Electron beam measurement device and electron beam measurement method

The electron beam measuring device minimizes resist shrinkage by selectively irradiating edges of the pattern, enabling precise and reliable measurements in semiconductor devices.

JP7569432B2Active Publication Date: 2024-10-17HORON CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023176576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2024-10-17
Estimated Expiration
2038-10-02

AI Technical Summary

Technical Problem

Conventional electron beam measurement methods cause resist shrinkage in semiconductor devices, leading to poor measurement accuracy and device defects, especially as feature sizes approach 10 nm, making precise length measurement without shrinkage impossible.

Method used

An electron beam measuring device that scans only necessary locations on the resist structure, using signal electrons to automatically set the electron beam irradiation range and generate an electron beam OFF signal at predetermined intervals to minimize irradiation and shrinkage.

Benefits of technology

The method significantly reduces resist shrinkage by irradiating the electron beam only at the edges of the pattern, allowing for accurate and reproducible measurements without damaging the resist structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569432000001
    Figure 0007569432000001
  • Figure 0007569432000002
    Figure 0007569432000002
  • Figure 0007569432000003
    Figure 0007569432000003
Patent Text Reader

Abstract

PURPOSE: To provide an electron beam measurement device and an electron beam measurement method, which involve blocking an electron bream in real time after a predetermined period of time from real-time detection of an edge of a peak, thereby preventing irradiation to a pattern to prevent damage and shrinkage of the pattern.CONSTITUTION: An electron beam measurement device disclosed herein comprises: scanning means for scanning a lightly focused electron beam on a resist pattern obtained by replacing an organic solvent that evaporates in vacuum contained in a measurement target resist pattern with an ionic liquid that does not evaporate in vacuum; and measurement means for making measurement based on a signal waveform acquired by the scanning made by the scanning unit. Reducing evaporation of the organic solvent of the resist pattern in vacuum causes a reduction in shrinkage.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electron beam measurement apparatus and method for measuring the dimensions and area of ​​a pattern of a distance measurement target formed on a sample or extracting the contour of the pattern. [Background technology]

[0002] For nearly half a century, the minimum feature size of semiconductor devices has been shrinking year by year, and with each new process development, devices with higher transistor density are being created. This has enabled a dramatic reduction in the cost per unit transistor. Today, devices with billions of transistors packed into a 1 cm2 chip can be purchased for just a few tens of thousands of yen, and computers with performance far exceeding that of conventional mainframe computers can now be realized inside smartphones.

[0003] This principle of economic expansion through shrinking feature sizes, commonly known as Moore's Law, has kept the semiconductor industry thriving for over half a century.

[0004] Currently, devices with minimum dimensions on the order of 10 nm are being developed and used, and the trend for transistors to become smaller is expected to continue to 7 nm, 5 nm, and 3 nm in the future.

[0005] Lithography, an exposure technique for printing wiring patterns, is important for manufacturing small transistors on silicon wafers on which semiconductor devices are made. Since the limit of microfabrication depends on the wavelength of the light used for exposure, efforts have been made to shorten the wavelength.

[0006] Currently, double or triple exposure using ArF 193 nm light or exposure using EUV 13.5 nm light are mainly used. Nanoimprint and Directed Self-Assembly (DSA) are also used as nm-order miniaturization processes that do not use exposure technology but use resists with a similar chemical composition.

[0007] The generation efficiency of short-wavelength laser light sources such as ArF or EUV used in exposure equipment is very low, so the amount of laser light finally obtained is also small. For example, with an EUV light source, only 1% of the input energy becomes EUV light, and only about 1% of that reaches the wafer surface and is used for actual exposure. More specifically, a pumping laser of several tens of kilowatts is used to generate EUV light of several hundred watts, and finally, light of several watts reaches the wafer. Therefore, if a normal low-sensitivity resist is used, the exposure time is too long, resulting in a significant decrease in throughput. Therefore, a high-sensitivity resist called a chemically amplified resist has been developed and is used, which can be exposed with weak light in the same exposure time as conventional resists and improve throughput.

[0008] A typical chemically amplified resist is based on esterified methacrylic acid resin and contains a photoacid generator (PAG) that generates an acid that acts as a reaction catalyst to increase sensitivity. When the resist is exposed to light, acid is generated, accelerating the decomposition reaction of the resist and increasing sensitivity. In addition to onium salts, other known photoacid generators include nitrobenzyl esters, diazomethane, and triazines.

[0009] In the positive type, the acid labile protecting group that protects the alkali soluble group of the alkali soluble resin undergoes a deprotection reaction with the acid as a catalyst by heating in the post-exposure bake (PEB), and the polarity of the resin changes from alkali insoluble to alkali soluble, resulting in a positive pattern after development with an alkaline solution. The alkali soluble group is a phenolic hydroxyl group or a carboxyl group, and the acid labile protecting group is tert-butyl tert-butoxycarbonyl (t-Boc) or a tetrahydropyranyl group. In the negative type, the alkali soluble resin and the crosslinking agent undergo a crosslinking reaction with the acid as a catalyst by heating in the post-exposure bake, changing from alkali soluble to alkali insoluble, resulting in a negative pattern after development with an alkaline solution. The crosslinking agent used is hexamethoxymethylmelamine or tetramethoxyglycoluryl (TMCU). In either case, the reaction proceeds with the acid as a catalyst, resulting in a resist with extremely high sensitivity compared to conventional resists.

[0010] On the other hand, such chemically amplified resists have a sensitivity amplification mechanism due to acid generation as mentioned above, so even electron beam irradiation, which is unrelated to light exposure, generates acid in the resist, which decomposes the resist and causes the resist to shrink. For example, it is known that when a resist structure containing the above-mentioned materials is irradiated with an electron beam converged to a few nm in order to perform length measurements with a CDSEM, the resist shrinks at the irradiated area, resulting in a difference in length and structure from the original. This problem has been widely recognized for many years as an obstacle to precise length measurements of resist structures using CDSEM, but a major challenge remains in that a method for CD measurement without shrinkage has not yet been found.

[0011] Currently, in major manufacturers' wafer CDSEMs, etc., a method is widely used in which, based on the premise that resist shrink of several nm to several tens of nm naturally occurs when measuring length using an electron beam, the dimensions when not irradiated with an electron beam are estimated or predicted from the results of multiple consecutive measurements of the same measurement location. DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0012] However, as mentioned above, as a result of the miniaturization of semiconductor devices, the minimum width of the resist structure is now on the order of 10 nm, and shrinkage of a few nm causes random dimensional changes of 10% or more of the main body dimensions, which not only results in a loss of dimensional measurement accuracy, but also has a major impact on device characteristics.Furthermore, it has become a major problem in that defects may occur due to SEM observation.

