CURABLE RESIN COMPOSITION, METHOD FOR PRODUCTION THEREOF, AND CURED PRODUCT THEREOF

A curable resin composition using bismuth catalysts and alkaline water with epoxy resin and hydrolyzable silyl groups addresses the slow curing and adhesion issues of organotin-based systems, providing rapid and uniform curing across adhesive surfaces and interiors.

JP7568940B2Active Publication Date: 2024-10-17THREE BOND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021563832
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-11
Filing Date
2020-11-24
Publication Date
2024-10-17
Estimated Expiration
2040-11-24

AI Technical Summary

Technical Problem

Conventional curable resin compositions using organotin catalysts for epoxy resins and modified silicone polymers face issues with poor surface and internal curability during bonding of adhesive members, particularly when exposed to humid environments, leading to slow curing and potential cracking due to differential hardening rates.

Method used

A curable resin composition comprising epoxy resin, bismuth catalyst, water with a pH of 8.0 or higher, an organic polymer with hydrolyzable silyl groups, and an epoxy resin hardener, which eliminates the need for organotin catalysts and enhances both surface and internal curability.

Benefits of technology

The composition achieves rapid and uniform curing across the surface and interior of bonded adhesive members, ensuring strong adhesion and flexibility without the use of toxic organotin catalysts, suitable for various applications including adhesives, sealants, and thermally conductive resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568940000001
    Figure 0007568940000001
  • Figure 0007568940000002
    Figure 0007568940000002
Patent Text Reader

Abstract

[Problem] The present invention provides a curable resin composition that, without the use of an organic tin catalyst, has superior surface curability and has superior interior curability when used to adhere together adhesion members. [Solution] A curable resin composition including components (A) to (E). Component (A) is an epoxy resin having two or more epoxy groups per molecule, component (B) is a bismuth-based catalyst, component (C) is water with a pH of 8.0 or higher, component (D) is an organic polymer having two or more hydrolyzable silyl groups per molecule, and component (E) is a curing agent for epoxy resins.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable resin composition that has excellent curability without using an organotin catalyst, a method for producing the same, and a cured product thereof. [Background technology]

[0002] Epoxy resins have excellent adhesive strength, sealing properties, high strength, heat resistance, electrical properties, and chemical resistance. For this reason, epoxy resins have been used in various applications such as adhesives, sealing agents, sealants, potting agents, coating agents, and conductive pastes. However, although the cured products of such epoxy resins exhibit high mechanical strength, they may lack flexibility. Therefore, the cured products of epoxy resins may not be able to follow the movement of the adherend, and may crack or peel off.

[0003] For this reason, modified silicone resins are blended into epoxy resins in order to impart flexibility to the resins.As one such technique, JP2007-099806A discloses an adhesive that is characterized by comprising an A-liquid blended with an epoxy resin, a curing catalyst for modified silicone polymers, and a filler, and a B-liquid blended with a modified silicone polymer having an alkoxysilyl group at its end, and an epoxy resin curing agent. Summary of the Invention

[0004] However, the curable resin composition disclosed in JP 2007-099806 A uses an organotin catalyst as a curing catalyst for modified silicone polymers (curing agent for modified silicone resins). Tin catalysts are highly toxic and harmful to the human body, and there are moves to restrict their use in various countries. Therefore, there is a strong demand for alternative catalysts to organotin catalysts.

[0005] Examples of catalysts that substitute for organotin include titanium catalysts. However, as a result of the study, the present inventors found that the curable resin composition using a titanium catalyst has a problem of poor surface curability and poor internal curability when bonding adhesive members, as shown in Comparative Example 5 of the present specification described later. The problem of poor internal curability when bonding adhesive members is as follows. When bonding substrates with a moisture-curable resin composition to each other over a large area, the moisture-curable resin composition in the peripheral area that is in contact with the air containing moisture cures first. And, because the cured product blocks moisture from penetrating into the uncured center, it takes a long time for the moisture-curable resin composition in the center to cure.

[0006] Therefore, an object of the present invention is to provide a curable resin composition that does not use an organotin catalyst and has excellent surface curing properties and internal curing properties when bonding members are attached.

[0007] The gist of the present invention is as follows: The present invention overcomes at least one of the problems associated with conventional curable resin compositions containing an epoxy resin, a modified silicone polymer, and a titanium catalyst.

[0008] One aspect of the present invention relates to the following [1]: [1] A curable resin composition comprising the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; (B) component: bismuth-based catalyst; (C) Component: Water having a pH of 8.0 or more (i.e., a water-containing liquid having a pH of 8.0 or more); Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): Hardener for epoxy resin.

[0009] Furthermore, the present invention includes the following embodiments [2] to [11-2] as non-limiting examples of preferred embodiments: [2] The curable resin composition according to [1], wherein the component (C) is alkaline electrolyzed water; [3] The curable resin composition according to [1] or [2], wherein the component (C) is water containing at least one compound selected from the group consisting of sodium hydroxide, calcium hydroxide, potassium carbonate, and sodium metasilicate; [4] The curable resin composition according to any one of [1] to [3], wherein the component (B) is a bismuth carboxylate; [5] The curable resin composition according to any one of [1] to [4], comprising 0.05 to 30 parts by mass of the (C) component per 100 parts by mass of the (A) component; [6] The curable resin composition according to any one of [1] to [5], wherein the component (E) is an amine compound that is liquid at 25°C; [7] The curable resin composition according to any one of [1] to [6], further comprising a filler as a component (F); [8] The curable resin composition according to any one of [1] to [7], which is a room temperature curable resin composition; [9] The curable resin composition according to any one of [1] to [8], which is a two-component curable resin composition;

[10] The curable resin composition according to [9], characterized in that the two-component curable resin composition contains an A component and a B component, the A component contains the (A) to (C) components, and the B component contains the (D) component and the (E) component; [10-2] The curable resin composition according to any one of [1] to

[10] , which is substantially free of an organotin catalyst; [10-3] The curable resin composition according to any one of [1] to [10-2], characterized in that the component (A) is at least one selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, diglycidyl ethers of alkylene oxide adducts of bisphenol A type, diglycidyl ethers of alkylene oxide adducts of bisphenol F type, and alkylene oxide adducts of bisphenol E type; [10-4] The curable resin composition according to any one of [1] to [10-3], wherein the hydrolyzable group constituting the hydrolyzable silyl group is at least one selected from the group consisting of a halogen atom, an alkoxy group, an acyloxide group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxide group; [10-5] The curable resin composition according to any one of [1] to [10-4], wherein the hydrolyzable silyl group is at least one selected from the group consisting of a trimethoxysilyl group, a triethoxysilyl group, a triisopropoxysilyl group, a triphenoxysilyl group, a methyldimethoxysilyl group, a methyldiethoxysilyl group, a dimethylmethoxysilyl group, and a dimethylethoxysilyl group; [10-6] The curable resin composition according to any one of [1] to [10-5], wherein the component (D) has at least one structure selected from the group consisting of polyoxyalkylene, polyester, polycarbonate, polyurethane, polyamide, polyurea, polyimide, polyethylene, polypropylene, polyisobutylene, poly(meth)acrylate, polystyrene, polyvinyl chloride, polybutadiene, polyisoprene, polyvinyl butyral, and polyvinyl ether; [10-7] The curable resin composition according to any one of [1] to [10-6], wherein the component (E) is at least one selected from the group consisting of an aliphatic polyamine, an alicyclic polyamine, an aromatic polyamine, a secondary amine, a tertiary amine, a polyamidoamine, and a polyamide; [10-8] The curable resin composition according to any one of [1] to [10-7], characterized in that the component (E) is at least one selected from the group consisting of piperidine, pyridine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethylenediamine, dimethylcyclohexylamine, dimethylbenzylamine, dimethylhexylamine, dimethylaminophenol, 2,4,6-tris(dimethylaminomethyl)phenol, dimethylamino-p-cresol, piperidine, 1,4-diazadicyclo[2.2.2]octane, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo[5.4.0]undecene-1; [10-9] The curable resin composition according to any one of [1] to [10-8], further comprising a filler as component (F), the component (F) being at least one selected from the group consisting of talc, silica, clay, calcium carbonate, magnesium carbonate, calcium silicate, glass, alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, carbon, diamond, gold, silver, copper, and nickel; [10-10] The curable resin composition according to any one of [1] to [10-9], further comprising a filler as component (F), the component (F) including a filler having a small average particle size of 0.01 μm or more and less than 5.0 μm, and a filler having a large average particle size of 5.0 μm or more and 150 μm or less; [10-11] The curable resin composition according to any one of [1] to [10-10], further comprising a silane coupling agent; [10-12] The curable resin composition according to any one of [1] to [10-11], wherein the silane coupling agent is a vinyl group-containing silane coupling agent; [10-13] The curable resin composition according to any one of [10-2] to [10-12], which is a room temperature curable resin composition; [10-14] The curable resin composition according to any one of [10-2] to [10-13], which is a two-component curable resin composition; [10-15] The curable resin composition according to [10-14], characterized in that the two-component curable resin composition contains an A component and a B component, the A component contains the (A) to (C) components, and the B component contains the (D) component and the (E) component;

