the acid is sulfuric acid and the final pH is selected from the range of 2.5 to 4.5. . ( 6 ) The acid may be one or more inorganic acids. R, (1) Or (2) 2. The method for recovering rare earth elements according to claim 1 . (7) Furthermore, after the solid-liquid separation step and prior to said extraction step, The pH of the rare earth element-containing leachate is adjusted by adding a base or acid to the rare earth element-containing leachate to obtain a pH-adjusted rare earth element-containing leachate. pH adjustment engineering The process The method for recovering rare earth elements according to any one of (1) to (6), (8) The solvent extractant used in the extraction step is an extractant of any one of an amine type, an organic phosphoric acid type, and a carboxylic acid type, and the solid phase extractant used in the extraction step is a resin having iminodiacetic acid as a functional group. ru, (1)~ (7) Any one of the following 2. The method for recovering rare earth elements according to claim 1 . (9) The method for recovering rare earth elements according to any one of (1) to (8), further comprising a precipitation step of adding a precipitating agent to the rare earth element concentrated solution after the extraction step to obtain a rare earth element precipitate, and a roasting step of roasting the rare earth element precipitate to obtain an oxide of the rare earth element. (10 ) The precipitating agent used in the precipitation step is any one of oxalic acid, carbonic acid, tartaric acid, and a base. Characterized by: (9) 2. The method for recovering rare earth elements according to claim 1 . ( 11 ) The iron and steel slag is blast furnace slag. 10 ) The method for recovering rare earth elements according to any one of claims 1 to 5. Effect of the Invention
[0011] According to the present invention, there is provided a method for recovering rare earth elements in steel slag, which allows easy control of the separation ratio between the main component elements and / or radioactive elements of the steel slag. Furthermore, by selecting the final pH of the leaching solution from a specific range, high-purity rare earth elements can be recovered from the steel slag at a high recovery rate. In particular, by controlling the pH in the leaching process to control the leaching rates of rare earth elements and main component elements and / or radioactive elements, leaching of rare earth elements and separation of main component elements and / or radioactive elements can be performed simultaneously, thereby reducing the burden on the refining process following the leaching process. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a flow chart illustrating an example of a method for recovering rare earth elements. [Diagram 2] FIG. 2 is a flow chart illustrating an example of a solid phase extraction process. [Diagram 3] FIG. 3 is a diagram showing the particle size distribution of the iron and steel slag used in the examples. [Figure 4] FIG. 4 shows the leaching rate of rare earth elements as a function of the final pH of the leaching solution. [Diagram 5] Figure 5 shows the separation ratios of rare earth elements, aluminum, and silicon as a function of the final pH of the leachate. [Figure 6] Figure 6 shows the separation ratio of rare earth elements and thorium as a function of the final pH of the leachate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A specific embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described in detail below with reference to the drawings. However, the present invention is not limited to the following embodiment, and can be implemented with appropriate modifications within the scope that does not change the gist of the present invention.
[0014] There are multiple definitions of the elements included in the term rare earth elements, but the definition of the term rare earth elements shown in this disclosure is a group of elements including a total of 17 elements, consisting of lanthanides (Ln) consisting of lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu), plus yttrium (Y) and scandium (Sc).
[0015] In this disclosure, the term "steel slag" is defined as including blast furnace slag produced in the iron-making process, steelmaking slag produced in the steelmaking process, and electric furnace slag produced in electric furnaces.
[0016] 1 and 2 are flow diagrams for explaining an exemplary method for recovering rare earth elements. In the method for recovering rare earth elements, a leachate obtained by leaching steel slag with an acid such as sulfuric acid, nitric acid, or hydrochloric acid is introduced into a refining process, and rare earth elements are separated from elements such as aluminum, magnesium, calcium, and silicon that are main components of steel slag, and from radioactive elements such as thorium and uranium, to recover the rare earth elements.
