Manufacturing method of electrical steel sheet

The method enhances magnetic properties and film adhesion in electrical steel sheets by replacing Mn in MnS precipitates with Cu and other elements, addressing the challenges of transformer efficiency and reliability.

JP7568948B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 21 Cites 0 Cited by

Patent Information

Application Number
JP2022532514
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-24
Filing Date
2021-06-23
Publication Date
2024-10-17
Estimated Expiration
2041-06-23

AI Technical Summary

Technical Problem

Existing electrical steel sheets, particularly grain-oriented and non-oriented types, face challenges in achieving sufficient magnetic properties and film adhesion, which are crucial for transformer efficiency and reliability, while also requiring improvements in manufacturing ease and environmental considerations.

Method used

A manufacturing method involving specific elemental compositions and treatments, including contact with solutions containing Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, to replace Mn in MnS precipitates on the steel surface, enhancing inhibitor strength and improving heat resistance, film adhesion, and heat removal performance.

Benefits of technology

The method results in electrical steel sheets with improved magnetic properties, specifically higher magnetic flux density and better film adhesion, contributing to stable transformer operation and reduced iron loss, applicable to both grain-oriented and non-oriented sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568948000001
    Figure 0007568948000001
  • Figure 0007568948000002
    Figure 0007568948000002
  • Figure 0007568948000003
    Figure 0007568948000003
Patent Text Reader

Abstract

Provided is a novel and improved method for producing an electromagnetic steel sheet, with which an electromagnetic steel sheet having excellent magnetic properties and coating film adhesion can be produced. This method for producing an electromagnetic steel sheet is characterized by including a step for bringing a solution into contact with an electromagnetic steel sheet which contains, in terms of mass%, more than 0% and not more than 0.10% of C, 2.5-4.5% of Si, 0.01-5.0% of Mn, a total of more than 0% and not more than 0.050% of one or more elements selected from among S, Se and Te, more than 0% and not more than 5.0% of acid-soluble Al, more than 0% and not more than 0.015% of N, and more than 0% and not more than 1.0% of P, with the remainder comprising Fe and impurities, with the solution containing one or more elements selected from among Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, and the total concentration of these elements being 0.00001-1.0000%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an electrical steel sheet. [Background technology]

[0002] Electrical steel sheets are generally classified into grain-oriented and non-oriented types. Grain-oriented electrical steel sheets contain about 2% to 5% by mass of Si, and the grain orientation of the steel sheet is called the Goss orientation {110} <001> It is a steel sheet in which the crystal axis orientation is highly integrated. Grain-oriented electrical steel sheets have excellent magnetic properties and are used, for example, as iron core materials for stationary inductors such as transformers. On the other hand, high-grade non-oriented electrical steel sheets contain about 2% by mass to 5% by mass of Si, just like grain-oriented electrical steel sheets, but the crystal axis orientation of each crystal is arranged as randomly as possible so as not to show magnetic properties biased toward a specific orientation of the steel sheet, and they have excellent magnetic properties just like grain-oriented electrical steel sheets and are used, for example, as iron core materials for the stators and rotors of rotating machines.

[0003] In order to improve the magnetic properties of such electrical steel sheets, various developments have been made. In particular, with the recent demand for energy saving, there is a demand for further reduction in iron loss in electrical steel sheets. Iron loss is composed of eddy current loss and hysteresis loss.

[0004] In order to reduce the iron loss of grain-oriented electrical steel sheets, it is effective to increase the concentration of crystal grains in the Goss orientation of the steel sheets, thereby improving the magnetic flux density and reducing hysteresis loss.

[0005] In the manufacture of grain-oriented electrical steel sheets, the crystal orientation is controlled by utilizing a catastrophic grain growth phenomenon called secondary recrystallization. However, in order to appropriately control the crystal orientation in secondary recrystallization, it is important to improve the heat resistance of fine precipitates in the steel, called inhibitors.

[0006] For example, the inhibitor is completely dissolved when the slab is heated before hot rolling, and then finely precipitated during hot rolling and the subsequent annealing process. Specifically, the inhibitor is used as an inhibitor in a method in which MnS and AlN are used as inhibitors and rolling is performed at a reduction rate of more than 80% in the final cold rolling process, as exemplified in Patent Document 1 below, or the inhibitor is used as an inhibitor in a method in which MnS and MnSe are used as inhibitors and two cold rolling processes are performed, as exemplified in Patent Document 2 below.

[0007] As mentioned above, iron loss includes eddy current loss. Regardless of whether the magnetic steel sheet is oriented or non-oriented, providing an insulating coating on the surface of the magnetic steel sheet makes it possible to suppress conduction between the magnetic steel sheets stacked as the magnetic core, thereby reducing the eddy current loss of the magnetic core, and further improving the practical magnetic properties of the magnetic steel sheet. In addition, a technique is also known in which magnetic domains are subdivided to reduce eddy current loss and, as a result, reduce iron loss. This effect is particularly applicable to grain-oriented electrical steel sheets.

[0008] Patent Documents 3 and 4 disclose techniques for producing grain-oriented electrical steel sheets with excellent coating properties by controlling the conditions for hot-rolled sheet annealing and the conditions for pickling treatment. Furthermore, Patent Document 5 discloses a technique for producing grain-oriented electrical steel sheets with excellent coating properties by controlling the conditions for pickling treatment, the conditions for additives in the annealing separator, and the conditions for finish annealing. Patent Document 6 discloses a technique for improving the coating adhesion of an insulating coating on a non-oriented electrical steel sheet. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Special Publication No. 40-15644 [Patent Document 2] Special Publication No. 51-13469 [Patent Document 3] JP 2003-193141 A [Patent Document 4] JP 2019-99827 A [Patent Document 5] JP 2014-196559 A [Patent Document 6] JP 2017-082276 A Summary of the Invention [Problem to be solved by the invention]

[0010] In recent years, with the progress of global regulations on transformer efficiency, there is an even greater demand for reduced iron loss in grain-oriented electrical steel sheets. On the other hand, since transformers are important equipment that support social infrastructure over the long term, it is important that they continue to operate stably. For this reason, grain-oriented electrical steel sheets, which are a major component of transformers, are also required to have the reliability to contribute to the stable operation of transformers. In addition, due to the growing concern about the global environment in recent years, electrical equipment is required to be small, have high output, and have high energy efficiency, and non-oriented electrical steel sheets, which are used as the iron core material for motors, are also required to have the reliability to contribute to the stable operation of motors.

