Composition for cured resin, cured product of said composition, methods for producing said composition and said cured product, and semiconductor device

A cured resin composition using a polyfunctional benzoxazine and epoxy compound with a norbornane structure addresses the need for high heat resistance and room temperature stability, achieving a glass transition temperature of 220°C or higher for semiconductor applications.

JP7569784B2Active Publication Date: 2024-10-18ENEOS MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021516225
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-23
Publication Date
2024-10-18
Estimated Expiration
2040-04-23

AI Technical Summary

Technical Problem

There is a need for a cured resin composition that exhibits excellent room temperature stability and high heat resistance, suitable for applications such as adhesives, encapsulants, and semiconductor sealing materials, as existing compositions do not adequately meet these requirements.

Method used

A composition comprising a polyfunctional benzoxazine compound, a specific epoxy compound with a norbornane structure, and a curing agent, with a weight average molecular weight between 350 and 650, which when cured, forms a resin with enhanced stability and heat resistance.

Benefits of technology

The composition achieves a cured product with a glass transition temperature of 220°C or higher, demonstrating excellent heat resistance and stability at room temperature, making it suitable for semiconductor devices and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569784000001
    Figure 0007569784000001
  • Figure 0007569784000002
    Figure 0007569784000002
  • Figure 0007569784000003
    Figure 0007569784000003
Patent Text Reader

Abstract

[Problem] To provide: a curable-resin composition that has excellent room-temperature stability and is for producing a cured product that is highly heat-resistant, etc.; a cured product of the curable-resin composition; a production method for the curable-resin composition and the cured product; and a semiconductor device that uses the cured product as a sealing material. [Solution] A curable-resin composition that contains (A) a polyfunctional benzoxazine compound that has at least two benzoxazine rings, (B) an epoxy compound that includes at least one type of epoxy compound that has at least one norbornane structure and at least two epoxy groups, and (C) a curing agent, the polystyrene-equivalent weight average molecular weight of a mixture of (A), (B), and (C) being 350–650. A cured product of the curable-resin composition. A production method for the curable-resin composition and the cured product. A semiconductor device in which a semiconductor element is arranged in a cured product that is formed by curing a curable-resin composition that contains components (A)–(C) and, optionally, (D) and (E).
Need to check novelty before this filing date? Find Prior Art

Description

REFERENCE TO RELATED APPLICATIONS

[0001] This patent application claims priority to Japanese Patent Application No. 2019-086689, filed on April 26, 2019, the entire disclosure of which is incorporated herein by reference. [Technical field]

[0002] The present invention relates to a composition for curing resins for obtaining a highly heat-resistant cured product, a cured product thereof, and a method for producing the composition for curing resins and the cured product.Furthermore, the present invention relates to a semiconductor device using the cured product as an encapsulant. [Background technology]

[0003] Thermosetting resins are used for various applications such as semiconductor encapsulation materials and fiber-reinforced plastics, and benzoxazine compounds are used as one of the raw materials for them. A benzoxazine compound refers to a compound having a benzoxazine ring that contains a benzene skeleton and an oxazine skeleton, and benzoxazine resins, which are cured products (polymers), have excellent physical properties such as heat resistance and mechanical strength, and are used as high-performance materials in many fields.

[0004] Patent Document 1 discloses an epoxy resin composition containing a benzoxazine compound having a specific structure and an epoxy compound containing an aromatic ring in the main chain, and describes that the epoxy resin has a glass transition point (Tg) of about 200°C or higher. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-254895 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the fields of adhesives, sealing materials, paints, matrix resins for composite materials, etc., there is a demand for curable resin compositions that are highly heat-resistant resin cured products and have excellent room temperature stability so as to be compatible with various usage environments and market conditions. However, a curable resin composition that has excellent room temperature stability to obtain a highly heat-resistant cured product has not yet been obtained.

[0007] Therefore, the present invention aims to provide a curable resin composition having excellent room temperature stability for obtaining a highly heat-resistant cured product. Another object of the present invention is to provide a cured product obtained by curing the above-mentioned curable resin composition, as well as a method for producing the above-mentioned curable resin composition and the cured product. Another object of the present invention is to provide a semiconductor device using the above-mentioned curable resin composition as an encapsulant. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have developed a composition for a curable resin, which contains (A) a polyfunctional benzoxazine compound, (B) a specific epoxy compound, and (C) a curing agent, and which has a specific weight average molecular weight in polystyrene equivalent, and have found that the composition for a curable resin has excellent stability at room temperature and that the cured product thereof has excellent heat resistance, thereby completing the present invention.

[0009] That is, according to the present invention, the following inventions are provided. [1] (A) at least one polyfunctional benzoxazine compound having at least two benzoxazine rings, selected from a polyfunctional benzoxazine compound having a structural unit of formula (1) and a polyfunctional benzoxazine compound represented by a structure of formula (2); (B) an epoxy compound including at least one epoxy compound having at least one norbornane structure and at least two epoxy groups; (C) a hardener; Contains A composition for curable resins, comprising (A), (B) and (C), the weight average molecular weight of which is calculated as polystyrene of 350 or more and 650 or less. [ka] [In formula (1), R represents a chain alkyl group having 1 to 12 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and the aryl group may have a halogen or a chain alkyl group having 1 to 12 carbon atoms as a substituent. Z represents hydrogen, a hydrocarbon group having 1 to 8 carbon atoms, and / or a linking group, which may be the same or different, and at least one of them is a linking group, and the benzoxazine rings are linked to each other by the linking group.] [ka] [In formula (2), L is a divalent organic group having 1 to 5 aromatic rings or an alkylene group having 2 to 10 carbon atoms, and the organic group and the alkylene group may contain oxygen and / or sulfur.] [2] The composition for curable resins according to [1], wherein the (B) epoxy compound having at least one norbornane structure and at least two epoxy groups is an alicyclic epoxy compound. [3] The composition for curable resins according to [1] or [2], wherein the (B) epoxy compound having at least one norbornane structure and at least two epoxy groups does not have a glycidyl group. [4] The composition for curable resins according to any one of [1] to [3], wherein the (B) epoxy compound further comprises at least one selected from the group consisting of epoxy compounds having a biphenyl skeleton, trisphenolmethane type epoxy compounds, naphthalene type epoxy compounds, novolac type epoxy compounds, and phenol aralkyl type epoxy compounds. [5] The composition for curable resins according to any one of [1] to [4], further comprising (D) a curing accelerator. [6] The composition for curable resins according to any one of [1] to [5], further comprising (E) an inorganic filler. [7] A cured product obtained by curing the composition for a curable resin according to any one of [1] to [6]. [8] A semiconductor device comprising a semiconductor element disposed in a cured product obtained by curing the composition for a curable resin according to any one of [1] to [6]. [9] A method for producing a composition for curable resin according to any one of [1] to [6], (A) at least one polyfunctional benzoxazine compound having at least two benzoxazine rings, selected from a polyfunctional benzoxazine compound having a structural unit of formula (1) and a polyfunctional benzoxazine compound represented by a structure of formula (2); (B) an epoxy compound including at least one epoxy compound having at least one norbornane structure and at least two epoxy groups; (C) a hardener; to obtain a mixture; Processing the mixture into a powder, pellet, or granular curable resin composition. The method for producing a composition for cured resin comprising the steps of: [ka] [In formula (1), R represents a chain alkyl group having 1 to 12 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and the aryl group may have a halogen or a chain alkyl group having 1 to 12 carbon atoms as a substituent. Z represents hydrogen, a hydrocarbon group having 1 to 8 carbon atoms, and / or a linking group, which may be the same or different, and at least one of them is a linking group, and the benzoxazine rings are linked to each other by the linking group.] [ka] [In formula (2), L is a divalent organic group having 1 to 5 aromatic rings or an alkylene group having 2 to 10 carbon atoms, and the organic group and the alkylene group may contain oxygen and / or sulfur.]

[10] The method according to [9], further comprising mixing (D) a curing accelerator and / or (E) an inorganic filler in the step of obtaining the mixture.

[11] A method for producing a cured product, comprising the step of heating the curable resin composition produced by the method according to [9] or

[10] at 150 to 300°C for 20 seconds to 5 hours to cure the composition. Effect of the Invention

[0010] The curable resin composition of the present invention is a novel curable resin composition containing components (A) to (C) and, if desired, components (D) and (E), and is characterized in that the curable resin composition has excellent room temperature stability and the cured product thereof has excellent heat resistance. Therefore, the curable resin composition of the present invention can be used in applications that require room temperature stability and heat resistance in the cured product, such as adhesives, encapsulants, paints, and matrix resins for composite materials. The curable resin composition of the present invention exhibits excellent encapsulation performance, particularly as a semiconductor element encapsulant, and can contribute to high reliability of semiconductor devices. In addition, according to the present invention, a blend consisting of components (A) to (C) can be used as an agent for improving the room temperature stability of the curable resin composition and / or the heat resistance of the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Composition for cured resin] The present invention will be described in detail below. The "compound" in components (A), (B) and (C) of the present invention includes not only the monomers shown in the respective formulas, but also oligomers in which the monomers are polymerized in small amounts, that is, prepolymers before forming a cured resin. Therefore, the composition for cured resin of the present invention may be a curable resin composition.