[0017] The first feature of the present invention is that in the leaching step K, the ratio of the amounts of the steel slag and the acid to be contacted is controlled to control the pH of the leachate, thereby controlling the leaching rates of the rare earth elements and the main element and / or the radioactive element, and thus leaching of the rare earth elements is performed. By selecting an appropriate final pH, a high leaching rate of the rare earth elements and a high separation ratio from the main element and / or the radioactive element can be obtained. Although not an essential aspect, the second feature of the present invention is that the rare earth elements in the rare earth-containing leachate obtained in the leaching step K are purified in an extraction step M including either one or both of a solid-phase extraction step M1 and a solvent extraction step M2.
[0018] By using the method of the present invention, rare earth elements can be leached from steel slag at the desired leaching rate and separation ratio. Therefore, rare earth elements in steel slag can be recovered at a high recovery rate, and high-purity rare earth elements can be recovered even from raw materials containing many impurities such as steel slag. In addition, by simultaneously performing leaching of rare earth elements and rough separation of main component elements and / or radioactive elements in the leaching step K, the burden of the refining step can be reduced and rare earth elements can be recovered at a lower cost. In particular, by roughly separating thorium, a natural radioactive element, in the leaching step, which is the first stage of the entire rare earth element recovery process, the risk of generating thorium concentrate can be eliminated.
[0019] Although not essential, the steel slag may be pulverized to increase its surface area prior to the leaching step K. Alternatively, the molten steel slag may be subjected to a water granulation process when cooled to produce fine granulated slag with a large surface area. Increasing the surface area of the steel slag can increase the leaching rate of the rare earth elements in the steel slag.
[0020] <Leaching process K> In the leaching step K, the steel slag is immersed in an acid to leach the rare earth elements into the solvent. More specifically, the pH of the leachate obtained by contacting the steel slag with the acid is adjusted to a predetermined final pH to obtain a rare earth element-containing leachate. The pH can be adjusted by controlling the amount of acid or base added while monitoring the pH of the leachate obtained by contacting the steel slag with the acid. The acid can be an inorganic acid or an organic acid, and an inorganic acid is preferred. Specific examples of the inorganic acid include sulfuric acid, nitric acid, and hydrochloric acid. From the viewpoint of the leaching rate of the rare earth elements and the separation ratio between the rare earth elements and aluminum and silicon, hydrochloric acid and nitric acid are preferred, and from the viewpoint of the separation ratio between the rare earth elements and thorium, hydrochloric acid and nitric acid are preferred, and hydrochloric acid is more preferred. From the viewpoint of the balance between the separation ratio and the leaching rate, sulfuric acid is preferred. The acid is preferably a strong acid from the viewpoint of obtaining a high leaching rate of the rare earth elements. From the same viewpoint, the pK a is preferably not more than −2. One or more acids can be used.
[0021] A specific method for carrying out the leaching step K is exemplified below. Steel slag is charged into a leaching reaction vessel, and acid is added. At this time, the solid-liquid ratio of steel slag to acid is preferably 1:1 to 1:100. The pH of the acid to be added may be 1.0 or less. Since steel slag contains 10 to 70% oxides and hydroxides of calcium and magnesium, the amount and pH of the acid to be added initially may be determined in anticipation of neutralization by these. As a method for monitoring the pH, a method may be used in which a pH sensor is immersed in the leachate obtained by contacting the steel slag with acid, and the pH of the leachate is monitored at any time. In addition, it is preferable to appropriately perform stirring or the like so that the pH of the leachate becomes uniform. In addition, the rare earth elements can be sufficiently leached even under conditions where the leachate temperature is normal temperature of 15 to 35°C and the pressure is normal pressure of about 1013 hpa, but the rare earth elements may be