[0013] Therefore, the conventional method of estimating the dimensions after the resist has actually shrunk and before the electron beam is irradiated is no longer meaningful, and CDSEM measurements, which are originally performed to improve yields, are now even causing a drop in the yield of device manufacturing. This has become a major problem in that although TEGs (test element groups) can be measured, it is impossible to measure devices or elements that actually function.

[0014] Therefore, in consideration of the issues and defects of conventional measurement methods using electron beams, the present invention proposes a measurement method and SEM observation method that introduces a method that is completely opposite to the conventional CDSEM measurement concept, essentially reducing the shrinkage of the resist itself or preventing it from occurring, and that allows accurate and highly reproducible measurement of the resist dimensions of actually operating devices or does not reduce yield. [Means for solving the problem]

[0015] The present invention provides an electron beam measurement device for extracting the dimensions, area measurement or contour of a pattern of a distance measurement target formed on a sample, comprising a setting means for setting a partial scanning area including the edge of the pattern of the distance measurement target, a detection means for scanning an electron beam over the partial scanning area to detect the generated electrons to obtain a partial scanning image, and for detecting the edges of the pattern in real time during the acquisition, an electron beam OFF signal generating means for detecting the edge in real time by the detection means and generating an electron beam OFF signal in real time after a predetermined interval has elapsed, and an electron beam blocking means for blocking the electron beam in real time when the electron beam OFF signal generating means generates the electron beam OFF signal in real time to block irradiation of the pattern, so as to automatically obtain the minimum image required for measurement.

[0016] At this time, edge extraction is performed on each of the partial scan images acquired facing the measurement target pattern, and the distance between the opposing edges of the pattern is obtained from the respective edge position information.

[0017] In addition, edge extraction is performed on the partial scan image acquired from the measurement target pattern, and the contour of the measurement target pattern is extracted.

[0018] In addition, the specified interval is set to an interval corresponding to N scan lines (an integer) when the electron beam is scanned parallel to the edge of the pattern to be measured, or an interval corresponding to M pixels (an integer) of the scan line when the electron beam is scanned perpendicular to the edge of the pattern to be measured.

[0019] The pattern to be measured is a resist pattern or a pattern that is reduced by electron beam irradiation. Effect of the Invention

[0020] The feature of the present invention is that it is completely opposite to the conventional method, and basically measures the width and length of a resist structure without irradiating the resist structure (pattern) with an electron beam. In particular, the present invention has a major feature in that it can automatically set the electron beam scanning area to a very narrow range used for measurement using signal electrons obtained from the structure.

[0021] In conventional measurement or inspection methods using electron beams, an electron beam focused to the nm order is scanned thoroughly over the entire area of ​​the FOV, which ranges from several microns to several mm and includes the resist structure, to obtain an image. Parts in the obtained image where the brightness changes significantly are defined as the edges of the structure, and the distance between those edges is calculated to perform length measurement or shape recognition.

[0022] This invention uses a technology that reduces measurement time by irradiating the electron beam only to the necessary places on the measurement target. By using this technology, it is possible to irradiate the electron beam only to the edge of the resist, making it possible to reduce shrinkage. For example, for a line pattern with a width of about 100 nm, it is possible to measure by irradiating the electron beam only to an area with a width of about 10 nm that constitutes the edge. In this way, resist shrinkage can be made much smaller than when the electron beam is irradiated to the entire line.

[0023] However, because there is error in the line formation position, it is extremely difficult to quickly and accurately irradiate and measure only the edge parts of a line pattern, which has a line width on the order of 10 nm, with an electron beam while relying only on positions that are determined in advance by the design (CAD data).

[0024] Therefore, the present invention utilizes a caliper-like measurement method for an electron beam. In other words, the electron beam scan is mainly performed in the area outside the boundary created by the resist structure to be measured, and the length is measured by sandwiching the structure. In particular, the present invention has a major feature in that the range to be irradiated with the electron beam is automatically set (self-aligned ESR) by using the signal electrons obtained from the structure to match the edge position of the line actually formed using CAD data as a guide.

[0025] In other words, the major feature of this method is that it has a novel electron beam scanning method that uses the signal electrons generated from the structure irradiated with the electron beam in real time during measurement to instantly modulate the ongoing electron beam scanning method or change the measurement method (real-time measurement). This makes it possible to automatically change the scanning method according to changes in the signal (electrons, electromagnetic waves, heat, etc.) generated as a result of irradiating the object to be measured.

[0026] As a more specific example, a major feature of this method is that it uses signal electrons from the structure of the object to be measured to recognize the boundary of a pattern on the object to be measured, and blanks or stops the electron beam being irradiated to the object to be measured, thereby reliably protecting the object to be measured. BEST MODE FOR CARRYING OUT THEINVENTION

[0027] The present invention sets partial scanning areas each including opposing edges of a pattern to be measured for distance, scans the partial scanning areas with an electron beam, detects the generated electrons, and acquires the partial scanning image.After detecting the peak of the edge existing at the boundary from the outside to the inside of the pattern in real time, an electron beam OFF signal is generated in real time after a predetermined interval has elapsed, and irradiation of the electron beam onto the pattern is blocked in real time, thereby automatically acquiring only the minimum amount of images required for measurement, thereby suppressing irradiation of the pattern and preventing damage and shrinkage of the pattern. Example 1

[0028] The embodiments of the present invention will be described in detail below. (1) The electron beam scan starts from a position where there is no resist structure based on CAD data, and the scanning position is gradually moved toward the boundary with the resist structure. Secondary electrons or reflected electrons generated from the object to be measured as a function of the scanning position are detected, and their intensity is converted into a digital value and then recorded in a semiconductor memory or a storage device. (2) Since the intensity and emission direction of secondary electrons or reflected electrons in areas without resist structures differ from those in areas with resist, it is possible to automatically distinguish between resist areas and areas other than resist by setting an appropriate threshold value using the intensity signal difference or emission direction difference, and to decide to stop electron beam irradiation as soon as the electron beam enters the resist area or to stop after scanning N pixels. The signal waveform acquired up until the end of scanning is stored as one block in a storage device such as a memory. (3) The key point is that since the area without resist does not affect the measurement target no matter how much the electron beam is scanned, the above process can be repeated as many times as necessary to obtain the required image SNR, and an image with a very high SNR can be obtained. As a result of this characteristic, it is possible to suppress the noise floor to a very low level, and it is possible to detect a small signal that represents a boundary that protrudes slightly above the noise floor, making it easy to distinguish between the resist area and other areas, which is the basic principle of the present invention. In addition, the interval at which the electron beam is scanned may be controlled to approach the resist structure in the shortest time and with the greatest efficiency by using a learning function such as AI to learn the relationship between the interval and the waveform change.