[11] A cured product obtained by curing the curable resin composition according to any one of [1] to

[10] ; [11-2] A cured product obtained by curing the curable resin composition according to any one of [10-2] to [10-15].

[0010] Another aspect of the present invention relates to the following

[12] :

[12] A method for producing a curable resin composition, comprising mixing the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; (B) component: bismuth-based catalyst; (C) Component: Water having a pH of 8.0 or more (i.e., a water-containing liquid having a pH of 8.0 or more); Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): Hardener for epoxy resin.

[0011] Furthermore, the present invention includes the following embodiments [12-2 to 13-2] as non-limiting examples of preferred embodiments: [12-2] The method for producing a curable resin composition according to

[12] , wherein the component (C) is alkaline electrolyzed water; [12-3] The method for producing a curable resin composition according to

[12] or [12-2], wherein the component (C) is water containing at least one compound selected from the group consisting of sodium hydroxide, calcium hydroxide, potassium carbonate, and sodium metasilicate; [12-4] The method for producing a curable resin composition according to any one of

[12] to [12-3], wherein the component (B) is bismuth carboxylate; [12-5] A method for producing a curable resin composition according to any one of

[12] to [12-4], characterized in that the (C) component is contained in an amount of 0.05 to 30 parts by mass per 100 parts by mass of the (A) component; [12-6] A method for producing a curable resin composition according to any one of

[12] to [12-5], wherein the component (E) is an amine compound that is liquid at 25°C; [12-7] A method for producing a curable resin composition according to any one of

[12] to [12-6], further comprising a filler as the component (F); [12-8] A method for producing a curable resin composition according to any one of

[12] to [12-7], which is substantially free of an organotin catalyst; [12-9] A method for producing a curable resin composition according to any one of

[12] to [12-8], characterized in that the component (A) is at least one selected from the group consisting of bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, diglycidyl ethers of alkylene oxide adducts of bisphenol A type, diglycidyl ethers of alkylene oxide adducts of bisphenol F type, and alkylene oxide adducts of bisphenol E type; [12-10] The method for producing a curable resin composition according to any one of

[12] to [12-9], wherein the hydrolyzable group constituting the hydrolyzable silyl group is at least one selected from the group consisting of a halogen atom, an alkoxy group, an acyl oxide group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyl oxide group; [12-11] The method for producing a curable resin composition according to any one of

[12] to [12-10], wherein the hydrolyzable silyl group is at least one selected from the group consisting of a trimethoxysilyl group, a triethoxysilyl group, a triisopropoxysilyl group, a triphenoxysilyl group, a methyldimethoxysilyl group, a methyldiethoxysilyl group, a dimethylmethoxysilyl group, and a dimethylethoxysilyl group; [12-12] A method for producing a curable resin composition according to any one of

[12] to [12-11], characterized in that the component (D) has at least one structure selected from the group consisting of polyoxyalkylene, polyester, polycarbonate, polyurethane, polyamide, polyurea, polyimide, polyethylene, polypropylene, polyisobutylene, poly(meth)acrylate, polystyrene, polyvinyl chloride, polybutadiene, polyisoprene, polyvinyl butyral, and polyvinyl ether; [12-13] A method for producing a curable resin composition according to any one of

[12] to [12-12], characterized in that the component (E) is at least one selected from the group consisting of an aliphatic polyamine, an alicyclic polyamine, an aromatic polyamine, a secondary amine, a tertiary amine, a polyamidoamine, and a polyamide; [12-14] The method for producing a curable resin composition according to any one of

[12] to [12-13], characterized in that the component (E) is at least one selected from the group consisting of piperidine, pyridine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethylenediamine, dimethylcyclohexylamine, dimethylbenzylamine, dimethylhexylamine, dimethylaminophenol, 2,4,6-tris(dimethylaminomethyl)phenol, dimethylamino-p-cresol, piperidine, 1,4-diazadicyclo[2.2.2]octane, 2,4,6-tris(dimethylaminomethyl)phenol and 1,8-diazabicyclo[5.4.0]undecene-1; [12-15] A method for producing a curable resin composition according to any one of

[12] to [12-14], further comprising a filler as component (F), the component (F) being at least one selected from the group consisting of talc, silica, clay, calcium carbonate, magnesium carbonate, calcium silicate, glass, alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, carbon, diamond, gold, silver, copper and nickel; [12-16] A method for producing a curable resin composition according to any one of

[12] to [12-15], further comprising a filler as component (F), the component (F) including a filler having a small average particle size of 0.01 μm or more and less than 5.0 μm, and a filler having a large average particle size of 5.0 μm or more and 150 μm or less; [12-17] A method for producing a curable resin composition according to any one of

[12] to [12-16], further comprising a silane coupling agent; [12-18] The method for producing a curable resin composition according to any one of

[12] to [12-17], wherein the silane coupling agent is a vinyl group-containing silane coupling agent; [12-19] A method for producing the curable resin composition according to any one of

[12] to [12-18], which is a room temperature curable resin composition; [12-20] A method for producing the curable resin composition according to any one of

[12] to [12-19], which is a two-component curable resin composition; [12-21] The method for producing a curable resin composition according to [12-20], characterized in that the two-component curable resin composition contains an A component and a B component, the A component contains the (A) to (C) components, and the B component contains the (D) component and the (E) component;

[13] A method for producing a curable resin composition by the method for producing a curable resin composition according to

[12] , and curing the produced curable resin composition; [13-2]. A method for producing a curable resin composition, comprising producing a curable resin composition by the method for producing a curable resin composition according to any one of [12-2] to [12-21], and curing the produced curable resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In this specification, "X to Y" is used to mean that the numerical values ​​before and after it (X and Y) are included as the lower limit and upper limit, and means "at least X and at most Y."

[0013] Unless otherwise specified, operations and measurements of physical properties are performed at room temperature (20 to 25°C) and a relative humidity of 40 to 50% RH.

[0014] In this specification, the term "(meth)acrylate" is a general term for acrylate and methacrylate. Similarly, compounds containing (meth), such as (meth)acrylic acid, are a general term for compounds having "meth" in their names and compounds not having "meth".

[0015] One aspect of the present invention relates to a curable resin composition comprising the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; (B) component: bismuth-based catalyst; (C) Component: Water with a pH of 8.0 or higher (a water-containing liquid with a pH of 8.0 or higher); Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): Hardener for epoxy resin.

[0016] Such a curable resin composition has excellent surface curing properties and internal curing properties when bonding members are attached to each other without using an organotin catalyst.

[0017] The details of the invention are described below.

[0018] <Component (A)> A curable resin composition according to one embodiment of the present invention includes component (A): an epoxy resin having two or more epoxy groups in one molecule. The component (A) in the present invention is not particularly limited as long as it is an epoxy resin having two or more epoxy groups in one molecule. The component (A) may be used alone or in a mixture of two or more kinds. From the viewpoint of workability, the component (A) is preferably liquid at 25°C.

[0019] In this specification, the term "epoxy resin" refers to a curable epoxy compound that can be polymerized (cured) to form a resin. Here, the curable epoxy compound may be any of a monomer, an oligomer, and a polymer.