leached while heating or pressurizing in order to increase the leaching rate. When the pH of the leachate is higher than the target final pH, an acid can be added in small amounts while monitoring the pH value to adjust the pH to the final pH. On the other hand, when the pH of the leachate is lower than the target final pH, an iron and steel slag or a basic substance can be added in small amounts while monitoring the pH value to adjust the pH to the final pH. In this disclosure, the final pH of the leachate is the pH at which the rate of change of the pH after the addition of an acid or base becomes 1 / min or less. Examples of the basic substance include, but are not limited to, sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, etc. The final pH can be appropriately determined depending on the purpose, and may be selected from a range consisting of any combination of an upper limit of less than 7.0, 6.0, 5.5, 5.0, 4.5, or 4.0 and a lower limit of 0.0, 1.0, 1.5, 2.0, 2.5, or 3.0. In one embodiment, from the viewpoint of improving the leaching rate of rare earth elements, the final pH can be selected from 5.0 or less. By selecting the final pH from 5.0 or less, the leaching rate of rare earth elements represented by the following (Equation 1) can be, for example, 20% or more. [Rare earth element leaching rate (%)] = [leached rare earth elements (μg)] ÷ [rare earth elements in steel slag (μg)] × 100 (Equation 1) In another embodiment, the final pH may be selected from the range of 1.5 to 5.0. By controlling the final pH to a value within this range, the separation ratio of rare earth elements and thorium calculated from the following (Equation 2) and (Equation 3) can be set to, for example, about 5 to about 350. That is, rare earth elements can be leached at a high leaching rate and the rare earth elements and thorium can be separated simultaneously. By separating thorium, which is a radioactive element, at an early stage of the entire rare earth element recovery process, the amount of by-products containing radioactive substances produced can be significantly reduced. This allows the management cost of concentrates of natural radioactive elements in rare earth element recovery to be significantly reduced. [Thorium leaching rate (%)] = [Leaked thorium (μg)] ÷ [Thorium in steel slag (μg)] × 100 (Equation 2) [Rare earth element and thorium separation ratio] = [Rare earth element leaching rate] ÷ [Thorium leaching rate] (Equation 3) Also, by selecting the final pH in the range of 1.5 or more and 5.0 or less, the leaching rates of aluminum and silicon in the steel slag represented by the following (Formula 4) decrease. Therefore, since the rough separation of the main component elements and the leaching of rare earth elements can be carried out simultaneously, it becomes possible to reduce the burden on the purification process following the leaching process. The separation ratio of the rare earth element to aluminum or silicon is calculated from the following (Formula 5). [Leaching rate of aluminum or silicon (%)]=[Leached aluminum or silicon (μg)]÷[Aluminum or silicon in steel slag (μg)]×100 (Formula 4) [Separation ratio of rare earth element to aluminum or silicon]=[Leaching rate of rare earth element]÷[Leaching rate of aluminum or silicon] (Formula 5) In other embodiments, the final pH may be selected from the range of 3.0 or more and 5.0 or less. When the final pH is controlled to a value within this range, the separation ratio of the rare earth element to thorium can be made higher.
[0022] <Solid-liquid separation step L> The solid-liquid separation step L is a step of separating solid components from the rare earth element-containing leachate obtained in the leaching step K. In the solid-liquid separation step L, the rare earth element-containing leachate obtained in the leaching step K and the leaching residue can be physically separated. As the separation method, known solid-liquid separation devices such as a continuous thickener, a deep cone thickener, a lamella thickener, a drum filter, a disk filter, a horizontal belt filter, a filter press, a pressure filter, and centrifugation may be used.
[0023] By subjecting the rare earth element-containing leachate obtained by the leaching step K and the solid-liquid separation step L to an optional purification step, the purity of the rare earth element can be further increased. Examples of the optional purification step include a pH adjustment step, an extraction step M, a precipitation step N, a roasting step O, and the like. Hereinafter, exemplary methods of each step will be described.