[0029] The above mechanism makes it possible to automatically obtain the minimum number of images required for measurement in small areas that would not be possible using CAD data alone.

[0030] FIG. 1 shows a system configuration diagram of the present invention.

[0031] In Fig. 1, the electron gun 1 generates and reduces an electron beam, and the electron generating source can be a thermionic electron source using a W filament, a Schottky type using ZrO, a cold emitter made of electrolytically polished W, a cold field emitter made using micromachining technology, a CNT cathode, LaB6, a photoexcited emitter (photocathode), etc. It is a well-known device composed of an accelerating electrode that accelerates the generated electrons to a desired energy.

[0032] The aperture 2 is a circular stop that passes the central portion (within a predetermined solid angle) of the electron beam emitted from the electron gun 1 and blocks the rest, and here, can be automatically switched to a plurality of hole diameters. A stepping motor, a servo motor, an ultrasonic motor using a piezoelectric element, a shape memory alloy, or the like can be used as a moving means for changing the aperture diameter. The illustrated aperture 2 is placed above CL3, but is not limited to this, and may be placed on the main surface (center of the lens) or below CL3.

[0033] The CL (condenser lens) 3 is a known lens that converges the electron beam that is emitted from the electron gun 1 and passes through the center of the aperture 2. The CL 3 shown in the figure is shown diagrammatically, and is actually composed of a magnetic lens or an electrostatic lens.

[0034] The blanking electrode 13 is used together with the blanking aperture 14 to turn on / off the electron beam according to a signal from the automatic blanking control device 11 to determine whether or not the electron beam is irradiated onto the sample 8. To enable ultra-high speed operation, the blanking electrode 13 is designed to have as small a capacitance between the electrodes as possible. Also, it is advisable to place the blanking aperture 14 at the location where the electron beam is converged so that complete blanking can be achieved by applying a small voltage.

[0035] The automatic blanking control means 11 is a device that receives a secondary electron or reflected electron signal generated by the electron beam scanning in the sample 8, detects a large change in the sample structure or a change in the constituent material (e.g., an edge) at ultra-high speed, automatically generates a blanking signal, and prevents the electron beam from being irradiated to the resist structure. As described above, the location where the electron beam irradiation actually starts to stop can be set to any pixel (or line) after receiving the signal. CAD data that determines the design dimensions and layout of the structure can also be used to determine this ON / OFF. For example, when a certain amount of electron beam scanning enters the range of the resist structure defined by the CAD data, blanking is performed automatically or forcibly to completely protect the resist structure. In the above example, an example of blanking using signal electrons generated by the sample is shown, but it is also possible to control so that the resist does not actually shrink by changing the scanning interval, current amount, or duty of the irradiated electron beam in response to a signal from the measurement target.

[0036] The blanking device 12 applies a voltage to a blanking electrode 13 based on a signal from the automatic blanking control means 11, thereby blocking the electron beam.

[0037] The blanking aperture 14 is an aperture that blocks the electron beam deflected by the blanking electrode 13 .

[0038] DEF(1)4 and DEF(2)5 represent two-stage deflectors, which are electrostatic deflectors with opposing electrodes, and irradiate the electron beam 111, narrowed to the nm order, onto the sample 8 while performing planar scanning (scanning in the X and Y directions). It is desirable for this deflector to be designed with small electrode capacitance and high-speed response so that the electron beam can be scanned only where it is needed. It is also possible to use a two-stage magnetic deflector specially designed to have small hysteresis.

[0039] MCP6 is an example of a secondary electron detector, which detects the secondary electrons emitted when the electron beam is irradiated onto the sample 8 and scanned in a plane, and has a positive voltage applied to the front. The detector can be any currently available detector, including MCP, scintillator, PIN diode, APD, MPPC, and other semiconductor detectors. In order to perform boundary detection in real time, it is desirable to accelerate the secondary electrons generated on the sample surface to minimize delays. For this purpose, it is advisable to apply an accelerating electric field between the sample and the electron detector. Naturally, it is desirable to amplify the signal using an amplifier capable of ns frequency response.

[0040] The objective lens 7 is used to focus the electron beam 111 on the sample 8 to a fine focal length of nm and is usually a magnetic objective lens. Of course, it can also be configured with an electrostatic lens. To reduce the objective lens aberration, it is also possible to use a method in which highly accelerated electrons are injected into the objective lens and a reverse bias is applied to the sample to brake the electron beam and control the landing energy of the electron beam (the so-called retarding method or intermediate acceleration method). The sample 8 is a sample with a resist pattern (such as a photomask or a semiconductor wafer) fixed on a stage 9.

[0041] The stage 9 fixes the sample 8 and moves it to a predetermined location while a length measuring device 27 precisely measures the coordinate positions in the X and Y directions.

[0042] The electron beam 111 is a primary electron beam emitted from the electron gun 1 .

[0043] The secondary electron beam 121 is a collection of secondary electrons emitted when the electron beam 111 is narrowed and irradiated onto the sample 8 while scanning the surface of the sample 8. The secondary electrons 121 emitted from the sample 8 spiral on the axis due to the magnetic field of the objective lens 7, proceed toward the MCP 6 to which a positive voltage is applied, collide with the detection surface of the MCP 6, are amplified, and become a signal current, which is appropriately amplified, then AD converted and taken into the PC, and a secondary electron image with the amount of signal current as a gray scale is generated on the display. The secondary electron beam also includes reflected electrons, etc.

[0044] The high voltage power supply 21 applies a positive high voltage to the electron gun 1 and supplies a heating voltage to the cathode in accordance with instructions from the PC 31 .

[0045] The CL power supply 22 supplies a predetermined current to the CL 3 in accordance with an instruction from the PC 31 .

[0046] The deflection power supply 23 applies a predetermined deflection voltage to the DEF( 1 ) 4 and the DEF( 2 ) 5 in accordance with an instruction from the PC 31 .

[0047] The secondary electron detector 24 applies a predetermined voltage to the MCP 6 , further amplifies the signal amplified by the MCP 6 , and sends a secondary electron signal (secondary electron image) to the PC 31 .

[0048] The objective lens power supply 25 supplies a predetermined current to the objective lens 7 according to an instruction from the PC 31 .

