Electrolyte and method for producing chromium layer
By adding metallic chromium to the electrolyte, the chromium(III) ion concentration is stabilized, preventing Cr(VI) formation and ensuring consistent chromium deposition, addressing the challenges of concentration reduction and anion accumulation in electrolytic chromium deposition.
Patent Information
- Application Number
- JP2021535302
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-21
- Filing Date
- 2019-12-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-12-12
AI Technical Summary
The precipitation of chromium from trivalent chromium electrolytes leads to a reduction in chromium(III) ion concentration, requiring periodic dilution and additional ingredient administration, and results in the accumulation of anions and potential Cr(VI) formation.
Incorporating metallic chromium into the electrolyte maintains a constant chromium(III) content over extended periods by dissolving it, preventing Cr(VI) formation without the need for semipermeable membranes, using a composition that includes chromium(III) salts, metallic chromium, formic acid, and additives like sulfate and glycine to stabilize the electrolyte.
Maintains chromium(III) ion concentration for several hours to months, prevents Cr(VI) formation, and allows for uniform chromium deposition without membrane separation, ensuring high-quality chromium layers on objects like gravure cylinders.
Smart Images

Figure 0007569788000001 
Figure 0007569788000002 
Figure 0007569788000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte for the electrolytic deposition of chromium as metal, to the use of the electrolyte for this purpose, and to a method for producing a chromium layer.
[0002] A method for electrolytically depositing chromium from an electrolyte containing Cr(III) is well known. The electrolyte for electrolytically depositing chromium metal has the following composition: (a) Chromium(III) salts, (b) A compound of formula (I) JPEG0007569788000001.jpg24166(I), Here, R represents NH2, OH, or SO3H, and n is an integer from 1 to 3. (c) Formic acid (d) at least one additive, as known, for example, from DE 10 2014 116 717 A1, from which electrolyte chromium can be deposited by passing a direct current through an object used as a cathode. Summary of the Invention [Problem to be solved by the invention]
[0003] The disadvantage is that the precipitation of chromium from the trivalent chromium electrolyte reduces the concentration of chromium(III) ions in the electrolyte. Cr(III) can only be added in the form of chromium(III) salts, but the anions present in the salts will accumulate in the electrolyte, necessitating periodic dilution and additional dosing of other components.
[0004] The present invention is therefore based on the object of providing an electrolyte in which the Cr(III) content remains more or less constant over a long period of time, up to at least several months, while electrolysis is being carried out, and in which, even if Cr(III) is subsequently supplied to the electrolyte from which Cr(III) has been depleted, no Cr(VI) is produced in the process. [Means for solving the problem]
[0005] According to the present invention, this is achieved by an electrolyte for electrolytic deposition of chromium metal, the electrolyte comprising (a) a chromium (III) salt and (b) metallic chromium.
[0006] It has been found that the incorporation of metallic chromium in the Cr(III) electrolyte allows the chromium(III) content to be kept approximately constant over a long period of time, at least from a few hours to several months, during electrolysis. How long the chromium(III) content can be kept constant depends on the amount of metallic chromium used and the conditions of electrolysis, so that the period can be controlled in a simple and convenient way by means of these parameters. It is also possible to observe the state of dissolution of metallic chromium. It is assumed - without being bound thereto - that in the presence of Cr(III), cathodic Cr(II) is produced during reduction. This should promote the dissolution of metallic Cr. At the same time, the formation of Cr(VI) during oxidation can be prevented. That is, Cr(VI) is not produced even if metallic chromium is dissolved during electrolysis. Furthermore, the electrolytic deposition can be advantageously carried out without the use of a semipermeable membrane. Up to now, semipermeable membranes have been used to separate the anode and the cathode so that Cr(VI) is not produced. With the use of the electrolyte according to the invention, this is not necessary, since the composition of the electrolyte here prevents the formation of Cr(VI).