[0024] <pH adjustment step> Although not essential, a pH-adjusted rare earth element-containing leachate may be obtained by adding a base or an acid to the leachate that has been subjected to the leaching step K or the solid-liquid separation step L to adjust the pH. By adjusting the pH of the leachate to between 0.5 and 8, the adsorption rate of the rare earth element to the solid phase is improved in the solid-phase extraction step M1 described below, and separation from the main components of the steel slag, such as calcium and magnesium, becomes possible. <Extraction process M> The extraction step M is, for example, a step of extracting rare earth elements from the rare earth element-containing leachate after the solid-liquid separation step L to obtain a rare earth element-concentrated solution. The extraction step M preferably includes one or both of a solid-phase extraction step M1 for concentrating rare earth elements by the principle of solid-phase extraction and a solvent extraction step M2 for concentrating rare earth elements by the principle of solvent extraction. When both the solid-phase extraction step M1 and the solvent extraction step M2 are used, the order in which the rare earth element-containing leachate after the solid-liquid separation step is treated may be any. When only one of the solid-phase extraction step M1 and the solvent extraction step M2 is used in the extraction step M, there is an advantage that the equipment can be simplified and the rare earth elements can be recovered at low cost, but the purity of the obtained rare earth elements is lower than when both the solid-phase extraction step M1 and the solvent extraction step M2 are used. On the other hand, when rare earth elements are recovered using both the solid-phase extraction process M1 and the solvent extraction process M2, there is an advantage that rare earth elements can be recovered with high purity, but compared to using only one of the solid-phase extraction process M1 and the solvent extraction process M2, the equipment becomes larger and the equipment costs become higher. The above advantages and disadvantages can be used according to the purpose. For example, when rare earth elements are used for applications such as misch metals where the inclusion of a small amount of impurities is not a problem, one extraction process is sufficient. On the other hand, when the application is such as for the electronics industry where the purity of the product is particularly important, an extraction process that combines the solid-phase extraction process M1 and the solvent extraction process M2 is desirable.
[0025] <Solid phase extraction process M1> The solid-phase extraction step M1 is a step included in the extraction step M, and includes, for example, a rare earth element adsorption step M11, a cation removal step M12, and a rare earth element elution step M13. If necessary, a solid-phase washing step M14 can be performed in the solid-phase extraction step M1. In the rare earth element adsorption step M11, for example, the leaching solution may be contacted with a solid-phase extraction agent such as a solid phase made of a resin having iminodiacetic acid as a functional group to adsorb cations onto the solid phase to obtain a cation-adsorbed solid phase. In the subsequent cation removal step M12, for example, an inorganic acid of less than 0.3N may be contacted with the cation-adsorbed solid phase to elute cations other than rare earth elements from the solid phase to obtain a rare earth element adsorbed solid phase. In the rare earth element elution step M13, for example, an inorganic acid of 0.3N or more and less than 3N may be contacted with the rare earth element adsorbed solid phase to elute rare earth elements to obtain a rare earth element solid phase eluent. In the solid phase washing step M14, for example, the solid phase that has been subjected to the rare earth element elution step M13 may be contacted with an inorganic acid of 3N or more to elute impurity cations.
[0026] Although not essential, the solid phase that has been subjected to the solid phase washing step M14 can be reused as the solid phase in the rare earth element adsorption step M11. By repeatedly using the solid phase, the consumption of the resin having iminodiacetic acid as a functional group can be reduced, which is economically advantageous. However, if the same solid phase is used repeatedly, the resin having iminodiacetic acid as a functional group deteriorates and its performance decreases, resulting in a decrease in the ability to separate impurities and rare earth elements. In this case, the performance can be restored to the original state by replacing it with a new resin having iminodiacetic acid as a functional group.
[0027] <Solvent extraction process M2> The solvent extraction step M2 is a step included in the extraction step M, and is, for example, a step including an extraction step M21 and a stripping step M22. In the extraction step M21, for example, an organic solvent containing a solvent extractant may be mixed with the leaching solution to distribute the rare earth element into the organic solvent to obtain a rare earth element-containing organic phase. In the stripping step M22, for example, the rare earth element-containing organic phase obtained in the extraction step M21 may be mixed with water to distribute the rare earth element from the organic phase to the aqueous phase for stripping. In the stripping step M22, pH adjustment may be performed as necessary. The pH may be a pH suitable for the organic solvent used, etc.
[0028] In the extraction step M21 and the stripping step M22, when the organic phase and the aqueous phase are mixed, a known solvent extraction device such as a centrifugal extractor or a pulse column may be used.