[0012] (Component A) The component (A) constituting the curable resin composition is at least one type of polyfunctional benzoxazine compound having at least two benzoxazine rings, selected from polyfunctional benzoxazine compounds having a structural unit of formula (1) and polyfunctional benzoxazine compounds having a structure of formula (2). In addition, Z in the above formula (1) represents hydrogen, a substituent and / or a linking group (spacer), which may be the same or different, and at least one is a linking group, and the benzoxazine rings are linked to each other by the linking group. In addition, the linking group here includes two benzoxazine rings directly bonded without any other group. In addition, the above-mentioned substituent can be, for example, a hydrocarbon group having 1 to 8 carbon atoms. Therefore, the above formula (1) represents a structural unit of a compound in which two or more benzoxazine rings are linked at a benzene ring portion, among the options for component (A).

[0013] More specifically, the polyfunctional benzoxazine compound of formula (1) can be represented by the structure shown in formula (1a). [ka] [In formula (1a), R represents a chain alkyl group having 1 to 12 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and the aryl group may have a halogen or a chain alkyl group having 1 to 12 carbon atoms as a substituent. R may be the same or different. X represents hydrogen or a hydrocarbon group having 1 to 8 carbon atoms, and may be the same or different. Y represents an alkylene group having 1 to 6 carbon atoms, oxygen, sulfur, an SO2 group, or a carbonyl group. m is 0 or 1. n is an integer of 1 to 10.]

[0014] Specific examples of R in the formulae (1) and (1a) include the following groups. Examples of the chain alkyl group having 1 to 12 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a t-butyl group. Examples of the cyclic alkyl group having 3 to 8 carbon atoms include a cyclopentyl group and a cyclohexyl group. Examples of the aryl group having 6 to 14 carbon atoms include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a phenanthryl group, and a biphenyl group. The aryl group having 6 to 14 carbon atoms may be substituted, and examples of the substituent include a chain alkyl group having 1 to 12 carbon atoms or a halogen. Examples of the aryl group having 6 to 14 carbon atoms and substituted with a chain alkyl group having 1 to 12 carbon atoms or a halogen include an o-tolyl group, a m-tolyl group, a p-tolyl group, a xylyl group, an o-ethylphenyl group, a m-ethylphenyl group, a p-ethylphenyl group, an ot-butylphenyl group, a mt-butylphenyl group, a pt-butylphenyl group, an o-chlorophenyl group, and an o-bromophenyl group. In terms of ease of handling, R is preferably selected from a methyl group, an ethyl group, a propyl group, a phenyl group, and a p-tolyl group. Furthermore, component (A) may be a mixture of two or more compounds represented by formula (1) or (1a), each of which has a different R.

[0015] Examples of the hydrocarbon group having 1 to 8 carbon atoms in Z in formula (1) and X in formula (1a) include an alkyl group, an aryl group, and an aralkyl group, and preferably an aryl group.

[0016] Examples of the polyfunctional benzoxazine compound represented by formula (1) or (1a) include a compound represented by the following formula (1X) and an oligomer in which the compound is polymerized in small amounts. [ka] JPEG0007569784000007.jpg123162

[0017] The polyfunctional benzoxazine compound of formula (2), which is another option for component (A), is a compound in which the nitrogen atoms (N atoms) of two benzoxazine rings are bonded to each other via a linking group L. [ka] [In formula (2), L is a divalent organic group having 1 to 5 aromatic rings or an alkylene group having 2 to 10 carbon atoms, and the organic group and the alkylene group may contain oxygen and / or sulfur.] The composition of the present invention may contain, as component (A), a plurality of polyfunctional benzoxazine compounds represented by formula (2) each having different L's.

[0018] When L in formula (2) is a group having an aromatic ring, the number of aromatic rings is 1 to 5, and examples thereof include monocyclic compounds, polycyclic compounds, and condensed ring compounds. Furthermore, L may contain at least one selected from the group consisting of oxygen and sulfur. A specific example is a group shown in the following formula (3). [ka]

[0019] When L in formula (3) is an alkylene group, the carbon number thereof is, for example, 1 to 10, and preferably 1 to 6. Specific examples of the alkylene group include a methylene group, an ethylene group, and an isopropylidene group, and preferably a methylene group.

[0020] Examples of the polyfunctional benzoxazine compound of formula (2) include a compound represented by the following formula (2X) and an oligomer obtained by polymerizing the compound, for example, an oligomer obtained by polymerizing a small amount of the compound. [ka]

[0021] The polyfunctional benzoxazine compound of component (A) may be a commercially available product, such as bisphenol F-aniline (Fa) type benzoxazine or phenol-diaminodiphenylmethane (Pd) type benzoxazine (both manufactured by Shikoku Kasei Co., Ltd.).

[0022] (Component B) Component (B) constituting the curable resin composition is an epoxy compound. Such an epoxy compound includes at least one epoxy compound having at least one norbornane structure and at least two epoxy groups. The composition of the present invention may further include an epoxy compound other than the epoxy compound having at least one norbornane structure and at least two epoxy groups as component (B) as long as it does not impede the effects of the present invention. Examples of epoxy compounds other than the epoxy compound having at least one norbornane structure and at least two epoxy groups include epoxy compounds having a biphenyl skeleton, trisphenolmethane type epoxy compounds, naphthalene type epoxy compounds, novolac type epoxy compounds, and phenol aralkyl type epoxy compounds, and are preferably epoxy compounds having a biphenyl skeleton and trisphenolmethane type epoxy compounds. The epoxy compounds other than the epoxy compound having at least one norbornane structure and at least two epoxy groups may be of multiple types.

[0023] (Epoxy compound having at least one norbornane structure and at least two epoxy groups) The epoxy compound having at least one norbornane structure and at least two epoxy groups is not particularly limited as long as it does not interfere with the effects of the present invention, but is preferably an alicyclic epoxy compound, and more preferably has an epoxy structure bonded to a 5-membered ring, a 6-membered ring or a norbornane ring as shown in the following formula (4). Here, the alicyclic epoxy compound is a compound having an epoxy group, which is a reactive group, on an alicyclic skeleton. Therefore, a more preferred alicyclic epoxy compound is an epoxy compound having a structure in which a carbon-carbon bond forming a 5-membered ring, a 6-membered ring or a norbornane ring and a carbon-carbon bond of an epoxy group are shared as shown in the following formula (4), and is preferably a compound without a glycidyl group. By using such a compound, high heat resistance can be achieved. These may be used alone or in combination of two or more. [ka]

[0024] A specific example of the alicyclic epoxy compound is a compound represented by the following formula (5). [ka]

[0025] A production example of the polyfunctional epoxy compound of component (B) will be described. The compound of the following formula (5-1) can be produced, for example, by synthesizing a compound (a) having the following norbornane structure by the Diels-Alder reaction of butadiene and dicyclopentadiene, and then reacting the compound (a) with metachloroperbenzoic acid as shown in the following formula (6). [ka]

[0026] The compound of the following formula (5-2) can be produced, for example, by synthesizing a compound (b) (tricyclopentadiene) having the following norbornane structure by the Diels-Alder reaction of cyclopentadiene and dicyclopentadiene, and then reacting the compound (b) with metachloroperbenzoic acid as shown in the following formula (7). [ka]

[0027] The compound of the following formula (5-3) can be produced, for example, by synthesizing a compound (c) having the following norbornane structure by the Diels-Alder reaction of butadiene and cyclopentadiene, and then reacting the compound (c) with metachloroperbenzoic acid as shown in the following formula (8). [ka]

[0028] The compound of the following formula (5-4) can be produced, for example, by reacting dicyclopentadiene with potassium peroxymonosulfate (Oxone). The dicyclopentadiene diepoxide, which is the compound of formula (5-4), may be a commercially available product, and an example of a commercially available product is dicyclopentadiene diepoxide manufactured by SHANDONG QIHUAN BIOCHEMICAL CO., LTD. [ka]

[0029] (Epoxy compounds having a biphenyl skeleton) The epoxy compound having a biphenyl skeleton is not particularly limited as long as it does not impede the effects of the present invention, but is preferably an epoxy compound represented by the structure of the following formula (9-1) or formula (9-2). As the epoxy compound having a biphenyl skeleton, either one of the epoxy compound represented by the structure of the following formula (9-1) and the epoxy compound represented by the structure of the following formula (9-2) may be used, or a mixture of the two may be used. A more preferred epoxy compound having a biphenyl skeleton is an epoxy compound represented by the structure of the following formula (9-1). [ka] [In formula (9-1), R1 is a substituent and is an alkyl group having 1 to 4 carbon atoms, and may be the same or different. m is the number of the substituents R1 and is an integer of 0 to 4. n is an average value of 1 to 5.] [ka] [In formula (9-2), R1 to R8 are a hydrogen atom, a halogen atom, or an alkyl group having 1 to 4 carbon atoms, and may be the same or different.]

