How to recover precious metals

The method uses iodine, potassium iodide, and lactam compounds to dissolve and phase-separate precious metals, overcoming low yields and high energy costs in existing methods, achieving efficient and environmentally friendly recovery.

JP7569048B2Active Publication Date: 2024-10-17MITSUBISHI MATERIALS CORP +1

Patent Information

Application Number
JP2020176673
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-21
Publication Date
2024-10-17
Estimated Expiration
2040-10-21

AI Technical Summary

Technical Problem

Existing methods for recovering precious metals from waste materials face challenges such as low yields, high energy costs, environmental impact, and inefficiencies in dissolution processes, particularly when using iodine and potassium iodide without organic solvents.

Method used

A method involving the use of an extract containing iodine, potassium iodide, and an organic solvent like lactam compounds to dissolve precious metals, followed by pH adjustment to 2 or less and dilution with water to induce phase separation, allowing for high-yield recovery without thermal energy.

Benefits of technology

This method enables high-yield recovery of precious metals like gold and palladium from waste materials at low energy costs and with minimal environmental impact, using simple configurations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569048000002
    Figure 0007569048000002
  • Figure 0007569048000003
    Figure 0007569048000003
  • Figure 0007569048000004
    Figure 0007569048000004
Patent Text Reader

Abstract

To provide a noble metal recovery method capable of separating and recovering a noble metal from a noble metal-containing material in a high yield at a low energy cost.SOLUTION: A noble metal recovery method comprises: a dissolving process for obtaining a metal solution by immersing a noble metal-containing material having at least one of gold and palladium in an extract solution containing an organic solvent and iodine; a pH adjusting process for adjusting the pH to 2 or less by adding an acid to the metal solution; and a hydrolysis step for diluting the metal solution so that the volume becomes 2.7 times or more by adding water to prepare an iodide of the noble metal. The organic solvent contains a lactam compound.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for recovering precious metals from a material containing at least one of gold and palladium. [Background technology]

[0002] Recycling of precious metals (Au, Ag, Pt, Pd, Rh, Ir, Ru, Os) is being carried out to recover precious metals from waste materials that contain them. For example, discarded smartphone and computer circuit boards contain gold and palladium, and the content of these metals per unit weight can be greater than that of natural ores. In recent years, due to the soaring prices of precious metals, many methods have been proposed to efficiently extract precious metals from such waste materials.

[0003] For example, Patent Documents 1 and 2 disclose methods of heating and melting waste containing precious metals at high temperatures of several hundred degrees, and separating and extracting the precious metals. Furthermore, Patent Document 3 discloses a method of recovering gold by dissolving gold contained in waste using an extraction solution containing iodine and potassium iodide, and then performing electrolysis. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5761258 [Patent Document 2] Patent No. 6604515 [Patent Document 3] Patent No. 2571591 Summary of the Invention [Problem to be solved by the invention]

[0005] However, the methods disclosed in Patent Documents 1 and 2 have the problem that resin components and heavy metal components generated by heating the waste circuit boards have a detrimental effect on the separation of precious metals, reducing the yield of precious metals. In addition, there is a problem that the cost of the thermal energy required to melt the waste at high heat is high, and furthermore, a large amount of CO2 is generated during melting, which places a heavy burden on the environment.

[0006] On the other hand, in the method disclosed in Patent Document 3, the precious metals contained in the waste were not sufficiently dissolved when the extracting solution contained only iodine and potassium iodide. In order to sufficiently dissolve the precious metals by simply immersing the waste in the extracting solution, it is necessary to add an organic solvent to the extracting solution. In this case, there was a problem that the method of precipitating gold by adjusting the pH to 12 or higher as disclosed in Patent Document 3 could not be applied.

[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a method for recovering precious metals that can separate and recover precious metals from precious metal-containing materials at low energy cost and in high yield. [Means for solving the problem]

[0008] In order to solve the above-mentioned problems, the method for recovering precious metals of the present invention comprises the steps of: Organic solvents, iodine and potassium iodide the organic solvent containing a lactam compound, and the method for producing the metal solution further comprises: a dissolving step of immersing a material containing at least one of a precious metal, gold or palladium, in an extraction solution containing the organic solvent to obtain a metal solution; a pH adjustment step of adding an acid to the metal solution to adjust the pH to 2 or less; and a hydration step of adding water to the metal solution to dilute it to a volume 2.7 times or more, thereby producing an iodide of the precious metal.