[0029] The solvent extractant used in the extraction step M21 may be a conventionally known one, for example, a carboxylic acid extractant such as neodecanoic acid, an organic phosphoric acid extractant such as di(2-ethylhexyl)phosphoric acid, tributyl phosphate, or trioctylphosphine oxide, or an amine extractant such as triisooctylamine. The solvent extractant may be used without a solvent, or may be dissolved in an organic solvent that is immiscible with water, such as kerosene, xylene, or toluene. The solvent extractant may be added to the aqueous phase.
[0030] <Precipitation process N> The precipitation step N is a step of obtaining a rare earth element precipitate by adding a precipitant to the rare earth element concentrated solution obtained, for example, through the extraction step M. Examples of the precipitant include bases and acids. Examples of the base include metal-containing basic salts such as sodium hydroxide and potassium hydroxide, and organic bases such as tetramethylammonium hydroxide (TMAOH), with organic bases being preferred from the viewpoint of obtaining rare earth elements of higher purity. Examples of the acid include acids such as tartaric acid, carbonic acid, and oxalic acid, with oxalic acid being preferred.
[0031] In the precipitation step N, when oxalic acid is used as a precipitant, it has the advantage that rare earth elements can be separated from impurities such as uranium, aluminum, and iron contained in the rare earth element concentrated solution with high efficiency, but has the disadvantage that the separation ability from magnesium and calcium is low. On the other hand, when a base is used as a precipitant, it has the advantage that rare earth elements can be separated from impurities such as uranium, magnesium, and calcium contained in the rare earth element concentrated solution with high efficiency, but has the disadvantage that the separation ability from iron and aluminum is low. Since the impurities contained in the rare earth element concentrated solution vary depending on the components of the steel slag and the impurity elements that cause problems vary depending on the use of the rare earth elements, it is only necessary to use a different precipitant depending on the purpose.
[0032] The resulting rare earth element precipitate and the post-precipitation solution can be physically separated using known solid-liquid separation devices such as a continuous thickener, deep cone thickener, lamellar thickener, drum filter, disc filter, horizontal belt filter, filter press, pressure filter, and centrifuge.
[0033] <Roasting process O> The roasting step O is a step of roasting the rare earth element precipitate obtained in the precipitation step N to obtain an oxide of the rare earth element. The roasting step O may include a washing step O1 and a heating step O2. In the washing step O1, for example, the rare earth element precipitate obtained in the precipitation step N may be washed with water to remove impurities. In the heating step O2, for example, the rare earth element precipitate that has been subjected to the washing step O1 may be heated to remove moisture, and volatile elements such as carbon, phosphorus, and nitrogen may be vaporized and removed, and the rare earth element may be reacted with oxygen to obtain an oxide of the rare earth element.
[0034] In the roasting step O, the roasting conditions are not limited, but may be, for example, placed in a tubular furnace and heated at about 900° C. for about 2 hours. Alternatively, by using a continuous furnace such as a rotary kiln, drying and roasting can be carried out in the same device, making it possible to produce rare earth oxides industrially with high efficiency. EXAMPLES
[0035] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these descriptions in any way.
[0036] Example 1 Prior to the leaching process, 1 cm 3 From 4cm 3 An example of the particle size distribution of steel slag in which the surface area was increased by pulverizing steel slag having a particle size of about 100 nm using a ball mill is shown in Fig. 3. In addition, the elemental composition of the steel slag used in the experiment, which was determined by measuring the steel slag using X-ray fluorescence analysis, is shown in Table 1 as an example. In this example, blast furnace slag was used as the target of the steel slag. [Table 1]
[0037] Next, the steel slag was contacted with an acid (hydrochloric acid, nitric acid, or sulfuric acid) having a pH of 1.0 or less at a solid-liquid weight ratio of 1:100. After 24 hours, the pH was measured to confirm whether the pH of the leachate reached a predetermined value (hydrochloric acid: pH 9.9, 4.3, 0.97, 0.47, -0.5; nitric acid: pH 9.9, 3.8, 0.82, 0.39, -0.5; sulfuric acid: pH 9.9, 3.6, 0.67, 0.35, -0.6). If the pH was higher than the target value, acid was added, and if the pH was lower than the target value, steel slag was added. After performing these operations and confirming that the pH reached the predetermined value 24 hours later, the leachate was subjected to elemental analysis using an inductively coupled plasma mass spectrometer.