[0011] The above Patent Documents 3 to 5 disclose a method for obtaining grain-oriented electrical steel sheets with excellent magnetic properties and / or excellent coating adhesion by causing a difference in the concentration of Mn and Cu between the surface and the center of the sheet thickness. Patent Document 6 discloses a method for obtaining non-oriented electrical steel sheets with excellent coating adhesion by segregating Cu and Ni together with Sb and Sn on the surface of the base steel sheet. However, the magnetic properties and coating adhesion of these steel sheets may not be sufficient, and further improvement and ease of production are required.

[0012] The present invention has been made in view of the above problems, and an object of the present invention is to provide a new and improved method for manufacturing an electrical steel sheet that is capable of manufacturing an electrical steel sheet having excellent magnetic properties and coating adhesion. In this specification, unless otherwise specified, the electrical steel sheet may be either a grain-oriented electrical steel sheet or a non-oriented electrical steel sheet. [Means for solving the problem]

[0013] In order to solve the above problems, the present invention provides the following aspects. [1] The method includes a step of contacting an electrical steel sheet containing, by mass%, C: more than 0% and not more than 0.10%, Si: 2.5% or more and not more than 4.5%, Mn: 0.01% or more and not more than 5.0%, the total of one or more of S, Se and Te: more than 0% and not more than 0.050%, acid-soluble Al: more than 0% and not more than 5.0%, N: more than 0% and not more than 0.015%, P: more than 0% and not more than 1.0%, with the balance being Fe and impurities, with a solution; The solution contains one or more elements selected from Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, and the total concentration of each element is 0.00001% or more and 1.0000% or less. [2] The method for producing an electrical steel sheet according to [1], characterized in that the electrical steel sheet contains, in place of a portion of the Fe, one or more elements selected from the group consisting of Cu: 1.0% or less, Sn: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Sb: 1.0% or less, and Bi: 1.0% or less. [3] The method for producing an electrical steel sheet according to [1] or [2], characterized in that a step in which the electrical steel sheet comes into contact with the solution is an acid pickling step, the pH of the solution is -1.5 or more and less than 7, the solution temperature is 15°C or more and 100°C or less, and the time for which the electrical steel sheet is in contact with the solution is 5 seconds or more and 200 seconds or less. [4] The method for producing an electrical steel sheet according to any one of [1] to [3], characterized in that a step in which the electrical steel sheet is brought into contact with the solution occurs after a hot rolling step and before a finish annealing step. [5] The method for producing an electrical steel sheet according to any one of [1] to [4], characterized in that a step in which the electrical steel sheet is brought into contact with the solution occurs after a finish annealing step and before an insulating coating application step. Effect of the Invention

[0014] According to the present invention, an electrical steel sheet is contacted with a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni (these may be referred to as "Cu, etc." in this specification). The electrical steel sheet contains MnS, MnSe, and MnTe (these may be referred to as "MnS, etc." in this specification) as precipitates, and the precipitates of MnS, etc. act as inhibitors. In the present invention, when MnS, etc. comes into contact with a solution containing Cu, etc., a part of Mn in MnS, etc., particularly Mn in the surface layer of MnS, etc., is replaced with Cu, etc., and this phenomenon is utilized to improve the heat resistance of the precipitates, thereby improving the inhibitor strength of the grain-oriented electrical steel sheet and achieving high magnetic properties. Furthermore, when a steel sheet containing MnS or the like on its surface is brought into contact with a solution containing Cu or the like, the above-mentioned phenomenon in which elements such as Cu become concentrated on the steel sheet surface can be utilized to realize the magnetic domain control effect due to improved heat transfer, the improvement of coating adhesion due to improved wettability of the coating liquid, and the improvement of heat extraction in laminated cores in transformers and motors. These effects can be enjoyed not only in grain-oriented electrical steel sheets but also in non-oriented electrical steel sheets. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Preferred embodiments of the present invention will be described in detail below. Unless otherwise specified, the expression "A to B" for numerical values ​​A and B means "A or more and B or less." In such an expression, when a unit is added only to numerical value B, the unit is also applied to numerical value A.

[0016] [Method of manufacturing electrical steel sheets] The present inventors conducted extensive research into a manufacturing method for grain-oriented electrical steel sheet in order to improve the adhesion between the coating of the electrical steel sheet and the steel sheet while also improving the magnetic properties, and as a result, discovered the following.

[0017] Specifically, the inventors have discovered that when an electrical steel sheet containing MnS, etc. is brought into contact with a solution containing Cu, etc., part of the Mn in the MnS, etc., particularly the Mn in the surface layer of the MnS, etc., is replaced with Cu, etc., by utilizing this phenomenon, the heat resistance of the MnS, etc. is improved, thereby improving the inhibitor strength and thereby the magnetic properties.

[0018] In addition, when a steel sheet containing MnS or the like on its surface is brought into contact with a solution containing Cu or the like, the above-mentioned phenomenon occurs, causing elements such as Cu to concentrate on the steel sheet surface. By utilizing this phenomenon, the researchers have discovered that the magnetic domain control effect is realized by improving the heat conductivity of the steel sheet, the coating adhesion is improved by improving the wettability of the coating liquid, and the heat removal performance of laminated iron cores in transformers and motors is improved.

[0019] The present inventors have taken the above findings into consideration and arrived at the present invention. One embodiment of the present invention is a method for producing an electrical steel sheet having the following configuration.

[0020] The method includes a step of contacting an electrical steel sheet containing, by mass%, C: more than 0% and not more than 0.10%, Si: 2.5% or more and not more than 4.5%, Mn: 0.01% or more and not more than 5.0%, the total of one or more of S, Se and Te: more than 0% and not more than 0.050%, acid-soluble Al: more than 0% and not more than 5.0%, N: more than 0% and not more than 0.015%, P: more than 0% and not more than 1.0%, with the balance being Fe and impurities, with a solution; The solution contains one or more elements selected from Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni, and the total concentration of each element is 0.00001% or more and 1.0000% or less.

[0021] The method for manufacturing an electrical steel sheet according to this embodiment will be specifically described below.

