Recovery agent, recovery method for non-aqueous electrolyte secondary battery, and manufacturing method for non-aqueous electrolyte secondary battery
A recovery agent with an aromatic hydrocarbon compound and metal ions in a specific concentration range in an ether solvent addresses the complexity of third electrode methods, enhancing the recovery efficiency and capacity of non-aqueous electrolyte secondary batteries.
Patent Information
- Application Number
- JP2021040205
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Existing methods for restoring the capacity of non-aqueous electrolyte secondary batteries, such as those involving a third electrode, complicate the battery structure and require a novel recovery method without a third electrode.
A recovery agent containing an aromatic hydrocarbon compound in a reduced state and metal ions of the same type as the carrier ions, at a concentration of 1.7 mol/L to 5.0 mol/L in an ether solvent, is injected into the battery to restore capacity.
The recovery agent facilitates a smooth supply of electrons and metal ions to the positive electrode, enhancing the battery's recovery reaction efficiency and improving the capacity of the non-aqueous electrolyte secondary battery.
Smart Images

Figure 0007569719000007 
Figure 0007569719000008 
Figure 0007569719000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a recovery agent, a method for recovering a nonaqueous electrolyte secondary battery, and a method for manufacturing a nonaqueous electrolyte secondary battery. [Background technology]
[0002] Conventionally, as a method for restoring the capacity of a nonaqueous electrolyte secondary battery whose capacity has deteriorated due to long-term storage or charge-discharge cycles, a method has been proposed in which a third electrode is provided in addition to a positive electrode and a negative electrode, the third electrode and the positive electrode are externally short-circuited, and carrier ions are supplied from the third electrode to the positive electrode (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-076358 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in Patent Document 1, there is a problem that the structure of the battery becomes complicated by incorporating a third electrode. For this reason, a new recovery method for a nonaqueous electrolyte secondary battery that can recover the capacity without using a third electrode has been desired.
[0005] The present disclosure has been made to solve such problems, and has as its main object to provide a novel method for restoring a non-aqueous electrolyte secondary battery. [Means for solving the problem]
[0006] As a result of intensive research to achieve the above-mentioned object, the present inventors have found that the capacity of a non-aqueous electrolyte secondary battery is restored when a solution containing a reduced aromatic hydrocarbon compound and the same type of metal ion as the carrier ion of the non-aqueous electrolyte secondary battery is injected into the non-aqueous electrolyte secondary battery. In particular, the present inventors have found that the capacity of the battery after restoration is further improved when the reduced aromatic hydrocarbon compound and the metal ion are at a predetermined high concentration relative to the ether solvent in the restoration agent, and have completed the present disclosure.
[0007] That is, the recovery agent disclosed in the present specification is A recovery agent for recovering the capacity of a non-aqueous electrolyte secondary battery having a metal ion as a carrier ion, a reduced aromatic hydrocarbon compound, a metal ion of the same type as the carrier ion, and a solvent which is an ether compound, wherein the concentrations of the reduced aromatic hydrocarbon compound and the metal ion relative to the solvent are 1.7 mol / L or more and 5.0 mol / L or less; It is something.
[0008] The method for recovering a non-aqueous electrolyte secondary battery disclosed in the present specification includes the steps of: A method for recovering the capacity of a non-aqueous electrolyte secondary battery that uses metal ions as carrier ions, comprising: a recovery step of injecting the recovery agent into the nonaqueous electrolyte secondary battery to recover the capacity of the nonaqueous electrolyte secondary battery; It includes.
[0009] The method for producing a nonaqueous electrolyte secondary battery disclosed in the present specification further comprises the steps of: a battery preparation step of preparing a capacity-degraded nonaqueous electrolyte secondary battery having metal ions as carrier ions; a recovery step of recovering the capacity of the nonaqueous electrolyte secondary battery in the above-mentioned method for recovering the capacity of the nonaqueous electrolyte secondary battery; It includes. Effect of the Invention
[0010] This recovery agent and the recovery method for a non-aqueous electrolyte secondary battery can provide a novel recovery method for a non-aqueous electrolyte secondary battery. The reason for obtaining such an effect is presumed to be as follows. For example, it is presumed that the recovery agent containing a reduced aromatic hydrocarbon compound and a metal ion acts directly on the positive electrode by simply injecting it into a non-aqueous electrolyte secondary battery, and generates a recovery reaction that supplies electrons and metal ions to the positive electrode. In particular, the recovery agent in which the concentration of each of the reduced aromatic hydrocarbon compound and the metal ion in the ether solvent is 1.7 mol / L or more and 5.0 mol / L or less improves the capacity of the battery after recovery. The reason for this is presumed to be as follows. For example, the recovery agent in which the concentration of each of the reduced aromatic hydrocarbon compound and the metal ion in the ether solvent is 1.7 mol / L or more and 5.0 mol / L or less has high diffusibility of the reduced aromatic hydrocarbon compound and the metal ion to the positive electrode. Therefore, when this recovery agent is added to a non-aqueous electrolyte secondary battery, it is considered that the supply of electrons and metal ions to the positive electrode is smooth, the recovery reaction proceeds efficiently, and the capacity of the battery after recovery is further improved. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery 20. FIG. [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a recovery reaction scheme. [Diagram 3] 1 is a graph showing the capacity at constant voltage in Experimental Example 1. [Figure 4] 1 is a graph showing recovery capacity in Experimental Example 1. [Diagram 5] 1 is a graph showing the relationship between the capacity at constant voltage and the recovery capacity in Experimental Examples 1 to 10. [Figure 6] 1 is a graph showing the relationship between the concentration of naphthalene and lithium and the recovery capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The recovery agent disclosed in this specification is for recovering the capacity of a non-aqueous electrolyte secondary battery. Further, the method for recovering a non-aqueous electrolyte secondary battery disclosed in this specification is a method for recovering the capacity of a non-aqueous electrolyte secondary battery. Preferred embodiments of the recovery agent and the method for recovering a non-aqueous electrolyte secondary battery will be described below.