[0009] According to the present invention, a metal solution containing a precious metal can be obtained by simply immersing a precious metal-containing material in an extracting solution containing an organic solvent having a lactam compound. Then, by simply adjusting the pH of this metal solution and diluting it with water, phase separation occurs and the precious metal can be transferred to a solid phase or an oil phase. This makes it possible to recover the precious metal contained in the precious metal-containing material at a high yield, at low cost, and with a simple configuration, with almost no use of thermal energy.

[0011] In addition, in the present invention, the extraction liquid may contain iodine and potassium iodide, the concentration of the potassium iodide being 30 g / L or more and the concentration of the iodine being 5 g / L or more, and the concentration of the potassium iodide being higher than the concentration of the iodine.

[0012] In the present invention, the concentration of the lactam compound contained in the extract may be 100 g / L or more and 600 g / L or less.

[0013] In the present invention, the water addition step may be a step of reducing the concentration of the lactam compound contained in the extract to half or less.

[0014] In the present invention, the hydration step may be a step of precipitating the noble metal iodide in the form of tabular crystals or needle crystals.

[0015] In the present invention, the amount of the precious metal contained in the precious metal iodide obtained in the hydration step may be 90% or more of the amount of the precious metal contained in the metal solution.

[0016] In the present invention, the material containing a precious metal may be a circuit board. Effect of the Invention

[0017] According to the present invention, it is possible to provide a method for recovering precious metals, which is capable of separating and recovering precious metals from materials containing precious metals at low energy cost and in high yield. [Brief description of the drawings]

[0018] [Figure 1] 1 is a flow chart showing a step-by-step process for recovering precious metals according to one embodiment of the present invention. [Diagram 2] 2 is an enlarged photograph of the precipitate (solid phase) after solid-liquid separation obtained in Example 1. [Diagram 3] 1 is an enlarged photograph of the precipitate (solid phase) after solid-liquid separation obtained in Example 13. [Figure 4] 1 shows a photograph and a composition table illustrating the results of composition analysis by energy dispersive X-ray analysis (EDX) of the Au-containing precipitate (solid phase) obtained in Example 1. [Diagram 5] 1 shows a photograph and a composition table illustrating the results of composition analysis by energy dispersive X-ray analysis (EDX) of the Pd-containing precipitate (solid phase) obtained in Example 13. [Figure 6] 1 is a graph showing peaks in powder X-ray diffraction (XRD) of the Au-containing precipitate (solid phase) obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, a method for recovering precious metals according to an embodiment of the present invention will be described with reference to the drawings. Note that the embodiment shown below is specifically described to better understand the gist of the invention, and does not limit the present invention unless otherwise specified.

[0020] FIG. 1 is a flow chart showing a step-by-step process for recovering precious metals according to one embodiment of the present invention. In the method for recovering precious metals according to the present embodiment, a procedure for separating and recovering precious metals from, for example, a circuit board (material containing precious metals) of an electronic device will be described. The circuit board of an electronic device contains precious metals such as Au and Pd in ​​soldered portions and wiring. Note that the precious metals in this embodiment refer to the following eight elements: Au, Ag, Pt, Pd, Rh, Ir, Ru, and Os.

[0021] First, an extracting solution is prepared that selectively dissolves Au and Pd as precious metals and Al and Ni as valuable metals that are industrially useful. The extracting solution of this embodiment is prepared by dissolving iodine, potassium iodide, and an organic solvent in water (pure water or ion-exchanged water).

[0022] Iodine has low solubility in water, but the solubility in water can be increased by adding water-soluble potassium iodide, so the concentration of potassium iodide in the extract is preferably higher than the concentration of iodine.

[0023] It is preferable that the concentration of potassium iodide contained in the extract is 30 g / L or more, and the concentration of iodine is 5 g / L or more. If the concentrations of potassium iodide and iodine are below the above-mentioned lower limits, the solubility of the precious metal decreases in the dissolution step described below, which is not practical. In addition, if the concentration of potassium iodide is less than 30 g / L, there is a concern that iodine will not dissolve in water to an extent of 5 g / L or more.