[0022] [Slab composition] First, the composition of the electromagnetic steel sheet according to this embodiment will be described. In the following, unless otherwise specified, the notation "%" will represent "mass %". The remainder other than the elements described below is Fe and impurities. Here, the impurities refer to components contained in the raw materials or components mixed in during the manufacturing process, and components that are not intentionally contained in the steel sheet. The chemical composition of the slab, which is the raw material of the electromagnetic steel sheet, is basically similar to the composition of the electromagnetic steel sheet. However, in the manufacture of general electromagnetic steel sheets, particularly grain-oriented electromagnetic steel sheets, some of the contained elements are discharged outside the system by decarburization annealing and purification annealing during the manufacturing process, so that the chemical composition of the slab, which is the raw material, and the electromagnetic steel sheet, which is the final product, particularly grain-oriented electromagnetic steel sheets, differ from each other. The slab composition can be appropriately adjusted in consideration of the effects of decarburization annealing and purification annealing during the manufacturing process so that the characteristics of the electromagnetic steel sheet, particularly grain-oriented electromagnetic steel sheets, are desired. Furthermore, unless otherwise specified, the expression "electromagnetic steel sheet" in the present invention refers to an electromagnetic steel sheet at any step in the manufacturing process of the electromagnetic steel sheet from the slab to the final product. In other words, unless otherwise specified, the expression "electromagnetic steel sheet" in the manufacturing process of the electromagnetic steel sheet in the present invention refers to an electromagnetic steel sheet at any step in the manufacturing process of the electromagnetic steel sheet from the slab to before the insulating coating application step.

[0023] The C (carbon) content is more than 0% and 0.10% or less. C has various roles, but when C is not contained (when C is 0%), the grain size becomes excessively large when the slab is heated, which may increase the iron loss value of the final electrical steel sheet, which is not preferable. When the C content exceeds 0.10%, the decarburization time becomes long during decarburization after cold rolling, which is not preferable because the manufacturing cost increases. In addition, when the C content exceeds 0.10%, decarburization is likely to be incomplete, which is not preferable because there is a possibility that magnetic aging may occur in the final electrical steel sheet. Therefore, the C content is more than 0% and 0.10% or less, and in the case of manufacturing a grain-oriented electrical steel sheet, it is preferably 0.02% or more and 0.10% or less. More preferably, it is 0.05% or more and 0.09% or less.

[0024] The Si (silicon) content is 2.5% or more and 4.5% or less. Si increases the electrical resistance of the steel sheet, thereby reducing eddy current loss, which is one of the causes of iron loss. If the Si content is less than 2.5%, it is not preferable because it becomes difficult to sufficiently suppress the eddy current loss of the final electrical steel sheet. If the Si content exceeds 4.5%, it is not preferable because the workability of the electrical steel sheet decreases. Therefore, the Si content is 2.5% or more and 4.5% or less, and preferably 2.7% or more and 4.0% or less.

[0025] The content of Mn (manganese) is 0.01% or more and 5.0% or less. Mn forms MnS, MnSe, MnTe, etc., which are inhibitors that affect secondary recrystallization. In addition, Mn has the effect of increasing electrical resistance like Si, and reduces eddy current loss, which is one of the causes of iron loss. If the content of Mn is less than 0.01%, it is not preferable because the absolute amount of MnS, MnSe, and MnTe that cause secondary recrystallization is insufficient. If the content of Mn is more than 5.0%, it is not preferable because it becomes difficult to form a solid solution of Mn during slab heating. In addition, if the content of Mn is more than 5.0%, it is not preferable because the precipitate size of MnS, MnSe, and MnTe, which are inhibitors, tends to become coarse, and the optimal size distribution as an inhibitor is impaired. Therefore, the Mn content is 0.01% or more and 5.0% or less, and in the case of manufacturing grain-oriented electrical steel sheets, it is preferably 0.01% or more and 0.50% or less, more preferably 0.01% or more and 0.30% or less, and even more preferably 0.03% or more and 0.15% or less. The above content may be acceptable from the viewpoint of reducing iron loss (eddy current loss).

[0026] The total content of S (sulfur), Se (selenium) and Te (tellurium) is more than 0% and 0.050% or less. S, Se and Te form an inhibitor together with the above-mentioned Mn. All three of S, Se and Te may be contained in the electrical steel sheet, but at least one of them may be contained in the electrical steel sheet. If the total content of S, Se and Te is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained. However, in the case of non-oriented electrical steel sheets, an inhibitor is not necessary, so the less the better, and 0% is preferable, but it may be costly to make it 0%, so it is made to be more than 0%. In addition, if the content exceeds the above upper limit, a large number of sulfides such as MnS are precipitated, causing a significant increase in iron loss. Therefore, the total content of one or more of S, Se and Te is more than 0% and 0.050% or less, preferably 0.001% or more and 0.040% or less.

[0027] The content of acid-soluble Al (acid-soluble aluminum) is more than 0% and not more than 5.0%. Acid-soluble Al constitutes an inhibitor (AlN) useful for producing electrical steel sheets with high magnetic flux density, particularly grain-oriented electrical steel sheets. In addition, Al has the effect of increasing electrical resistance like Si, and reduces eddy current loss, which is one of the causes of iron loss. When the content of acid-soluble Al is 0, AlN does not exist, and the inhibitor strength is insufficient, so that good magnetic properties may not be obtained, which is not preferable. When the content of acid-soluble Al is more than 5.0%, AlN precipitated as an inhibitor becomes coarse, which reduces the inhibitor strength, which is not preferable. Therefore, the content of acid-soluble Al is more than 0% and not more than 5.0%, and in the case of producing grain-oriented electrical steel sheets, it is preferably more than 0% and not more than 0.05%. More preferably, it is more than 0% and not more than 0.04%.

[0028] The N (nitrogen) content is more than 0% and not more than 0.015%. N forms AlN, which is an inhibitor, together with the above-mentioned acid-soluble Al. If the N content is outside the above range, it is not preferable because a sufficient inhibitor effect cannot be obtained and good magnetic properties cannot be obtained. Furthermore, if the N content exceeds the above upper limit, the increase in nitrides causes a significant increase in iron loss. Therefore, the N content is more than 0% and not more than 0.015%, and preferably more than 0% and not more than 0.012%.

[0029] The content of P (phosphorus) is more than 0% and not more than 1.0%. P has the effect of increasing strength without decreasing magnetic flux density. However, excessive P content impairs the toughness of the steel, making the steel sheet more susceptible to fracture. Therefore, the upper limit of the P content is set to 1.0%, preferably 0.150% or less, and more preferably 0.120% or less. There is no particular lower limit for the P content, but taking into consideration the manufacturing cost, it is set to 0.001% or more.

[0030] Furthermore, the slab used to manufacture the electrical steel sheet according to this embodiment, particularly the grain-oriented electrical steel sheet, may contain, in addition to the above-mentioned elements, one or more of Cu, Sn, Ni, Cr, Sb, and Bi as elements that stabilize secondary recrystallization, each in a content of 0% to 1.0%. The content of each of these elements may preferably be 0.0005% to 0.3000%. When the slab contains the above-mentioned elements, the magnetic flux density of the manufactured electrical steel sheet, particularly the grain-oriented electrical steel sheet, can be further improved.

