Grain-oriented electrical steel sheet and its manufacturing method

The method enhances grain-oriented electrical steel sheet production by aligning crystal grains with the rolling direction through controlled annealing and rolling stages, addressing yield and magnetic deviation issues, resulting in improved magnetic properties and productivity.

JP7569381B2Active Publication Date: 2024-10-17CLEANSOLUTION CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022538348
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-20
Filing Date
2020-12-17
Publication Date
2024-10-17
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheet production processes face challenges such as temperature differences between coil windings leading to magnetic deviations, surface defects during high-temperature annealing, and divided production stages that reduce yield, while continuous annealing limits the formation of exact Goss-oriented grains and hinders iron loss improvement.

Method used

A method involving hot rolling, primary and secondary decarburization annealing, and continuous annealing with controlled temperature increases and dew point temperatures, along with multiple cold rolling stages, to promote crystal grains aligned with the rolling direction, avoiding high-temperature phases and inhibitors like AlN and MnS, thus enhancing magnetic properties.

Benefits of technology

The method produces a grain-oriented electrical steel sheet with improved magnetic properties, reduced defects, and increased productivity by forming numerous crystal grains parallel to the rolling direction, achieving low iron loss and high magnetic flux density without the need for high-temperature heating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569381000003
    Figure 0007569381000003
  • Figure 0007569381000001
    Figure 0007569381000001
  • Figure 0007569381000002
    Figure 0007569381000002
Patent Text Reader

Abstract

A grain-oriented electrical steel sheet with improved magnetic properties and a manufacturing method thereof are provided. [Solution] A method for manufacturing a grain-oriented electrical steel sheet according to the present invention includes the steps of hot-rolling a slab to manufacture a hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet after annealing, first cold-rolling the hot-rolled steel sheet after the first cold-rolling, first decarburization annealing the steel sheet after the first cold-rolling, second cold-rolling the steel sheet after the decarburization annealing, second decarburization annealing the steel sheet after the second cold-rolling, and continuous annealing the steel sheet after the second decarburization annealing.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a grain-oriented electrical steel sheet having improved magnetic properties by including multiple cold rolling and decarburization annealing steps, and a manufacturing method thereof. [Background technology]

[0002] Grain-oriented electrical steel sheets are steel sheets with a crystal orientation of {110} <001> It is also known as a soft magnetic material that has excellent magnetic properties in the rolling direction and is made up of crystal grains with a Goss orientation.

[0003] Such grain-oriented electrical steel sheets are manufactured by rolling the slab to the final thickness through hot rolling, hot-rolling, annealing, and cold rolling after heating, and then undergoing primary recrystallization annealing and high-temperature annealing for secondary recrystallization formation.

[0004] Generally, the secondary recrystallization annealing process of grain-oriented electrical steel requires a low heating rate and long-term purification annealing at high temperature, which is a process that consumes a lot of energy. In order to manufacture grain-oriented electrical steel with excellent magnetic properties by forming secondary recrystallization through such an extreme process, the following difficulties arise in the process.

[0005] First, temperature deviation occurs between the outer and inner coil parts due to heat treatment in the coil state, and the same heat treatment pattern cannot be applied to each part, resulting in magnetic deviation between the outer and inner coil parts. Second, after decarburization annealing, MgO is coated on the surface and various surface defects occur in the process of forming a base coating during high-temperature annealing, reducing actual yield. Third, the production process is divided into three steps, as the decarburized sheet is wound into a coil, then high-temperature annealed, flattened again, and then insulated coated, resulting in a problem of reduced actual yield.

[0006] In order to overcome these process limitations, a technology has been proposed that utilizes normal crystal growth without secondary recrystallization by adjusting the decarburization annealing and cold rolling reduction rate. However, continuous annealing can cause the crystal orientation to change to {110} due to the short heat treatment time of water. <001> However, it was not possible to form a large number of grains with an exact Goss orientation that exactly matched the Goss orientation, and there was a limit to the improvement in iron loss. Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a grain-oriented electrical steel sheet having improved magnetic properties and a manufacturing method thereof, specifically, to provide a grain-oriented electrical steel sheet having improved magnetic properties by including multiple cold rolling and decarburization annealing steps, and a manufacturing method thereof. [Means for solving the problem]