[0013] [Non-aqueous electrolyte secondary battery] First, the non-aqueous electrolyte secondary battery to be recovered will be described. The non-aqueous electrolyte secondary battery is not particularly limited as long as it is a non-aqueous electrolyte secondary battery having metal ions as carrier ions. For example, it may be one having Group 1 ions such as lithium, sodium, and potassium, or Group 2 ions such as magnesium, calcium, and strontium as carrier ions. Further, the non-aqueous electrolyte secondary battery may be an ion secondary battery such as a lithium-ion secondary battery, or a metal secondary battery such as a lithium metal secondary battery. Hereinafter, as an example, the case where the non-aqueous electrolyte secondary battery is a lithium-ion secondary battery will be mainly described.
[0014] The non-aqueous electrolyte secondary battery includes a positive electrode, a negative electrode, and a non-aqueous electrolyte. The positive electrode may have a positive electrode active material capable of occluding and releasing lithium ions. The negative electrode may have a negative electrode active material capable of occluding and releasing lithium ions. The non-aqueous electrolyte may be interposed between the positive electrode and the negative electrode and conduct lithium ions.
[0015] The positive electrode may be formed, for example, by mixing a positive electrode active material, a conductive material, and a binder, adding an appropriate solvent to form a paste-like positive electrode mixture, applying and drying it on the surface of a current collector, and compressing it as necessary to increase the electrode density. As the positive electrode active material, sulfides containing transition metal elements, oxides containing lithium and transition metal elements, etc. can be used. Specifically, transition metal sulfides such as TiS2, TiS3, MoS3, and FeS2, and lithium manganese composite oxides having a basic composition formula of Li (1-x) MnO2 (0 < x < 1, etc., the same applies hereinafter), and Li (1-x) Mn2O4, etc., and lithium cobalt composite oxides having a basic composition formula of Li (1-x)Lithium cobalt composite oxide with CoO2, etc., with the basic composition formula Li (1-x) Lithium nickel composite oxide such as NiO2, with the basic composition formula Li (1-x) Ni a Co b Mn c Lithium nickel cobalt manganese composite oxides having a basic composition formula of LiV2O2(a+b+c=1), lithium vanadium composite oxides having a basic composition formula of LiV2O3, transition metal oxides having a basic composition formula of V2O5, etc. can be used. Among these, lithium transition metal composite oxides, such as LiCoO2, LiNiO2, LiMnO2, LiV2O3, etc., are preferred. The term "basic composition formula" means that other elements may be included. The positive electrode active material may have an oxidation-reduction potential of 3.5V or more, 4.0V or more, or 4.5V or more based on Li metal.
[0016] In the positive electrode, the conductive material may be, for example, one or more of graphite such as natural graphite (scale graphite, flake graphite) or artificial graphite, acetylene black, carbon black, Ketjen black, carbon whisker, needle coke, carbon fiber, metal (copper, nickel, aluminum, silver, gold, etc.), etc. Among these, from the viewpoint of electronic conductivity and coating property, carbon black and acetylene black are preferable as the conductive material. The binder plays a role of binding the active material particles and the conductive material particles, and may be, for example, fluorine-containing resin such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, etc., or thermoplastic resin such as polypropylene and polyethylene, ethylene propylene diene monomer (EPDM) rubber, sulfonated EPDM rubber, natural butyl rubber (NBR), etc., used alone or as a mixture of two or more kinds. In addition, aqueous binders such as cellulose-based carboxymethylcellulose (CMC), styrene butadiene copolymer (SBR), and aqueous dispersions of polyvinyl alcohol can also be used. As a solvent for dispersing the positive electrode active material, conductive material, and binder, for example, organic solvents such as N-methylpyrrolidone, dimethylformamide, dimethylacetamide, methyl ethyl ketone, cyclohexanone, methyl acetate, methyl acrylate, diethylenetriamine, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran can be used. In addition, a dispersant, a thickener, and the like can be added to water, and the active material can be slurried with latex such as SBR. As a thickener, for example, polysaccharides such as carboxymethylcellulose and methylcellulose can be used alone or as a mixture of two or more kinds. Examples of application methods include roller coating such as an applicator roll, screen coating, doctor blade method, spin coating, and bar coater, and any thickness and shape can be obtained by using any of these. The basis weight of the positive electrode mixture is not particularly limited, but for example, 5 mg / cm 2 May exceed 6mg / cm 2 or more, 7 mg / cm 2The weight of the positive electrode mixture may be, for example, 20 mg / cm 2 The following may be used. As the current collector, in addition to aluminum, titanium, stainless steel, nickel, iron, baked carbon, conductive polymer, conductive glass, etc., aluminum or copper whose surface is treated with carbon, nickel, titanium, silver, etc. for the purpose of improving adhesion, conductivity, and oxidation resistance can be used. The surface of these can also be subjected to oxidation treatment. The shape of the current collector can be a foil, film, sheet, net, punched or expanded one, lath, porous body, foam, fiber group formation, etc. The thickness of the current collector used is, for example, 1 to 500 μm.