[0031] A slab is formed by casting molten steel adjusted so that the electrical steel sheet has the above-described composition. The method for casting the slab is not particularly limited. In research and development, even if a steel ingot is formed in a vacuum melting furnace or the like, the same effect as when a slab is formed can be confirmed for the above-described composition.

[0032] [Process to make hot-rolled steel sheet] The slab is then heated and hot-rolled to be processed into a hot-rolled steel sheet. The slab heating temperature is not particularly limited. When the inhibitor components in the slab are completely dissolved, the slab may be heated to, for example, 1280°C or higher. The upper limit of the slab heating temperature is not particularly specified, but is preferably 1450°C from the viewpoint of equipment protection, and the slab heating temperature may be 1280°C or higher and 1450°C or lower. On the other hand, when the inhibitor components in the slab are not completely dissolved, the slab heating temperature may be less than 1280°C, for example. In this case, the steel sheet may be subjected to a nitriding treatment in any of the steps from the hot-rolled sheet annealing step to the finish annealing step. In addition, in the case of a non-oriented electrical steel sheet, in order to prevent the re-dissolved S compounds, N compounds, etc. during slab heating from subsequently finely precipitating and deteriorating the magnetic properties, the normal slab heating temperature may be 1150°C or lower, preferably 1100°C or lower, and more preferably 1050°C or lower.

[0033] Next, the heated slab is hot-rolled to be processed into a hot-rolled steel sheet. The thickness of the hot-rolled steel sheet after processing may be, for example, 1.8 mm or more and 3.5 mm or less. If the thickness of the hot-rolled steel sheet is less than 1.8 mm, the shape of the steel sheet after hot rolling may be inferior, which is not preferable. If the thickness of the hot-rolled steel sheet is more than 3.5 mm, the rolling load in the cold rolling process becomes large, which is not preferable.

[0034] [Process to make cold-rolled steel sheet] Next, the processed hot-rolled steel sheet is subjected to hot-rolled sheet annealing, and then rolled by one cold rolling or multiple cold rolling with intermediate annealing in between, to be processed into a cold-rolled steel sheet. When rolling by multiple cold rolling with intermediate annealing in between, it is also possible to omit the hot-rolled sheet annealing in the previous stage. However, when hot-rolled sheet annealing is performed, the steel sheet shape becomes better, so that the possibility of the steel sheet breaking during cold rolling can be reduced. Before being subjected to cold rolling, it is preferable to perform pickling in order to remove scale and the like attached to the surface of the steel sheet. For the purpose of controlling the plate thickness direction inhibitor described later, pickling may be performed at least once between hot rolling and primary recrystallization annealing. When rolling by multiple cold rolling, it is preferable to perform pickling before each cold rolling step from the viewpoint of reducing roll wear in cold rolling.

[0035] In addition, the steel sheet may be heat-treated at about 300°C or less between passes of cold rolling, between rolling roll stands, or during rolling. In such a case, the magnetic properties of the final magnetic steel sheet can be improved. The hot-rolled steel sheet may be rolled by three or more cold rolling passes, but since multiple cold rolling passes increase the manufacturing cost, it is preferable that the hot-rolled steel sheet is rolled by one or two cold rolling passes. When cold rolling is performed by reverse rolling such as a Sendzimir mill, the number of passes in each cold rolling pass is not particularly limited, but is preferably 9 passes or less from the viewpoint of manufacturing cost.

[0036] [Process of contacting the electromagnetic steel sheet with the solution] The manufacturing method of the electrical steel sheet of the present invention is characterized in that the electrical steel sheet is brought into contact with a solution containing one or more elements selected from Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni (these may be referred to as "Cu, etc." in this specification), in which the total concentration of each element is 0.00001% or more and 1.0000% or less (this may be referred to as "solution contact treatment" or "solution contact step" in this specification).

[0037] Electrical steel sheets contain MnS, MnSe, and MnTe (sometimes referred to as "MnS, etc." in this specification) as precipitates, and these precipitates act as inhibitors. In the present invention, by utilizing the phenomenon that when MnS, etc., comes into contact with a solution containing Cu, etc., a part of the Mn in MnS, etc., particularly the Mn in the surface layer of MnS, etc., is replaced with Cu, etc., the heat resistance of the precipitates is improved, thereby improving the inhibitor strength of the grain-oriented electrical steel sheet and realizing high magnetic properties. In addition, by utilizing the above phenomenon in which elements such as Cu become concentrated on the steel sheet surface, it is possible to realize the magnetic domain control effect by improving heat transfer, the coating adhesion by improving the wettability of the coating liquid, and the heat extraction in laminated cores in transformers and motors. These effects can be enjoyed not only in grain-oriented electrical steel sheets but also in non-oriented electrical steel sheets.

[0038] The mechanism by which the inhibitor control in the sheet thickness direction is possible by contacting the electrical steel sheet with a solution containing Cu, etc. is presumed to be as follows. When the solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, these elements have a very high affinity with S, Se, and Te in the solution, and therefore replace Mn in the MnS, MnSe, and MnTe precipitates exposed on the steel sheet surface to form compounds. This reaction is particularly likely to occur on the surface side of the MnS precipitates that come into contact with the solution. When Mn is replaced with other metal elements (Cu, etc.) on the surface side of the MnS precipitates, these surface side compounds act as a barrier and suppress the dissolution of Mn, S, Se, and Te on the center side of the MnS precipitates into the steel. This suppresses the Ostwald ripening of MnS, etc. in the final annealing process, and it is believed that the heat resistance of the MnS precipitates, i.e., the inhibitor strength, increases. This reaction occurs when a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni comes into contact with MnS, MnSe, and MnTe. Therefore, if there are defects such as cracks and voids in the surface layer of the steel sheet, the solution penetrates into the steel sheet through those spaces and reacts not only with MnS exposed on the outermost surface of the steel sheet, but also with MnS within a certain depth range of the steel sheet surface, increasing the inhibitor strength. In order to increase the inhibitor strength of MnS within a certain depth range, defects such as cracks may be introduced into the steel sheet surface by shot blasting or the like before the electrical steel sheet comes into contact with the solution. In addition to the heat resistance described above, that is, the increase in inhibitor strength, the concentrated elements such as Cu can realize the magnetic domain control effect due to improved heat transfer, the improvement of coating adhesion due to improved wettability of the coating liquid, and the improvement of heat extraction in laminated cores in transformers and motors.