[0020] The component (A) is not particularly limited, but examples thereof include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, diglycidyl ethers of bisphenol A type alkylene oxide adducts, diglycidyl ethers of bisphenol F type alkylene oxide adducts, diglycidyl ethers of bisphenol E type alkylene oxide adducts, hydrogenated bisphenol A type epoxy resins, hydrogenated bisphenol F type epoxy resins, hydrogenated bisphenol E type epoxy resins, epoxy resins having a glycidylamine skeleton, cresol novolac type epoxy resins, phenol novolac type epoxy resins, hydrogenated cresol novolac type epoxy resins, hydrogenated phenol novolac type epoxy resins, resorcinol diglycidyl ether, alicyclic epoxy resins, aliphatic epoxy resins, and urethane-modified epoxy resins. Among these, from the viewpoint of being compatible with the component (D) described later and being superior in surface curing property and internal curing property when bonding the adhesive member, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol E type epoxy resin, diglycidyl ether of alkylene oxide adduct of bisphenol A type, diglycidyl ether of alkylene oxide adduct of bisphenol F type, and diglycidyl ether of alkylene oxide adduct of bisphenol E type are preferably used. Among these, diglycidyl ether of alkylene oxide adduct of bisphenol A type is particularly preferable. These may be used alone or in combination of two or more.

[0021] As the component (A), a commercially available product or a synthetic product may be used. Examples of commercially available products of the component (A) include jER (registered trademark) series 825, 827, 828, 828EL, 828US, 828XA, 834, 806, 806H, 807, 604, 630, 871, YX8000, YX8034, and YX4000 (all manufactured by Mitsubishi Chemical Corporation), and EPICLON (registered trademark) series. 840, 840-S, 850, 850-S, 850-LC, EXA-850CRP, 830, 830-S, 835, EXA-830LVP, EXA-850CRP, 835LV, HP4032D, 703, 720, 726, HP820, N-660, N-680, N-695, N-655-EXP-S, N-665-EXP-S, N-685-EXP-S, N-740, N-775, N-865 (all manufactured by DIC Corporation), ADEKA RESIN (registered trademark) EP4100, Examples of the esters include, but are not limited to, EP4000, EP4080, EP4085, EP4088, EP4100HF, EP4901HF, EP4000S, EP4000L, EP4003S, EP4010S, EP4010L, EPU6, EPR4023, EPR1309, EP49-20 (all manufactured by ADEKA CORPORATION), TEPIC (registered trademark), TEPIC (registered trademark)-S, TEPIC (registered trademark)-VL (all manufactured by Nissan Chemical Industries, Ltd.). These may be used alone or in combination of two or more.

[0022] The epoxy equivalent of the component (A) is preferably from 50 to 5000 g / ep, more preferably from 100 to 1000 g / ep, and particularly preferably from 120 to 600 g / ep.

[0023] <(B) component> A curable resin composition according to one embodiment of the present invention includes component (B): a bismuth-based catalyst.

[0024] The component (B) in the present invention is not particularly limited as long as it is a bismuth catalyst. The silanol catalyst is a catalyst that reacts a compound having a silanol group. The silanol catalyst acts to react the silanol group obtained after hydrolysis of an organic polymer having two or more hydrolyzable silyl groups in one molecule, which is the component (D) described later, and a silane coupling agent, which is another component described later. By selecting the component (B) of the present invention from among silanol catalysts and combining it with the other components of the present invention, a remarkable effect of excellent surface curing properties and internal curing properties when bonding adhesive members together can be achieved without using an organic tin catalyst.

[0025] The (B) component is not particularly limited, but examples thereof include bismuth neodecanoate, bismuth carboxylate, bismuth benzoate, bismuth abietate, bismuth neoabietate, and bismuth octylate. Among these, bismuth neodecanoate and bismuth carboxylate are preferred from the viewpoint of superior internal curing properties and adhesion to aluminum when bonding the adhesive member. Among these, bismuth carboxylate is particularly preferred. These may be used alone or in combination of two or more.

[0026] As the component (B), a commercially available product or a synthetic product may be used. The commercially available product of the component (B) is not particularly limited, but examples thereof include Pucat (registered trademark) B7, Pucat (registered trademark) 25, bismuth neodecanoate (all manufactured by Nippon Chemical Industry Co., Ltd.), K-KAT (registered trademark) 348, K-KAT (registered trademark) XC-C227, K-KAT (registered trademark) XK-628, K-KAT (registered trademark) XK-640 (all manufactured by KING INDUSTRIES), Borchi (registered trademark) Kat 315, Borchi (registered trademark) Kat 320, Borchi (registered trademark) Kat 24 (all manufactured by Borchers), and the like.

[0027] The blending amount of the (B) component is not particularly limited, but is preferably in the range of 0.01 to 50 parts by mass, more preferably 0.05 to 30 parts by mass, and particularly preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the (D) component. By being within the above range, the adhesive member is more excellent in internal curing property when bonded together and in adhesion to aluminum.

[0028] <(C) component> The curable resin composition according to one embodiment of the present invention includes component (C): water having a pH of 8.0 or more (i.e., a water-containing liquid having a pH of 8.0 or more). The component (C) of the present invention is not particularly limited as long as it is water having a pH of 8.0 or more (i.e., a water-containing liquid having a pH of 8.0 or more). The component (C) of the present invention, when combined with other components, can provide a remarkable effect of excellent surface curing properties and internal curing properties when bonding adhesive members together without using an organotin catalyst. On the other hand, when water having a pH of less than 8.0 (i.e., a water-containing liquid having a pH of less than 8.0) is used or when water is not used, the surface curing properties and internal curing properties when bonding adhesive members together are poor. In addition, the adhesiveness tends to be lower than when the component (C) of the present invention is used.

[0029] The pH of component (C) is not particularly limited as long as it is 8.0 or higher, but is preferably 8.5 to 13.5, more preferably 9.0 to 13.3, and particularly preferably 9.5 to 13.0. The method for evaluating the pH of component (C) is not particularly limited, but for example, the value calculated using a glass electrode type hydrogen ion concentration indicator D-54 manufactured by HORIBA STEC Co., Ltd. can be used.

[0030] The water (water-containing liquid having a pH of 8.0 or more, or water as a raw material thereof) is not particularly limited, and for example, distilled water, ion-exchanged water, tap water, alkaline electrolyzed water, etc. can be used. These may be used alone or in combination of two or more. Among these, it is preferable to use alkaline electrolyzed water. Therefore, in a preferred embodiment of the present invention, the component (C) is alkaline electrolyzed water.

[0031] In this specification, alkaline electrolyzed water refers to water that exhibits alkalinity after electrolyzing water to which an electrolyte has been added and being obtained from the cathode side. Therefore, alkaline water obtained from the cathode side by electrolyzing water to which an electrolyte has been added is alkaline electrolyzed water. In addition, water obtained by diluting the alkaline water obtained from the cathode side by electrolyzing water to which an electrolyte has been added with other water such as distilled water, ion-exchanged water, tap water, etc. is also treated as alkaline electrolyzed water. In addition, water obtained by removing the remaining electrolyte and ions that may be generated from the electrolyte from the alkaline water obtained from the cathode side by electrolyzing water to which an electrolyte has been added is also considered to be alkaline electrolyzed water. Therefore, the alkaline electrolyzed water is not particularly limited, but examples thereof include water containing hydroxide ions generated from the cathode side by electrolyzing water. In addition, the alkaline electrolyzed water is not particularly limited, but examples thereof include water obtained by diluting water containing hydroxide ions generated from the cathode side by electrolyzing water with pure water. Among these, water containing hydroxide ions generated from the cathode side by electrolyzing water is preferable.