[0017] The negative electrode may be formed by bonding a negative electrode active material and a current collector, or may be formed by mixing a negative electrode active material, a conductive material, and a binder, adding an appropriate solvent to form a paste-like negative electrode composite, applying it to the surface of a current collector, drying it, and compressing it to increase the electrode density as necessary. Examples of the negative electrode active material include inorganic compounds such as lithium, lithium alloys, and tin compounds, carbonaceous materials capable of absorbing and releasing lithium ions, composite oxides containing multiple elements, and conductive polymers. Examples of the carbonaceous material include cokes, glassy carbons, graphites, non-graphitizable carbons, pyrolytic carbons, and carbon fibers. Among these, graphites such as artificial graphite and natural graphite are preferred because they have an operating potential close to that of metallic lithium, can be charged and discharged at a high operating voltage, and can suppress self-discharge when a lithium salt is used as a supporting salt, and can reduce irreversible capacity during charging. Examples of the composite oxide include lithium titanium composite oxide and lithium vanadium composite oxide. Of these, carbonaceous materials are preferred as the negative electrode active material from the viewpoint of safety. The conductive material, binder, solvent, etc. used in the negative electrode can be the same as those exemplified for the positive electrode. The negative electrode active material may have an oxidation-reduction potential of 1.0 V or less, 0.5 V or less, or 0.3 V or less, based on Li metal. The weight of the negative electrode composite material is, for example, 3 mg / cm. 2 May exceed 4mg / cm 2The weight of the negative electrode mixture may be, for example, 15 mg / cm. 2 The negative electrode current collector may be made of copper, nickel, stainless steel, titanium, aluminum, baked carbon, conductive polymer, conductive glass, Al-Cd alloy, etc., or may be made of copper or the like whose surface has been treated with carbon, nickel, titanium, silver, etc., for the purpose of improving adhesion, conductivity, and reduction resistance. The surface of these materials may also be oxidized. The shape of the current collector may be the same as that of the positive electrode.
[0018] The non-aqueous electrolyte may contain a supporting salt and an organic solvent. Examples of the supporting salt include inorganic salts such as LiPF6, LiClO4, LiAsF6, and LiBF4, and organic salts such as LiN(FSO2)2 (also referred to as LiFSI), LiN(CF3SO2)2 (also referred to as LiTFSI), and LiN(C2F5SO2)2 (also referred to as LiBETI). These supporting salts may be used alone or in combination. The concentration of the supporting salt is preferably 0.1 to 2.0 M, and more preferably 0.8 to 1.2 M. Examples of the organic solvent include aprotic organic solvents. Examples of such organic solvents include cyclic carbonates, chain carbonates, cyclic esters, cyclic ethers, and chain ethers. Examples of the cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, and vinylene carbonate. Examples of the chain carbonate include dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. Examples of the cyclic ester include gamma butyrolactone and gamma valerolactone. Examples of the cyclic ether include tetrahydrofuran and 2-methyltetrahydrofuran. Examples of the chain ether include dimethoxyethane and ethylene glycol dimethyl ether. These may be used alone or in combination. In addition, the non-aqueous electrolyte may include nitrile-based solvents such as acetonitrile and propylnitrile, ionic liquids, gel electrolytes, and the like. The non-aqueous electrolyte may include additives such as a film-forming agent and a flame retardant.
[0019] The non-aqueous electrolyte secondary battery may have a separator between the positive electrode and the negative electrode. The separator is not particularly limited as long as it has a composition that can withstand the range of use of the non-aqueous electrolyte secondary battery, and examples thereof include polymer non-woven fabrics such as polypropylene non-woven fabrics and polyphenylene sulfide non-woven fabrics, and thin microporous films of olefin resins such as polyethylene and polypropylene. These may be used alone or in combination.
[0020] The nonaqueous electrolyte secondary battery may have an openable / closable electrolyte injection port in a battery case that houses the positive electrode, the negative electrode, and the nonaqueous electrolyte, allowing the recovery agent to be easily injected through the electrolyte injection port.
[0021] The shape of the nonaqueous electrolyte secondary battery is not particularly limited, and examples thereof include coin type, button type, sheet type, laminated type, cylindrical type, flat type, and square type. The nonaqueous electrolyte secondary battery may also be applied to large batteries used in electric vehicles and the like. FIG. 1 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery 20. The nonaqueous electrolyte secondary battery 20 includes a cup-shaped battery case 21, a positive electrode 22 having a positive electrode active material and provided at the bottom of the battery case 21, a negative electrode 23 having a negative electrode active material and provided at a position facing the positive electrode 22 via a separator 24, a gasket 25 formed of an insulating material, and a sealing plate 26 disposed at the opening of the battery case 21 and sealing the battery case 21 via the gasket 25. In the nonaqueous electrolyte secondary battery 20, a nonaqueous electrolyte 27 is filled in the space between the positive electrode 22 and the negative electrode 23.