[0039] If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution is less than 0.00001%, the inhibitor control effect in the sheet thickness direction, and the effects of magnetic domain control effect manifestation, coating adhesion improvement, and heat extraction improvement due to the concentration of Cu, etc. are insufficient, which is not preferable. If the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution is more than 1.0000%, the effect of improving magnetism is saturated, which is not preferable. Therefore, the total concentration of one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni in the solution is 0.00001% or more and 1.0000% or less.

[0040] Generally, the pH of the solution is preferably low. A solution with a low pH has a pickling effect, and is thought to react not only with MnS exposed on the outermost surface of the steel sheet, but also with MnS within a certain depth range of the steel sheet surface layer, thereby increasing the inhibitor strength and promoting the concentration of Cu and the like. However, if the pH of the solution is less than -1, it is not preferable because the acidity becomes too strong and the solution becomes difficult to handle. If the pH of the solution is 7 or more, the effect of the pickling treatment cannot be sufficiently obtained, and the effect of inhibitor control in the plate thickness direction may be insufficient. Therefore, the pH of the solution may be -1.5 or more and less than 7. The lower the pH of the solution, the higher the pickling effect and the more the inhibitor strengthening is promoted, so the pH of the solution is preferably -1.5 or more and 6 or less, and more preferably -1.5 or more and 5 or less. Examples of acid components contained in the solution include sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and the like.

[0041] Furthermore, if the temperature of the solution is less than 15°C, the pickling effect is not sufficient, and the inhibitor control effect in the thickness direction may be insufficient. If the temperature of the solution is more than 100°C, the solution may be difficult to handle. Therefore, the temperature of the solution may be 15°C or more and 100°C or less.

[0042] Furthermore, if the steel sheet is in contact with the solution for less than 5 seconds, the contact time is insufficient, and the effects of pickling, inhibitor strengthening, Cu concentration, etc. may be insufficient. If the steel sheet is in contact with the solution for more than 200 seconds, the equipment for contacting the steel sheet becomes long and large, which is not preferable. Therefore, the contact time of the steel sheet with the solution may be 5 seconds or more and 200 seconds or less.

[0043] Therefore, the step in which the electrical steel sheet comes into contact with the solution (solution contact step) may be a pickling step, and the above-mentioned pH value, solution temperature, and contact time (pickling time) may be adopted as the pickling conditions. In general, in the manufacturing process of steel sheets, pickling treatment is performed before a subsequent step for the purpose of removing scale and cleaning the steel sheet surface. Typically, pickling treatment may be performed before each cold rolling step from the viewpoint of reducing roll wear in cold rolling, pickling treatment may be performed before primary recrystallization annealing from the viewpoint of controlling oxidation of the steel sheet surface in primary recrystallization annealing, pickling treatment may be performed before finish annealing from the viewpoint of improving the applicability of the annealing separator, and pickling treatment may be performed before planarization annealing from the viewpoint of improving the adhesion of the insulating coating, or these pickling treatments may be performed in combination. The inhibitor (precipitate) heat resistance improving effect of the present technology can be applied to other steel types, for example, non-oriented electrical steel sheets. When applied to other steel types, the slab components and process conditions are not limited to those described above.

[0044] (Method to confirm that the surface of "MnS, etc." precipitates is replaced with "Cu, etc.") A method for confirming whether the surfaces of precipitates such as MnS are replaced with Cu or the like will be described. First, the steel plate sample to be confirmed is mirror-polished and observed by SEM-EDX. The presence of precipitates such as MnS can be confirmed in the SEM observation image. The EDX element mapping and intensity ratio of Cu, for example, Mn, S, and Cu, are superimposed on the observation image. This makes it possible to confirm the constituent elements of the precipitate particles. In a typical example, when a precipitate particle and its vicinity are observed, the mapping intensity ratio of Mn and S is increased in the precipitate particle area, confirming that the particle is a MnS particle, and if the mapping intensity ratio of Cu is also increased in the surface vicinity of the particle, it is estimated that the surface of the precipitate is replaced with Cu.

[0045] Furthermore, the element distribution state within the precipitate particle is confirmed by Auger electron spectroscopy. More specifically, element analysis is performed by sputtering the surface layer of the MnS or other precipitate with Ar at intervals of several nm (typically 1 nm) by Auger electron spectroscopy, so that the distribution of the constituent elements can be confirmed from the surface layer of the precipitate particle to its interior. If Cu or the like is detected in high concentration only in the surface layer of the MnS or other precipitate and the concentration of Cu or the like is reduced inside the precipitate, it can be considered that the surface of the precipitate has been substituted with Cu or the like.

[0046] The instruments and measurement conditions used for SEM, EDS and Auger electron spectroscopy can be appropriately selected depending on the object to be measured. In the analysis in this specification, the SEM instrument used was a JEOL7001F FE-SEM manufactured by JEOL with a WD of 10 mm and an accelerating voltage of 15 kV. The Auger electron spectroscopy instrument used was a PHI FE-AES PHI-700 with an electron beam of 10 kV, 10 nA, and an ion beam of Ar / 2 kV.

[0047] [Primary recrystallization annealing process] Next, the cold-rolled steel sheet is heated and then decarburized. These processes are also called primary recrystallization annealing, and are preferably performed continuously. In addition, intermediate treatment may be performed between the heating and decarburization annealing for the purpose of improving the coating properties by suppressing color unevenness.

[0048] The decarburization annealing may be performed in a wet atmosphere containing hydrogen and nitrogen at a temperature of 900° C. or less. In order not to inhibit the decarburization, the oxygen partial pressure ratio of the decarburization annealing atmosphere, i.e., the water vapor partial pressure P H2O and hydrogen partial pressure P H2 Compared to P H2O / P H2 may be set to 0.35 or more.

[0049] In the step of primary recrystallization annealing, the cold-rolled steel sheet may be subjected to reduction annealing following decarburization annealing in order to improve magnetic properties and coating adhesion.

[0050] [Finish annealing process] Thereafter, the cold-rolled steel sheet after the primary recrystallization annealing is subjected to a finish annealing. In this case, an annealing separator mainly composed of MgO may be applied before the finish annealing for the purpose of preventing seizure between steel sheets, forming a primary coating, controlling secondary recrystallization behavior, etc. The annealing separator is generally applied to the steel sheet surface in the form of a water slurry and dried, but an electrostatic application method or the like may also be used. Here, by adding sulfides, sulfate compounds, nitrides, etc. to MgO, sulfur, nitrogen, etc. may be infiltrated into the steel sheet during the subsequent finish annealing, and secondary recrystallization control may be performed through inhibitor control.