[0030] In formula (9-1), m is preferably 0 to 2, more preferably 0. In formula (9-1), n ​​is preferably 1 to 5, more preferably 1 to 4. Examples of the alkyl group having 1 to 4 carbon atoms in the substituent R1 in formula (9-1) include a methyl group, an ethyl group, a propyl group, and a butyl group. As the substituent R1, a methyl group and an ethyl group are preferable. Furthermore, the epoxy compound having a biphenyl skeleton may be a mixture of compounds represented by formula (9-1) having different R1, m, and n.

[0031] Examples of the alkyl group having 1 to 4 carbon atoms in R1 to R8 of formula (9-2) include a methyl group, an ethyl group, a propyl group, and a butyl group. R1, R2, R3, R4, R5, R6, R7, and R8 are preferably a hydrogen atom or a methyl group. Furthermore, the epoxy compound having a biphenyl skeleton may be a mixture of compounds represented by formula (9-2) in which R1 to R8 are different from each other.

[0032] According to another preferred embodiment of the present invention, the epoxy compound having a biphenyl skeleton used in the present invention is a compound represented by formula (9-2) in which R1, R2, R3 and R4 are alkyl groups having 1 to 4 carbon atoms, and R5, R6, R7 and R8 are hydrogen atoms. According to another further preferred embodiment of the present invention, the epoxy compound having a biphenyl skeleton used in the present invention is a compound represented by formula (9-2) in which R1, R2, R3 and R4 are methyl groups, and R5, R6, R7 and R8 are hydrogen atoms.

[0033] As the epoxy compound having a biphenyl skeleton, a commercially available product can also be used. Commercially available epoxy compounds represented by the structure of formula (9-1) include NC-3000 (trade name, Nippon Kayaku Co., Ltd.), NC-3000-L (trade name, Nippon Kayaku Co., Ltd.), NC-3000-H (trade name, Nippon Kayaku Co., Ltd.), NC-3000-FH-75M (trade name, Nippon Kayaku Co., Ltd.), and NC-3100 (trade name, Nippon Kayaku Co., Ltd.). Commercially available epoxy compounds represented by the structure of formula (9-2) include YX4000 (trade name, Mitsubishi Chemical Co., Ltd.), YX4000H (trade name, Mitsubishi Chemical Co., Ltd.), and YL6121H (trade name, Mitsubishi Chemical Co., Ltd.). These may be used alone or in combination of two or more.

[0034] (Trisphenolmethane type epoxy compound) The trisphenolmethane type epoxy compound is not particularly limited as long as it does not impede the effects of the present invention, but is preferably an epoxy compound represented by the structure of the following formula (10). [ka] [In formula (10), R is a substituent, each of which is independently an alkyl group having 1 to 6 carbon atoms, an allyl group, or a phenyl group. m is the number of the substituents R, each of which is an integer of 0 to 3. n is an average value, and 0≦n≦10.]

[0035] In formula (10), m is preferably 0 to 2, and more preferably 0. In formula (10), n is preferably 0 to 5. Examples of the alkyl group having 1 to 6 carbon atoms in the substituent R in formula (10) include a methyl group, an ethyl group, a propyl group, a butyl group, and a cyclohexyl group. The substituent R is preferably a methyl group. Furthermore, the trisphenolmethane type epoxy compound may be a mixture of compounds represented by formula (10) having different R, m, and n.

[0036] As the trisphenolmethane type epoxy compound, commercially available products can be used. Examples of commercially available products include EPPN-501H (trade name, manufactured by Nippon Kayaku Co., Ltd.), EPPN-501HY (trade name, manufactured by Nippon Kayaku Co., Ltd.), EPPN-502H (trade name, manufactured by Nippon Kayaku Co., Ltd.), and EPPN-503 (trade name, manufactured by Nippon Kayaku Co., Ltd.). These may be used alone or in combination of two or more.

[0037] (Naphthalene type epoxy compound) The naphthalene type epoxy compound is not particularly limited as long as it does not impede the effects of the present invention, and examples thereof include naphthylene ether type epoxy compounds, binaphthalene type epoxy compounds, naphthol type epoxy compounds, and the like. Of these, naphthylene ether type epoxy compounds and binaphthalene type epoxy compounds are preferred.

[0038] (Naphthylene ether type epoxy compound) The naphthylene ether type epoxy compound is not particularly limited as long as it does not impede the effects of the present invention, but is preferably an epoxy compound represented by the structure of the following formula (11). [ka] [In formula (11), n ​​is an integer of 1 to 20, l is an integer of 0 to 2, R1 is a substituent, each of which is independently a benzyl group, an alkyl group, or a structure represented by formula (11a), and R2 is independently a hydrogen atom or a methyl group.] [ka] [In formula (11a), each Ar is independently a phenylene group or a naphthylene group, each R2 is independently a hydrogen atom or a methyl group, and m is an integer of 1 or 2.] Furthermore, the naphthylene ether type epoxy compound may be a mixture of compounds represented by formula (11) in which R1, R2, l and n are different from each other.

[0039] An example of the naphthylene ether type epoxy compound represented by the above general formula (11) is one represented by formula (11-1). [ka] (In formula (11-1), n ​​is an integer of 1 or more and 20 or less, preferably an integer of 1 or more and 10 or less, more preferably an integer of 1 or more and 8 or less. R is a substituent, each of which is independently a benzyl group, an alkyl group, or a structure represented by the following general formula (11a-1), or is absent, and preferably the substituent R is absent.) [ka] (In the above general formula (11a-1), m is an integer of 1 or 2.)

[0040] Examples of the naphthylene ether type epoxy compound represented by formula (11-1) include those represented by formulas (11-2) to (11-6). [ka] [ka] [ka] [ka] [ka]

[0041] As the naphthylene ether type epoxy compound, commercially available products can be used. Commercially available naphthylene ether type epoxy compounds include HP-6000 (trade name, DIC Corporation), EXA-7310 (trade name, DIC Corporation), EXA-7311 (trade name, DIC Corporation), EXA-7311L (trade name, DIC Corporation), and EXA-7311-G3 (trade name, DIC Corporation). These may be used alone or in combination of two or more.

[0042] (Binaphthalene type epoxy compound) The binaphthalene type epoxy compound is not particularly limited as long as it does not impair the effects of the present invention and does not include the naphthylene ether type epoxy compound, but is preferably an epoxy compound represented by the structure of the following formula (12). [ka] [In formula (12), X represents an alkylene group having 1 to 8 carbon atoms. R1 to R4 represent any one of a group represented by the following formula (12a), a hydrogen atom, a halogen atom, a phenyl group, and an alkyl group having 1 to 4 carbon atoms. R1 to R4 may be added to either ring of the naphthalene skeleton, or may be added to both rings at the same time. Among R1 to R4, it is necessary to include, on average, at least two or more groups represented by the following general formula (12a), and the other Rs may be the same or different from each other.] [ka] Furthermore, the binaphthalene type epoxy compound may be a mixture of compounds represented by the formula (12) in which R1 to R4 and X are different from each other.

[0043] The binaphthalene type epoxy compound includes a bifunctional or higher binaphthalene type epoxy compound, preferably a bifunctional, trifunctional or tetrafunctional binaphthalene type epoxy compound, more preferably a bifunctional binaphthalene type epoxy compound represented by the following formula (12-1). [ka]

[0044] Commercially available binaphthalene type epoxy compounds can also be used. Commercially available bifunctional binaphthalene type epoxy compounds include HP-4770 (product name, DIC Corporation). Commercially available trifunctional binaphthalene type epoxy compounds include EXA-4750 (product name, DIC Corporation). Commercially available tetrafunctional binaphthalene type epoxy compounds include HP-4710 (product name, DIC Corporation), HP-4700 (product name, DIC Corporation). These may be used alone or in combination of two or more.