[0008] In order to achieve the above object, a method for manufacturing a grain-oriented electrical steel sheet according to one aspect of the present invention includes the steps of hot rolling a slab to manufacture a hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet after the hot-rolled sheet annealing, first cold rolling the hot-rolled steel sheet after the first cold rolling, first decarburization annealing the steel sheet after the first cold rolling, second cold rolling the steel sheet after the decarburization annealing, second decarburization annealing the steel sheet after the second cold rolling, and continuous annealing the steel sheet after the second decarburization annealing. The method is characterized in that the temperature is increased in the temperature range of 950 to 1000° C. at a rate of 10° C. / sec or less after the secondary decarburization annealing step and before the continuous annealing step.

[0009] The slab preferably contains, by weight, 1.0% to 4.0% Si, 0.1% to 0.4% C, and the remainder being Fe and unavoidable impurities. The slab may further comprise Mn: 0.1 wt. % or less and S: 0.005 wt. % or less. The hot-rolled sheet annealing step may include a decarburization process. The hot-rolled sheet annealing step is preferably performed at a temperature of 850°C to 1000°C and a dew point temperature of 70°C or lower. The primary decarburization annealing step is preferably performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. The first decarburization annealing step is preferably performed in an austenite single phase region or a region where a composite phase of ferrite and austenite exists. After the first decarburization annealing step, the average diameter of the crystal grains may be 150 to 250 μm. It is preferable that the first decarburization annealing step and the second cold rolling step are repeated two or more times. The secondary decarburization annealing step is preferably performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. The secondary decarburization annealing step is preferably performed for 30 seconds to 5 minutes. In the continuous annealing step, annealing is preferably performed at a temperature of 1000° C. to 1200° C. and a dew point temperature of −20° C. or lower. The continuous annealing step is preferably performed for 30 seconds to 5 minutes. The continuous annealing step preferably includes a primary annealing step at 1000°C to 1100°C and a secondary annealing step at 1130°C to 1200°C.

[0010] In order to achieve the above object, a grain-oriented electrical steel sheet according to one aspect of the present invention has a grain-oriented electrical steel sheet in which 90% or more of all grains have a ratio (D2 / D1) of a circumscribing circle diameter (D1) to an inscribing circle diameter (D2) of 0.4 or more, <100> It is characterized by having 15% or more of crystal grains whose crystal orientation is parallel to the rolling direction (RD direction) of the steel plate at an angle of 5° or less.

[0011] The fraction of crystal grains having a grain size of 50 μm to 5000 μm among all the crystal grains may be 80% or more. <100> The crystal grains whose direction forms an angle of 10 to 15° with the rolling direction (RD direction) of the steel sheet may account for 30% or less. The grain-oriented electrical steel sheet according to one embodiment of the present invention preferably contains, by weight, 1.0% to 4.0% Si, 0.005% or less (excluding 0%) C, and the balance being Fe and unavoidable impurities. The grain-oriented electrical steel sheet according to one embodiment of the present invention may further contain Mn: 0.1% by weight or less and S: 0.005% by weight or less. Effect of the Invention

[0012] The grain-oriented electrical steel sheet according to the present invention utilizes normal crystal growth, <100> It is possible to form a large number of crystal grains whose direction is parallel to the rolling direction (RD) of the steel sheet, and the percentage of crystal grains with excellent sharpness of 5° or less is high, resulting in excellent magnetic properties. In addition, since AlN and MnS are not used as grain growth inhibitors, there is no need to heat the slab to high temperatures of 1300° C. or higher. In addition, there is no need to remove precipitates such as N and S, and the purification annealing time is relatively short, improving productivity. It is also possible to provide a grain-oriented electrical steel sheet having magnetic properties in which cracks are formed in the width direction. [Brief description of the drawings]

[0013] [Figure 1] 1 is a photograph of the surface of a grain-oriented electrical steel sheet manufactured using invention material 10, analyzed by EBSD. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below will be referred to as the second part, component, region, layer or section within the scope of the present invention.

[0015] The terminology used herein is merely for the purpose of describing particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. As used herein, the meaning of "comprising" embodies certain properties, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other properties, regions, integers, steps, operations, elements and / or components.