[0051] Subsequently, a finish annealing is performed for the purpose of forming a primary coating and secondary recrystallization. The finish annealing may be performed by heat treating the coiled steel sheet using, for example, a batch-type heating furnace. Furthermore, in order to further reduce the iron loss value of the final electrical steel sheet, the coiled steel sheet may be subjected to a purification treatment in which the temperature is raised to about 1200°C and then maintained at that temperature.

[0052] Finish annealing is generally performed by raising the temperature from about room temperature, and the temperature raising rate of finish annealing is various, but is not particularly limited in the present invention, and general finish annealing conditions can be used. For example, the rate may be 5°C / h to 100°C / h from the viewpoint of productivity and general equipment constraints. In addition, other known heat patterns may be used. The heat pattern in the cooling process is also not particularly limited.

[0053] The atmosphere gas composition in the final annealing is not particularly limited. In the secondary recrystallization process, a mixed gas of nitrogen and hydrogen may be used. A dry atmosphere or a wet atmosphere may be used. The atmosphere in the purification annealing may be dry hydrogen gas.

[0054] The present inventors have discovered that coating adhesion is improved by contacting an electrical steel sheet with a solution containing one or more elements selected from the group consisting of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni at specific concentrations.

[0055] Although not bound by a specific theory, the following mechanism is considered for this effect. In some of the MnS, MnSe, and MnTe on the surface layer side of the steel sheet, Mn is replaced with these elements (Cu, etc.), and the elements such as Cu are concentrated. Mn is an element with a relatively low thermal conductivity compared to elements such as Cu. Therefore, the thermal conductivity is improved in the areas where Mn is replaced by Cu, etc., and heat transfer by heating in primary recrystallization annealing and finish annealing is promoted, so the temperature distribution in the steel sheet is more likely to be uniform, the surface roughness of the steel sheet surface is suppressed, and the wettability of the coating liquid of the coating in the subsequent coating process is improved and it can be applied uniformly. Even at the stage where the coating is formed by baking, etc., the temperature distribution by heating and the coating liquid application state are uniform, so it is thought that the coating adhesion is improved. It should be noted that the same effect can be obtained even if some of the MnS, MnSe, and MnTe are present in the coating such as forsterite. In addition, the improved thermal conductivity also improves heat dissipation in laminated cores in transformers and motors.

[0056] Therefore, a step of contacting the electrical steel sheet with a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni at specific concentrations may be performed after the finish annealing step and before the insulating coating application step, which can improve the adhesion of the insulating coating.

[0057] [Planarization annealing process] (insulating coating) Subsequently, after finish annealing, an insulating coating containing, for example, aluminum phosphate or colloidal silica as a main component is applied to the surface of the steel sheet for the purpose of imparting insulation and tension to the steel sheet. (flattening annealing) Thereafter, flattening annealing is performed for the purpose of baking the insulating coating and flattening the shape of the steel sheet by finish annealing. Note that the composition of the insulating coating is not particularly limited as long as it imparts insulation and tension to the steel sheet. Note that in this embodiment, it goes without saying that the grain-oriented electrical steel sheet may be subjected to magnetic domain control treatment depending on the purpose of the customer. According to the manufacturing method of the present embodiment, by contacting the magnetic steel sheet with a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni at a specific concentration, Mn is replaced with these elements in some of MnS, MnSe, and MnTe on the surface layer side of the steel sheet, improving the heat conductivity. When heat input such as laser processing or electron beam processing is performed as the magnetic domain control treatment, the improved heat conductivity allows uniform heat input and also promotes the realization of the magnetic domain control effect. In this respect, the step of contacting the magnetic steel sheet with a solution containing one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni at a specific concentration is preferably performed before the magnetic domain control treatment, and the step of contacting with the acid may be performed before or after the final annealing depending on the timing of the magnetic domain control treatment.

[0058] The final electrical steel sheet can be manufactured through the above steps. According to the manufacturing method according to this embodiment, a grain-oriented electrical steel sheet excellent in magnetic properties and coating adhesion can be manufactured.

[0059] From the viewpoint of excellent magnetic properties, the magnetic flux density B8 value may be further controlled in the magnetic steel sheet according to this embodiment. Specifically, in the magnetic steel sheet according to this embodiment, the magnetic flux density B8 value is preferably 1.90 T or more, more preferably 1.91 T or more, even more preferably 1.92 T or more, and even more preferably 1.93 T or more. Here, the magnetic flux density B8 value is the magnetic flux density when a magnetic field of 800 A / m at 50 Hz is applied to the magnetic steel sheet. If the magnetic flux density B8 value is less than 1.90 T, the iron loss value (particularly, hysteresis loss) of the magnetic steel sheet becomes large, which is not preferable. The upper limit of the magnetic flux density B8 value is not particularly limited, but may be, for example, 2.0 T in reality. The magnetic properties of the magnetic steel sheet, such as the magnetic flux density, can be measured by a known method. For example, the magnetic properties of the magnetic steel sheet can be measured by using a method based on the Epstein test specified in JIS C2550, or the Single Sheet Tester (SST) method specified in JIS C2556. In research and development, when a steel ingot is formed in a vacuum melting furnace or the like, it is difficult to take a test piece of the same size as that of the actual manufacturing. In this case, for example, a test piece with a width of 60 mm and a length of 300 mm may be taken and a measurement based on the Single Sheet Magnetic Property Test Method may be performed. Furthermore, a correction factor may be multiplied to the obtained result so that a measurement value equivalent to that of the method based on the Epstein test is obtained. In this embodiment, the measurement is performed by a measurement method based on the Single Sheet Magnetic Property Test Method.

[0060] The electromagnetic steel sheet thus obtained is processed into wound cores or stacked cores when manufacturing transformers and motors. High coating adhesion, no peeling during processing or long-term operation, and suppression of powder generation during slitting are important factors in gaining trust from consumers. In particular, the insulating coating not only ensures insulation between steel sheets, but also has the function of applying tension to the steel sheet surface, and the coating adhesion between the primary coating and the insulating coating is important. From the viewpoint of excellent coating adhesion, in one embodiment of the present invention, a test piece having a length of 300 mm in the rolling direction and 30 mm in the direction perpendicular to the rolling direction is taken from the obtained electromagnetic steel sheet, adhesive tape is attached to the steel sheet surface, and the test piece is bent 180° while being pressed against round bars having various diameters, and then the adhesive tape is peeled off, and the smallest diameter at which the insulating coating does not adhere to the bent part of the adhesive tape is evaluated. The smaller the minimum diameter of peeling upon bending, the better the adhesion of the insulating coating. In normal applications, a minimum diameter of 20 mm or less is required, and if the minimum diameter is 10 mm or less, it may be determined that the bending adhesion is excellent. Note that the peeling property of the insulating coating may be easily detected by using, for example, a transparent tape as the adhesive tape. Note that the effect of improving the adhesion of the insulating coating by the technology of the present application may be applied to other steel types, for example, it may be applied to non-oriented electrical steel sheets.