[0045] (Novolac type epoxy compound) The novolac type epoxy compound is not particularly limited as long as it does not interfere with the effects of the present invention, but commercially available products can also be used. Commercially available novolac type epoxy compounds include N-730A (trade name, DIC Corporation), N-865 (trade name, DIC Corporation), etc. These may be used alone or in combination of two or more.

[0046] (Phenol aralkyl type epoxy compound) The phenol aralkyl type epoxy compound is not particularly limited as long as it does not impair the effects of the present invention, and commercially available products can also be used.

[0047] The blending ratio of the polyfunctional benzoxazine compound (A) and the epoxy compound (B) is preferably 30 parts by mass or more and 180 parts by mass or less, more preferably 50 parts by mass or more and 130 parts by mass or less, per 100 parts by mass of the component (A). When the blending ratio of the components (A) and (B) is within the above range, better heat resistance can be obtained. When the composition of the present invention contains multiple types of polyfunctional benzoxazine compounds as component (A), the total of these compounds is taken as 100 parts by mass. When the composition of the present invention contains multiple types of epoxy compounds as component (B), the component (B) means the total of the multiple compounds.

[0048] When the epoxy compound of component (B) further contains an epoxy compound other than an epoxy compound having at least one norbornane structure and at least two epoxy groups (hereinafter also referred to as an epoxy compound containing a norbornane structure), the blending ratio (mass ratio) of the epoxy compound containing a norbornane structure to the epoxy compound other than the epoxy compound containing a norbornane structure (epoxy compound containing a norbornane structure: epoxy compound other than the epoxy compound containing a norbornane structure) is, for example, 85:15 to 15:85, preferably 70:30 to 30:70, more preferably 60:40 to 40:60. When the blending ratio is within the above range, a composition for cured resin having better room temperature stability and a cured product having better heat resistance can be obtained. In addition, when the composition of the present invention contains multiple types of epoxy compounds other than the norbornane structure-containing epoxy compound as component (B), the above-mentioned blending amount of the epoxy compounds other than the norbornane structure-containing epoxy compound means the total blending amount of the multiple types of compounds.

[0049] (Component C) Component (C) constituting the curable resin composition is a curing agent. Specific examples of component (C) include phenolic curing agents, aromatic amines (e.g., diethyltoluenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, metaxylenediamine, derivatives thereof, etc.), aliphatic amines (e.g., triethylenetetramine, isophoronediamine, etc.), imidazoles (e.g., imidazole, imidazole derivatives, etc.), dicyandiamide, tetramethylguanidine, carboxylic acid anhydrides (e.g., methylhexahydrophthalic anhydride, etc.), carboxylic acid hydrazides (e.g., adipic acid hydrazide, etc.), carboxylic acid amides, polymercaptans, carboxylates, and Lewis acid complexes (e.g., boron trifluoride ethylamine complexes, etc.). Examples of the phenol-based curing agent include monofunctional phenols, polyfunctional phenol compounds (e.g., bisphenol A, bisphenol F, dihydroxynaphthalene, bisphenol sulfides (e.g., bis(4-hydroxyphenyl) sulfide, etc.), polyphenol compounds (e.g., pyrogallol, etc.), phenol resins (e.g., novolac-type phenol resins, phenol aralkyl resins having a phenylene skeleton, phenol aralkyl resins having a biphenyl skeleton, naphthol aralkyl resins having a phenylene skeleton, trisphenolmethane-type phenol resins (also called triphenylmethane-type phenol resins, or phenol resins mainly composed of a reaction product of hydroxybenzaldehyde, formaldehyde, and phenol), copolymers of triphenylmethane-type phenol compounds and novolac-type phenol compounds, and dicyclopentadiene-modified phenol resins). Component (C) is preferably a phenol-based curing agent, more preferably a polyfunctional phenol compound, even more preferably bisphenol F or a phenol resin, and even more preferably bisphenol F, a novolac-type phenol resin, a phenol aralkyl resin having a phenylene skeleton, or a phenol aralkyl resin having a biphenylene skeleton. These may be used alone or as a mixture of two or more kinds.

[0050] As the phenol-based curing agent of component (C), commercially available products can be used. For example, bisphenol F (manufactured by Honshu Chemical Industry Co., Ltd.), bis(4-hydroxyphenyl)sulfide (TDP, manufactured by Tokyo Chemical Industry Co., Ltd.), 2,7-dihydroxynaphthalene (manufactured by Tokyo Chemical Industry Co., Ltd.), pyrogallol (manufactured by Tokyo Chemical Industry Co., Ltd.), novolac-type phenolic resin (e.g., Ferrite TD-2106, manufactured by DIC Corporation; Ferrite TD-2090, manufactured by DIC Corporation), phenol aralkyl resin having a phenylene skeleton (e.g., MEH-7800-4S, manufactured by Meiwa Kasei Co., Ltd.), phenol aralkyl resin having a biphenyl skeleton (e.g., MEHC-7851SS, manufactured by Meiwa Kasei Co., Ltd.), triphenylmethane-type phenolic resin (HE910-20, manufactured by Air Water Inc.; TPM-100, manufactured by Gun-ei Chemical Industry Co., Ltd.), etc. may be used alone or in combination of two or more of these.

[0051] The blending ratio of the polyfunctional benzoxazine compound (A) to the total of the epoxy compound (B) and the curing agent (C) is preferably from 40 to 200 parts by mass, and more preferably from 60 to 150 parts by mass, of the total of the components (B) and (C) per 100 parts by mass of the component (A). When the blending ratio of component (A) to the total of components (B) and (C) is within the above range, it is possible to obtain a curable resin composition having better room temperature stability and a cured product having better heat resistance. In addition, when the composition of the present invention contains multiple types of polyfunctional benzoxazine compounds as component (A), the total of these compounds is considered to be 100 parts by mass. When the composition of the present invention contains multiple types of epoxy compounds as component (B), the above "mixing ratio of component (B)" means the total ratio of multiple types of compounds. Furthermore, when the composition of the present invention contains multiple types of curing agents as component (C), the above "mixing ratio of component (C)" means the total ratio of multiple types of curing agents.

[0052] The weight average molecular weight of the blend consisting of (A), (B) and (C) in terms of polystyrene is 350 to 650, preferably 350 to 600 or 400 to 650, more preferably 350 to 550 or 450 to 600. By setting the weight average molecular weight to 350 to 650, the cured resin composition is thought to be less sticky at room temperature and easier to handle. Therefore, when the weight average molecular weight is 350 to 650, a cured resin composition with better room temperature stability can be obtained. In the present invention, the weight average molecular weight of the blend consisting of (A), (B) and (C) in terms of polystyrene can be obtained by measuring by gel permeation chromatography (GPC) and converting to standard polystyrene. Such measurement and conversion can be easily performed by using a commercially available GPC device (e.g., manufactured by Tosoh Corporation) and column (e.g., TSKgel superHZ2000 (manufactured by Tosoh Corporation) and TSKgel superHZ1000 (manufactured by Tosoh Corporation)). The above measurement and conversion can be performed, for example, under the following conditions. Apparatus: GPC system HLC-8420GPC (with built-in RI detector) (manufactured by Tosoh Corporation), columns: 1 x TSKgel superHZ2000 (manufactured by Tosoh Corporation) (inner diameter 4.5 mm × 150 mm) and 2 x TSKgel superHZ1000 (manufactured by Tosoh Corporation) (inner diameter 4.5 mm × 150 mm), eluent: tetrahydrofuran, flow rate: 0.35 mL / min, detector: RI detector, column temperature: 40°C, injection volume: 5 μL, molecular weight standard: standard polystyrene (PStQuick F, manufactured by Tosoh Corporation). As the blend consisting of the above-mentioned (A), (B), and (C), a blend obtained by kneading (A), (B), and (C) for 5 minutes under atmospheric pressure on a hot plate whose surface temperature is set at 100°C, cooling to room temperature to obtain a mixture, and then pulverizing the mixture into powder in a mortar can be used.