[0016] When an element is referred to as being "on" another element, this means that it is directly on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them.

[0017] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the currently disclosed content, and are not interpreted in an ideal or very formal sense unless defined.

[0018] Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight.

[0019] In one embodiment of the present invention, the term "additionally contain an additional element" means that the remaining iron (Fe) is replaced by an additional amount of the additional element.

[0020] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof so that those skilled in the art can easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.

[0021] A method for manufacturing a grain-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of hot rolling a slab to manufacture a hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet, hot-rolling the hot-rolled steel sheet after the hot-rolled sheet annealing, first cold rolling the hot-rolled steel sheet after the first cold rolling, first decarburization annealing the steel sheet after the first cold rolling, second cold rolling the steel sheet after the decarburization annealing, second decarburization annealing the steel sheet after the second cold rolling, and continuous annealing the steel sheet after the second decarburization annealing.

[0022] Each step will be explained in detail below.

[0023] First, the slab is hot rolled.

[0024] The slab contains, by weight, 1.0% to 4.0% Si, 0.1% to 0.4% C, and the remainder being Fe and unavoidable impurities.

[0025] The reasons for limiting the composition are as follows.

[0026] Silicon (Si) reduces the magnetic anisotropy of the electrical steel sheet, increases the resistivity, and improves the core loss. If the Si content is less than 1.0 wt%, the core loss is poor, and if it exceeds 4.0 wt%, the brittleness increases. Therefore, after the slab and final annealing stages, the Si content in the grain-oriented electrical steel sheet is 1.0-4.0 wt%. More specifically, the Si content may be 1.5-3.5 wt%.

[0027] Regarding carbon (C), since the Goss crystal grains in the surface layer diffuse to the center during intermediate decarburization annealing and final decarburization annealing, a process is required in which C in the center escapes to the surface layer, so the C content in the slab is 0.1 to 0.4 wt%. More specifically, the C content in the slab may be 0.15 to 0.3 wt%. Furthermore, the carbon content in the grain-oriented electrical steel sheet finally manufactured after the continuous annealing stage in which decarburization is completed is 0.0050 wt% or less. More specifically, it may be 0.002 wt% or less.

[0028] The slab may further comprise Mn: 0.1 wt. % or less and S: 0.005 wt. % or less.

[0029] Mn and S form MnS precipitates and impede the growth of Goss grains that diffuse to the center during the decarburization process. Therefore, it is preferable not to add Mn and S. However, taking into consideration the amount that inevitably gets mixed in during the steelmaking process, the Mn and S contents in the slab and grain-oriented electrical steel sheets after the final annealing stage are controlled to Mn: 0.1 wt% or less and S: 0.005 wt% or less, respectively.

[0030] The balance is composed of Fe and inevitable impurities. The inevitable impurities are impurities that are mixed in during the steelmaking stage and the manufacturing process of the grain-oriented electrical steel sheet, and are widely known in the art, so a detailed description will be omitted. Specifically, components such as Al, N, Ti, Mg, and Ca react with oxygen in the steel to form oxides, and therefore need to be strongly suppressed, so each component is controlled to 0.005 wt% or less. In one embodiment of the present invention, the addition of elements other than the above-mentioned alloy components is not excluded, and various elements are included within a range that does not impair the technical idea of ​​the present invention. When an additional element is further included, it is included in place of the balance Fe.

[0031] More specifically, the slab contains, by weight, 1.0% to 4.0% Si, 0.1% to 0.4% C, and the remainder being Fe and unavoidable impurities.

[0032] Before hot rolling the slab, the slab is heated. The heating temperature of the slab is 1100°C to 1350°C, which is higher than the usual heating temperature. If the temperature is high when heating the slab, the hot-rolled texture becomes coarse, which has a negative effect on magnetic properties. However, in the method for producing a grain-oriented electrical steel sheet according to an embodiment of the present invention, the carbon content of the slab is relatively high, so that even if the reheating temperature of the slab is high, the hot-rolled texture does not become coarse, and since the slab is reheated at a higher temperature than usual, it is more advantageous during hot rolling.