[0049] A stage control power supply 26 supplies a predetermined control power supply to a motor that drives the stage 9 to move the sample 8 to a predetermined location.

[0050] The length measuring device 27 is a laser interferometer or the like that precisely measures the position of the stage 9 or the sample 8. The position coordinates where the electron beam irradiates the sample are obtained by combining the measurement position of the laser interferometer and the scanning position of the electron beam. The irradiation start position is determined using this value and the coordinates of the CAD data or the like.

[0051] The PC 31 is a known personal computer that performs various controls and processes using programs, and in this embodiment is composed of a scanning area setting means 32, a scanning method designation means 33, a global alignment means 34, an image acquisition means 35, a length measurement means 36, a reliability determination means 37, a DB 41, etc.

[0052] The scanning area setting means 32 sets the scanning area (scanning area, partial scanning area) of the pattern on the sample 8.

[0053] The scanning method designation means 33 designates a scanning method for scanning the scanning area of ​​the pattern on the sample 8 .

[0054] The global alignment means 34 generates a coordinate conversion formula between the pattern on the sample 8 and the pattern on the design data. Here, the precise position of the measurement target to be irradiated with the electron beam on the sample, such as a semiconductor wafer or a photomask, can be precisely specified using CAD data used in the design of semiconductor devices after performing an appropriate alignment procedure. Of course, if there is no CAD data, the boundary between the resist and other places can be determined and the place to be scanned with the electron beam can be automatically determined by specifying the range of the measurement target while observing the SEM image at a low magnification that does not affect the resist and with the electron beam irradiation amount as small as possible. Of course, a high-magnification optical microscope or AFM can also be used. When using a tool other than an electron beam, alignment is performed so that the electron beam irradiation position and the center position of the optical microscope coincide with each other.

[0055] The image acquisition means 35 scans a scanning area (scanning area, partial scanning area) of a pattern on the sample 8 with a finely focused electron beam and acquires an image (scanning area image, partial scanning area image) using the amount of signal electrons generated on the sample as brightness information.

[0056] The length measuring means 36 extracts a boundary portion from the image (scanning area image, partial scanning area image) acquired by the image acquiring means 35, and measures the length of the pattern.

[0057] The reliability determination means 37 extracts the resist boundary area from the acquired images (scanned area image, partial scanned area image) and determines the reliability of the measured pattern length. DB 41 stores various data in an easy-to-search format, and in this example stores CAD data for determining wiring patterns and measurement positions, measurement result data, reliability data, and the like.

[0058] FIG. 2 shows an example of a photocathode type electron source capable of being turned on / off at high speed according to the present invention.

[0059] FIG. 2(a) shows a configuration diagram, and FIG. 2(b) shows an example of a beam-off signal.

[0060] In FIG. 2(a), a laser 51 oscillates a laser.

[0061] The condenser lens 52 serves to focus the laser light generated by the laser 51 onto a photoelectric film 53 as shown in the figure.

[0062] The electron beam 54 is formed by accelerating electrons emitted when the photoelectric film 53 is irradiated with a laser by an electrode (not shown).

[0063] The automatic blanking control means 11 is the automatic blanking control means in FIG. 1, which generates a blanking signal when a predetermined interval (for example, an interval of N lines or M pixels) has elapsed from the edge of the pattern, stops (blocks) the emission of the laser 51, and stops the irradiation of the electron beam to the sample (described later using FIG. 3, FIG. 4, etc.).

[0064] Here, this is realized by combining a semiconductor laser 51 that can be turned on / off at high speed with a photocathode type electron gun that irradiates a photoelectric film 53 such as GaAs to generate electrons. A semiconductor laser can be turned on / off at a speed much faster than ns, and the electron beam can be stopped in a time shorter than the time it takes for the electron beam to move in the XY direction by one pixel of deflection scanning. Therefore, by inputting a signal that determines the resist boundary into the laser control signal, it is possible to reliably stop the electron beam irradiation with an error of one pixel or less and prevent the resist from shrinking. Naturally, if 2 pixels, 3 pixels, or N pixels are specified after receiving the resist boundary signal, the electron beam irradiation will stop at that position. Similarly, by using a gated microemitter created using MEMS or semiconductor manufacturing technology, it is possible to give a blanking signal to the gate of the electron gun itself and turn the electron beam on / off at high speed. In other words, the blanking signal can be used as the ONF / OFF signal for the electron source to control the on / off of the electron beam irradiation. It is advisable to correct the signal point so that the blanking signal correctly corresponds to the boundary.

[0065] Next, the operation of the configuration in FIG. 2 will be described. (1) When the electronic detector in FIG. 2(a) scans a line, for example, from left to right and detects the left edge of the line in real time, the automatic blanking control means 11 generates a beam OFF signal a predetermined interval (an interval of N lines or an interval of M pixels) after the edge. (2) Based on the beam OFF signal (1), the laser 51 is turned OFF to stop laser emission. This turns OFF the electron beam 54 emitted from the photoelectric film 53, and the electron beam can be blocked extremely quickly.

[0066] As described above, after the edge of the line is detected, a beam OFF signal is output after a specified interval, the laser is turned OFF, and the electron beam is also turned OFF. As a result, the electron beam passes the edge of the line and is shut off at ultra-high speed after a specified interval, eliminating unnecessary electron beam irradiation and making it possible to reduce damage and shrinkage to the line (made of resist) to a minimum.

[0067] FIG. 3 shows an explanatory diagram (part 1) of the operation of the present invention.

[0068] 3A shows an example of scanning along the longitudinal direction of a line. The vertical direction represents the main scanning direction (Y axis), and the horizontal direction represents the sub-scanning direction (X axis).

[0069] In Figure 3(a), the electron beam starts scanning (main scanning) vertically parallel to the lines from the space, then scans (main scanning) sequentially to the right toward the lines, and when it reaches the boundary, the intensity of the detected secondary electrons reaches a strong peak, allowing the edge (boundary between the space and the line) to be detected. After detecting the edge, when it reaches a gap of N lines (e.g., 3 lines), an electron beam OFF signal is generated, blocking the electron beam and blocking irradiation of the electron beam to the inner part thereafter. This prevents excess electron beam from being irradiated to the inside of the line, reducing damage and shrinkage of the line.

[0070] FIG. 3(a) will now be described in detail.