[0024] Examples of organic solvents used in the extract include lactam compounds. Lactam compounds are cyclic compounds formed by dehydration condensation of amino groups and carboxy groups, and contain a [-CO-NH-] group in part of the cyclic portion. Lactam compounds are classified into α-lactams (three-membered rings), β-lactams (four-membered rings), and γ-lactams (five-membered rings) depending on the number of carbon atoms in the cyclic portion, and lactam compounds of any number of carbon atoms can be used.

[0025] When a lactam compound is used in the extract, the concentration of the lactam compound in the extract is preferably in the range of 100 g / L or more and 600 g / L or less. If the concentration of the lactam compound is less than 100 g / L, there is a concern that the precious metal will not be sufficiently dissolved in the dissolving step described below. Also, if the concentration of the lactam compound is more than 600 g / L, there is a concern that the phase separation will be adversely affected in the water addition step described below.

[0026] In this embodiment, N-methyl-2-pyrrolidone (NMP) and N-ethyl-2-pyrrolidone (NEP) are used as lactam compounds. NMP is a liquid obtained by condensing γ-butyrolactone and methylamine, and dissolves in water at any ratio. The organic solvent is not limited to NMP or NEP, and various compounds having a lactam structure can be used.

[0027] Using the extracting solution having the above composition, a material containing at least one of gold and palladium, in this embodiment a circuit board, is immersed in the extracting solution (dissolving step S1). Many of these circuit boards contain precious metals such as gold and palladium in the solder or bonding wire. Many circuit boards also contain Al and Ni as valuable metals that are industrially useful in the conductive patterns, etc.

[0028] In the dissolving step S1, the circuit board is immersed in the extract at a temperature of about 10°C to 80°C for about 1 hour to 72 hours. If the extract is stirred at this time, the dissolution rate of the precious metals can be increased. Through this dissolving step S1, precious metals such as gold and palladium, and valuable metals such as Al and Ni become metal ions and dissolve in the extract, thereby obtaining a metal solution.

[0029] Next, the pH of the metal solution obtained in the dissolving step S1 is adjusted (pH adjustment step S2). In the pH adjustment step S2, an acid is added to the metal solution to adjust the pH to 2 or less. The acid used for the pH adjustment is not particularly limited, but for example, hydrochloric acid (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), etc. can be used. In this embodiment, hydrochloric acid is used. Even after the pH adjustment step S2, the metal solution remains in a homogeneous liquid state.

[0030] Next, the pH-adjusted metal solution is diluted with water so that its volume becomes 2.7 times or more (water-adding step S3). This water-adding step S3 produces iodides of the precious metals dissolved in the pH-adjusted metal solution, which then separates into two phases.

[0031] In the water addition step S3, the metal solution is separated into two phases, a solid phase and a liquid phase, or an oil phase and an aqueous phase, by the addition of water. Iodides containing Au and Pd move to either the solid phase or the oil phase. Whether the iodides move to the solid phase or the oil phase depends on the concentration of the organic solvent in the extract, the amount of water added in the water addition step S3, and the concentration of the precious metal dissolved in the metal solution.

[0032] In the water addition step S3, the concentration of the lactam compounds in the extract is reduced to less than half due to phase separation caused by the addition of water. This is thought to be because the lactam compounds promote phase separation caused by the addition of water.

[0033] For example, when the iodide containing the precious metal is transformed into a solid phase by the hydration step S3, the solid phase is precipitated and precipitated as a plate-like or needle-like crystal of the precious metal iodide. The main components of the resulting solid phase are the precious metal, iodine, and carbon. In addition, when the iodides containing the precious metals are transferred to the oil phase by the water addition step S3, the oil phase precipitates at the bottom of the aqueous phase as an oily substance having a high specific gravity. The main components of the resulting oil phase are the precious metals, iodine, and carbon.

[0034] In this embodiment, the metal solution is subjected to the pH adjustment step S2 and then the hydration step S3, but the metal solution may be subjected to the hydration step S3 and then the pH adjustment step S2. Also, the metal solution may be subjected to the pH adjustment step S2 and the hydration step S3 simultaneously.