[0033] Hot rolling is performed to produce a hot-rolled sheet having a thickness of 1.5 to 4.0 mm so that the final product thickness can be produced by applying an appropriate rolling ratio in the final cold rolling stage. The hot rolling temperature and the cooling temperature are not particularly limited, but in one embodiment that provides excellent magnetic properties, the hot rolling end temperature is set to 950°C or less, and the steel is rapidly cooled with water and coiled at 600°C or less.

[0034] Next, the hot-rolled steel sheet is annealed. At this time, the hot-rolled steel sheet annealing may include a decarburization process. Specifically, the hot-rolled steel sheet is annealed at a temperature of 850°C to 1000°C and a dew point temperature of 70°C or less. After the above-mentioned annealing, additional annealing is performed at a temperature of 1000°C to 1200°C and a dew point temperature of 0°C or less. After the hot-rolled steel sheet annealing, the hot-rolled steel sheet is pickled.

[0035] Next, a first cold rolling is carried out to produce a cold-rolled steel sheet.

[0036] In the manufacturing process of a conventional grain-oriented electrical steel sheet, it is known that it is effective to perform cold rolling once with a high reduction rate of nearly 90%. This is because it creates an environment favorable for grain growth of only the Goss crystal grains in the primary recrystallized grains. However, the manufacturing method of a grain-oriented electrical steel sheet according to an embodiment of the present invention does not utilize the abnormal grain growth of the Goss oriented crystal grains, but instead reduces the surface layer defects generated by decarburization annealing and cold rolling. <100> The direction of the grains is parallel to the rolling direction (RD) of the steel plate, so in the surface layer <100> It is advantageous to form the steel sheet so that a large number of crystal grains are distributed parallel to the rolling direction (RD) of the steel sheet.

[0037] Therefore, when cold rolling is performed at a rolling reduction of 50% to 70%, a large amount of Goss texture is formed in the surface layer portion. More specifically, the rolling reduction may be 55% to 65%.

[0038] Next, the cold-rolled steel sheet is subjected to primary decarburization annealing. At this time, the decarburization annealing step is performed in the austenite single phase region or the region where a composite phase of ferrite and austenite exists. Specifically, annealing is performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. The atmosphere may be a mixed gas atmosphere of hydrogen and nitrogen. The amount of decarburization during the decarburization annealing may be 0.0300% by weight to 0.0600% by weight. After the above-mentioned annealing, additional annealing is performed at a temperature of 1000°C to 1200°C and a dew point temperature of 0°C or less.

[0039] During this primary decarburization annealing process, the crystal grains on the surface of the electrical steel sheet grow coarse, but the crystal grains inside the electrical steel sheet remain as a fine structure. The average diameter of the crystal grains after this primary decarburization annealing may be 150 μm to 250 μm. In this case, the crystal grains are ferrite crystal grains on the surface. The diameter of the crystal grains means the diameter of a virtual circle having the same area as the crystal grain. The reference plane is a plane parallel to the rolled surface (ND plane).

[0040] Next, the steel sheet that has been subjected to the first decarburization annealing is subjected to a second cold rolling. The second cold rolling is the same as the first cold rolling, so a detailed description thereof will be omitted.

[0041] The above-mentioned first decarburization annealing step and the second cold rolling step are repeatedly performed two or more times. <100> A large number of textures whose directions are parallel to the rolling direction (RD) of the steel sheet are formed in the surface layer.

[0042] Next, the steel sheet that has completed the second cold rolling undergoes secondary decarburization annealing.

[0043] The secondary decarburization annealing stage is annealed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C. The cold-rolled sheet before the secondary annealing is in a state where the decarburization annealing has progressed to the point where the carbon content is 40% to 60% of the weight of the carbon in the slab. Therefore, in the secondary decarburization annealing stage, the crystal grains formed in the surface layer diffuse inward as the carbon is released. In the secondary decarburization annealing stage, decarburization is carried out so that the carbon content in the steel sheet is 0.005% by weight or less.

[0044] The secondary decarburization annealing step is performed for 30 seconds to 5 minutes. Decarburization is sufficiently performed within the above-mentioned time range.

[0045] Next, the steel sheet that has been subjected to secondary decarburization annealing is subjected to continuous annealing.