[0032] The alkaline electrolyzed water may contain impurities, or may be free of impurities after the impurities have been removed. The impurities are not particularly limited, but may include, for example, electrolytes added during electrolysis in the preparation of alkaline electrolyzed water or ions that may be generated from the electrolyte. The electrolytes added during electrolysis in the preparation of alkaline electrolyzed water are not particularly limited, and known electrolytes may be used. The electrolyte is not particularly limited, but is preferably a compound that is a component other than the (A), (B), (D), and (E) components and dissolves in water. Here, the other components may include, for example, components other than the (A), (B), (D), (E), and (F) components. In addition, for example, the (A) component, the (B) component, the (D) component, the (E) component, the (F) component, silane coupling agents, various elastomers such as styrene copolymers, polythiol compounds, storage stabilizers, antioxidants, light stabilizers, heavy metal deactivators, tackifiers, plasticizers, defoamers, dyes, pigments, rust inhibitors, leveling agents, dispersants, rheology adjusters, and components other than surface active agents can be mentioned. In addition, the electrolyte contained in the (C) component is not particularly limited, but for example, a basic compound can be mentioned. In addition, for example, sodium hydroxide, calcium hydroxide, potassium carbonate, sodium metasilicate, etc. can be mentioned.

[0033] The (C) component may be water alone, or may be a liquid obtained by mixing water with other compounds. The other compounds mixed with the (C) component are not particularly limited, but may be, for example, the same as the electrolytes described above. The other compounds contained in the (C) component are not particularly limited, but are preferably compounds that can at least make the pH of water 8.0 or higher, and may be, for example, basic compounds. Other compounds include, for example, sodium hydroxide, calcium hydroxide, potassium carbonate, and sodium metasilicate.

[0034] For these reasons, the (C) component according to a preferred embodiment of the present invention is water containing an electrolyte. The (C) component according to a more preferred embodiment of the present invention is water containing a basic compound. The (C) component according to a further preferred embodiment of the present invention is water containing at least one compound selected from the group consisting of sodium hydroxide, calcium hydroxide, potassium carbonate, and sodium metasilicate.

[0035] The pH of the (C) component is not particularly limited, and can be adjusted, for example, with an electrolyte. The pH of the (C) component can be adjusted, for example, with a basic compound. The pH of the (C) component can be adjusted, for example, with sodium hydroxide, calcium hydroxide, potassium carbonate, or sodium metasilicate. When the (C) component is alkaline electrolytic water, the pH of the (C) component can be adjusted, for example, by the type and amount of the electrolyte, and the conditions of electrolysis. The pH of the (C) component can be adjusted, for example, by the amount of water (e.g., pure water) added to the water obtained from the cathode as a result of electrolysis. When the (C) component is a liquid obtained by mixing water and other compounds, the pH of the (C) component can be adjusted, for example, by adding a basic compound to the water. The pH of the (C) component can be adjusted by adding sodium hydroxide, calcium hydroxide, potassium carbonate, sodium metasilicate, or the like to the water. In this case, a preferred example of the ratio of the amounts of water and other compounds contained in component (C) is, without being particularly limited, a ratio that enables the pH to be 8.0 or higher when the water and other compounds are mixed.

[0036] As the component (C), a commercially available product or one prepared by oneself may be used. In addition, a product prepared using a commercially available product as a raw material may be used. The commercially available products that are the raw materials for the component (C) are not particularly limited, but examples thereof include ThreeBond 6658 (manufactured by ThreeBond Co., Ltd.) and First Alkaline Water (manufactured by Daiichi Sangyo Co., Ltd.).

[0037] The amount of component (C) is not particularly limited, but is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 0.3 to 10 parts by mass, relative to 100 parts by mass of component (D). By being within the above range, the surface curability, the internal curability when the adhesive member is attached, and the adhesion to aluminum are further excellent.

[0038] The amount of the (C) component is not particularly limited, but is preferably 0.05 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 0.3 to 10 parts by mass, relative to 100 parts by mass of the (A) component. By being within the above range, the surface curability, the internal curability when the adhesive member is attached, and the adhesion to aluminum are further excellent.

[0039] <(D) component> The curable resin composition according to one embodiment of the present invention includes component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule. The component (D) of the present invention is an organic polymer having two or more hydrolyzable silyl groups in one molecule, and is preferably an organic polymer in which a crosslinking reaction is initiated by moisture. The hydrolyzable silyl group may be bonded to the end or side chain of the organic polymer, but from the viewpoint of superior internal curing properties when bonding the adhesive member, it is preferable that the hydrolyzable silyl group is bonded to the end, and more preferably to both ends.

[0040] In this specification, the hydrolyzable silyl group refers to a group in which 1 to 3 hydrolyzable groups are bonded to a silicon atom. The hydrolyzable group is not particularly limited, but preferred examples include halogen atoms, alkoxy groups such as methoxy groups, ethoxy groups, propyloxy groups, isopropyloxy groups, and butoxy groups, acyloxide groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, mercapto groups, and alkenyloxide groups. Among these, alkoxy groups are preferred, and methoxy groups are particularly preferred, from the viewpoint of superior internal curing properties and adhesion to aluminum when bonding the adhesive member.

[0041] The alkoxysilyl group in which an alkoxy group is bonded to a silicon atom is not particularly limited, and examples thereof include trialkoxysilyl groups such as trimethoxysilyl group, triethoxysilyl group, triisopropoxysilyl group, and triphenoxysilyl group; dialkoxysilyl groups such as methyldimethoxysilyl group and methyldiethoxysilyl group; and monoalkoxysilyl groups such as dimethylmethoxysilyl group and dimethylethoxysilyl group. Among these, dialkoxysilyl groups and trialkoxysilyl groups are preferred, and trialkoxysilyl groups are more preferred from the viewpoint of superior internal curing properties and adhesion to aluminum when bonding the adhesive member. In addition, among these, trimethoxysilyl groups are particularly preferred. These may be used alone or in combination of a plurality of these.

[0042] The structure of the organic polymer of the component (D) is not particularly limited, and examples thereof include structures such as polyoxyalkylene, polyester, polycarbonate, polyurethane, polyamide, polyurea, polyimide, polyethylene, polypropylene, polyisobutylene, poly(meth)acrylate, polystyrene, polyvinyl chloride, polybutadiene, polyisoprene, polyvinyl butyral, and polyvinyl ether. Among these, structures such as polyoxyalkylene, polyisobutylene, and poly(meth)acrylate are preferred from the viewpoint of superior surface curing properties, and structures such as polyoxyalkylene and poly(meth)acrylate are more preferred from the viewpoint of superior internal curing properties when bonding the adhesive members. Among these, polyoxyalkylene is particularly preferred. As the component (D), polymers of these structures may be used alone or in the form of a mixture of two or more kinds. As the component (D), a polymer having a plurality of these structures may be used.

[0043] From the viewpoint of handling, the component (D) is preferably liquid at 25°C. The range of the viscosity (25°C) of the component (D) is not particularly limited, but is preferably in the range of 0.5 to 3000 Pa·s, more preferably in the range of 1 to 2000 Pa·s, and particularly preferably in the range of 3 to 1500 Pa·s. By being within the above range, a curable resin composition having excellent internal curing properties and better workability when bonding the adhesive members can be obtained. Unless otherwise specified, the viscosity is measured by measuring the viscosity at 25°C using a cone-plate viscometer in accordance with JIS K6833-1:2008.

[0044] For these reasons, a preferred example of component (D) is a polyoxyalkylene containing trimethoxysilyl groups at both ends, etc. A more preferred example is a polyoxyalkylene containing trimethoxysilyl groups at both ends, etc., having a viscosity (25°C) of 0.5 to 3000 Pa s (more preferably 1 to 2000 Pa s, and even more preferably 3 to 1500 Pa s).

[0045] As the component (D), a commercially available product or a synthetic product may be used. The commercially available product of the component (D) is not particularly limited, but examples thereof include Silyl (registered trademark) SAT010, SAX115, SAT030, SAT030, SAT200, SAT350, SAT400, SAX220, SAX510, SAX530, SAX580, SAX710, SAX720, SAX725, SAX770, MA440, MA447, MA451, MA903, MA903M, MA904, S943, MAX923, MAX951, SAX520, Examples of such polymers include OR100S, MS Polymer (registered trademark) S203, S303, S203H, S303H, S943S, S911S, XMAP (registered trademark) SA100S, SA310S, Epion (registered trademark) EP100S, EP103S, EP303S, EP505S, etc. (all manufactured by Kaneka Corporation), and Exestar (registered trademark) ES-S2410, ES-S2420, ES-S3430, ES-S3610, ES-S3630 (all manufactured by Asahi Glass Co., Ltd.).