[0071] The present invention is characterized by the fact that the measurement is performed without irradiating the lines, which are resist structures, with the electron beam as little as possible. Therefore, by using design CAD data, it is possible to accurately know in advance the design positions of the lines of the measurement target structure and the space around them. The electron beam scan starts from the space area where there is no resist, and scans the required length in the direction along the longitudinal direction of the line. For example, scanning starts from the left side of the line for a preset distance (number of pixels) along the longitudinal direction of the line (scan 1). As with conventional SEM, information on signal electrons generated during scanning (amount, emission direction, energy, etc.) is detected in real time as a function of the scanning position.

[0072] When scanning the space area, secondary electrons are emitted that are determined by the secondary electron emission capacity of the substrate (quartz, metal film, etc.). Since there is no resist in the space area, even if a large amount of electron beam irradiation is performed, it does not affect resist shrink, so electron beam scanning is performed by irradiating a sufficient amount of electrons so that an image signal with a necessary and sufficient SNR can be obtained. When scanning gradually from the space area toward the right and approaching the line, it comes to an area where a very thin residual film of the resist structure that forms the line structure remains. Scanning further to the right enters an even thicker resist residual area. Although it depends on the energy of the primary electrons, the resist has the property of absorbing electrons, so the signal intensity decreases at first. The secondary electron detection capacity is sensitive enough to detect changes in resist film thickness of less than a few nm on the surface of the measurement target. After that, when it hits the side wall of the resist structure, the secondary electron emission increases suddenly due to the cosine effect. As described above, two opposing partial scanning images obtained by sandwiching the measurement target structure are used as a pair. In the present invention, the signal SNR is very high, so it is possible to precisely measure these signal changes.

[0073] The relationship between the electron beam scanning position and the signal electron intensity can be replaced with a simple approximation formula, etc. By defining a first threshold value that predetermines the resist boundary for the obtained approximation formula, it becomes possible to distinguish the boundary between the space and the resist structure.

[0074] The signal used for the judgment may be a mixture of the secondary electron signal and the backscattered electron signal, or the energy of the secondary electron signal and the backscattered electron signal may be filtered to use only electrons with the desired energy so that the signal change corresponding to the boundary change is more clearly indicated, or multiple signals may be combined.

[0075] Figure 3(b) shows an example of a scanned image along the longitudinal direction of the line. This shows an example of an image obtained by scanning in the same manner as Figure 3(a), where the vertical direction represents the main scanning direction (Y axis) and the horizontal direction represents the sub-scanning direction (X axis). The image shown is a secondary electron image.

[0076] In FIG. 3(b), the electron beam is blocked when it enters the interior of the vertical lines (made of resist) for N lines at the left and right ends of the image, so that the electron beam is not irradiated within that area, causing it to become completely black (the entire area is shown in the scanned image in the figure for the sake of explanation).

[0077] As described above, the electron beam is irradiated from both ends of the line up to N lines and the electron beam is blocked inside. This makes it possible to limit the irradiation of the electron beam inside in real time and reduce damage and shrinkage of the line.

[0078] Figure 4 shows an explanatory diagram (part 2) of the operation of the present invention. Figure 4 shows the cross section of a resist structure (line) and the signal electron waveform generated by electron beam scanning. Unlike the conventional signal electron waveform, there is a waveform corresponding to the edge part, but there is no waveform corresponding to the structure.

[0079] FIG. 4(c) shows an explanatory diagram for stopping scanning when the edge (+N line) is reached, and FIG. 4(d) shows an example of electron beam irradiation.

[0080] Next, the operation will be described. (1) As shown in Figure 4(c), for example, a first threshold is set as a threshold for measuring the length reflecting the bottom structure of the resist, and a second threshold is set as a threshold for measuring the length reflecting the top structure of the resist (the user decides by experiment what is defined as the bottom or top, taking into consideration measurement reproducibility, etc.). Usually, it is decided by comparing with values ​​obtained by other measurement methods such as peak position, waveform height %, differential waveform, or cross-sectional SEM or TEM.

[0081] When the amount of electronic signals generated from the sample exceeds or falls below the respective thresholds, the automatic blanking control means determines that the scanning electron beam has reached the boundary between the space and the line (resist), and stops the electron beam irradiation or performs electron beam blanking to stop the electron beam irradiation and prevent the electron beam from irradiating the resist structure (line). The position of the boundary obtained in this way is recorded as boundary position 1 (X1, Y1). (2) Next, in the opposite direction to the previous step, scanning begins on the space to the right of the line (scan 2). The two scans are in a straight line with the resist structure in between. The scan gradually moves leftward and approaches the line. As it approaches the line, it enters an area with thin resist film residue, and as it scans further left, it enters an area with thicker resist residue. As mentioned earlier, the change in resist thickness changes the amount of secondary electron signal to a level that can be detected sufficiently. By expressing this change in an approximate formula and distinguishing it with a second threshold value that defines the resist boundary, it is possible to accurately determine the boundary between the space to the right of the line and the resist area (line). Using this signal, the automatic blanking control means operates and turns off the electron beam. The position of the boundary (edge) found in this way is recorded as boundary position 2 (X2, Y2). The resolution of the CD measurement is proportional to the increment of each line, so when high resolution is required, the line scan increment should be set to a small value such as sub-nm, and when high resolution is not required, it is recommended to set it to 3 nm or the like. (3) By using the position difference (X2-X1) between the two left and right resist boundaries (line edges) calculated as described above as the width of the resist structure, measurement can be performed without shrinking the resist structure. (4) As with conventional CDSEM, the best place to set the threshold for the signal waveform can be optimized to the threshold with the highest measurement reproducibility by learning the correlation with measurement reproducibility using AI or other tools.

[0082] Fig. 5 shows an explanatory diagram of a line profile according to the present invention. When the threshold values ​​(first threshold value, second threshold value) shown in Fig. 5 are associated, the amount of secondary electrons or reflected electrons may be expressed by an approximation formula on an X1-dimensional or XY2-dimensional plane relative to the electron beam scanning position, and the boundary may be obtained by applying the threshold value to the approximation formula. Alternatively, an approximation curve (boundary) connecting the coordinates of the respective boundary points obtained as the left and right boundaries of the resist structure may be considered, and the distance may be measured using the approximation curve.

[0083] In this case, since the distances obtained by each electron beam scan have variations due to edge roughness, if the results of electron beam scanning of parts that are designed to have the same distance are accumulated and statistically averaged to obtain the length, measurement results with higher accuracy and better reproducibility can be obtained.

[0084] 6 shows an operation explanatory diagram (part 3) of the present invention. This shows an example of scanning in a direction perpendicular to the line.