[0035] Thereafter, the two phases generated in the water addition step S3 are separated from each other (separation step S4). In the separation step S4, if the metal solution is separated into a solid phase and a liquid phase, the solid phase containing the precious metal is recovered using a filter or the like. Also, if the metal solution is separated into an oil phase and an aqueous phase, the oil phase containing the precious metal is recovered by dispensing them at the oil-water interface. The recovered solid phase or oil phase containing the precious metals can be redissolved and purified to isolate the precious metals.

[0036] The amount of precious metal contained in the precious metal iodide obtained in the water addition step S3 is 90% or more of the amount of precious metal contained in the metal solution. In other words, most of the precious metal dissolved in the metal solution moves to the solid phase or oil phase recovered in the separation step S4, and the precious metal can be recovered with a high yield from the metal solution in which the precious metal is dissolved.

[0037] As described above, according to the method for recovering precious metals of the present invention, a metal solution in which precious metals are dissolved can be obtained by simply immersing a material containing precious metals in an extracting solution containing an organic solvent. Then, by simply adjusting the pH of this metal solution and diluting it with water, phase separation can be caused and the precious metals can be transferred to a solid phase or an oil phase. This makes it possible to recover the precious metals contained in the precious metal-containing material at a high yield, at low cost, and with a simple configuration, without using much thermal energy.

[0038] Although the embodiment of the present invention has been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention. EXAMPLES

[0039] The effect of the present invention was verified. First, it was verified that Au or Pd was contained in the precipitates (solid phases) of Examples 1 and 13 shown below, which were obtained by the above-mentioned precious metal recovery method.

[0040] Example 1 The extract of Example 1 was prepared by dissolving potassium iodide at 31 g / L, iodine at 5 g / L, and N-methyl-2-pyrrolidone (NMP) as an organic solvent at 400 g / L in ion-exchanged water.

[0041] A precious metal-containing waste (a material containing a precious metal) containing Au as a precious metal was immersed in the extraction solution of Example 1, and the temperature of the extraction solution was kept at 60°C and left for 24 hours (dissolving step). As a result, a metal solution in which Au was selectively dissolved in the extraction solution of Example 1 was obtained. A portion of this metal solution was collected, and the components were analyzed by inductively coupled plasma (ICP) emission spectroscopy. When the Au concentration in the metal solution was 700 ppm or less, precious metal-containing waste was added until the Au concentration in the metal solution exceeded 700 ppm, thereby increasing the Au concentration in the metal solution. When the predetermined concentration was reached, the precious metal-containing waste was removed from the metal solution. In addition, a polyimide film on which a thin Au film was formed by sputtering was used as the precious metal-containing waste.

[0042] This metal solution was adjusted to pH 1 or less by adding 0.4 times by volume of 1M hydrochloric acid (pH adjustment step). Furthermore, 2.6 times by volume of ion-exchanged water was added to the metal solution after pH adjustment to dilute it (water addition step). This resulted in a 4-fold dilution of the concentration of the extract. In this water addition step, a precipitate (solid phase) was formed immediately after water addition in Example 1, but a sufficient amount of precipitate can be obtained by leaving it to stand for about 1 hour. In this way, the precipitate (solid phase) of Example 1 was obtained. Figure 2 shows an enlarged photograph of the precipitate (solid phase) obtained in Example 1 after solid-liquid separation. Note that a portion of the aqueous phase of the solution after water addition was collected, and it was confirmed by component analysis that 90% or more of Au had been transferred to the precipitate.

[0043] Example 13 The extract of Example 13 was prepared by dissolving potassium iodide at 62 g / L, iodine at 10 g / L, and NMP at 500 g / L in ion-exchanged water. A precious metal-containing waste containing Pd as a precious metal was immersed in the extract of Example 13, and the temperature of the extract was kept at 60° C. and left for 24 hours (dissolving step). As a result, a metal solution in which Pd was selectively dissolved in the extract of Example 13 was obtained. A portion of this metal solution was collected, and the components were analyzed by inductively coupled plasma (ICP) emission spectroscopy. When the Pd concentration in the metal solution was 700 ppm or less, precious metal-containing waste was added until it exceeded 700 ppm, and the Pd concentration in the metal solution was increased. When the predetermined concentration was reached, the precious metal-containing waste was taken out from the metal solution. In addition, a Pd metal piece was used as a simulation for the precious metal-containing waste containing Pd.