[0022] A non-aqueous electrolyte secondary battery has an internal resistance of 5 Ωcm when the capacity of the battery is not degraded (also called a pre-degraded battery). 2 It may be in excess of 7 Ωcm 2 It may be 10 Ωcm or more. 2In non-aqueous electrolyte secondary batteries, such as batteries for electric vehicles, in which the thickness or weight of the electrode composite is large and the internal resistance is relatively high, the capacity and cycle capacity retention rate of the battery after recovery are often low simply by injecting a recovery agent, so it is highly meaningful to apply the recovery method for non-aqueous electrolyte secondary batteries of the present disclosure. Note that the internal resistance of the battery before deterioration is 50 Ω cm 2 It may be the following:
[0023] [Recovery potion] Next, the recovery agent will be described. The recovery agent includes an aromatic hydrocarbon compound in a reduced state, metal ions of the same type as the carrier ions of the nonaqueous electrolyte secondary battery, and a solvent that is an ether compound. The recovery agent may be a recovery agent prepared in advance, or may be prepared in a preparation step for preparing the recovery agent. In the recovery agent, the aromatic hydrocarbon compound in a reduced state and the metal ions may be dissociated or associated. The recovery agent may include an electrolyte in addition to a recovery agent stock solution that includes an aromatic hydrocarbon compound in a reduced state, metal ions of the same type as the carrier ions of the nonaqueous electrolyte secondary battery, and a solvent that is an ether compound. The recovery agent may be a recovery agent stock solution without including an electrolyte.
[0024] In the recovery agent, the aromatic hydrocarbon compound is preferably polyacene or polyphenyl. Polyacene is a compound having a structure in which a plurality of benzene rings are condensed, and examples thereof include naphthalene, anthracene, tetracene, and pentacene. Polyphenyl is a compound having a structure in which a plurality of phenyl groups are linked by single bonds, and examples thereof include biphenyl, ortho-terphenyl, meta-terphenyl, para-terphenyl, para-quaterphenyl, and para-quinquiphenyl. Polyacene and polyphenyl may have a substituent on the aromatic ring, or may contain a heteroatom in the aromatic ring. Examples of the substituent include a halogen atom, an alkyl group, an aryl group, an alkenyl group, an alkoxy group, an aryloxy group, a sulfonyl group, an amino group, a cyano group, a carbonyl group, an acyl group, an amide group, and a hydroxyl group. Examples of the heteroatom include nitrogen, oxygen, and sulfur. Examples of polyacene containing a heteroatom in an aromatic ring include quinoline, chromene, and acridine. Examples of polyphenyl containing a heteroatom in an aromatic ring include bipyridine. The aromatic hydrocarbon compound is preferably one or more of naphthalene, biphenyl, anthracene, ortho-terphenyl, and para-terphenyl among the above-mentioned compounds, and more preferably one or more of naphthalene and biphenyl. The aromatic hydrocarbon compound may be, for example, one or more of formula (1) and formula (2). The aromatic hydrocarbon compound in a reduced state is, for example, the above-mentioned aromatic hydrocarbon compound in a reduced state (also called a reduced form), for example, a radical anion. The aromatic hydrocarbon compound in a reduced state may be, for example, one or more of the reduced form of the compound of formula (1) and the reduced form of the compound of formula (2).
[0025] [ka]
[0026] In the recovery agent, the metal ions may be of the same type as the carrier ions in the nonaqueous electrolyte secondary battery, but are preferably one or more of alkali metal ions such as lithium ions, sodium ions, and potassium ions.
[0027] The restoring agent may include one or more compounds of formula (3) and formula (4). In the compounds of formula (3) and formula (4), the radical anion portion is the above-mentioned aromatic hydrocarbon compound in a reduced state, and the metal cation portion is the above-mentioned metal ion.
[0028] [ka]
[0029] In the recovery agent, the solvent is an ether compound. The ether compound may be a compound having an ether skeleton, and may be a cyclic ether or a chain ether. The solvent may be one or more of tetrahydrofuran (THF), dimethoxyethane (DME), diethoxyethane (DEE), dioxolane (DOL), and dioxane (DOX). The solvent is preferably one or more of tetrahydrofuran and dimethoxyethane.
[0030] The recovery agent may be obtained by adding an aromatic hydrocarbon compound and a metal in a metallic state, not an ion state, to a solvent. For example, the recovery agent may be obtained by one or more of formulas (5) and (6). More specifically, the recovery agent may be obtained by reacting naphthalene, diphenyl, or terphenyl with Li metal in a THF solvent, as shown in formulas (7) to (9). Also, the recovery agent may be obtained by reacting naphthalene, diphenyl, or terphenyl with Li metal in a DME solvent, according to formulas (7) to (9). In this way, a recovery agent containing an aromatic hydrocarbon compound in a reduced state and a metal ion can be easily prepared. The recovery agent may be prepared by adding a metal to a precursor obtained by adding an aromatic hydrocarbon compound to a solvent. The recovery agent may be prepared under an inert atmosphere such as an argon atmosphere. The recovery agent may be prepared under a low dew point environment, such as a dew point of -20°C or less, -40°C or less, or -60°C or less. The recovery agent may be prepared by stirring a solvent, an aromatic hydrocarbon compound, and a metal, and a stirrer or the like may be used in this case.
[0031] [ka]
[0032] [ka]
[0033] The restoring agent described above is also referred to as a restoring agent stock solution. In the restoring agent stock solution, the concentrations of the aromatic hydrocarbon compound in a reduced state and the metal ions are each 1.7 mol / L or more and 5.0 mol / L or less. This concentration may be 1.8 mol / L or more and 4.5 mol / L or less, 2.0 mol / L or more and 4.0 mol / L or less, or 2.5 mol / L or more and 3.5 mol / L or less. This concentration may also be equal to or less than the solubility. Also, the number of moles M of the aromatic hydrocarbon compound in a reduced state contained in the restoring agent is A (mol) and the number of moles of metal ion M B (mol) M A / M B is preferably 1 / 1, but may be 1.1 / 1.0 to 1.0 / 1.1, or may be 1.2 / 1.0 to 1.0 / 1.2.