[0038] The total amount of rare earth elements in the steel slag was determined by completely dissolving the steel slag using the acid decomposition method and the melting method, and measuring the sample with the inductively coupled plasma mass spectrometer described above. The leaching process was performed at room temperature of 25°C and at a pressure of 1013 hPa.
[0039] The above measured values were substituted into the above (Equation 1) to calculate the leaching rate of rare earth elements, and the relationship between the final pH and the leaching rate of rare earth elements is shown in Figure 4. As is clear from Figure 4, the leaching rate of rare earth elements can be changed by changing the final pH of the leaching solution. In particular, it was confirmed that a rare earth leaching rate of 20% or more can be achieved by setting the final pH of the leaching solution to be between -0.5 and 5. In other words, it was shown that controlling the pH of the leaching solution is effective in controlling the leaching rate of rare earth elements.
[0040] In addition, the leaching rates of aluminum and silicon were calculated using (Equation 4), and the leaching rates of rare earth elements were substituted into (Equation 5) to calculate the separation ratios of rare earth elements and aluminum or silicon. The results are shown in Figure 5. As is clear from Figure 5, the separation ratios of rare earth elements and aluminum or silicon can be changed by changing the final pH of the leaching solution. In other words, it was shown that controlling the pH of the leaching solution is effective in controlling the separation ratios of rare earth elements and aluminum or silicon. In particular, when the final pH was selected from the range of 1.5 to 5.0, the separation ratios of rare earth elements and aluminum or silicon were higher than those under other pH conditions. Furthermore, when the final pH of the leaching solution was selected from the range of 1.5 to 5.0 using hydrochloric acid or nitric acid, the separation ratios of rare earth elements and aluminum or silicon could be set to about 2 to 9. In other words, by selecting the final pH of the leachate from within the above range, it is possible to simultaneously carry out rough separation of aluminum and silicon, the main components of steel slag, from rare earth elements and leaching of the rare earth elements, thereby reducing the burden on the refining process that follows the leaching process. By treating the leachate obtained by this method through steps L to O shown in Figures 1 and 2, rare earth elements can be efficiently recovered.
[0041] Next, the leaching rate of thorium was calculated in the same manner. That is, the experimental values were substituted into (Equation 2) and (Equation 3), and the leaching rate of thorium and the separation ratio of rare earth elements and thorium were calculated and shown in Figure 6. As is clear from Figure 6, the separation ratio of rare earth elements and thorium can be changed by changing the final pH of the leaching solution. That is, it was shown that controlling the pH of the leaching solution is effective in controlling the separation ratio of rare earth elements and thorium. In particular, by selecting the final pH from the range of 1.5 to 5.0, the separation ratio can be set to about 5 to 350. By selecting the final pH of the leaching solution from the above range, it is possible to simultaneously perform crude separation of thorium and rare earth elements, which are radioactive elements, and leaching of the rare earth elements, thereby reducing the burden of the refining process following the leaching process. In particular, by separating thorium at the early stage of the entire rare earth element recovery process, the amount of by-products containing radioactive substances can be significantly reduced, and the management cost of concentrates of natural radioactive elements can be significantly reduced. By treating the leachate obtained by the above method through steps L to O shown in Figures 1 and 2, rare earth elements can be efficiently recovered.