[0046] In the heating step after the secondary decarburization annealing step and before the continuous annealing step, the temperature range is 950-1000°C, and the heating rate is 10°C / sec or less. By controlling the heating rate to a low level in this manner, the selectivity of the orientation that facilitates crystal growth is increased in the crystal growth process after the decarburization annealing is completed. This is because when a high heating rate is applied, the rapid supply of thermal energy does not allow enough time for selective growth according to the peculiar crystal orientation of each crystal grain, and crystal grains of various orientations all grow. According to the composition and characteristics of the cold-rolled steel sheet of the present invention, <100> Since crystal grains whose direction is parallel to the rolling direction (RD) of the steel plate tend to grow, it can be said that an appropriate heating rate is necessary for their selective growth. <100> Among the grains whose direction is parallel to the rolling direction (RD) of the steel sheet, many grains with a deviation of 5° or less are formed. <100> / / The number of crystal grains that form angles of 10 to 15 degrees among the RD crystal grains is small. More specifically, the temperature range is 950 to 1000°C, and the heating rate is 3 to 8°C / sec.

[0047] The continuous annealing stage is performed at a temperature of 1000℃~1200℃ and a dew point temperature of -20℃ or less. The purpose of the continuous annealing stage is to grow the carbon in the steel to a certain size after decarburization. The reason is that the decarburization and the subsequent grain growth process continue to grow. <100> This is because the fraction of crystal grains whose direction is parallel to the rolling direction (RD) of the steel plate increases.

[0048] The continuous annealing step is performed for 30 seconds to 5 minutes.

[0049] In the time range mentioned above <100> The growth of crystal grains parallel to the rolling direction (RD) of the steel plate is sufficiently achieved.

[0050] After the first cold rolling step, the process is carried out continuously up to the continuous annealing step. A continuous process means that there is no batch process in which the steel sheet is wound into a coil and annealed. As mentioned above, the decarburization annealing step and the continuous annealing step can be completed in a few minutes, making this a continuous process.

[0051] The continuous annealing step includes a primary annealing step at 1000° C. to 1100° C. and a secondary annealing step at 1130° C. to 1200° C. Each of the primary annealing step and the secondary annealing step is performed for 30 seconds to 2 minutes.

[0052] In this way, the continuous annealing step has the advantage of lowering the average heating rate by applying two-step soaking temperature. In particular, by adjusting the soaking temperature in the first annealing step to a relatively low temperature, the decarburization annealing <100> When the selective growth of grains parallel to the rolling direction (RD) of the steel plate is completed, <100> The advantage of this method is that it gives additional selective growth of crystal grains whose direction is parallel to the rolling direction (RD) of the steel sheet. As mentioned above, when the temperature is increased rapidly, sufficient time cannot be given for selective growth due to the special crystal orientation of each crystal grain, whereas when the temperature is increased relatively slowly, the selective growth due to the special crystal orientation of the test piece after decarburization annealing in the present invention can be obtained. <100> This is because it is possible to maximize the selective growth of crystal grains whose direction is parallel to the rolling direction (RD) of the steel sheet.

[0053] In the grain-oriented electrical steel sheet finally manufactured after the continuous annealing step, 90% or more of the crystal grains have a ratio (D2 / D1) of 0.4 or more between the diameter of the circumscribing circle (D1) and the diameter of the inscribing circle (D2). This is because the secondary decarburization annealing and the continuous annealing are performed for a short period of time, as described above. When annealing is performed for a long period of time, such as one hour or more, by batch annealing as in the past, the diameter of the circumscribing circle (D1) becomes much larger than the diameter of the inscribing circle (D2), and the ratio does not become 0.4 or more. Here, the circumscribing circle means the smallest circle among the imaginary circles surrounding the outside of the crystal grain, and the inscribing circle means the largest circle among the imaginary circles included inside the crystal grain. More specifically, 95% or more of the crystal grains may have a ratio (D2 / D1) of 0.4 or more between the diameter of the circumscribing circle (D1) and the diameter of the inscribing circle (D2). More specifically, 95% to 99% of all crystal grains may have a ratio (D2 / D1) of the circumscribing circle diameter (D1) to the inscribing circle diameter (D2) of 0.4 or more.