[0034] When the recovery agent contains an electrolyte in addition to the recovery agent stock solution, the electrolyte may be, for example, a nonaqueous electrolyte exemplified in the nonaqueous electrolyte of the nonaqueous electrolyte secondary battery, or may contain an organic solvent exemplified in the nonaqueous electrolyte and a supporting salt exemplified in the nonaqueous electrolyte. The solvent of the electrolyte may be different from the solvent of the recovery agent stock solution, and is preferably one or more of cyclic carbonate, chain carbonate, and cyclic ester, and more preferably one or more of cyclic carbonate and chain carbonate. The solvent of the electrolyte may be one or more of ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The supporting salt of the electrolyte may be different from the solute of the recovery agent stock solution, and may be an inorganic salt such as LiPF6, or an organic salt such as LiFSI. The electrolyte may contain additives such as a film-forming agent and a flame retardant. The composition of the electrolyte may be the same as that of the nonaqueous electrolyte of the nonaqueous electrolyte secondary battery to be recovered. When the recovery agent contains an electrolyte solution, the content of the electrolyte solution may be 30% by volume to 70% by volume, 30% by volume to 60% by volume, or 30% by volume to 50% by volume. When preparing a recovery agent containing an electrolyte solution, the recovery agent stock solution and the electrolyte solution may be mixed, and the recovery agent stock solution and the electrolyte solution may be stirred, or may be stirred using a stirrer or the like.
[0035] The redox potential of the recovery agent may be higher than that of the negative electrode and lower than that of the positive electrode. The redox potential of the recovery agent may be, for example, 0.5 V to 2.5 V, 1.0 V to 2.0 V, or 1.2 V to 1.9 V, based on Li metal.
[0036] [Recovery method for non-aqueous electrolyte secondary batteries] Next, a method for restoring a non-aqueous electrolyte secondary battery will be described. This method for restoring a capacity of a non-aqueous electrolyte secondary battery includes a restoring step of restoring the capacity of the non-aqueous electrolyte secondary battery using the above-mentioned restoring agent.
[0037] (Recovery process) In this process, a recovery agent is injected into the nonaqueous electrolyte secondary battery to recover the capacity of the nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery to be recovered is a battery in a state of capacity degradation (also called a degraded battery), and may be, for example, a battery in a state of capacity degradation relative to the rated capacity of the nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery to be recovered may be an unused product or a used product. Even an unused product may experience capacity degradation due to long-term storage, etc.
[0038] In this step, it is preferable to inject a recovery agent into the nonaqueous electrolyte secondary battery and maintain a predetermined voltage lower than the full charge voltage by applying a constant voltage to recover the capacity of the nonaqueous electrolyte secondary battery. The predetermined voltage is preferably a voltage lower than the full charge voltage and a voltage at which the potential of the positive electrode is higher than the potential of the recovery agent. The full charge voltage may be the upper limit charging voltage set for the nonaqueous electrolyte secondary battery (battery before deterioration). The predetermined voltage may be appropriately determined according to the configuration of the battery to be recovered, and may be, for example, 3.0 V or more and less than 4.1 V, 3.5 V or more and 4.0 V or less, or 3.7 V or more and 4.0 V or less. If the battery is left in an open circuit state without applying a constant voltage, the positive electrode potential decreases as the recovery reaction progresses, and the potential difference between the positive electrode and the recovery agent, which is the driving force of the recovery reaction, decreases as the recovery reaction progresses, and the effect of the recovery agent may gradually attenuate. On the other hand, when the recovery agent is injected and a predetermined voltage is maintained by applying a constant voltage, the decrease in the positive electrode potential is suppressed, and therefore even if the recovery reaction proceeds, the potential difference between the positive electrode, which is the driving force of the reaction, and the recovery agent is kept substantially constant, so that the effect of the recovery agent is unlikely to attenuate, and the capacity of the battery after recovery can be further increased. In addition, the activity of the radical anions of the aromatic hydrocarbon compound is appropriately suppressed by applying a constant voltage, and the residual radical anions of the aromatic hydrocarbon compound are suppressed by effectively using the recovery agent, so that the cycle capacity retention rate of the battery after recovery is also thought to be improved.
[0039] In this step, prior to injecting the recovery agent, the voltage of the nonaqueous electrolyte secondary battery may be adjusted to the above-mentioned predetermined voltage. In this case, for example, the nonaqueous electrolyte secondary battery may be charged by constant current charging (CC charging) or constant current constant voltage charging (CCCV charging) to adjust the voltage of the nonaqueous electrolyte secondary battery. This voltage adjustment is not necessary, but it is preferable that the voltage of the nonaqueous electrolyte secondary battery to be recovered is the above-mentioned predetermined voltage.