[0046] The blending amount of the (D) component is preferably 30 to 300 parts by mass, more preferably 30 to 200 parts by mass, and particularly preferably 50 to 150 parts by mass, per 100 parts by mass of the (A) component. By being within the above range, the surface curability, the internal curability when the adhesive member is attached, and the adhesion to aluminum are further excellent.

[0047] <(E) component> The curable resin composition according to one embodiment of the present invention includes component (E): a curing agent for epoxy resins. That is, the component (E) of the present invention is a curing agent for epoxy resins. The component (E) is preferably an amine compound that is liquid at 25°C.

[0048] The component (E) is not particularly limited, but examples thereof include aliphatic polyamines, alicyclic polyamines, aromatic polyamines, secondary amines, tertiary amines, polyamidoamines, polyamides, etc. The amine compounds may be used alone or in combination of two or more kinds.

[0049] Examples of aliphatic polyamines include, but are not limited to, ethylenediamine, diethylenetriamine, triethylenetetramine, hexamethylenediamine, etc. Examples of alicyclic polyamines include, but are not limited to, menthene diamine (MDA), isophorone diamine (IPDA), N-aminoethylpiperazine (N-AEP), diaminodicyclohexylmethane, norbornane diamine (NBDA), etc. Examples of aromatic polyamines include, but are not limited to, metaxylylenediamine (MXDA), metaphenylene diamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldiphenylmethane, etc.

[0050] The secondary amine or tertiary amine is not particularly limited, but examples thereof include piperidine, pyridine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, triethylenediamine, dimethylcyclohexylamine, dimethylbenzylamine, dimethylhexylamine, dimethylaminophenol, 2,4,6-tris(dimethylaminomethyl)phenol, dimethylamino-p-cresol, piperidine, 1,4-diazadicyclo[2.2.2]octane, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo[5.4.0]undecene-1, and the like.

[0051] As the component (E), a commercially available product or a synthetic product may be used. The commercially available product of the component (E) is not particularly limited, but examples thereof include Ancamine (registered trademark) series K-54 (manufactured by Air Products Japan Co., Ltd.) and the like.

[0052] The blending amount of the (E) component is not particularly limited, but is preferably 1 to 300 parts by mass, more preferably 1 to 150 parts by mass, and particularly preferably 3 to 100 parts by mass, of the (E) component relative to 100 parts by mass of the (A) component. By keeping the blending amount within the above range, a curable resin composition that is excellent in internal curing property when bonding adhesive members together and has better workability can be obtained.

[0053] <(F) Component> The curable resin composition according to one embodiment of the present invention preferably further contains a filler as component (F). That is, the filler as component (F) can be used in the curable resin composition according to one embodiment of the present invention, as long as the object of the present invention is not impaired. In the conventional moisture-curable resin composition, when a large amount of filler is blended, moisture does not easily penetrate into the moisture-curable resin composition, so that the internal curing tends to be significantly slow. On the other hand, the curable resin composition according to one embodiment of the present invention has excellent internal curing properties, so that a large amount of filler can be blended, and various functions can be imparted.

[0054] The (F) component is not particularly limited, but examples thereof include talc, silica, clay, calcium carbonate, magnesium carbonate, calcium silicate, glass, alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, carbon, diamond, gold, silver, copper, nickel, etc. The (F) component may be surface-treated. These may be used alone or in combination.

[0055] As the (F) component, in order to impart high modulus to the cured product of the curable resin composition, talc, silica, clay, calcium carbonate, magnesium carbonate, calcium silicate, and glass are preferred. In order to impart thermal conductivity to the curable resin composition, thermally conductive powders such as alumina, zinc oxide, magnesium oxide, aluminum nitride, boron nitride, carbon, and diamond are preferred. In order to impart flame retardancy to the curable resin composition, aluminum hydroxide is preferred. In order to impart conductivity to the curable resin composition, conductive fillers such as gold, silver, copper, and nickel are preferred.

[0056] From the viewpoint of obtaining a curable resin composition having excellent surface curability and internal curability when bonding members are bonded together, the average particle size (50% average particle size) of component (F) is preferably from 0.01 μm to 150 μm, more preferably from 0.1 μm to 100 μm, and most preferably from 0.5 μm to 70 μm. In the present invention, the average particle size is, for example, the particle size at 50% cumulative in a particle size distribution determined by a laser diffraction / scattering method (also referred to as D50).

[0057] As the component (F), a commercially available product or a synthetic product may be used. The commercially available product of the component (F) is not particularly limited, but examples thereof include low soda alumina LS-210B (manufactured by Nippon Light Metal Co., Ltd.) and AO-509 (manufactured by Admatechs Co., Ltd.).

[0058] The content of the (F) component is not particularly limited, but is, for example, preferably 5 to 95 mass%, more preferably 10 to 90 mass%, and particularly preferably 20 to 85 mass%, based on the entire curable resin composition according to one embodiment of the present invention. By having the content of the (F) component within the above range, a curable resin composition having even better surface curability and internal curability when bonding adhesive members is obtained.

[0059] When the curable resin composition of the present invention is used as a thermally conductive resin composition, the content of the (F) component is not particularly limited, but is, for example, preferably 30 to 95 mass %, more preferably 40 to 90 mass %, and particularly preferably 50 to 85 mass %, based on the entire curable resin composition according to one embodiment of the present invention.

[0060] When the curable resin composition according to one embodiment of the present invention is used as a thermally conductive resin composition, it is preferable to use two or more fillers having different average particle diameters in combination as the component (F) since a curable resin composition having low viscosity, excellent thermal conductivity, and excellent internal curing properties when bonding adhesive members is obtained. Specifically, the filler having a small average particle diameter is preferably 0.01 μm or more and less than 5.0 μm, and more preferably 0.1 μm or more and 3.5 μm or less. In addition, the filler having a large average particle diameter is preferably 5.0 μm or more and 150 μm or less, more preferably 6.0 μm or more and 100 μm or less, and most preferably 7.0 μm or more and 70 μm or less, since a curable resin composition having low viscosity before curing and excellent thermal conductivity is obtained. In addition, the content of the filler having a large average particle diameter relative to 100 parts by mass of the filler having a small average particle diameter is preferably 10 to 700 parts by mass, more preferably 20 to 600 parts by mass, and particularly preferably 30 to 500 parts by mass. By adding the filler having a small average particle size and the filler having a large average particle size in the above-described ranges, it is possible to obtain a curable resin composition that has even better surface curability and internal curability when adhesive members are bonded together.

[0061] <Other additives> Other additives such as silane coupling agents, various elastomers such as styrene copolymers, polythiol compounds, storage stabilizers, antioxidants, light stabilizers, heavy metal deactivators, tackifiers, plasticizers, defoamers, dyes, pigments, rust inhibitors, leveling agents, dispersants, rheology adjusters and surfactants can be used in the curable resin composition according to one embodiment of the present invention, within the scope that does not impair the object of the present invention. Among these, the curable resin composition according to one embodiment of the present invention preferably contains a silane coupling agent, a storage stabilizer or an antioxidant, and particularly preferably contains a silane coupling agent.

[0062] The silane coupling agent is not particularly limited, and examples thereof include alkyl group-containing silane coupling agents such as dimethyldimethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, and hexyltrimethoxysilane; vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane; phenyl group-containing silane coupling agents such as phenyltrimethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane; N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyltriethoxysilane, and 3-aminopropyltrimethoxysilane. silane coupling agents containing an amino group, such as 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxysilyltriethoxysilane; silane coupling agents containing a glycidyl group, such as 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropyltriethoxysilane; and silane coupling agents containing a (meth)acryloyl group, such as 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropyltriethoxysilane; and other silane coupling agents, such as γ-mercaptopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, styrylsilane, ureidosilane, sulfide silane, isocyanate silane, etc. Among these, since the surface curing property and the internal curing property at the time of bonding the adhesive member are more excellent while maintaining the storage stability of the curable resin composition, the alkyl group-containing silane coupling agent, the phenyl group-containing silane coupling agent, the vinyl group-containing silane coupling agent, and the amino group-containing silane coupling agent are preferred, and the vinyl group-containing silane coupling agent is more preferred.In addition, among these, vinyltrimethoxysilane is particularly preferred.These may be used alone or in combination of two or more kinds.The amount of the silane coupling agent added is not particularly limited, but is, for example, preferably in the range of 0.05 to 100 parts by mass, more preferably 0.1 to 50 parts by mass, and particularly preferably 1 to 30 parts by mass, relative to 100 parts by mass of the component (D) of the present invention. By being within the above range, the storage stability of the curable resin composition is maintained, and the surface curability and the internal curability when the adhesive member is attached are more excellent.