[0053] (Component D) The curable resin composition of the present invention may further contain a curing accelerator (D) if desired. As the curing accelerator, known curing accelerators can be used, including amine compounds such as tributylamine and 1,8-diazabicyclo(5,4,0)undecene-7, imidazole compounds such as 2-methylimidazole, 2-ethylimidazole, and 1,2-dimethylimidazole, organic phosphorus compounds in which phosphorus is bonded only by covalent bonds such as triphenylphosphine, and organic phosphorus compounds such as salt-type organic phosphorus compounds in which phosphorus is bonded by covalent bonds and ionic bonds such as tetraphenylphosphonium tetraphenylborate, bis(tetrabutylphosphonium)(BTBP)-pyromellitic acid, and tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate (TBP-3PC), but are not limited thereto. In addition, the above-mentioned curing accelerators may be used alone, or two or more of them may be used in combination. Among these, organic phosphorus compounds such as triphenylphosphine, tetraphenylphosphonium tetraphenylborate, BTBP-pyromellitic acid, and TBP-3PC are preferred because they have a greater effect of improving the curing rate. The organic phosphorus compound is preferably one that exhibits a function of promoting a crosslinking reaction between an epoxy group and a phenolic hydroxyl group, as described in JP-A-55-157594, and further preferably exhibits a function of promoting a reaction between an epoxy group and a hydroxyl group generated when the polyfunctional benzoxazine compound (A) undergoes a cleavage reaction at high temperature.

[0054] The blending ratio of component (D) is preferably in the range of 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the total of components (A), (B) and (C). By including component (D) in this range, a curable resin composition having superior rapid curing properties can be obtained.

[0055] (Component E) The curable resin composition of the present invention may further contain an inorganic filler (E) if desired. For example, when the curable resin composition of the present invention is used for sealing materials such as semiconductor elements, it is preferable to contain component (E). The inorganic filler used in the present invention is not particularly limited, and can be selected in consideration of the use of the curable resin composition or its cured product or the properties to be imparted. Hereinafter, this inorganic filler is referred to as component (E). Examples of component (E) include oxides such as silica, alumina, titanium oxide, zirconium oxide, magnesium oxide, cerium oxide, yttrium oxide, calcium oxide, antimony trioxide, and zinc oxide; carbonates such as calcium carbonate, magnesium carbonate, barium carbonate, and strontium carbonate; sulfates such as barium sulfate, aluminum sulfate, and calcium sulfate; nitrides such as aluminum nitride, silicon nitride, titanium nitride, boron nitride, and manganese nitride; silicon compounds such as calcium silicate, magnesium silicate, and aluminum silicate; boron compounds such as aluminum borate; zirconium compounds such as barium zirconate and calcium zirconate; phosphorus compounds such as zirconium phosphate and magnesium phosphate; strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium Examples of the suitable materials include titanium compounds such as barium phosphate and potassium titanate; minerals such as mica, talc, kaolin, kaolin clay, kaolinite, halloysite, cordierite, pyrophyllite, montmorillonite, sericite, amesite, bentonite, asbestos, wollastonite, sepiolite, xonotlite, zeolite, hydrotalcite, hydrated gypsum, alum, diatomaceous earth, and boehmite; fly ash, dewatered sludge, glass beads, glass fiber, silica sand, magnesium oxysulfate, silicon oxide, silicon carbide, and the like; metals such as copper, iron, and nickel, or alloys containing any of these; magnetic materials such as ferrites such as sendust, alnico magnets, and soft magnetic ferrites, iron oxide, chromium oxide, cobalt, and non-oxidized metal magnetic materials (oxides); graphite, coke, and the like. The component (E) is preferably silica, alumina, and a magnetic material. Examples of silica include fused silica, spherical silica, crystalline silica, amorphous silica, synthetic silica, hollow silica, etc., and preferably spherical silica and crystalline silica. Examples of alumina include spherical alumina, crushed alumina, and microspherical alumina, and preferably spherical alumina and microspherical alumina. Preferred magnetic materials include soft magnetic ferrite, iron oxide, chromium oxide, cobalt, non-oxidized metal magnetic material (oxide), etc. Component (E) may be used alone or in combination of two or more.

[0056] Component (E) may be granular, and in that case, the average particle size is not particularly limited, but may be, for example, 0.01 μm to 150 μm, preferably 0.1 μm to 120 μm, more preferably 0.5 μm to 75 μm. Within this range, for example, when the composition of the present invention is used as an encapsulant for semiconductor elements, the filling property into a mold cavity is improved. The average particle size of component (E) can be measured by a laser diffraction / scattering method. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample is preferably one in which the inorganic filler is dispersed in water by ultrasonic waves. As the laser diffraction particle size distribution measuring device, "LA-500", "LA-750", "LA-950", "LA-960" and the like manufactured by Horiba, Ltd. can be used.

[0057] The blending ratio of component (E) is not particularly limited as long as a highly heat-resistant cured product can be obtained, and can be appropriately set depending on the application. For example, when the composition is used for semiconductor encapsulation, the blending ratio shown below is preferable. The lower limit of the blending ratio of component (E) is, for example, 150 parts by mass or more, preferably 400 parts by mass or more, and more preferably 500 parts by mass or more, relative to 100 parts by mass of the total of components (A), (B) and (C). The upper limit of the blending ratio of component (E) is, for example, 1300 parts by mass or less, preferably 1150 parts by mass or less, and more preferably 950 parts by mass or less. If the lower limit of the blending ratio of component (E) is 400 parts by mass or more, the increase in moisture absorption amount and the decrease in strength due to the curing of the curable resin composition can be further suppressed, and therefore a cured product having better solder crack resistance can be obtained. If the upper limit of the blending ratio of component (E) is 1300 parts by mass or less, the fluidity of the curable resin composition is improved, it is easier to fill the mold, and the cured product exhibits better sealing performance.

[0058] (Other Ingredients) The composition of the present invention may contain a benzoxazine compound other than component (A) within the range that does not impair the effects of the present invention. For example, when it is desired to reduce the viscosity of the composition, a monofunctional benzoxazine compound having one benzoxazine ring may be added to the composition.

[0059] Furthermore, the curable resin composition of the present invention may contain, for example, nanocarbon, a flame retardant, a release agent, a colorant, a low-stress additive, a metal hydroxide, etc., within the scope of not impairing the performance of the composition. Examples of nanocarbons include carbon nanotubes, fullerenes, and derivatives of each. Examples of the flame retardant include red phosphorus, phosphoric acid esters such as triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, resorcinol bisphenyl phosphate, and bisphenol A bisdiphenyl phosphate, boric acid esters, and phosphazenes. Examples of the release agent include stearic acid esters, natural waxes such as carnauba wax, synthetic waxes such as oxidized polyethylene wax, higher fatty acids such as stearic acid or esters thereof, metal salts such as zinc stearate, paraffin, and silicone oil. Examples of colorants include carbon black, red iron oxide, and titanium oxide. Low stress additives include silicone oil and silicone rubber. Metal hydroxides include hydroxides such as calcium hydroxide, aluminum hydroxide, and magnesium hydroxide. When component (E) an inorganic filler is contained, a silane coupling agent may be added.

[0060] The blending ratio of the other components is preferably in the range of 0.01 parts by mass or more and 10 parts by mass or less, and more preferably in the range of 0.1 parts by mass or more and 9 parts by mass or less, per 100 parts by mass of the total of components (A), (B), and (C).

[0061] (Characteristics of the curable resin composition) The room temperature stability of the composition for a curable resin of the present invention can be evaluated by the glass transition temperature (also called powder Tg), stickiness, and / or caking property of the composition for a curable resin before curing.

[0062] The glass transition temperature of the composition for curable resin is 3° C. or higher, preferably 5° C. or higher, and more preferably 6° C. or higher. The glass transition temperature can be measured by differential scanning calorimetry (DSC). Such a measurement can be easily performed by using a commercially available differential scanning calorimeter (for example, manufactured by Hitachi High-Tech Science Corporation).

[0063] It is preferable that the curable resin composition of the present invention is not sticky. The stickiness of the curable resin composition can be confirmed by the following confirmation test to determine whether the curable resin composition is sticky or not. Verification test: The composition for curable resin before curing is put into a bottle, sealed with a lid, and then stored for 24 hours in a temperature-controlled room adjusted to a temperature of 23±1°C and humidity of 50±5°C. After that, the bottle is turned upside down and left to stand for 5 minutes, after which it can be judged whether the composition has adhered to the bottom of the bottle or not. Further details of the above confirmation test can be described in accordance with Example 1 below.

[0064] When the curable resin composition of the present invention contains component (E), it is preferable that the curable resin composition does not solidify, or if it does solidify, it can be loosened by turning the bottle upside down. The solidification property of the curable resin composition can be confirmed by the following confirmation test to confirm whether the curable resin composition solidifies or not. Verification test: Put the composition for curable resin before curing into a bottle, seal it with a lid, and store it for 24 hours in a temperature-controlled room adjusted to a temperature of 23±1°C and humidity of 50±5°C. After that, turn the bottle upside down and leave it for 5 minutes, then visually check the composition to determine whether it has solidified or not. Further details of the above confirmation test can be described in accordance with the description of Example 15 below.