[0054] In addition, the final manufactured grain-oriented electrical steel sheet is <100> Many grains are formed whose orientation is parallel to the rolling direction (RD) of the steel sheet at 5° or less. <100> The number of crystal grains whose orientation forms an angle of 10 to 15 degrees with the rolling direction (RD) of the steel sheet is small. <100> The crystal grains whose orientation is parallel to the rolling direction (RD direction) of the steel plate is 15% or more. <100> The crystal grains whose orientation forms an angle of 10 to 15 degrees with the rolling direction (RD direction) of the steel sheet may be 30% or less. <100> The formation of a large number of crystal grains with accurate orientation contributes to improving magnetic properties. More specifically, <100> The crystal grains having an orientation parallel to the rolling direction (RD direction) of the steel sheet at an angle of 5° or less may account for 15% to 30%. <100> The proportion of crystal grains whose orientation forms an angle of 10 to 15° with the rolling direction (RD direction) of the steel sheet may be 5% to 30%.

[0055] The area fraction of crystal grains with a grain size of 50 μm to 5000 μm in the entire crystal grains is preferably 80% or more. This is because, as described above, the secondary decarburization annealing and continuous annealing are performed for a short period of time. When annealing is performed for a long period of time of 1 hour or more by batch annealing as in the past, the average grain size becomes larger by 5 mm or more, which is completely different from the grain size distribution of the grains in the grain-oriented electrical steel sheet according to one embodiment of the present invention. More specifically, the fraction of crystal grains with a grain size of 50 μm to 5000 μm in the entire crystal grains may be 90% or more. More specifically, the fraction of crystal grains with a grain size of 50 μm to 5000 μm in the entire crystal grains may be 90% to 99%.

[0056] In the grain-oriented electrical steel sheet according to one embodiment of the present invention, 90% or more of all crystal grains have a ratio (D2 / D1) of the circumscribing circle diameter (D1) to the inscribing circle diameter (D2) of 0.4 or more.

[0057] <100> The crystal grains whose orientation is parallel to the rolling direction (RD direction) of the steel plate is 15% or more.

[0058] <100> It is preferable that the proportion of crystal grains whose orientation forms an angle of 10 to 15° with the rolling direction (RD direction) of the steel sheet is 30% or less.

[0059] It is preferable that the percentage of crystal grains having a grain size of 50 μm to 5000 μm among all the crystal grains is 80% or more.

[0060] The orientation, shape and size of crystal grains have been described in detail in relation to the manufacturing method of grain-oriented electrical steel sheet, so duplicated description will be omitted.

[0061] The electrical steel sheet contains, by weight, 1.0% to 4.0% Si, 0.005% or less (except 0%) C, and the balance being Fe and unavoidable impurities.

[0062] The electrical steel sheet may further contain Mn: 0.1% by weight or less and S: 0.005% by weight or less.

[0063] Except for C, the compositional limitations are the same as those for slabs, so duplicate explanations will be omitted.

[0064] The grain-oriented electrical steel sheet according to an embodiment of the present invention has a high percentage of crystal grains with excellent sharpness of 5° or less, and has excellent magnetic properties.

[0065] Specifically, iron loss (W 17 / 50 ) is 1.55W / kg or less. More specifically, the iron loss (W 17 / 50 ) may be 1.00 to 1.50 W / kg. More specifically, it may be 1.10 to 1.50 W / kg. Iron loss W 17 / 50 is the magnitude of iron loss (W / kg) induced at 1.7 Tesla and 50 Hz.

[0066] In addition, the magnetic flux density (B8) is equal to or greater than 1.83 T. Specifically, the magnetic flux density (B8) may be 1.85 to 2.00 T. More specifically, it may be 1.87 to 1.95 T.

[0067] Magnetic flux density B8 is the magnetic flux density induced in a magnetic field of 800 A / m.

[0068] Hereinafter, specific examples of the present invention will be described. However, the following examples are merely specific examples of the present invention, and the present invention is not limited to the following examples.

[0069] Example 1 A slab containing, by weight, 2.0% Si, 0.20% C, with the balance being Fe and unavoidable impurities, was heated at a temperature of 1250°C, hot rolled, and then hot-rolled at an annealing temperature of 950°C and a dew point temperature of 60°C. After that, the steel sheet was cooled, pickled, and cold-rolled at a reduction ratio of 50% to produce a cold-rolled sheet with a thickness of 1.4 mm.