[0063] An antioxidant may be added to the curable resin composition according to one embodiment of the present invention. Examples of the antioxidant include quinone compounds such as β-naphthoquinone, 2-methoxy-1,4-naphthoquinone, methylhydroquinone, hydroquinone, hydroquinone monomethyl ether, mono-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, p-benzoquinone, 2,5-diphenyl-p-benzoquinone, and 2,5-di-tert-butyl-p-benzoquinone; phenothiazine, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), catechol, and tert-butylcatechol. , 2-butyl-4-hydroxyanisole, 2,6-di-tert-butyl-p-cresol, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, 4,4'-butylidenebis(6-tert-butyl-3-methylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 3,9- Bis[2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N, N'-Hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide], benzenepropanoic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy, C7-C9 side chain alkyl ester, 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3”,5,5',5”-hexa-tert-butyl-a,a',a”-(mesitylene-2,4,6-tolyl)tri-p-cresol, calcium diethyl bis[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,3,5-tris(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, reaction products of N-phenylbenzenamine with 2,4,6-trimethylpentene, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)phenol, picric acid, citric acid and other phenols; bis(2,4-di-tert-butylphenyl)phosphite, tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphen-6-yl]oxy]ethyl]amine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ester phosphorous acid, tetrakis(2,4-di-tert-butylphenyl)[1,1-bisphenyl]-4,4'-di Examples of the phosphorus-based compounds include aryl bisphosphonite, 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1,3,2]dioxaphosphene, and the like; dilauryl 3,3'-thiodipropionate, dimyristyl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythrityl tetrakis(3-laurylthiopropionate), lactone-based compounds; and vitamin E-based compounds. Among these, phenol-based compounds are preferred. These may be used alone or in combination of two or more.

[0064] The storage stabilizer is not particularly limited, but examples thereof include silicate compounds such as ethyl silicate, propyl silicate, and butyl silicate; borate esters such as triethyl borate, tripropyl borate, and tributyl borate; etc. These may be used alone or in combination of two or more kinds.

[0065] The curable resin composition according to one embodiment of the present invention is preferably substantially free of an organotin catalyst. In this specification, "substantially free of an organotin catalyst" means that the content of the organotin catalyst is less than 0.1 mass% relative to the total mass of the curable resin composition. The content of the organotin catalyst is preferably as small as possible, preferably less than 0.01 mass%, more preferably less than 0.001 mass%, and most preferably free of an organotin catalyst.

[0066] <Method for producing curable resin composition> Another aspect of the present invention relates to a method for producing a curable resin composition, comprising mixing the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; (B) component: bismuth-based catalyst; (C) Component: Water having a pH of 8.0 or more (i.e., a water-containing liquid having a pH of 8.0 or more); Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): Hardener for epoxy resin.

[0067] Details of the types, amounts added, characteristics, preferred embodiments, etc. of the above components (A) to (E) are the same as those described above for the curable resin composition.

[0068] In addition, in the production method according to one embodiment of the present invention, other additives may be mixed in addition to the above-mentioned components (A) to (E). Details of the types, amounts, properties, preferred aspects, etc. of the other additives are the same as those described above for the curable resin composition.

[0069] <Curing method, cured product and manufacturing method thereof> The curable resin composition according to one embodiment of the present invention is preferably a room temperature curable resin composition that can be cured in a room temperature (25° C.) environment by mixing two liquids or by moisture.

[0070] In addition, the curable resin composition produced by the production method according to one embodiment of the present invention is preferably a room temperature curable resin composition that can be cured in a room temperature (25°C) environment by mixing two liquids or by moisture.

[0071] The curable resin composition according to one embodiment of the present invention and the curable resin composition produced by the production method according to one embodiment of the present invention can be cured in a short time by heating. The heating conditions are not particularly limited, but for example, a temperature of 45 to 200°C is preferable, a temperature of 50 to 170°C is more preferable, and a temperature of 55 to 150°C is further preferable.

[0072] A cured product obtained by curing the curable resin composition according to one embodiment of the present invention is also another embodiment of the present invention. In addition, a method for producing a cured product, which includes producing a curable resin composition by the production method according to one embodiment of the present invention and curing the produced curable resin composition, is yet another embodiment of the present invention.

[0073] The term "hardening by mixing two liquids" means that the material can be hardened by mixing two liquids when in use.

[0074] <Two-component curable resin composition and its manufacturing method> The curable resin composition according to one embodiment of the present invention is preferably a two-component curable resin composition. The two-component curable resin composition is not particularly limited, but may be, for example, a composition containing an A component and a B component, the A component being a composition containing components (A) to (C), and the B component being a composition containing components (D) and (E). That is, the curable resin composition according to a preferred embodiment of the present invention is a two-component curable resin composition containing an A component and a B component, the A component being a composition containing components (A) to (C), and the B component being a composition containing components (D) and (E).

[0075] Moreover, a production method according to one embodiment of the present invention is a method for producing a two-component curable resin composition, and preferably includes a step of preparing a liquid A, which includes mixing components (A) to (C), and a step of preparing a liquid B, which includes mixing components (D) and (E).

[0076] By dividing the components into separate liquids in this way, unnecessary reactions during storage can be suppressed and storage stability can be improved. Furthermore, by mixing the two liquids when in use, the product can be quickly cured.

[0077] In addition, optional components such as component (F) and a silane coupling agent may be contained in either or both of component A and component B. Among these, component (F) is preferably contained in at least component B, and more preferably contained only in component B. In addition, the silane coupling agent is preferably contained in at least component B, and more preferably contained only in component B.

[0078] In addition, optional components such as component (F) and a silane coupling agent may be mixed in the preparation process of one or both of the A and B agents. Among these, component (F) is preferably mixed at least in the preparation process of the B agent, and more preferably only in the preparation process of the B agent. In addition, the silane coupling agent is preferably mixed at least in the preparation process of the B agent, and more preferably only in the preparation process of the B agent.

[0079] Furthermore, relative to 100 parts by mass of agent A, the amount of agent B is preferably in the range of 0.1 to 1000 parts by mass, more preferably in the range of 1 to 900 parts by mass, even more preferably in the range of 5 to 800 parts by mass, and particularly preferably in the range of 10 to 700 parts by mass.

[0080] Moreover, it is particularly preferable that the room temperature curable resin composition according to one embodiment of the present invention and the room temperature curable resin composition produced by the production method according to one embodiment of the present invention are two-component curable resin compositions.

[0081] <Application> The curable resin composition according to one embodiment of the present invention and the curable resin composition produced by the production method according to one embodiment of the present invention have excellent surface curing properties and internal curing properties when bonding adhesive members together without using an organotin catalyst.Therefore, the applications of these curable resin compositions or their cured products are not particularly limited, but are preferably used for various applications such as adhesives, sealants, sealants, potting agents, coating agents, thermally conductive resins, flame-retardant resins, and conductive pastes.These curable resin compositions or their cured products are particularly suitable for applications such as automobile parts, electrical and electronic parts, and building materials. Furthermore, the thermally conductive moisture-curable composition (thermally conductive moisture-curable resin composition) according to one embodiment of the present invention, the thermally conductive moisture-curable composition (thermally conductive moisture-curable resin composition) produced by the production method according to one embodiment of the present invention, or a cured product thereof can be used in various applications such as heat dissipation from electronic substrates; heat dissipation from electronic devices such as mobile phones and personal computers; heat dissipation from lighting such as LEDs; heat dissipation from optical pickup modules; heat dissipation from camera modules; heat dissipation from sensing devices; heat dissipation from power semiconductors; heat dissipation from inverters for HEVs, FCVs, and EVs; heat dissipation from converters for HEVs, FCVs, and EVs; and heat dissipation from battery packs and ECU parts for HEVs, FCVs, and EVs.