[0044] This metal solution was adjusted to pH 1 or less by adding 0.4 times by volume of 1M hydrochloric acid (pH adjustment step). Furthermore, 1.3 times by volume of ion-exchanged water was added to the metal solution after pH adjustment to dilute it (water addition step). This resulted in dilution to 2.7 times the concentration of the extract. In this water addition step, a precipitate (solid phase) was generated immediately after water addition in Example 13, but a sufficient amount of precipitate can be obtained by leaving it to stand for about 1 hour. In this way, the precipitate (solid phase) of Example 13 was obtained. Figure 3 shows an enlarged photograph of the precipitate (solid phase) obtained in Example 13 after solid-liquid separation. Note that a portion of the aqueous phase of the solution after water addition was collected, and it was confirmed by component analysis that 90% or more of Pd had been transferred to the precipitate.

[0045] Next, the precipitates (solid phases) obtained in the above-mentioned Examples 1 and 13 were used to perform composition analysis by energy dispersive X-ray analysis (EDX). The results of the EDX in Example 1 are shown in Figure 4, and the results of the EDX in Example 13 are shown in Figure 5. The numbers in the photographs indicate the analyzed locations.

[0046] According to the results shown in Figure 4, it was confirmed that the precipitate (solid phase) obtained in Example 1 was composed of C, Au, and I, and contained Au at a concentration of 5% or more. This gold content is sufficiently high compared to, for example, general gold ore.

[0047] Moreover, according to the results shown in FIG. 5, it was confirmed that the precipitate (solid phase) obtained in Example 13 was composed of C, Pd, and I, with Pd being contained at a concentration of 4% or more. From these results, it was confirmed that precious metals such as Au and Pd of the precious metal-containing material were transferred to the precipitate (solid phase) obtained by the precious metal recovery method of this embodiment.

[0048] Next, powder X-ray diffraction (XRD) was performed on the precipitate (solid phase) obtained in Example 1. Figure 6 shows the peaks of the precipitate in Example 1 obtained by XRD. According to the results shown in Figure 4, the precipitate (solid phase) is not derived from either Au or I, but is considered to be a substance containing organic matter, and is considered to be a complex composition or mixture containing C, I, and Au. In addition, a peak was generated at the same position as the Au peak, and it was also confirmed from the results of XRD that Au had migrated to the precipitate (solid phase). It was confirmed that a part of Au had precipitated as simple Au.

[0049] Next, for the above-mentioned Examples 1 and 13, as well as Examples 2 to 12, 14 to 19, and Comparative Examples 1 to 7, it was confirmed whether a precipitate (solid phase) or an oil phase containing precious metals was generated by phase separation from the metal solution in which precious metals were dissolved by immersing precious metal-containing waste in an extraction solution of each composition. The conditions for each Example and Comparative Example and the results of phase separation are shown in Table 1.

[0050] The formation of a precipitate (solid phase) was defined as the following state. A plate-like or needle-like crystalline solid with a side length exceeding 1 μm is produced from a metal solution, and composition analysis using energy dispersive X-ray analysis (EDX) shows that it contains 5 mass% or more of Au or Pd relative to iodine. The formation of the oil phase was defined as follows: A liquid separation layer is generated from the metal solution, and composition analysis of this separation layer using X-ray fluorescence analysis (XRF) shows that it contains 1 mass% or more of Au or Pd relative to iodine.

[0051] [Table 1]

[0052] (Examples 2 to 4) The same operations as in Example 1 were carried out, except that the water addition ratios to the metal solutions containing Au were 8, 16, and 24 times, respectively (both the amount of hydrochloric acid and ion-exchanged water were increased). The formation of precipitates was confirmed in all cases, and the amount of precipitates formed was almost the same as in Example 1. Once precipitates formed, they did not redissolve no matter how many times the metal solution was diluted (water was added), and Au could be recovered.