[0085] In Fig. 6, this embodiment is characterized in that the direction of electron beam scanning is not parallel to the resist structure (line) but is rather scanning at an angle close to a right angle (it can be oblique). If scanning is performed obliquely, the line width appears longer, so the number of pixels in the image forming the boundary part can be increased, thereby improving the measurement accuracy. When scanning obliquely, the obtained distance is converted to the correct distance by performing scanning angle correction.

[0086] Fig. 7 shows an explanatory diagram (part 4) of the operation of the present invention. This explains the details of Fig. 6. The details will be explained below.

[0087] (1) The position on the sample where electron beam irradiation begins is precisely determined by CAD guidelines1,2 using CAD data or manually. Scanning begins from the space where there is no resist. Since the space and resist (lines) are made of different materials, they emit different amounts of secondary electrons when irradiated with the same electron beam. For example, the electron beam is scanned from the left space toward the resist area (line), and secondary electrons or reflected electrons are continuously detected as a function of the electron beam scanning position, and the amount of signal electrons is detected as a function of the scanning position. When moving from the space with the starting point specified by the CAD data toward the resist area (line), it comes across a residual area where a thin film of resist remains. At this time, the secondary electrons or reflected electrons cause a change in signal amount according to the thickness of the resist. When scanning proceeds to the resist area (line) where a thicker residual remains, an even greater change in signal amount occurs. By detecting the change in signal amount (signal intensity of the edge) at this time, the boundary (edge) between the space area and the resist area can be detected (boundary by signal electrons).

[0088] (2) Using this detected signal, the automatic blanking control means scans N or M pixels extra from the boundary point (edge) and then blocks the electron beam, thereby acquiring one partial image data.

[0089] (3) After stopping one electron beam scan, a second electron beam scan is started using the guidelines indicated by each CAD data. By repeating this a required number of times, a collection of partial images near the edge with the scan end point self-aligned is acquired. The pixel positions of adjacent scan lines can be determined arbitrarily as required. In the present invention, the next scan after one line has been scanned can be freely programmed and can be changed depending on the signal electrons from the structure. For example, if the required SNR is not reached, the same location can be scanned again, or the horizontal pixel start and end positions can be changed. It is also possible to perform a scan from the scan start point to the scan end point and then return to the scan start point again (variable ESR).

[0090] (4) To achieve high-speed blanking, the electrostatic blanking method is used and the blanking electrodes are designed to have as little electrostatic capacitance as possible. Similarly, for the output of the circuit, ultra-fast transistors with a response speed of less than a few nanoseconds and a large output current are used to achieve sharp rise and fall times. It is desirable to place the blanking aperture at a position where the width of the primary electron beam narrows. Since blanking has a finite speed, a tail occurs when the primary electron beam is turned on and off. Therefore, if necessary, a method can be used to reduce the effect of the tail by slowing down the clock speed so that blanking can be performed more accurately.

[0091] (5) As already described in Fig. 2, instead of performing blanking, the electron beam itself output from the electron source can be stopped by using an automatic blanking control means together with boundary detection (edge ​​detection). In particular, when a photoexcited electron gun is used, a similar effect can be obtained by turning off a high-speed light source such as a laser that irradiates the electron source in accordance with the blanking timing.

[0092] (6) In the embodiment, lines / spaces have been used for simplicity, but since any shape can be defined as a connection or collection of small lines, it goes without saying that any shape other than lines / spaces can be measured in the same way. In particular, when extracting the contour of a pattern having an arbitrary shape, a method is used in which the approximate contour is specified using CAD data, electron beam scanning is started from that position, and the electron beam scanning range is determined using the boundary of the actual structure, making it possible to scan only the contour portion of the pattern that needs to be inspected on the semiconductor wafer or photomask, and to extract the contour of the structure to be measured at ultra-high speed.

[0093] (7) Specifically, electron beam scanning begins from the electron beam scanning start point specified in the CAD data, and when an edge is detected, the electron beam is stopped N pixels from that point. Next, scanning begins with the CAD guideline corresponding to the pixel immediately to the side as the starting point. It is desirable to scan in the perpendicular direction to the partial lines that form the arbitrary shape. By repeating this process, it becomes possible to scan the electron beam only in the vicinity of the contour of the object to be measured, and the contour can be extracted by simply measuring a very small area.

[0094] (8) Normally, inspection equipment scans wafers and photomasks in two dimensions, so it is necessary to capture many pixels as an image. The number of captured pixels is proportional to the inspection time, and the more pixels there are, the longer the inspection time will be. In inspections, the outer shape is often important. By using this invention, the measurement object can be represented by scanning close to one dimension, so inspection can be performed by capturing a very small number of pixels, which makes it possible to perform inspections at much higher speeds than with conventional inspection equipment.

[0095] FIG. 8 shows another explanatory diagram of the present invention.

[0096] In FIG. 8, the container is a vessel for holding an ionic liquid.

[0097] An ionic liquid is a liquid that has ionic conductivity.

[0098] The substrate is a substrate on which a pattern is formed, such as a wafer or a mask.

[0099] The resist is a resist that forms a pattern on a substrate, and in this case is immersed in the ionic liquid.

[0100] Next, the configuration of FIG. 8 will be described. (1) Ionic liquids are salts (substances that form ionic crystals) with a melting point below 100°C, and because they are strongly ionic-bonded, they have the property of barely evaporating in a vacuum, even though they are liquid at room temperature. Therefore, even if they are left in the vacuum chamber of an electron microscope in a vacuum state, they do not evaporate and remain intact, and because they exhibit electrical conductivity, they are used as antistatic agents and lubricants. On the other hand, like salt, they are pure ion masses, so each of their constituent substances has positive and negative ions, and they mix well with polar solvents. (2) The following are the main types of ionic liquids known. Ionic liquids are new, so many more will be developed in the future, and these will also be useful.

[0101] Basically, they are broadly divided into three types based on the type of cation: pyridine, alicyclic amine, and aliphatic amine. By selecting the type of anion to combine with this, a variety of structures can be synthesized. The cations used include ammonium ions such as imidazolium salts and pyridinium salts, phosphonium ions, pyrrolidinium, and non-ionic ions, while examples of anions include halogen ions such as bromide ions and triflates, boron ions such as tetraphenylborate, and phosphorus ions such as hexafluorophosphate.