[0082] <Heat dissipation method> The heat dissipation method using the curable resin composition according to one embodiment of the present invention, the curable resin composition produced by the production method according to one embodiment of the present invention, or the cured product thereof includes a method of dissipating heat generated from an electric / electronic component to the outside by applying the heat conductive moisture curable composition (heat conductive moisture curable resin composition) according to one embodiment of the present invention, or the heat conductive moisture curable composition (heat conductive moisture curable resin composition) produced by the production method according to one embodiment of the present invention to the electric / electronic component. Examples of such electric / electronic components include, but are not limited to, electronic substrates; mobile phones; electronic devices such as personal computers; lighting devices such as LEDs; optical pickup modules; camera modules; sensing devices; power semiconductors; inverters for HEVs, FCVs, and EVs; converters for HEVs, FCVs, and EVs; ECU parts for HEVs, FCVs, and EVs. EXAMPLES

[0083] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.

[0084] The test methods used in the examples and comparative examples are as follows.

[0085] <Preparation of Agent A of Curable Resin Composition> [Preparation of Agent A-1] As the component (A), 100 parts by mass of a diglycidyl ether (a1) of an alkylene oxide adduct of bisphenol A type that is liquid at 25°C (ADEKA RESIN (registered trademark) EP4000 manufactured by ADEKA CORPORATION) (epoxy equivalent: 320 g / ep), As the component (B), 4 parts by mass of bismuth carboxylate (b1) (K-KAT XK640 manufactured by KING INDUSTRIES), As the component (C), 1 part by mass of alkaline electrolytic water (alkaline electrolyte water) (c1) (manufactured by ThreeBond Co., Ltd. (product name) ThreeBond 6658) having a pH of 12.7; The mixture was mixed at room temperature (25°C) for 60 minutes in a mixer to obtain Agent A-1.

[0086] [Preparation of Agent A-2] A preparation of A-2 was obtained in the same manner as A-1, except that (c1) in A-1 was changed to alkaline electrolyzed water (alkaline electrolyte water) (c2) of pH 10.0. The alkaline electrolyzed water of pH 10.0 was prepared as follows: [Preparation of alkaline electrolyzed water with pH 10.0] Alkaline electrolyzed water with a pH of 10.0 was prepared by adding pure water (pH 7) (manufactured by ThreeBond Co., Ltd.) to alkaline electrolyzed water with a pH of 12.7 (product name: ThreeBond 6658, manufactured by ThreeBond Co., Ltd.).

[0087] [Preparation of Agent A-3] Agent A-3 was obtained in the same manner as agent A-1, except that (c1) in agent A-1 was changed to water (c'1) having a pH of 7.0 (pure water manufactured by ThreeBond Co., Ltd.).

[0088] [Preparation of Agent A-4] Agent A-4 was obtained in the same manner as agent A-1, except that (c1) in agent A-1 was changed to water (c'2) having a pH of 2.5 (product name: ThreeBond 6658C, manufactured by ThreeBond Co., Ltd.).

[0089] [Preparation of Agent A-5] Agent A-5 was obtained in the same manner as agent A-1, except that (c1) was omitted.

[0090] [Preparation of Agent A-6] A component A-6 was obtained in the same manner as in the preparation of component A-1, except that (b1) in component A-1 was replaced with zinc catalyst (b'1) (KING INDUSTRIES K-KAT 670).

[0091] [Preparation of Agent A-7] Agent A-7 was obtained in the same manner as Agent A-1, except that (b1) in Agent A-1 was replaced with a chelate-type titanium catalyst (b'2) (TC-750 manufactured by Matsumoto Pharmaceutical Industries Co., Ltd.).

[0092] [Preparation of Agent A-8] Agent A-8 was obtained by preparing Agent A-1 in the same manner as Agent A-1, except that (b1) in Agent A-1 was replaced with an organotin catalyst (b'3) (Neostan (registered trademark) S-1 manufactured by Nitto Chemical Industry Co., Ltd.).

[0093] <Preparation of Agent B of Curable Resin Composition> [Preparation of Agent B-1] As the component (D), 100 parts by mass of a polyoxyalkylene (d1) containing trimethoxysilyl groups at both ends and having a viscosity (25°C) of 7 Pa s (Silyl (registered trademark) SAX530, manufactured by Kaneka Corporation); As component (E), 4 parts by mass of 2,4,6-tris(dimethylaminomethyl)phenol (e1) (liquid at 25°C, Ancamine (registered trademark) K-54 manufactured by Air Products Japan Co., Ltd.), As a silane coupling agent, 2 parts by mass of vinyltrimethoxysilane, The mixture was mixed at room temperature (25°C) for 60 minutes in a mixer to obtain Agent B-1.

[0094] The test methods used in the examples and comparative examples in Table 1 below are as follows.

[0095] <(1) Tack-free time test> As shown in Table 1 below, 105 parts by mass of agent A and 112 parts by mass of agent B of the curable resin composition were put into a polyethylene container and mixed for 10 minutes using a wooden stick in a 25°C environment. Next, the mixed curable resin composition was applied to a glass test piece in a thickness of 250 μm, and left in an atmosphere of 25°C x 55% RH. The surface of the mixed curable resin composition was touched with a wooden stick, and the time until the threading of the mixed curable resin composition disappeared was taken as the "tack-free time (min)". Here, when the tack-free time could not be measured within 600 minutes, it was recorded as "uncured". The tack-free time is preferably within 350 minutes, more preferably within 330 minutes. The results are shown in Table 1 below.

[0096] <(2) Tensile shear adhesive strength to aluminum> [Preparation of test specimen] As shown in Table 1 below, 105 parts by mass of agent A and 112 parts by mass of agent B of the curable resin composition were put into a polyethylene container and mixed for 10 minutes using a wooden stick in a 25°C environment. Next, the mixed curable resin composition of the Examples and Comparative Examples was applied to an aluminum (A1050P) test piece having a width of 25 mm, a length of 100 mm, and a thickness of 1 mm. Thereafter, another aluminum (A1050P) test piece was attached so that the overlap surface was 25 mm x 10 mm, and fixed with a clip. Note that the overlap surface is configured such that the curable resin composition exists between the two aluminum test pieces. Then, the test piece was left in a 25°C, 85% RH environment for 12 hours.

[0097] [Measurement of tensile shear adhesive strength] The shear bond strength (unit: MPa) of the test piece was measured at 25° C. using a universal tensile tester (tensile speed: 50 mm / min.) in accordance with JIS K 6850:1999. The shear bond strength was the value at the maximum strength. The results are shown in Table 1 below.

[0098] In the present invention, the shear adhesive strength to aluminum is preferably 1.3 MPa or more.

[0099] <(3) Internal hardening after bonding> [Preparation of test specimen] As shown in Table 1 below, 105 parts by mass of agent A and 112 parts by mass of agent B of the curable resin composition were put into a polyethylene container and mixed for 10 minutes using a wooden stick in a 25°C environment. Next, the mixed curable resin composition was applied to a glass plate (width 150 mm x length 150 mm x thickness 5 mm) with a polytetrafluoroethylene sheet attached to its surface. Thereafter, a glass plate with another polytetrafluoroethylene sheet attached to its surface was attached so that the overlapping surface was 25 mm x 10 mm, and fixed with a clip. Note that the overlapping surface is configured such that the curable resin composition exists between the glass plates with two polytetrafluoroethylene sheets attached to their surfaces, and each polytetrafluoroethylene sheet and the curable resin composition are in contact with each other. Then, the specimen was left in a 25°C, 55% RH environment for 8 hours and used as a test piece. The lamination was performed by sandwiching a glass plate (a glass plate (thickness: 0.5 mm) as a spacer) between the adherends and controlling the clearance to be 0.5 mm.