[0042] Example 2 In order to verify the effect of selecting the final pH of the leaching solution from a specific range, the weights of rare earth elements and thorium recovered from 10,000 tons of steel slag were calculated. That is, the weights of rare earth elements and thorium leached when the final pH was set to -0.5 using sulfuric acid and when the final pH was set to 3.6 were obtained by the same operation as in Example 1, and the weights of rare earth elements and thorium recovered from 1 ton of steel slag were calculated and shown in Table 2. To simplify the calculation, it was assumed that the behavior of rare earth elements and Th from the extraction process M to the roasting process O in Figure 1 was the same and that the yield was 100%. [Table 2]
[0043] As is clear from Table 2, if the final pH of the leachate is -0.5, more than 100 kg of thorium concentrate can be generated as waste when 10,000 tons of blast furnace slag are treated. On the other hand, if the final pH of the leachate is set to 3.6 in the leaching process, which is the initial stage of the recovery process, and thorium and rare earth elements are separated at a high separation ratio, the thorium concentration at a concentration level that requires treatment as a radioactive material can be reduced, and the amount of waste generated can be kept to 10 kg or less for the treatment of 10,000 tons of blast furnace slag. Separating rare earth elements and thorium through leaching with pH control can reduce the cost of thorium management, reduce the burden on the refining process, and allow rare earth elements to be recovered at lower cost. [Explanation of symbols]
[0044] K leaching process L Solid-liquid separation process M extraction process M1 solid phase extraction process M2 solvent extraction process N Precipitation process O Roasting process O1 Cleaning process O2 heating process M11 Rare earth element adsorption process M12 Cation removal process M13 Rare earth element elution process M14 Solid phase washing process
Claims
1. A method for recovering rare earth elements from iron and steel slag produced by a steelmaking process, comprising the steps of: a leaching step of adjusting the pH of a leachate obtained by contacting the iron and steel slag with an acid to a final pH of 1.5 to 5.0 to obtain a leachate containing rare earth elements; a solid-liquid separation step of separating solids from the rare earth element-containing leachate; and an extraction step of treating the rare earth element-containing leachate after the solid-liquid separation step by solid-phase extraction, or by both solvent extraction and solid-phase extraction, to obtain a rare earth element concentrated solution.
2. 2. The method for recovering rare earth elements according to claim 1, wherein the final pH is selected from the range of 3.0 to 5.
0.
3. A method for recovering rare earth elements as described in claim 1, wherein the acid is nitric acid and the final pH is selected from the range of 2.5 or more and 5.0 or less.
4. A method for recovering rare earth elements as described in claim 1, wherein the acid is hydrochloric acid and the final pH is selected from the range of 3.0 or more and 4.5 or less.
5. A method for recovering rare earth elements as described in claim 1, wherein the acid is sulfuric acid and the final pH is selected from the range of 2.5 or more and 4.5 or less.
6. 3. The method for recovering rare earth elements according to claim 1, wherein the acid comprises one or more inorganic acids.
7. The method for recovering rare earth elements according to any one of claims 1 to 5, further comprising a pH adjustment step of adjusting the pH of the rare earth element-containing leachate by adding a base or an acid after the solid-liquid separation step and before the extraction step to obtain a pH-adjusted rare earth element-containing leachate.
8. The method for recovering rare earth elements according to any one of claims 1 to 5, wherein the solvent extractant used in the extraction step is an extractant of any one of an amine type, an organic phosphoric acid type, and a carboxylic acid type, and the solid-phase extractant used in the extraction step is a resin having iminodiacetic acid as a functional group.
9. A method for recovering rare earth elements described in any one of claims 1 to 5, further comprising a precipitation step of adding a precipitating agent to the rare earth element concentrated liquid after the extraction step to obtain a rare earth element precipitate, and a roasting step of roasting the rare earth element precipitate to obtain an oxide of the rare earth element.
10. 10. The method for recovering rare earth elements according to claim 9, wherein the precipitating agent used in the precipitation step is any one of oxalic acid, tartaric acid, carbonic acid and a base.
11. The method for recovering rare earth elements according to any one of claims 1 to 5, wherein the iron and steel slag is blast furnace slag.
Citation Information
Patent Citations
Method for producing rare earth-containing niobium alloy with blast furnace waste slag after smelting from Baiyunebo mine
CN101067183A
Ionic type rare-earth fine ore acid leaching process
CN104328290A
Method for extracting rare earth from iron and thorium waste residues
CN106916975A
Method for recovering rear earth element
JP1993287405A
Method for recovering rare earth metal
JP2012224943A