[0061] The electromagnetic steel sheet according to the present embodiment has been described above. The electromagnetic steel sheet according to the present embodiment can be manufactured by the manufacturing method of the electromagnetic steel sheet according to the present embodiment described above. However, the manufacturing method is not limited to this method. EXAMPLES

[0062] The method for producing an electromagnetic steel sheet according to an embodiment of the present invention and the electromagnetic steel sheet will be described in more detail below with reference to examples. Note that the examples shown below are merely examples of the electromagnetic steel sheet according to this embodiment, and the electromagnetic steel sheet according to this embodiment is not limited to the examples shown below.

[0063] Example 1 First, a steel ingot was prepared containing, by mass%, C: 0.04%, Si: 3.3%, Mn: 0.10%, S: 0.001%, Se: 0.001%, Te: 0.001%, acid-soluble Al: 0.005%, N: 0.003%, P: 0.007%, and the balance being Fe and impurities. The steel ingot was annealed at 1200 ° C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1000 ° C for 140 seconds, pickled, and then subjected to two cold rolling steps including intermediate annealing and solution contact treatment (also serving as pickling), to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the solution contact conditions (pickling conditions) after intermediate annealing were as shown in Table 1.

[0064] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and the steel sheet was dried. Then, a finish annealing was performed, and the steel sheet after the finish annealing was washed with water. Then, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and the steel sheet was subjected to planarization annealing for the purpose of baking the insulating coating and planarizing the steel sheet.

[0065] The grain-oriented electrical steel sheet samples obtained above were sheared and annealed for stress relief, and then the magnetic flux density B8 value of the grain-oriented electrical steel sheets according to each of the present invention examples and comparative examples was measured using a single sheet magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm x 300 mm. Here, the B8 value is the magnetic flux density of the steel sheet when the grain-oriented electrical steel sheet is excited at 50 Hz and 800 A / m. In the present invention, the average value of five samples was used.

[0066] Here, the condition where the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.90 T or more was judged to be good (B). Furthermore, the condition where the magnetic flux density B8 value is 1.91 T or more was judged to be best (A). And the conditions other than the above were judged to be unacceptable (C).

[0067] Table 1 shows the manufacturing conditions, measurement results, and evaluations of the above examples of the present invention and comparative examples.

[0068] [Table 1]

[0069] Referring to the results in Table 1, it was found that the grain-oriented electrical steel sheet satisfying the conditions of this embodiment was judged to be good.

[0070] Example 2 First, a steel ingot containing C: 0.08%, Si: 3.3%, Mn: 0.08%, S: 0.026%, acid-soluble Al: 0.03%, N: 0.008%, P: 0.005%, and the balance being Fe and impurities was prepared. The steel ingot was annealed at 1350 ° C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1100 ° C for 140 seconds, subjected to a solution contact treatment (also acts as pickling), and then cold-rolled to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the solution contact conditions (pickling conditions) after hot-rolled sheet annealing were as shown in Table 2.

[0071] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and the steel sheet was dried. Then, a finish annealing was performed, and the steel sheet after the finish annealing was washed with water. Then, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and the steel sheet was subjected to planarization annealing for the purpose of baking the insulating coating and planarizing the steel sheet.

[0072] The grain-oriented electrical steel sheet samples obtained above were sheared and annealed for stress relief, and then the magnetic flux density B8 value of the grain-oriented electrical steel sheets according to each of the present invention examples and comparative examples was measured using a single sheet magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm x 300 mm. Here, the B8 value is the magnetic flux density of the steel sheet when the grain-oriented electrical steel sheet is excited at 50 Hz and 800 A / m. In the present invention, the average value of five samples was used.

[0073] Here, the condition where the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.91 T or more was judged to be good (B). Furthermore, the condition where the magnetic flux density B8 value is 1.92 T or more was judged to be best (A). And the other conditions were judged to be unacceptable (C).

[0074] Table 2 shows the manufacturing conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0075] [Table 2]

[0076] Referring to the results in Table 2, it was found that the grain-oriented electrical steel sheet satisfying the conditions of this embodiment was judged to be good.

[0077] Example 3 First, a steel ingot was produced containing, by mass%, C: 0.09%, Si: 3.3%, Mn: 0.09%, S: 0.023%, acid-soluble Al: 0.03%, N: 0.009%, P: 0.004%, with the balance being the components shown in Table 3, Fe, and impurities. The steel ingot was annealed at 1350°C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1100°C for 140 seconds, subjected to a solution contact treatment (which also served as pickling), and then cold-rolled to obtain a cold-rolled steel sheet with a thickness of 0.23 mm. Here, the solution contact conditions (pickling conditions) after annealing of the hot-rolled sheet were as follows: Cu concentration in the solution: 0.001%, solution (base): hydrochloric acid, solution pH: 3, solution temperature: 70°C, contact time between the solution and the steel sheet: 30 seconds.

[0078] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and the steel sheet was dried. Then, a finish annealing was performed, and the steel sheet after the finish annealing was washed with water. Then, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and the steel sheet was subjected to planarization annealing for the purpose of baking the insulating coating and planarizing the steel sheet.

[0079] The grain-oriented electrical steel sheet samples obtained above were sheared and annealed for stress relief, and then the magnetic flux density B8 value of the grain-oriented electrical steel sheets according to each of the present invention examples and comparative examples was measured using a single sheet magnetic property measurement method (based on the method described in JIS C2556) with a sample size of 60 mm x 300 mm. Here, the B8 value is the magnetic flux density of the steel sheet when the grain-oriented electrical steel sheet is excited at 50 Hz and 800 A / m. In the present invention, the average value of five samples was used.

[0080] Here, the condition where the magnetic flux density B8 value of the grain-oriented electrical steel sheet is 1.93 T or more was judged to be extremely good (S).

[0081] Table 3 shows the manufacturing conditions, measurement results, and evaluations of the above examples of the present invention and comparative examples.

[0082] [Table 3]

[0083] Referring to the results in Table 3, it was found that the grain-oriented electrical steel sheet satisfying the conditions of this embodiment was judged to be good.