[0065] [Method of producing curable resin composition] Next, a method for producing the composition for curable resin of the present invention will be described. The curable resin composition of the present invention can be produced by carrying out a step of kneading or mixing components (A) to (C) and, if desired, other components such as component (D), component (E), other additives, and a solvent to obtain a mixture, and a step of processing the mixture into a powder-like, pellet-like, or granular curable resin composition. The kneading or mixing method is not particularly limited, and for example, mixing devices or kneaders such as planetary mixers, twin-screw extruders, heat rolls, or kneaders can be used. When components (A), (B), and (C) are in a high-viscosity liquid or solid state at room temperature, or when component (E) is contained, they may be heated and kneaded as necessary, or further kneaded under pressure or reduced pressure. The heating temperature is preferably 80 to 120°C. Since the curable resin composition containing component (E) is solid at room temperature, it may be cooled and pulverized after heating and kneading to obtain a powder, and the powder may be tableted to obtain a pellet shape. Also, the powder may be granulated to obtain a granular shape.

[0066] When the curable resin composition of the present invention does not contain component (E) and is used for FRP prepregs or the like, the curable resin composition preferably has a viscosity of 10 to 3000 Pa·s at 50° C., more preferably 10 to 2500 Pa·s, and even more preferably 100 to 2000 Pa·s. When used as a sealant or coating material, the viscosity is not particularly limited as long as it does not interfere with sealing, coating, or other operations.

[0067] [Cured product] The cured product of the composition for curable resin of the present invention has a high glass transition temperature and excellent heat resistance. The reason why the composition for curable resin of the present invention forms such an excellent cured product is considered to be as follows. First, in the homopolymerization of benzoxazine, phenolic hydroxyl groups are generated by polymerization. At high temperatures, e.g., 200°C or higher, these phenolic hydroxyl groups are converted into ketoenol tautomers, which cause the polymer chain to break, resulting in low heat resistance and a low glass transition temperature. In contrast, the polyfunctional epoxy compound of the present invention having a norbornane structure and two or more epoxy groups is difficult to homopolymerize, and is believed to prevent the polymer chain from being cut by reacting with the phenolic hydroxyl group derived from the benzoxazine, thereby resulting in a cured product with high heat resistance.

[0068] (Characteristics of the cured product) The heat resistance of the cured product of the present invention can be evaluated by measuring the glass transition temperature of the cured product. The glass transition temperature of the cured product is 220°C or higher, preferably 225°C or higher, and more preferably 230°C or higher. In addition, when the curable resin composition contains component (E), the glass transition temperature of the cured product is 230°C or higher, preferably 235°C or higher, and more preferably 240°C or higher. The glass transition temperature can be measured by differential scanning calorimetry (DSC). Such measurements can be easily performed using a commercially available differential scanning calorimeter (for example, manufactured by Hitachi High-Tech Science Corporation).

[0069] [Method of manufacturing the cured product] The cured product of the present invention can be produced by carrying out ring-opening polymerization and curing under the same curing conditions as those for known benzoxazine compounds and / or epoxy compounds. For example, the following method can be mentioned. First, the composition for curable resin of the present invention is produced by the above-mentioned method. Then, the obtained composition for curable resin is heated, for example, at 150 to 300° C. for a curing time of, for example, 20 seconds to 5 hours, preferably 20 seconds to 1 hour, to obtain a cured product. When continuously producing a cured product, a curing time of 1 to 3 minutes is sufficient, but in order to obtain a higher strength, it is preferable to further heat for about 5 minutes to 5 hours as post-curing.

[0070] When a film-shaped molded product is to be obtained as the cured product, a solvent may be further added to the composition to obtain a solution viscosity suitable for forming a thin film. The solvent is not particularly limited as long as it can dissolve components (A) to (D), and examples of the solvent include hydrocarbons, ethers, esters, and halogen-containing solvents. In this way, in the case of a solution-like curable resin composition dissolved in a solvent, the solution-like curable resin composition can be applied to a substrate or the like, the solvent can be evaporated, and then the composition can be thermally cured to obtain a cured product.

[0071] [Semiconductor Devices] The semiconductor device of the present invention is a semiconductor device in which a semiconductor element is placed in a cured product obtained by curing the composition for curable resin of the present invention containing components (A) to (C) and, if desired, components (D) and (E) and other components. Here, the semiconductor element is usually supported and fixed by a lead frame, which is a thin plate of a metal material. "A semiconductor element is placed in a cured product" means that the semiconductor element is sealed with a cured product of the composition for curable resin, and represents a state in which the semiconductor element is covered with the cured product. In this case, the entire semiconductor element may be covered, or the surface of the semiconductor element placed on the substrate may be covered.

[0072] When the cured product of the present invention is used to encapsulate various electronic components such as semiconductor elements to produce a semiconductor device, the semiconductor device can be produced by carrying out the encapsulation step using a conventional molding method such as transfer molding, compression molding, or injection molding. EXAMPLES

[0073] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0074] <Component (A): Polyfunctional benzoxazine compound> The following compound was used as component (A). (A): Phenol-diaminodiphenylmethane (Pd)-type benzoxazine (manufactured by Shikoku Kasei Co., Ltd.) shown in the following formula (2-1) [ka]

[0075] <Component (B): Epoxy compound> As the component (B), the following (B1) to (B5) were used. (B1) Epoxy compound 1 (alicyclic epoxy compound); compound of formula (5-1) Compound (a) represented by the above formula (6) was synthesized in accordance with the method described in Shoichi Tsuchida et al., "Diels-Alder reaction of butadiene and cyclopentadiene - Determination of trimer -", Journal of Petroleum Science, Vol. 15, No. 3, pp. 189-192, 1972. Next, the reaction of the above formula (6) was carried out as follows: 23.5 kg of chloroform and 1.6 kg of compound (a) were placed in a reaction vessel, and 4.5 kg of metachloroperbenzoic acid was added dropwise while stirring at 0° C. The temperature was raised to room temperature, and the reaction was carried out for 12 hours. Next, the by-product metachlorobenzoic acid was removed by filtration, and the filtrate was washed three times with 1N aqueous sodium hydroxide solution and then washed with saturated saline. The organic layer was dried over magnesium sulfate, and the magnesium sulfate was removed by filtration. The filtrate was concentrated to obtain a crude product. 2 kg of toluene was added to the crude product and dissolved at room temperature. 6 kg of heptane was added dropwise to crystallize the product, and the product was aged at 5°C for 1 hour. The crystallized product was collected by filtration and washed with hexane. The product was dried under reduced pressure at 35°C for 24 hours to obtain 1.4 kg of the compound represented by the following formula (5-1) as a white solid. [ka]

[0076] (B2) Epoxy compound 2 (epoxy compound having a biphenyl skeleton): an epoxy compound having a biphenyl skeleton represented by the following formula (9-1-1) (NC-3000-H, manufactured by Nippon Kayaku Co., Ltd.) [ka] (In formula (9-1-1), n ​​is the average value, which is 3.9.)

[0077] (B3) Epoxy compound 3 (trisphenolmethane type epoxy compound): an epoxy compound represented by the following formula (10-1) (EPPN-502H, manufactured by Nippon Kayaku Co., Ltd.) [ka] (In formula (10-1), n ​​is the average value, which is 1.9.)

[0078] (B4) Epoxy compound 4 (alicyclic epoxy compound); compound of formula (5-2) (tricyclopentadiene diepoxide) Compound (b) was synthesized in the same manner as compound (a) described in (B1) above, according to the method described in the above literature. Next, the reaction of the above formula (7) was carried out as follows: 59.2 kg of chloroform and 4.0 kg of compound (b) were placed in a reaction vessel, and 10.6 kg of metachloroperbenzoic acid was added dropwise while stirring at -10°C. The temperature was raised to room temperature, and the reaction was carried out for 12 hours. Next, after removing the by-product metachlorobenzoic acid by filtration, the filtrate was washed with 42.0 kg of 5% aqueous sodium sulfite solution. The organic layer was further washed four times with 41.6 kg of 1N aqueous sodium hydroxide solution, and then washed with 48.0 kg of saturated saline. The organic layer was dried over magnesium sulfate, after which the magnesium sulfate was removed by filtration and the filtrate was concentrated to obtain 5.1 kg of crude product. 3.5 kg of toluene was added to the crude product and dissolved at room temperature. 13.7 kg of heptane was added dropwise to crystallize the product, and the product was aged at 5°C for 1 hour. The crystallized product was collected by filtration and washed with heptane. The product was dried under reduced pressure at 35°C for 12 hours to obtain 2.8 kg of the compound represented by the following formula (5-2) as a white solid. [ka]