[0070] The cold-rolled sheet was again subjected to decarburization annealing (1st stage), pickled and cold-rolled at a reduction of 54% to produce a cold-rolled sheet with a thickness of 0.65 mm. It was then decarburized annealed (2nd stage) at 950℃ in a wet mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60℃) and cold-rolled again to produce a cold-rolled sheet with a thickness of 0.282 mm.

[0071] Then, for the final annealing, decarburization annealing (third) was performed for 2 minutes in a wet mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60°C) at an ambient temperature of 950°C. Then, for crystal growth annealing, heat treatment was performed by dwelling for 60 seconds at the first soaking temperature summarized in Table 1 below, and then dwelling for 60 seconds at 1130°C. The heating rate and <100> The crystal grain fraction whose direction is parallel to the rolling direction (RD) of the steel sheet was classified by deviation of 0° to 5° and 10° to 15° by EBSD measurement, and is summarized in Table 1 below.

[0072] In addition, the area fractions of crystal grains with a ratio (D2 / D1) of the circumscribing circle diameter (D1) to the inscribing circle diameter (D2) of 0.4 or more and crystal grains with grain sizes of 50 μm to 5000 μm were analyzed by EBSD and are summarized in Table 1 below.

[0073] [Table 1]

[0074] As shown in Table 1, when the heating rate in the 950-1000°C range during the final annealing process is controlled to 10°C / s or less, the crystal grain orientation has a deviation of 5° or less, which is favorable for magnetic properties. <100> A large number of crystal grains are formed whose orientation is parallel to the rolling direction (RD) of the steel plate.

[0075] FIG. 1 shows a photograph of the surface of a grain-oriented electrical steel sheet manufactured using the invention material 10, analyzed by EBSD. <100> Grains whose orientation is parallel to the rolling direction of the steel sheet were classified using different colors at 5° intervals.

[0076] Example 2 A slab containing, by weight, 2.52% Si, 0.195% C, with the balance being Fe and unavoidable impurities, was heated at a temperature of 1220°C, hot rolled, and then hot-rolled at an annealing temperature of 950°C and a dew point temperature of 60°C. After that, the steel sheet was cooled, pickled, and cold-rolled at a reduction ratio of 60% to produce a cold-rolled sheet with a thickness of 0.9 mm.

[0077] The cold-rolled sheet was subjected to decarburization annealing (first step) at 950°C in a wet mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60°C), and then cold-rolled again to produce a cold-rolled sheet with a thickness of 0.35 mm.

[0078] Then, decarburization annealing (secondary) was performed for 150 seconds in a wet mixed gas atmosphere of hydrogen and nitrogen (dew point temperature 60°C) at an ambient temperature of 950°C. Then, for crystal growth annealing, heat treatment was performed at the primary soaking temperature summarized in Table 2 below. Heat treatment was performed for 60 seconds at each residence, and the heating rate and <100> The grain fraction in the / / RD direction was classified according to deviations of 0° to 5° and 10° to 15° based on EBSD measurements, and is summarized in Table 2 below.

[0079] In addition, the area fractions of crystal grains with a ratio (D2 / D1) of the circumscribing circle diameter (D1) to the inscribing circle diameter (D2) of 0.4 or more and crystal grains with grain sizes of 50 μm to 5000 μm were analyzed by EBSD and are summarized in Table 2 below.

[0080] [Table 2]

[0081] table 2 As shown in Fig. 1, even during continuous annealing processes with different Si and C contents, rolling times, and cold-rolled sheet thicknesses, when starting heat treatment for crystal growth, if a low crystal growth rate is set at the beginning of crystal growth, that is, the heating rate in the 950-1000°C range is set to 10°C / s or less, a crystal orientation favorable for magnetic properties is formed.

[0082] The present invention is not limited to the above-described embodiments and / or examples, and can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-described embodiments and / or examples are illustrative in all respects and not limiting.