[0053] Example 5 The same procedure as in Example 1 was carried out, except that 0.04 volumes of 1M hydrochloric acid were added to the Au-containing metal solution, and 2.96 volumes of ion-exchanged water were added to adjust the pH to 2. A precipitate was also formed, and Au could be recovered.

[0054] (Examples 6 and 7) The same operation as in Example 1 was carried out, except that the amount of precious metal-containing waste immersed in the extraction solution was adjusted to set the Au concentration in the solution to 2000 ppm and 350 ppm, respectively. A precipitate was also formed here, and Au could be recovered.

[0055] (Examples 8 to 10) The same operation as in Example 1 was performed, except that the amount of precious metal-containing waste immersed in the extraction solution was adjusted to set the Au concentration in the metal solution to 140 ppm, 100 ppm, and 10 ppm, respectively. No precipitate was formed, and multiple small black oil phases were separated from the solution. It was confirmed that 90% or more of the Au in the solution had migrated to this oil phase. The aqueous phase and the oil phase could be separated by passing through a filter paper or a filter, and Au could be recovered by heating the oil phase to remove the carbon component and the iodine component. The formation of the precipitate and the oil phase is influenced by the Au concentration relative to the organic solvent and iodine, and a high Au concentration results in a precipitate, while a low Au concentration results in an oil phase.

[0056] Example 11 The same procedure as in Example 1 was carried out except that the potassium iodide, iodine, and NMP in the extract were 62 g / L, 10 g / L, and 500 g / L, respectively. An oil phase was produced in this Example 11. When the iodine concentration is relatively high, an oil phase is produced instead of a precipitate.

[0057] Example 12 The same operation as in Example 1 was performed except that N-ethyl-2-pyrrolidone (NEP) was used as the organic solvent in the extraction solution and its concentration was 370 g / L. In this case, no precipitation occurs, but an oil phase occurs. NEP has a ketone group like NMP, and is an organic solvent that has a lactam structure like NMP. In comparison with Comparative Example 5 described later, it is considered that the organic solvent needs to have a lactam structure in order for a precipitation or an oil phase to occur.

[0058] Example 14 The same operation as in Example 13 was performed except that the amount of precious metal-containing waste immersed in the extraction solution was adjusted to set the Pd concentration in the metal solution to 100 ppm. Here, no precipitate was formed, and multiple small black oil phases were separated from the solution and formed. It was confirmed that 90% or more of the Pd in ​​the solution had migrated to this oil phase. The aqueous phase and the oil phase could be separated by passing through a filter paper or a filter, and Pd could be recovered by heating the oil phase to remove the carbon component and the iodine component. In addition, the formation of the precipitate and the oil phase was influenced by the Pd concentration relative to the organic solvent and iodine, as compared with Example 13, and a precipitate was formed when the Pd concentration was high, and an oil phase was formed when the Pd concentration was low.

[0059] (Examples 15 to 17) Except for changing the concentration of NMP in the extraction solution to 100 g / L, 200 g / L, and 300 g / L, respectively, the same operation as in Example 1 was carried out. In Examples 15 to 17, a precipitate was formed and Au could be recovered.

[0060] (Example 18) The same operation as in Example 1 was carried out except that the potassium iodide, iodine, and NMP in the extraction solution were set to 26 g / L, 4 g / L, and 500 g / L, respectively, the amount of precious metal-containing waste to be immersed in the extraction solution was adjusted, and the Au concentration in the solution was set to 600 ppm. In this Example 18, a precipitate was also formed, and Au was able to be recovered.

[0061] (Example 19) The same operation as in Example 1 was performed except that the potassium iodide, iodine, and NMP in the extraction solution were set to 21 g / L, 3 g / L, and 600 g / L, respectively, and the amount of precious metal-containing waste immersed in the extraction solution was adjusted to set the Au concentration in the solution to 480 ppm. In this Example 19, an oil phase was produced. When the iodine concentration was relatively high, an oil phase was produced instead of a precipitate.

[0062] Comparative Example 1 The same operation as in Example 1 was carried out, except that the metal solution containing Au was not diluted (no water addition step) and only 0.4 times hydrochloric acid was added. As in Comparative Example 1, simply setting the pH to 1 or less did not produce either a precipitate or an oil phase, and a uniform single layer was formed overall, making it impossible to separate Au. It was found that a water addition step was necessary to produce a precipitate or an oil phase.