[0079] (B5) Alicyclic epoxy compound 5; Compound of formula (5-4) (dicyclopentadiene diepoxide) A reaction vessel was charged with 10 kg of dicyclopentadiene, 68 kg of sodium bicarbonate, 100 L of acetone, and 130 L of ion-exchanged water, and cooled to below 10°C. After that, the cooling was controlled so as to maintain the temperature of the reaction liquid below 30°C, and 84 kg of oxone was gradually added, and the reaction was carried out for 10 hours with stirring. Next, the reaction product was extracted twice with 100 L of ethyl acetate, and the obtained organic layers were separated and combined. The organic layers were then washed with 100 L of a mixed aqueous solution of sodium chloride and sodium thiosulfate (20 wt% sodium chloride + 20 wt% sodium thiosulfate), and then washed twice with 100 L of ion-exchanged water. The washed organic layer was dried over magnesium sulfate, and then the magnesium sulfate was removed by filtration. The organic solvent was distilled off from the filtrate to obtain 11 kg of the compound represented by the following formula (5-4) as a white solid. [ka]

[0080] <Component (C): Hardener> As the component (C), the following (C1) to (C4) were used. (C1) Curing agent 1: Bisphenol F (manufactured by Honshu Chemical Industry Co., Ltd.) shown in the following formula (13-1) [ka]

[0081] (C2) Curing agent 2: A curing agent shown in the following formula (13-2) (MEHC-7851SS, manufactured by Meiwa Chemical Industry Co., Ltd.) [ka] (In formula (13-2), n is the average value, which is 2.0.)

[0082] (C3) Curing agent 3: A curing agent shown in the following formula (13-3) (MEH-7800-4S, manufactured by Meiwa Kasei Co., Ltd.) [ka] (In formula (13-3), n is the average value, which is 4.8.)

[0083] (C4) Curing agent 4: A curing agent represented by the following formula (13-4) (TD-2106, manufactured by DIC Corporation) [ka] (In formula (13-4), n is the average value, which is 8.7.)

[0084] <Component (D): Curing accelerator> As the component (D), the following (D1) to (D4) were used. (D1) Curing accelerator 1: Triphenylphosphine (TPP) represented by the following formula (manufactured by Hokko Chemical Industry Co., Ltd.) [ka]

[0085] (D2) Curing accelerator 2: Tetraphenylphosphonium tetraphenylborate (TPP-K (trademark)) represented by the following formula (manufactured by Hokko Chemical Industry Co., Ltd.) [ka]

[0086] (D3) Curing accelerator 3: Bis(tetrabutylphosphonium) (BTBP)-pyromellitic acid represented by the following formula (manufactured by Hokko Chemical Industry Co., Ltd.) [ka]

[0087] (D4) Curing accelerator 4: Tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate (TBP-3PC) represented by the following formula (manufactured by Hokko Chemical Industry Co., Ltd.) [ka]

[0088] <Component (E): Inorganic filler> As the component (E), the following (E1) to (E3) were used. Component (E1) Inorganic filler 1: Fused spherical silica having an average particle size D50 of 22 μm (FB-820, manufactured by Denka Co., Ltd.) Component (E2) Inorganic filler 2: Spherical alumina (TCH75H-SI, manufactured by Admatechs Co., Ltd.) Component (E3) Inorganic filler 3: Magnetic powder (iron oxide) (DAMPMS-B(-200), manufactured by Daido Steel Co., Ltd.)

[0089] <Other ingredients> Carnauba wax (Clariant Japan KK) was used as a release agent, and carbon black (MA600, Mitsubishi Chemical Corporation) was used as a colorant.

[0090] Example 1 A composition for a cured resin (hereinafter also referred to as "composition" or "cured composition before curing") and a cured product were prepared as described below, and the weight average molecular weight of the composition for a cured resin, the glass transition temperature of the cured product as an evaluation of heat resistance, and the powder Tg and stickiness of the composition for a cured resin as an evaluation of room temperature stability were measured. (A), (B1), and (C2) were mixed in the proportions shown in Table 1 under atmospheric pressure for 5 minutes on a hot plate whose surface temperature was set to 100°C, and then cooled to room temperature to obtain a mixture. The mixture was pulverized into powder in a mortar to obtain a composition.

[0091] <Glass transition temperature; Tg> Approximately 10 mg of the composition was weighed into an aluminum pan used in DSC and heated in an oven at 220°C for 5 hours to obtain a cured product. The Tg of the obtained cured product was measured by DSC under the following conditions. The results are shown in Table 1. Equipment: X-DSC-7000 (Hitachi High-Tech Science Corporation) Measurement conditions: N2 flow rate: 20 mL / min, heating rate: 20 °C / min

[0092] <Weight average molecular weight> (A), (B1), and (C2) were kneaded for 5 minutes under atmospheric pressure on a hot plate with a surface temperature set to 100°C in the blending ratio shown in Table 1, and then cooled to room temperature to obtain a mixture. The mixture was pulverized into powder in a mortar to obtain a blend. The weight average molecular weight of the obtained blend was measured in terms of standard polystyrene by gel permeation chromatography (GPC) under the following conditions. The results are shown in Table 1. Equipment: GPC system HLC-8420GPC (with built-in RI detector) (manufactured by Tosoh Corporation) Column: 1 x TSKgel superHZ2000 (Tosoh Corporation) (inner diameter 4.5 mm x 150 mm) and 2 x TSKgel superHZ1000 (Tosoh Corporation) (inner diameter 4.5 mm x 150 mm) connected in series Eluent: Tetrahydrofuran Flow rate: 0.35mL / min Detector: RI detector Column temperature: 40℃ Injection volume: 5μL Molecular weight standard: Standard polystyrene (PStQuick F, Tosoh Corporation)

[0093] <Powder Tg> About 10 mg of the composition for a curable resin before curing was placed in an aluminum pan, and the glass transition temperature Tg (powder Tg) was measured under the following conditions. The results are shown in Table 1. Equipment: X-DSC-7000 (Hitachi High-Tech Science Corporation) Measurement conditions: N2 flow rate: 20 mL / min, heating rate: 5°C / min, measurement range: -40 to 50°C

[0094] <Evaluation of stickiness> 1 g of the composition for curable resin before curing was placed in a screw bottle (lightweight standard bottle (soda glass) No. 7, Maruemu Co., Ltd.), the bottle was sealed with a lid, and then stored for 24 hours in a temperature-controlled room adjusted to a temperature of 23±1°C and a humidity of 50±5°C. The screw bottle was then turned upside down, and after 5 minutes of standing, if the composition had not adhered to the bottom of the bottle, it was judged as "○" (not sticky), and if the composition had not adhered to the bottom of the bottle and fallen toward the lid, it was judged as "×" (sticky). If part of the composition had adhered to the bottom of the bottle, it was also judged as "×" (sticky). The results are shown in Table 1.

[0095] (Examples 2 to 14, 26, and 27) The compositions of each example were prepared in the same manner as in Example 1, except that the blending ratio of each component was as shown in Table 1. The weight average molecular weight, heat resistance (glass transition temperature), and room temperature stability (powder Tg, stickiness) of each composition were measured in the same manner as in Example 1. The blends in Examples 4 to 6 consisted of components (A), (B), and (C), and did not contain component (D). The results are shown in Table 1.

[0096] (Comparative Examples 1 to 8) The compositions of each comparative example were prepared in the same manner as in Example 1, except that the blending ratio of each component was as shown in Table 2. The weight average molecular weight, heat resistance (glass transition temperature), and room temperature stability (powder Tg, stickiness) of each composition were measured in the same manner as in Example 1. The blend in Comparative Example 2 consisted of components (A), (B), and (C), and did not contain component (D). The results are shown in Table 2.

[0097] [Table 1]

[0098] [Table 2]

[0099] The cured product of the cured resin composition of each Example has a Tg of 220°C or more, which indicates high heat resistance. In addition, the powder Tg of the cured resin composition before curing in each Example is 3°C or more, and it is not sticky, which indicates excellent room temperature stability. The cured resin compositions of Examples 7 to 14 are not sticky even when stored in a constant temperature room for 24 hours, and when inverted, the entire amount falls into the lid while maintaining the shape of the bottle bottom. Therefore, the cured resin compositions of Examples 7 to 14 are considered to be less sticky than the cured resin compositions of Examples 1 to 6, 26 and 27. On the other hand, the cured products obtained by curing the cured resin compositions of Comparative Examples 4 to 8 have a low Tg and are inferior in heat resistance. In addition, the powder Tg of the cured resin compositions before curing in Comparative Examples 1 to 3 is less than 3°C, and it is sticky, which indicates poor room temperature stability. From the above results, it is clear that the curable resin composition according to an embodiment of the present invention has excellent room temperature stability, while the cured product thereof achieves high heat resistance.