[0040] In this step, when injecting the recovery agent, the nonaqueous electrolyte secondary battery may be opened and the recovery agent may be injected to seal the opening, or the recovery agent may be injected into the nonaqueous electrolyte secondary battery by injection or the like to seal the perforation. When injecting the recovery agent, it may be injected under an inert atmosphere such as an argon atmosphere. The recovery agent may be injected so as to contact at least the positive electrode, but may also be mixed with the nonaqueous electrolyte. The injection amount of the recovery agent may be appropriately determined depending on the configuration of the nonaqueous electrolyte secondary battery, the degree of deterioration, and the like. The injection amount of the recovery agent may be, for example, 1% or more and 100% or less, 10% or more and 75% or less, or 25% or more and 50% or less with respect to the volume [mL] of the nonaqueous electrolyte contained in the nonaqueous electrolyte secondary battery. When applying a constant voltage, the constant voltage application may be continued before or during the injection of the recovery agent, or may be started after the injection of the recovery agent while the voltage drop of the nonaqueous electrolyte secondary battery due to the supply of metal ions to the positive electrode is negligibly small (for example, within 5 minutes, preferably within 3 minutes, more preferably within 1 minute). The constant voltage application time can be appropriately determined according to the configuration of the nonaqueous electrolyte secondary battery, the degree of deterioration, the injection amount of the recovery agent, etc. For example, the injection amount of the recovery agent may be constant, and the constant voltage application time may be adjusted according to the configuration and degree of deterioration of the nonaqueous electrolyte secondary battery. The constant voltage application time may be, for example, 1 hour or more and 48 hours or less, 6 hours or more and 36 hours or less, or 12 hours or more and 24 hours or less. In addition, when applying a constant voltage before the completion of the injection of the recovery agent, the constant voltage application time is the constant voltage application time after the completion of the injection of the recovery agent.
[0041] In this step, when the recovery agent is injected, a recovery reaction such as that shown in FIG. 2 is thought to occur. FIG. 2 is an explanatory diagram showing an example of a recovery reaction scheme, and is an explanatory diagram showing a scheme in which the positive electrode active material is a lithium transition metal composite oxide. As shown in FIG. 2, the recovery agent reacts with the radical anion of an aromatic hydrocarbon compound (Are·- in FIG. 2) and a metal ion (Li + ) functions as a reducing agent that donates electrons, and reduces the amount of depleted positive electrode (Li in Figure 2). n-y By acting on MeO2), electrons and metal ions are donated from the reducing agent to the positive electrode, and the capacity can be restored. In particular, in a recovery agent in which the concentration of a compound (reducing agent) containing a radical anion of an aromatic hydrocarbon compound and a metal ion in an ether solvent is 1.7 mol / L or more and 5.0 mol / L or less, the reducing agent has high diffusibility to the positive electrode. Therefore, when this recovery agent is added to a nonaqueous electrolyte secondary battery, the supply of metal ions to the positive electrode is smoothly carried out without being inhibited by diffusion rate control, etc., and the recovery reaction proceeds efficiently, and it is considered that the capacity of the battery after recovery is further improved. In this way, the capacity of the nonaqueous electrolyte secondary battery is restored, and a nonaqueous electrolyte secondary battery with restored capacity (also called a restored battery) is obtained.
[0042] In the recovery agent and the recovery method for a non-aqueous electrolyte secondary battery described above, the capacity of the non-aqueous electrolyte secondary battery can be recovered by injecting the recovery agent into the non-aqueous electrolyte secondary battery. This recovery agent and the recovery method for a non-aqueous electrolyte secondary battery provide a novel recovery method that does not require a third electrode. In addition, in the recovery agent and the recovery method for a non-aqueous electrolyte secondary battery, the recovery agent is used in which the concentrations of the reduced aromatic hydrocarbon compound and the metal ion relative to the ether solvent are 1.7 mol / L or more and 5.0 mol / L or less, respectively, to further improve the capacity of the battery after recovery.
[0043] It goes without saying that the present disclosure is in no way limited to the above-described embodiment, and can be embodied in various forms as long as it falls within the technical scope of the present disclosure.
[0044] For example, in the above-mentioned embodiment, the method for recovering a nonaqueous electrolyte secondary battery has been described, but in this method for recovering a nonaqueous electrolyte secondary battery, a new nonaqueous electrolyte secondary battery with recovered capacity can be manufactured using a nonaqueous electrolyte secondary battery with deteriorated capacity. Therefore, the method for recovering a nonaqueous electrolyte secondary battery can also be said to be a method for manufacturing a nonaqueous electrolyte secondary battery. A nonaqueous electrolyte secondary battery may be manufactured using the above-mentioned method for recovering a nonaqueous electrolyte secondary battery. The method for manufacturing a nonaqueous electrolyte secondary battery may include a battery preparation step of preparing a capacity-deteriorated nonaqueous electrolyte secondary battery using a metal ion as a carrier ion, and a recovery step of recovering the capacity of the nonaqueous electrolyte secondary battery using the above-mentioned method for recovering a nonaqueous electrolyte secondary battery. The nonaqueous electrolyte secondary battery prepared in the battery preparation step may be the same as the deteriorated battery described in the above-mentioned embodiment. EXAMPLES
[0045] Hereinafter, examples of recovering a lithium ion battery using the method for recovering a non-aqueous electrolyte secondary battery of the present disclosure will be described as examples. Note that Experimental Examples 1 to 4 correspond to working examples, and Experimental Examples 5 to 10 correspond to reference examples. The present disclosure is not limited to the following examples, and it goes without saying that the present disclosure can be implemented in various aspects as long as it falls within the technical scope of the present disclosure.