[0102] ArF resists used in cutting-edge exposure processes contain many of the following solvents to adjust viscosity: Propylene glycol monomethyl ether (melting point -96°C, boiling point 120°C) Butyl acetate (melting point -74°C, boiling point 126°C) Organic solvents are also separated and generated as products of resist decomposition reactions. (3) When the resist is exposed to light to form a pattern, and then developed, washed, and baked, a large amount of the above-mentioned solvent still remains inside the resist. Therefore, when the resist structure after development or baking is placed in the vacuum chamber of an electron microscope, the solvent rapidly evaporates and the resist is reduced in volume. In particular, the resist temperature rises locally in the area irradiated with an electron beam focused to a few nm, and acid is generated by the acid generator, which causes the resist to cleave and the solvent to fly out, causing further evaporation of the solvent, resulting in the resist being reduced in volume or shrinking.

[0103] On the other hand, since the above-mentioned ionic liquid is conductive and has almost no vapor pressure, by replacing it with the solvent constituting the resist after development, it is possible to prevent the organic solvent from evaporating from the resist to the outside and losing weight even in a vacuum. In order to make the ionic liquid penetrate the resist structure quickly, ultrasonic waves or the like may be added to accelerate the replacement. In the present invention, since the electron beam irradiation is automatically stopped at the edge portion, it is sufficient that the edge portion is replaced with the ionic liquid, and therefore the replacement can be performed relatively easily. (4) Although the technique of applying an ionic liquid to the surface of a resist for the purpose of preventing charging of the resist after baking has been known for some time, this invention is the first to disclose a method of suppressing shrinkage by replacing the organic solvent that constitutes the resist with an ionic liquid after or during development, thereby preventing the organic solvent contained in the resist from evaporating in a vacuum.

[0104] When irradiated with an electron beam, it reacts with the acid generator contained in the resist, promoting the resist cleavage reaction. The organic solvent generated by this reaction flies into the vacuum, promoting loss and shrinkage, but when the present invention is used, the solvent is replaced with an ionic liquid with a low vapor pressure, so there is almost no evaporation. In other words, even if the resist is irradiated with an electron beam, shrinkage and shrinkage can be completely prevented. (5) By combining these technologies with the electron beam scanning method described above, it is possible to avoid slight changes in the resist that occur when the resist is scanned with the electron beam, and it goes without saying that damage to the resist caused by electron beam irradiation can be prevented, that is, the state before the electron beam irradiation can be maintained.

[0105] Fig. 9 shows another explanatory diagram (part 2) of the present invention. In Fig. 9, the resist or sample is cooled by a cooling device in a vacuum chamber during measurement.

[0106] In FIG. 9, the electron beam column is a known type for generating, converging, and narrowing an electron beam to perform planar scanning on a sample.

[0107] The sample may be a pattern formed on a substrate.

[0108] The cooling device is a stage that is cooled to a low temperature, and a sample is mounted thereon to cool the sample.

[0109] The XY stage moves the sample to a desired position.

[0110] The vacuum chamber is a container in which the sample, cooling device, XY stage, etc. are placed in a vacuum.

[0111] Cooled helium gas is N gas used to cool the cooling device to low temperatures.

[0112] Next, the operation will be described. (1) In Figure 9, the shrink phenomenon that occurs when the resist is irradiated with an electron beam is a type of chemical reaction. Chemical reactions have a reaction rate that is determined by chemical energy, so the rate at which a chemical reaction proceeds can generally be controlled by temperature. Generally, lowering the temperature by 10 degrees halves the reaction rate, so lowering the temperature by 100 degrees reduces the reaction rate to one-thousandth. To reduce the amount of shrinkage to one-hundredth, at which point no substantial change in the resist is observed, it is necessary to lower the temperature by about 60 degrees from room temperature, that is, to about -30 to -40 degrees, so the sample temperature can be lowered using a Peltier element, etc. (2) As shown in Fig. 9, a cooling device is provided on a metal or glass ceramic palette, XY stage, or electron beam column for carrying the sample, and the sample is cooled during measurement. The entire sample may be cooled, or only the measurement point may be cooled. Generally, the melting point of organic solvents generated or contained in resist is higher than -100 degrees, so the organic solvent can be solidified using a semiconductor cooling device using a Peltier element, etc. Of course, liquid nitrogen, its cooling gas, or helium gas may be used for cooling using piping to prevent leakage in a vacuum. When performing measurements in a low vacuum, cooling gas may be sprayed onto the measurement target.

[0113] By cooling in the manner described above, shrinkage is reduced to less than one-hundredth of that at room temperature, making it essentially shrink-free. (3) When the liquid is replaced with the ionic liquid described above, it is possible to achieve a shrink-free resist by simply cooling it to near 0°C. By combining this method with the previously described method, it becomes possible to perform accurate and highly reproducible measurements with even less damage to the resist.

[0114] 10 shows a diagram of the configuration of another embodiment of the present invention, which illustrates the case where the length of a sample is measured under atmospheric pressure and under a further increased pressure.

[0115] This will be explained in detail below. (1) As mentioned above, resist shrinkage is mainly caused by organic solvents contained in the resist or organic solvents generated when the resist is irradiated with an electron beam being locally heated and volatilizing into the vacuum. Therefore, if the measurement environment is atmospheric pressure or pressurized, the reaction can be suppressed by chemical equilibrium and the evaporation of the generated organic solvent can be reduced. (2) There are various methods for measuring samples under atmospheric pressure. A series of electron microscopes called atmospheric pressure SEM can achieve this purpose. The device disclosed by the present inventor is one of them (for details, see JP 2014-157772 A). In these electron microscopes, a thin film of light elements such as carbon or silicon that can pass through the electron beam but cannot pass through gases such as air is placed at the electron beam exit to block the atmosphere, and the electron beam can be irradiated through the film to the atmosphere. However, simply irradiating the electron beam at atmospheric pressure cannot completely stop the shrinkage of the resist, so it goes without saying that more effective methods can be obtained by combining the self-aligned ESR electron beam scanning method, ionic liquid replacement method, or sample cooling method described above.

[0116] FIG. 11 shows an explanatory diagram of the present invention.

[0117] Figure 11(a) shows scanning for each pixel. This shows the state of scanning when the spot size of the electron beam is equal to the scanning step interval. In this case, when scanning (main scanning) is performed from the left side toward the line as shown in the figure, scanning is performed sequentially with the spot size of the electron beam as shown in the figure, so the brightness (amplitude) of the secondary electrons detected at that time forms a stepped waveform as shown in the figure.

[0118] On the other hand, (b) of Fig. 11 shows sub-pixel scanning. This shows the state of scanning when the spot size of the electron beam is much larger (longer) than the scanning step interval. In this case, when scanning (main scanning) is performed from the left side toward the line as shown in the figure, the electron beam is scanned (shifted) sequentially to the right with a larger spot size as shown in the figure, so the brightness (amplitude) of the secondary electrons detected at that time forms a waveform with peaks at the edge parts (boundaries between spaces and lines) as shown in the figure.