[0100] Example 15 A composition for a cured resin (hereinafter also referred to as "composition" or "composition for a cured resin before curing") and a cured product were prepared as described below, and the weight average molecular weight of the composition for a cured resin, the glass transition temperature of the cured product as an evaluation of heat resistance, and the solidification property of the composition for a cured resin as an evaluation of room temperature stability were measured. (A), (B1), (C2), (D1), (E1), carnauba wax, and carbon black were kneaded for 10 minutes at atmospheric pressure using a hot roll kneader (BR-150HCV, Imex Co., Ltd.) having two rolls with surface temperatures of 90°C and 100°C in the mixing ratios shown in Table 3, and then cooled to room temperature to obtain a mixture. The resulting mixture was pulverized into a powder form using a mini speed mill MS-09 (Labonect Co., Ltd.) so that it could be easily filled into a mold, and a composition was obtained.

[0101] <Glass transition temperature; Tg> The prepared composition was cured using a transfer molding machine under the conditions of a mold temperature of 200°C, an injection pressure of 4MPa, and a curing time of 3 minutes, and then heated in an oven at 220°C for 4 hours as a post-curing treatment to produce a cured product of 3 mm length x 3 mm width x 15 mm length. The cured product was cut into test pieces of 3 mm length x 3 mm width x 2 mm length, and Tg was measured by DSC under the following conditions. The results are shown in Table 3. Equipment: X-DSC-7000 (Hitachi High-Tech Science Corporation) Measurement conditions: N2 flow rate: 20 mL / min, heating rate: 20 °C / min

[0102] <Weight average molecular weight> A blend consisting of components (A), (B) and (C) of the composition of Example 15 was produced, and the weight average molecular weight of the blend was measured in terms of standard polystyrene by GPC in the same manner as in Example 1. Specifically, (A), (B1) and (C2) were kneaded for 5 minutes under atmospheric pressure on a hot plate with a surface temperature set to 100°C in the blending ratio shown in Table 3, and then cooled to room temperature to obtain a mixture. The mixture was pulverized into powder in a mortar to obtain a blend. The weight average molecular weight of the resulting blend was measured by GPC. The results are shown in Table 3.

[0103] <Consolidation evaluation> 1 g of the composition for curable resin before curing was placed in a screw bottle (lightweight standard bottle (soda glass) No. 7, Maruemu Co., Ltd.), sealed with a lid, and stored for 24 hours in a temperature-controlled room adjusted to a temperature of 23±1°C and humidity of 50±5°C. The bottle was then turned upside down and left to stand for 5 minutes, after which the composition was visually inspected to confirm whether it had solidified or not. As a result, if no solidification of the composition was observed, or if it had solidified but could be loosened by turning the bottle upside down, it was judged as "Good", and if the composition was found to have solidified even when the bottle was turned upside down, it was judged as "Poor". The results are shown in Table 3.

[0104] (Examples 16 to 25) The compositions of each example were prepared in the same manner as in Example 15, except that the blending ratio of each component was as shown in Table 3. The weight average molecular weight, heat resistance evaluation (glass transition temperature), and room temperature stability (caking property) of each composition were measured in the same manner as in Example 15. The results are shown in Table 3.

[0105] (Comparative Examples 9 to 12) The compositions of each comparative example were prepared in the same manner as in Example 15, except that the blending ratio of each component was as shown in Table 4. The weight average molecular weight, heat resistance evaluation (glass transition temperature), and room temperature stability (caking property) of each composition were measured in the same manner as in Example 15. The results are shown in Table 4.

[0106] [Table 3]

[0107] [Table 4]

[0108] The cured products of the curable resin compositions of each Example had a Tg of 230°C or higher, indicating high heat resistance. The solidification of the curable resin compositions before curing in each Example was rated "○", indicating excellent room temperature stability. In particular, no solidification of the compositions was observed in Examples 24 and 25. On the other hand, the cured products obtained by curing the curable resin compositions of Comparative Examples 10 to 12 had low Tg and poor heat resistance. The solidification of the curable resin composition before curing in Comparative Example 9 was rated "×", indicating poor room temperature stability. From the above results, it is clear that the curable resin composition according to an embodiment of the present invention has excellent room temperature stability, while the cured product thereof achieves high heat resistance.

Claims

1. (A) at least one polyfunctional benzoxazine compound having at least two benzoxazine rings, selected from a polyfunctional benzoxazine compound having a structural unit of formula (1) and a polyfunctional benzoxazine compound represented by a structure of formula (2); (B) an epoxy compound including at least one epoxy compound having at least one norbornane structure and at least two epoxy groups, and further including at least one selected from an epoxy compound having a biphenyl skeleton and a trisphenolmethane type epoxy compound; (C) a curing agent; Contains A composition for curable resins, comprising a blend of (A), (B) and (C), the weight average molecular weight of which is in the range of 350 to 650 in terms of polystyrene. [Case 1] [In formula (1), R represents a chain alkyl group having 1 to 12 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and the aryl group may have a halogen or a chain alkyl group having 1 to 12 carbon atoms as a substituent. Z represents hydrogen, a hydrocarbon group having 1 to 8 carbon atoms, and / or a linking group, which may be the same or different, and at least one of them is a linking group, and the benzoxazine rings are linked to each other by the linking group.] [Case 2] [In formula (2), L is a divalent organic group having 1 to 5 aromatic rings or an alkylene group having 2 to 10 carbon atoms, and the organic group and the alkylene group may contain oxygen and / or sulfur.]

2. The composition for curable resins according to claim 1 , wherein the (B) epoxy compound having at least one norbornane structure and at least two epoxy groups is an alicyclic epoxy compound.

3. The composition for curable resins according to claim 1 or 2, wherein the (B) epoxy compound having at least one norbornane structure and at least two epoxy groups does not have a glycidyl group.

4. The curable resin composition according to any one of claims 1 to 3, wherein the epoxy compound (B) further comprises at least one selected from the group consisting of a naphthalene type epoxy compound, a novolac type epoxy compound, and a phenol aralkyl type epoxy compound.

5. The composition for curable resin according to any one of claims 1 to 4, further comprising (D) a curing accelerator.

6. The curable resin composition according to any one of claims 1 to 5, further comprising (E) an inorganic filler.

7. A cured product obtained by curing the composition for curable resin according to any one of claims 1 to 6.

8. A semiconductor device comprising a semiconductor element disposed in a cured product obtained by curing the composition for curable resin according to any one of claims 1 to 6.

9. A method for producing a curable resin composition according to any one of claims 1 to 6, comprising the steps of: (A) at least one polyfunctional benzoxazine compound having at least two benzoxazine rings, selected from a polyfunctional benzoxazine compound having a structural unit of formula (1) and a polyfunctional benzoxazine compound represented by a structure of formula (2); (B) an epoxy compound including at least one epoxy compound having at least one norbornane structure and at least two epoxy groups, and further including at least one selected from an epoxy compound having a biphenyl skeleton and a trisphenolmethane type epoxy compound; (C) mixing with a curing agent to obtain a mixture; Processing the mixture into a powder, pellet, or granular curable resin composition. The method for producing a composition for cured resin comprising the steps of: [C3] [In formula (1), R represents a chain alkyl group having 1 to 12 carbon atoms, a cyclic alkyl group having 3 to 8 carbon atoms, or an aryl group having 6 to 14 carbon atoms, and the aryl group may have a halogen or a chain alkyl group having 1 to 12 carbon atoms as a substituent. Z represents hydrogen, a hydrocarbon group having 1 to 8 carbon atoms, and / or a linking group, which may be the same or different, and at least one of them is a linking group, and the benzoxazine rings are linked to each other by the linking group.] [C4] [In formula (2), L is a divalent organic group having 1 to 5 aromatic rings or an alkylene group having 2 to 10 carbon atoms, and the organic group and the alkylene group may contain oxygen and / or sulfur.]

10. The method according to claim 9 , wherein in the step of obtaining the mixture, a hardening accelerator (D) and / or an inorganic filler (E) are further mixed to obtain the mixture.

11. A step of heating the curable resin composition produced by the method according to claim 9 or 10 at 150 to 300° C. for 20 seconds to 5 hours to cure the composition. The method for producing a cured product comprising the steps of:

Citation Information

Patent Citations

  • Epoxy resin composition and cured product from the same

    JP2010254895A

  • Resin composition, copper-clad laminate and printed circuit sheet using the same

    JP2017020011A

  • Resin composition and product made therefrom

    US20170327683A1

  • Photosensitive resin composition

    WO2015002071A1

  • Composition for curable resin, and cured product thereof

    WO2017188448A1