[0046] [Experimental Example 1] (Non-aqueous electrolyte secondary battery (battery before deterioration)) The positive electrode is LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A positive electrode composite material containing 92 wt% O2 (NCM, Toda Kogyo Co., Ltd.), 5 wt% acetylene black (Denka Co., Ltd.), and 3 wt% polyvinylidene fluoride (Kureha Co., Ltd.) was used with a weight of 7 mg / cm. 2 The negative electrode was made of a negative electrode composite material containing 98 wt% graphite (OMAC1.5s, Osaka Gas Chemicals), 1 wt% carboxymethyl cellulose (Daicel), and 1 wt% styrene butadiene rubber (JSR), with a weight of 4 mg / cm. 2The electrolyte was prepared by dissolving LiPF6 at a concentration of 1.1M in a mixed solvent containing 30 vol% ethylene carbonate, 40 vol% dimethyl carbonate, and 30 vol% ethyl methyl carbonate. A polypropylene separator impregnated with 1 mL of electrolyte was sandwiched between the positive and negative electrodes to prepare a laminate cell. This was used as the pre-degradation battery. The electrode area of the cell was 10 cm2 for both the positive and negative electrodes. 2 When the resistance of the battery before deterioration was measured with a digital multimeter, the cell resistance was 10 Ω cm 2 In this nonaqueous electrolyte secondary battery, the lower limit discharge voltage was 3.0V and the upper limit charge voltage was 4.1V, which are determined according to the battery configuration.
[0047] (Deteriorated battery) The laminated cell thus produced was charged to a capacity (SOC=50%) equivalent to 50% of the electric capacity of the cell in the voltage range of 3.0V to 4.1V, and Li was extracted from the positive electrode to obtain a positive electrode with a simulated reduced capacity (also called a degraded positive electrode). The cell was then disassembled, and the degraded positive electrode was removed. A laminated cell was produced in the same manner as the pre-degraded battery, except that the degraded positive electrode was used as the positive electrode. This was used as a degraded battery. The degraded battery was CC-charged at 0.9 mA to 4.1V, and then CC-discharged at 0.9 mA to 3.0V, and the discharge capacity was measured.
[0048] (Recovery Agent) In an inert atmosphere, naphthalene was dissolved in tetrahydrofuran (THF) solvent to a concentration of 2.0 mol / L, and then 2.0 mol / L of lithium metal was added and stirred, and a dark green radical anion liquid composition (lithium naphthalenide + THF) was prepared as a recovery agent stock solution by the reaction shown in the above formula (7). In addition, lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved in a mixed solvent containing 30 vol% ethylene carbonate, 40 vol% dimethyl carbonate, and 30 vol% ethyl methyl carbonate to a concentration of 1.1 M to prepare an electrolyte solution. Then, the recovery agent stock solution and the electrolyte solution were mixed in a volume ratio of 5:5 to prepare a recovery agent.
[0049] (Recovery of degraded batteries) The deteriorated battery was CC-charged at 0.9 mA to adjust the cell voltage to 4.0 V (adjustment process), and part of the deteriorated battery was opened under an argon atmosphere, 0.5 mL of recovery agent was injected with a pipette, the opened part was sealed, and immediately after (in the experimental example, within 3 minutes of injecting the recovery agent), a constant voltage of 4.0 V was applied to the deteriorated battery, and the application of the constant voltage was continued for 24 hours (recovery process). In this way, the deteriorated battery was restored, and a restored battery was obtained. During the constant voltage application, the current density [mA / cm 2 ] was measured, and the charge capacity [mAh] obtained when a constant voltage was applied (also referred to as the capacity at constant voltage) was calculated (see FIG. 3).
[0050] (Recovery battery evaluation) The recovered battery was CC-charged at 0.9 mA in the voltage range of 3.0 V to 4.1 V, and then CC-discharged at 0.9 mA to 3.0 V, and the discharge capacity was measured. The recovered capacity was calculated by subtracting the discharge capacity of the deteriorated battery from the discharge capacity of the recovered battery (see Figure 4).
[0051] [Experimental Examples 2-3] Experimental Example 2 was the same as Experimental Example 1, except that the concentrations of naphthalene and lithium in the THF solvent were changed to 3.0 mol / L. Experimental Example 3 was the same as Experimental Example 1, except that the concentrations of naphthalene and lithium in the THF solvent were changed to 4.0 mol / L.
[0052] [Experimental Example 4] Experimental Example 4 was the same as Experimental Example 1, except that in the recovery agent, dimethoxyethane (DME) solvent was used instead of THF solvent, and the supporting salt of the electrolyte was changed from LiFSI to LiPF6.
[0053] [Experimental Example 5] Experimental Example 5 was the same as Experimental Example 1, except that the concentration of naphthalene and lithium in the THF solvent in the recovery agent was changed to 1.0 mol / L.
[0054] [Experimental Example 6] Experimental Example 6 was the same as Experimental Example 5, except that in the recovery agent, the supporting salt of the electrolyte was changed from LiFSI to LiPF6.
[0055] [Experimental Examples 7-9] Experimental Example 7 was the same as Experimental Example 5, except that in the recovery agent, the supporting salt concentration of the electrolyte was changed to 1.5 M. Experimental Example 8 was the same as Experimental Example 5, except that in the recovery agent, the supporting salt concentration of the electrolyte was changed to 2.0 M. Experimental Example 9 was the same as Experimental Example 5, except that the supporting salt concentration of the electrolyte was changed to 3.0 M.
[0056] [Experimental Example 10] Experimental Example 10 was the same as Experimental Example 4, except that the concentration of naphthalene and lithium in the DME solvent in the recovery agent was changed to 1.5 mol / L. In addition to Experimental Example 10, an attempt was made to prepare a recovery agent in which the concentration of naphthalene and lithium in the DME solvent was changed to 3.0 mol / L, but some of the recovery agent did not dissolve and remained undissolved. No such undissolved residue was present in the recovery agents of Experimental Examples 1 to 10.