[0100] [Checking internal hardening] The glass test pieces (glass plates with polytetrafluoroethylene sheets attached to the surface) were peeled off from the test specimens, and the state of the cured product present in the gaps between the glass test pieces was visually confirmed. If it was confirmed that the cured product was uniformly formed, the result was judged as "passed", and if the liquid composition remained in the center and was not cured, the result was judged as "failed". The results are shown in Table 1 below.

[0101] [Table 1]

[0102] From the results of Examples 1 and 2 in Table 1 above, it was confirmed that the curable resin composition of the present invention has excellent surface curability, internal curability when bonding adhesive members are attached, and adhesion to aluminum without using an organotin catalyst.

[0103] On the other hand, in comparison with Example 1 of the present invention, Comparative Examples 1 and 2 in Table 1 above are curable resin compositions using water, which is not the component (C) of the present invention, and it was found that they were inferior in surface curability, internal curability when bonding adhesive members were attached, and adhesion to aluminum.

[0104] Comparative Example 3 is a curable resin composition not containing the component (C) of the present invention, but it was found to be significantly inferior in surface curability, adhesion to aluminum, and internal curability when bonding adhesive members together.

[0105] Comparative Examples 4 to 6 are curable resin compositions using a catalyst other than the component (B) of the present invention, but were found to be inferior in surface curability, adhesion to aluminum, and internal curability when bonding adhesive members are bonded together. In particular, Comparative Example 6 is a curable resin composition using an organotin catalyst that is known to be highly active among silanol catalysts, but it was surprising that the curable resin composition of Example 1 using the component (B) of the present invention was superior in terms of internal curability when bonding adhesive members and adhesion to aluminum.

[0106] Next, a curable resin composition containing a large amount of thermally conductive powder was evaluated.

[0107] <Preparation of Agent B of Curable Resin Composition> [Preparation of Agent B-2] Agent B-2 was obtained by preparing Agent B-1 in the same manner as Agent B-1, except that Agent B-1 further contained, as component (F), 120 parts by mass of alumina powder (f1) having an average particle size of 3 μm (low soda alumina LS-210B manufactured by Nippon Light Metal Co., Ltd.) and 280 parts by mass of alumina powder (f2) having an average particle size of 10 μm (AO-509 manufactured by Admatechs Co., Ltd.).

[0108] <(4) Initial hardening test after mixing> As shown in Table 2 below, 105 parts by mass of the A agent and 512 parts by mass of the B agent of the curable resin composition were put into a polyethylene container and mixed for 10 minutes using a wooden stick in a 25°C environment. Next, the mixed curable resin composition was applied to a glass test piece in a thickness of 250 μm, and left for 600 minutes in an atmosphere of 25°C x 55% RH. The surface of the mixed curable resin composition was then touched with a wooden stick to evaluate whether it had been cured or not. The results are shown in Table 2 below.

[0109] <(5) Tensile shear adhesive strength to aluminum> [Preparation of test specimen] As shown in Table 2 below, 105 parts by mass of agent A and 512 parts by mass of agent B of the curable resin composition were put into a polyethylene container and mixed for 10 minutes using a wooden stick in a 25°C environment. Next, the mixed curable resin composition of the Examples and Comparative Examples in Table 2 below was applied to an aluminum (A1050P) test piece with a width of 25 mm, a length of 100 mm, and a thickness of 1 mm. Thereafter, another aluminum (A1050P) test piece was attached to the test piece so that the overlap surface was 25 mm x 10 mm, and fixed with a clip. Then, the test piece was left in a 25°C environment for 60 hours and used as a test piece.

[0110] [Measurement of tensile shear adhesive strength] The shear bond strength (unit: MPa) of the test piece was measured at 25° C. using a universal tensile tester (tensile speed: 50 mm / min.) in accordance with JIS K 6850:1999. The shear bond strength was the value at the maximum strength. The results are shown in Table 2 below.

[0111] In the present invention, the shear adhesive strength to aluminum is preferably 1.3 MPa or more.

[0112] [Table 2]

[0113] The results of Example 3 in Table 2 above confirm that the present invention provides excellent surface curability and adhesion to aluminum even when the curable resin composition contains a large amount of filler, without using an organotin catalyst.

[0114] On the other hand, Comparative Example 7 is a curable resin composition not containing the component (C) of the present invention, but it was found that the surface curability and adhesion to aluminum were significantly inferior.

[0115] Next, in order to confirm that the curable resin composition of Example 3 has thermal conductivity, the thermal conductivity was measured.

[0116] <(6) Thermal conductivity measurement> The curable resin composition of Example 3 described in Table 2 below was applied to an aluminum (A1050P) plate of width 25 mm × length 100 mm × thickness 1 mm so that the thickness was 2.0 mm, and the plate was left to cure for 7 days under an environment of 25°C and 50% RH to prepare a test piece. The thermal conductivity was measured at 25°C using a thermal conductivity meter (QTM-500 manufactured by Kyoto Electronics Manufacturing Co., Ltd.). The higher the thermal conductivity, the easier it is to transfer heat, which is preferable. In particular, in the present invention, the thermal conductivity is preferably 1.0 W / (m·k) or more. The measurement result of Example 3 was 1.5 W / (m·k), and it was confirmed that the plate had excellent thermal conductivity. [Industrial Applicability]

[0117] The curable resin composition according to one embodiment of the present invention and the curable resin composition produced by the production method according to one embodiment of the present invention are excellent in surface curability, internal curability when bonding adhesive members are bonded, and adhesion to aluminum without using an organotin catalyst, and are therefore suitable for various applications such as adhesives, sealing agents, sealants, potting agents, coating agents, thermally conductive resins, flame-retardant resins, conductive pastes, etc. Therefore, they are industrially useful because they can be applied in a wide range of fields.

[0118] This application is based on Japanese Patent Application No. 2019-223576, filed on December 11, 2019, the disclosures of which are incorporated by reference in their entirety.

Claims

1. A curable resin composition comprising the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; Component (B): bismuth-based catalyst; (C) component: water having a pH of 8.0 or more; Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): A curing agent for epoxy resins.

2. The curable resin composition according to claim 1 , wherein the component (C) is alkaline electrolyzed water.

3. 3. The curable resin composition according to claim 1, wherein the component (C) is water containing at least one compound selected from the group consisting of sodium hydroxide, calcium hydroxide, potassium carbonate, and sodium metasilicate.

4. The curable resin composition according to any one of claims 1 to 3, wherein the component (B) is a bismuth carboxylate.

5. The curable resin composition according to any one of claims 1 to 4, comprising 0.05 to 30 parts by mass of the (C) component relative to 100 parts by mass of the (A) component.

6. The curable resin composition according to any one of claims 1 to 5, wherein the component (E) is an amine compound that is liquid at 25°C.

7. The curable resin composition according to any one of claims 1 to 6, further comprising a filler as a component (F).

8. The curable resin composition according to any one of claims 1 to 7, which is a room temperature curable resin composition.

9. The curable resin composition according to any one of claims 1 to 8, which is a two-component curable resin composition.

10. The two-component curable resin composition comprises an A component and a B component, the A component comprises the (A) to (C) components, and the B component comprises the (D) component and the (E) component. The curable resin composition according to claim 9.

11. A cured product obtained by curing the curable resin composition according to any one of claims 1 to 10.

12. A method for producing a curable resin composition, comprising mixing the following components (A) to (E): Component (A): an epoxy resin having two or more epoxy groups in one molecule; Component (B): bismuth-based catalyst; (C) component: water having a pH of 8.0 or more; Component (D): an organic polymer having two or more hydrolyzable silyl groups in one molecule; Component (E): A curing agent for epoxy resins.

13. A method for producing a cured product, comprising: producing a curable resin composition by the method for producing a curable resin composition according to claim 12; and curing the produced curable resin composition.

Citation Information

Patent Citations

  • Acid and alkali resistant room temperature curing adhesive and preparation method thereof

    CN106566451A

  • Epoxy resin composition, powder coating material, article, and laser marking method

    JP1997249735A

  • Curable composition

    JP2002088267A

  • Tacky adhesive composition, tacky-adhesive sheet and method for manufacturing semiconductor device

    JP2009127043A

  • Direct epoxidation method using improved catalyst composition

    JP2011500803A