[0119] As described above, when the spot size and scanning step of the electron beam are changed, the waveform of the detected secondary electrons differs. Therefore, in order to detect the boundary (edge) from a space to a line, it is necessary to obtain an approximation curve in advance by experiment based on the spot size and scanning step at that time, and then use this approximation curve to accurately detect the edge position.

[0120] 12 shows an explanatory diagram (part 2) of the present invention. This illustrates the operation of generating a blocking signal N pixels after detecting an edge detection signal, blocking the electron beam, and blocking the beam.

[0121] In FIG. 12, the scanning signal is a signal for scanning (main scanning) the electron beam.

[0122] The edge detection signal is a signal that detects the boundary (edge) between a space and a line.

[0123] The blocking signal is a signal for blocking an electron beam, and is a signal for blocking an electron beam that occurs N pixels (M lines) after an edge detection signal (edge) is detected.

[0124] Secondary electrons are the intensity of secondary electrons generated from spaces, lines, etc.

[0125] Next, the operation will be described.

[0126] (1) As already mentioned, for example as shown in FIG. 7, an electron beam is scanned from a space toward a line (resist), and when a peak of secondary electrons that is the boundary (edge) between the space and the line is detected, an edge signal is output.

[0127] (2) After the edge signal is output, a blocking signal is output when the scanning signal advances by N pixels.

[0128] (3) When the blocking signal is output, the electron beam is blocked (beam blocking). The inside of the line from this point onwards is not irradiated with the electron beam, preventing damage and shrinkage of the line (resist). [Brief description of the drawings]

[0129] [Figure 1] FIG. 1 is a system configuration diagram of the present invention. [Diagram 2] 2 is an example of a photocathode type electron source capable of being turned on / off at high speed according to the present invention. [Diagram 3] FIG. 1 is an explanatory diagram (part 1) of the operation of the present invention. [Figure 4] FIG. 2 is an explanatory diagram (part 2) of the operation of the present invention. [Diagram 5] FIG. 2 is a diagram illustrating a line profile of the present invention. [Figure 6] FIG. 3 is an explanatory diagram (part 3) of the operation of the present invention. [Figure 7] FIG. 4 is an explanatory diagram of the operation of the present invention. [Figure 8] FIG. [Figure 9]FIG. 2 is another explanatory diagram (part 2) of the present invention. [Figure 10] FIG. 11 is a configuration diagram of another embodiment of the present invention. [Figure 11] FIG. 1 is an explanatory diagram of the present invention. [Figure 12] FIG. 2 is an explanatory diagram (part 2) of the present invention. [Explanation of symbols]

[0130] 1: Electron gun 2: Aperture 3: CL (condenser lens) 4:DEF(1) 5:DEF(2) 6: MCP 7: Objective lens 8: Sample 9. Stage 11: Automatic blanking control means 12: Blanking device 13: Blanking electrode 14: Blanking aperture 111: Electron beam 121: Secondary electron 21: High voltage power supply 22:CL power supply 23: Deflection power supply 24: Secondary electron detector 25: Objective power supply 26: Stage control power supply 27: Length measuring device 31: PC (personal computer) 32: Scanning area setting means 33: Scanning method designation means 34: Global alignment method 35: Image acquisition means 36: Length measuring means 37: Means of determining reliability 41:DB

Claims

1. In an electron beam measurement device for measuring the dimensions, area, or contour of a pattern to be measured formed on a sample, a scanning means for irradiating and scanning a resist pattern, which is a pattern to be measured, with a narrowed electron beam, the resist pattern being obtained by replacing an organic solvent that evaporates in a vacuum with an ionic liquid that does not evaporate in a vacuum; a measuring means for measuring based on a signal waveform acquired by scanning while irradiating the signal; Equipped with 4. An electron beam measuring device, comprising: a resist pattern having a resist pattern that is evaporating in a vacuum to reduce shrinkage of the resist pattern;

2. In an electron beam measurement device for measuring the dimensions, area, or contour of a pattern to be measured formed on a sample, a scanning means for scanning a resist pattern, which is a pattern to be measured, in which an organic solvent that evaporates in a vacuum is replaced with an ionic liquid that does not evaporate in a vacuum, with a narrowed electron beam from a region where the resist pattern is not present to a region where the resist pattern is present; an electron beam stopping means for detecting in real time that the electron beam has entered an area where the resist pattern is present and stopping irradiation of the electron beam; a measuring means for measuring based on a signal waveform acquired by scanning until the electron beam stopping means stops the irradiation of the electron beam; Equipped with 4. An electron beam measuring device, comprising: a resist pattern having a resist pattern that is evaporating in a vacuum to reduce shrinkage of the resist pattern;

3. The electron beam measurement device according to claim 1 or 2, characterized in that the resist pattern replaced with an ionic liquid that does not evaporate in the vacuum is replaced with the resist pattern that has been cooled and solidified so as not to evaporate in the vacuum, and the scanning means scans the replaced resist pattern while irradiating it with a narrowed electron beam.

4. 4. The electron beam measurement device according to claim 1, further comprising: means for extracting edges in the signal waveforms acquired facing the resist pattern to be measured, and determining a distance between opposing edges of the resist pattern from the edge position information of each edge.

5. 4. The electron beam measuring device according to claim 1, further comprising: an edge extraction unit that extracts an outline of the resist pattern to be measured by extracting an edge of the signal waveform obtained from the resist pattern to be measured.

6. 1. An electron beam measurement method for measuring the dimensions, area, or contour of a pattern to be measured formed on a sample, comprising: a scanning step of irradiating and scanning a thin electron beam onto a resist pattern, the resist pattern being a pattern to be measured, in which an organic solvent that evaporates in a vacuum is replaced with an ionic liquid that does not evaporate in a vacuum; a measuring step of measuring based on a signal waveform acquired by scanning while irradiating the light; having 4. An electron beam measuring method, comprising: reducing evaporation of an organic solvent contained in the resist pattern in a vacuum to thereby reduce shrinkage.

Citation Information

Patent Citations

  • Resist coating method and apparatus therefor

    JP1985160614A

  • Method for applying liquid photosensitive resist

    JP1993335298A

  • Apparatus and method for measuring dimension of pattern

    JP2000321040A

  • Charged particle beam apparatus

    JP2017199453A

  • Scanning electron microscope having length measuring function and sample dimension length measuring method

    WO2008111365A1