[0063] (Comparative Examples 2 and 3) The same operations as in Example 1 were carried out, except that the Au-containing metal solution was adjusted to pH 3 by adding 1 M hydrochloric acid (Comparative Example 2), or the pH was adjusted to pH 6 without adding hydrochloric acid (Comparative Example 3). In Comparative Examples 2 and 3, no precipitate or oil phase was formed, and only a uniform single layer was observed overall. It was confirmed that the formation of precipitate or oil phase requires pH adjustment to 2 or less.

[0064] Comparative Example 4 The same procedure as in Example 1 was carried out except that the extract did not contain an organic solvent. When no organic solvent was added to the extract, neither precipitation nor oil phase was formed. It was also confirmed that the amount of Au dissolved in the extract was low.

[0065] Comparative Example 5 The same operation as in Example 1 was carried out except that acetone not containing a lactam structure was used as the organic solvent added to the extract and the acetone concentration was set to 320 g / L. Although acetone has a ketone group like NMP, it does not contain a lactam structure, so neither precipitation nor an oil phase occurs. It was confirmed that a lactam compound is necessary as an organic solvent to cause precipitation or an oil phase.

[0066] Comparative Example 6 After adding 1M hydrochloric acid to the metal solution in which Pd was dissolved to adjust the pH to 1, the same operation as in Example 13 was carried out except that no ion-exchanged water was added (no water-adding step was performed). In this way, simply adjusting the pH to 1 or less did not produce either a precipitate or an oil phase, and only a uniform single layer was obtained overall. It was confirmed that a water-adding step was necessary to produce a precipitate or an oil phase.

[0067] Comparative Example 7 The same operation as in Example 13 was carried out, except that the pH was set to 6 without adding hydrochloric acid (no pH adjustment step) and the amount of ion-exchanged water added was 1.7 times the volume ratio of the metal solution. In this way, simply diluting the solution 2.7 times does not produce either a precipitate or an oil phase, and only a uniform aqueous phase is produced. It was confirmed that a pH adjustment step of adjusting the pH to 2 or less is necessary to produce a precipitate or an oil phase.

Claims

1. A method for producing a metal solution by immersing a material containing at least one of gold and palladium in an extracting solution containing an organic solvent, iodine, and potassium iodide; a pH adjustment step of adding an acid to the metal solution to adjust the pH to 2 or less; and a water addition step of diluting the metal solution by adding water to the metal solution to a volume of at least 2.7 times to generate an iodide of the precious metal, 2. A method for recovering precious metals, wherein the organic solvent contains a lactam compound.

2. The method for recovering precious metals according to claim 1, characterized in that the extraction solution contains iodine and potassium iodide, the concentration of the potassium iodide is 30 g / L or more, the concentration of the iodine is 5 g / L or more, and the concentration of the potassium iodide is higher than the concentration of the iodine.

3. 3. The method for recovering precious metals according to claim 1, wherein the concentration of the lactam compound contained in the extract is 100 g / L or more and 600 g / L or less.

4. 4. The method for recovering precious metals according to claim 1, wherein the water addition step is a step of reducing the concentration of the lactam compound contained in the extract to half or less.

5. 5. The method for recovering a precious metal according to claim 1, wherein the hydration step is a step of precipitating the iodide of the precious metal in the form of tabular crystals or needle crystals.

6. A method for recovering precious metals according to any one of claims 1 to 5, characterized in that the amount of precious metal contained in the precious metal iodide obtained in the hydration process is 90% or more of the amount of precious metal contained in the metal solution.

7. 7. The method for recovering precious metals according to claim 1, wherein the material containing precious metals is a circuit board.

Citation Information

Patent Citations

  • Nonaqueous-electrolyte battery

    JP1982061258A

  • Gold plating liquid and gold plating method

    JP2004043958A

  • Solution for dissolving noble metal, and method for dissolving / recovering noble metal with the use of the solution

    JP2005154892A

  • System for collecting gold while recycling iodine ion in gold-removing liquid

    JP2007016259A

  • Methods for recovering precious metals

    JP2571591B2

Cited By

  • Manufacturing methods for precious metals

    JP2026122591A