Claims

1. hot rolling the slab to produce a hot rolled steel sheet; annealing the hot-rolled steel sheet; performing a first cold rolling on the hot-rolled steel sheet that has been annealed; subjecting the first cold-rolled steel sheet to a first decarburization annealing; subjecting the steel sheet having undergone the decarburization annealing to a second cold rolling; subjecting the steel sheet having undergone the second cold rolling to a second decarburization annealing; and subjecting the steel sheet that has been subjected to the secondary decarburization annealing to continuous annealing, In the heating step after the second decarburization annealing step and before the continuous annealing step, the temperature is heated to a temperature range of 950 to 1000 ° C. at a rate of 8 ° C. / sec or less; The slab contains, by weight, Si: 1.0% to 4.0%, C: 0.1% to 0.4%, and S: 0.005% or less, with the balance being Fe and unavoidable impurities; The first decarburization annealing step is performed at a temperature of 850° C. to 1000° C. and a dew point temperature of 50° C. to 70° C. After the second decarburization annealing step, no batch annealing is performed, The grain-oriented electrical steel sheet thus produced has a ratio (D2 / D1) of the circumscribed circle diameter (D1) to the inscribed circle diameter (D2) of 0.4 or more in all grains, and The crystal grains having a <100> orientation parallel to the rolling direction (RD direction) of the steel sheet at an angle of 5° or less account for 15% by area or more; A method for producing a grain-oriented electrical steel sheet, characterized in that crystal grains whose <100> direction forms an angle of 10 to 15 degrees with the rolling direction (RD) of the steel sheet account for 30 area % or less.

2. The method for producing a grain-oriented electrical steel sheet according to claim 1, wherein the step of annealing the hot-rolled sheet includes a decarburization process.

3. 3. The method of claim 1, wherein the hot-rolled sheet is annealed at a temperature of 850° C. to 1000° C. and a dew point temperature of 70° C. or less.

4. 4. The method for producing a grain-oriented electrical steel sheet according to claim 1, wherein the step of subjecting the primarily cold-rolled steel sheet to primary decarburization annealing comprises annealing the steel sheet in an austenite single phase region or in a region where a composite phase of ferrite and austenite exists.

5. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 4, wherein the average diameter of crystal grains is 150 to 250 μm after the step of subjecting the primarily cold-rolled steel sheet to a primary decarburization annealing.

6. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 5, wherein the first decarburization annealing step and the second cold rolling step are repeated two or more times.

7. The method of claim 1, wherein the secondary decarburization annealing is performed at a temperature of 850°C to 1000°C and a dew point temperature of 50°C to 70°C.

8. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 7, wherein the secondary decarburization annealing is performed for 30 seconds to 5 minutes.

9. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 8, wherein the continuous annealing step comprises annealing at a temperature of 1000°C to 1200°C and at a dew point temperature of -20°C or lower.

10. The method for producing a grain-oriented electrical steel sheet according to any one of claims 1 to 9, wherein the continuous annealing step comprises annealing for 30 seconds to 5 minutes.

11. The method for manufacturing a grain-oriented electrical steel sheet according to any one of claims 1 to 10, wherein the continuous annealing step includes a first annealing step at 1000°C to 1100°C and a second annealing step at 1130°C to 1200°C.

12. The ratio (D2 / D1) of the circumscribing circle diameter (D1) to the inscribing circle diameter (D2) of 0.4 or more in the entire crystal grains is 90% or more by area, The crystal grains having a <100> orientation parallel to the rolling direction (RD direction) of the steel sheet at an angle of 5° or less account for 15% by area or more; The crystal grains having a <100> direction that forms an angle of 10 to 15 degrees with the rolling direction (RD direction) of the steel sheet account for 30% by area or less, A grain-oriented electrical steel sheet comprising, by weight%, 1.0% to 4.0% Si, 0.005% or less (excluding 0%) C, 0.005% or less S, and the balance being Fe and unavoidable impurities.

13. The grain-oriented electrical steel sheet according to claim 12, characterized in that the fraction of crystal grains having a grain size of 50 μm to 5000 μm in the total crystal grains is 80 area % or more.

Citation Information

Patent Citations

  • Method for preparing low-cost oriented silicon steel by utilization of continuous annealing

    CN104846177A

  • Production of grain-oriented magnetic steel sheet excellent in magnetic property

    JP1994306473A

  • Production of high magnetix flux density grain oriented silicon steel sheet excellent in magnetic property and film property

    JP1995097631A

  • Grain oriented silicon steel sheet excellent in magnetic property, and its production

    JP2000026942A

  • Divided core for motor

    JP2011026682A