[0084] Example 4 First, a steel ingot was prepared containing, by mass%, C: 0.09%, Si: 3.3%, Mn: 0.09%, S: 0.023%, acid-soluble Al: 0.03%, N: 0.009%, P: 0.004%, and the balance being Fe and impurities. The steel ingot was annealed at 1350°C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet having a thickness of 2.3 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1100°C for 140 seconds, pickled, and then cold-rolled to obtain a cold-rolled steel sheet having a thickness of 0.23 mm. Here, the pickling conditions after the annealing of the hot-rolled sheet were as follows: Cu concentration in the pickling solution: 0.000005%, pickling solution: hydrochloric acid, pH of the pickling solution: 3, pickling solution temperature: 70°C, and contact time between the pickling solution and the steel sheet: 30 seconds.

[0085] The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing in a wet hydrogen atmosphere at 850°C for 180 seconds. Next, an annealing separator containing MgO was applied in the form of a water slurry to the surface of the steel sheet after the primary recrystallization annealing, and the steel sheet was dried. Then, the steel sheet after the final annealing was subjected to finish annealing, and the steel sheet after the finish annealing was brought into contact with a solution (also served as pickling). Then, an insulating coating mainly composed of aluminum phosphate and colloidal silica was applied to the surface of the steel sheet, and the steel sheet was subjected to planarization annealing for the purpose of baking the insulating coating and planarizing the steel sheet. Here, the solution contact conditions (pickling conditions) after the finish annealing were as shown in Table 4.

[0086] Furthermore, the above samples were sheared to a width of 30 mm, and bending tests were performed using cylinders of various diameters. Here, the minimum cylinder diameter (diameter) at which the insulating coating did not peel off was defined as the peeling diameter (mm). The test method is as follows. A bending test was performed on the test pieces of each test number at a curvature of 8 to 30 mm. The bending test was performed using a cylindrical mandrel bending tester, with the tester set on the test piece so that the axial direction of the cylinder coincided with the width direction of the test piece, until the test piece was bent at 180°. After applying adhesive tape to the surface of the bending test piece and performing bending tests at various curvatures, the adhesive tape was subsequently peeled off, and the peeling diameter was derived by checking whether the insulating coating was attached to the bent part of the adhesive tape.

[0087] Here, the condition where the peeled diameter was 20 mm or less was judged as good (B), and the condition where the peeled diameter was 10 mm or less was judged as best (A), and the other conditions were judged as poor (C).

[0088] Table 4 shows the manufacturing conditions, measurement results, and evaluations of the above-mentioned examples of the present invention and comparative examples.

[0089] [Table 4]

[0090] With reference to the results in Table 4, it was found that the grain-oriented electrical steel sheets that satisfied the conditions of this embodiment were judged to be good. When the magnetic flux density B8 value of each sample was measured in the same manner as in Examples 1 to 3, good results of 1.90 T or more were obtained in all cases.

[0091] Example 5 A steel ingot was produced containing, by mass%, C: 0.0016%, Si: 2.74%, Mn: 0.22%, S: 0.0008%, acid-soluble Al: 0.87%, N: 0.0014%, P: 0.02%, Sn: 0.06%, and the balance being Fe and impurities. The steel ingot was annealed at 1080°C for 1 hour, and then hot-rolled to obtain a hot-rolled steel sheet with a thickness of 1.8 mm. The obtained hot-rolled steel sheet was annealed at a maximum temperature of 1050°C for 120 seconds, subjected to a solution contact treatment (also acts as pickling), and then cold-rolled to obtain a cold-rolled steel sheet with a thickness of 0.25 mm. Here, the solution contact conditions (pickling conditions) after hot-rolled sheet annealing were as shown in Table 5. The cold-rolled steel sheet thus obtained was then subjected to primary recrystallization annealing at 950° C. for 30 seconds, and then an insulating coating was applied thereto. From the non-oriented electrical steel sheet samples obtained above, ring-shaped cores with an outer diameter of 125 mm and an inner diameter of 100 mm were punched out, and after stacking to a thickness of 20 mm (80 sheets), they were magnetized at 50 Hz and 1.5 T, and the core temperature rise was measured. Here, the condition where the core temperature rise was 20°C or less was judged as good (A), and the other cases (over 20°C) were judged as unacceptable (C).

[0092] Table 5 shows the solution contact conditions (pickling conditions) and evaluations for the above-mentioned invention examples and comparative examples.

[0093] [Table 5]

[0094] Referring to the results in Table 5, it can be seen that the non-oriented electrical steel sheet satisfying the conditions of this embodiment has improved heat conductivity and therefore good heat dissipation properties, which suppresses the temperature rise of the laminated core and results in a good evaluation.

Claims

1. the method includes a step of contacting, with a solution, an electrical steel sheet containing, by mass%, C: more than 0% and not more than 0.10%, Si: 2.5% or more and not more than 4.5%, Mn: 0.01% or more and not more than 5.0%, the total of one or more of S, Se and Te: more than 0% and not more than 0.050%, acid-soluble Al: more than 0% and not more than 5.0%, N: more than 0% and not more than 0.015%, P: more than 0% and not more than 1.0%, with the balance being Fe and impurities; the solution contains one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn, and Ni, and the total concentration of each element is 0.000010% or more and 1.0000% or less by mass%, the pH of the solution is -1.5 or more and less than 7, the liquid temperature is 15°C or more and 100°C or less, and the contact time of the electrical steel sheet with the solution is 5 seconds or more and 200 seconds or less, the electrical steel sheet contains one or more of MnS, MnSe and MnTe, a step of contacting the magnetic steel sheet with a solution, in which a portion of Mn in one or more of MnS, MnSe and MnTe of the magnetic steel sheet is replaced with one or more of Cu, Hg, Ag, Pb, Cd, Co, Zn and Ni.

2. 2. The method for producing an electrical steel sheet according to claim 1, characterized in that the electrical steel sheet contains, in place of a portion of the Fe, one or more elements selected from the group consisting of Cu: 1.0% or less, Sn: 1.0% or less, Ni: 1.0% or less, Cr: 1.0% or less, Sb: 1.0% or less, and Bi: 1.0% or less.

3. 3. The method for producing an electrical steel sheet according to claim 1, wherein the step of contacting the electrical steel sheet with the solution is a pickling step.

4. The method for producing an electrical steel sheet according to any one of claims 1 to 3, characterized in that a step of contacting the electrical steel sheet with the solution occurs after a hot rolling step and before a finish annealing step.

Citation Information

Patent Citations

  • Non-oriented electrical steel for rotor of large-size generator and production method

    CN105296849A

  • JP1965-015644B

  • hifunsaibutsushitsuofunsaisurutamenoshindomiru

    JP1976013469A

  • Manufacture of hot rolled steel plate with superior chemical treatability

    JP1981130475A

  • Preparation of pickling solution

    JP1984159989A