[0057] The results of Experimental Examples 1 to 10 are summarized in Table 1. In addition, the relationship between the capacity at constant voltage and the recovered capacity for Experimental Examples 1 to 10 is summarized in FIG. 5. As shown in FIG. 5, it was found that the recovered capacity is roughly proportional to the capacity at constant voltage. As shown in Table 1 and FIG. 5, Experimental Examples 1 to 4, in which the concentrations of naphthalene and lithium were 2 mol / L or more and 4 mol / L or less, showed high recovered capacity. On the other hand, in Experimental Examples 5, 7 to 9, the supporting salt concentration of the electrolyte contained in the recovery agent was increased, but the recovered capacity was hardly improved, and when the supporting salt concentration was about 2 mol / L, the recovered capacity decreased. From this, it was found that the recovered capacity can be improved by adjusting the concentration of naphthalene and lithium in the recovery agent relative to the solvent, which is an ether compound.
[0058] The reason why Experimental Examples 1 to 4 showed high recovery capacities is presumed to be as follows. + The anion radicals of arenes such as naphthalene and biphenyl function as reducing agents that donate electrons, so by applying them to a deteriorated positive electrode, the reducing agent transfers electrons and Li to the positive electrode. + It was speculated that the capacity could be restored by providing Li + Li, which has a recovery effect by increasing the concentration of anion radicals of arenes such as naphthalene and biphenyl. + It was speculated that improving the diffusivity of the anion radicals of arenes such as naphthalene and biphenyl would result in efficient recovery and a high recovery capacity.
[0059] The preferred range of the concentrations of naphthalene and lithium was examined using FIG. 6. As shown in FIG. 6, it was inferred that if the concentrations of naphthalene and lithium are 1.7 mol / L or more and 5.0 mol / L or less, the recovery capacity is, for example, 1.2 mAh or more in both cases of THF and DME, which is preferable. As described above, it was difficult to dissolve naphthalene and lithium at 3.0 mol / L or more in the case of DME as the solvent. For this reason, it was inferred that, for example, it is more preferable to set the concentrations of naphthalene and lithium to 1.7 mol / L or more and less than the solubility in the case of DME as the solvent.
[0060] [Table 1] [Explanation of symbols]
[0061] 20 nonaqueous electrolyte secondary battery, 21 battery case, 22 positive electrode, 23 negative electrode, 24 separator, 25 gasket, 26 sealing plate, 27 nonaqueous electrolyte.
Claims
1. A recovery agent for recovering the capacity of a non-aqueous electrolyte secondary battery having a metal ion as a carrier ion, a solvent that is an ether compound, and the solvent is an aromatic hydrocarbon compound in a reduced state, the aromatic hydrocarbon compound in a reduced state and the metallic ion in a solvent that is an ether compound, the aromatic hydrocarbon compound in a reduced state and the metallic ion each having a concentration of 1.7 mol / L or more and 5.0 mol / L or less; Recovery agent.
2. The recovery agent has a concentration of the reduced aromatic hydrocarbon compound and the metal ion in the solvent of 2.0 mol / L or more and 4.0 mol / L or less. The recovery agent according to claim 1.
3. The restoring agent contains, as the reduced aromatic hydrocarbon compound, at least one of a reduced product of a compound of formula (1) and a reduced product of a compound of formula (2). The recovery agent according to claim 1 or 2. [Formula 1]
4. The recovery agent includes one or more of tetrahydrofuran and dimethoxyethane as the solvent; The recovery agent according to any one of claims 1 to 3.
5. The recovery agent includes a recovery agent stock solution containing the aromatic hydrocarbon compound in a reduced state, metal ions of the same type as the carrier ions, and the solvent, and an electrolyte solution. The recovery agent according to any one of claims 1 to 4.
6. A method for recovering the capacity of a non-aqueous electrolyte secondary battery that uses metal ions as carrier ions, comprising the steps of: A recovery step of injecting the recovery agent according to any one of claims 1 to 5 into the nonaqueous electrolyte secondary battery to recover the capacity of the nonaqueous electrolyte secondary battery; Including, A method for recovering a non-aqueous electrolyte secondary battery.
7. In the recovery step, the recovery agent is injected into the nonaqueous electrolyte secondary battery, and a predetermined voltage lower than a full charge voltage is maintained by applying a constant voltage. The method for restoring a nonaqueous electrolyte secondary battery according to claim 6 .
8. In the recovery process, the predetermined voltage is set to 3.0 V or more and 4.0 V or less. The method for restoring a nonaqueous electrolyte secondary battery according to claim 7 .
9. a battery preparation step of preparing a capacity-degraded nonaqueous electrolyte secondary battery having metal ions as carrier ions; The method for recovering a capacity of a nonaqueous electrolyte secondary battery according to any one of claims 6 to 8, comprising: The method for producing a non-aqueous electrolyte secondary battery includes the steps of:
Citation Information
Patent Citations
Liquid composition and manufacturing method thereof, non-aqueous electrolyte secondary battery and capacity recovery method thereof
CN112490506A
Electrolyte for lithium cell
JP1989286262A
Lithium second battery
JP1999185809A
Method for producing lithium-containing iron oxyhydroxide and nonaqueous electrolyte electrochemical cell using electrode containing lithium-containing iron oxyhydroxide obtained by the same
JP2005281128A
Nonaqueous electrolytic secondary battery