[0007] In one embodiment, the metallic chromium is available in the form of one or more moulds in the electrolyte. These, as mentioned above, are dissolved during the electrolysis over a particularly long period of time, so that the required Cr(III) can then be provided in a particularly convenient manner. The moulds can have a regular or irregular morphology. They can be smooth or porous. Examples of moulds are pieces, nuggets, chunks, plates, ingots, wires and meshes. Powders are not considered as moulds within the meaning of the present invention.
[0008] In one embodiment, the electrolyte contains, as component (c), sulfate (SO 42-), in particular sodium sulfate and / or potassium sulfate. The amount of sulfate can be 5 mM to 30 mM, for example 10 mM to 20 mM. By adding sulfate, the aforementioned advantages are particularly advantageously achieved.
[0009] In a further embodiment, the electrolyte comprises: (d) a compound of formula (I) JPEG0007569788000002.jpg24166(I), wherein R represents NH2, OH or SO3H, and n is an integer ranging from 1 to 3, and / or a salt thereof, e.g., Na + and / or K. + and / or salts with monovalent or divalent cations such as (e) formic acid and / or its salts, e.g., Na + and / or K. + and salts with monovalent or divalent cations such as
[0010] Formic acid, which may be contained in the electrolyte according to the invention, serves, for example, to convert the oxygen produced from the chromium(III) salt into CO2 and H2O and remove it.
[0011] The amount of formic acid and its salts in the electrolyte according to the invention is, for example, 1.0 mol / l to 3.0 mol / l relative to the electrolyte. A particularly convenient removal of oxygen occurs with this amount of formic acid in the electrolyte according to the invention. The indication of this amount refers to the electrolyte before the deposition of chromium. In the course of the deposition of chromium, the pH value of the electrolyte may change. To set the pH value, additional formic acid can be added. This additional amount is not meant to take into account the amount of formic acid in the electrolyte according to the invention, i.e. the amount of formic acid before the start of deposition.
[0012] Preferably, the compound of formula (I) is glycine, glycolic acid, sodium sulfoacetate, potassium sulfoacetate, or a mixture of at least two of these compounds. In the electrolyte according to the invention, the amount of the compound of formula (I) can be between 0.5 mol / l and 1.5 mol / l relative to the electrolyte.
[0013] The compounds of formula (I) serve to set the pH value of the electrolyte, which can be particularly advantageously set in the amounts indicated.
[0014] In one embodiment of the electrolyte according to the present invention, the chromium (III) salt comprises inorganic and / or organic chromium (III) salt. The term "chromium (III) salt" as used herein is understood to mean any chromium (III) salt from which chromium can be deposited as a metal layer on an object. Preferably, the inorganic chromium (III) salt is potassium chromium alum, ammonium chromium alum, chromium sulfate, chromium chloride, chromium sulfamate (amidosulfonate), chromium bromide, chromium iodide, chromium phosphate, chromium pyrophosphate (diphosphate), chromium phosphonate, chromium hydroxysulfate (alkali chromium sulfate), chromium chloride, and mixtures of two or more thereof. The organic chromium (III) salt may preferably be chromium citrate, chromium formate, chromium oxalate, chromium methanesulfonate, chromium dimethanesulfonate, and mixtures of two or more thereof.
[0015] The amount of chromium(III) salt is advantageously between 0.25 mol / l and 2.0 mol / l relative to the electrolyte. These amounts make it possible to produce chromium layers on metal objects by electrolytic deposition in a particularly convenient manner.
[0016] Furthermore, as component (f), additives known per se can be used in the electrolyte, which are usually used for the electrolytic deposition of chromium. Examples include wetting agents and complexing agents. These wetting agents reduce the surface tension and allow the H2 bubbles to leave the cathode. This makes it possible to simply and easily prevent the formation of pores and obtain a uniform chromium layer. As a complexing agent, for example, N,N-dimethyldithiocarbamylsulfonic acid sodium salt (DPS) can be used. With DPS, a chromium layer of particularly good quality can be obtained.
[0017] The amount of the common additive present in the electrolyte according to the invention can be between 0.01 g / l and 2.0 g / l relative to the electrolyte. In this process, the amount of the complexing agent can be between 0.5 mol / l and 4.0 mol / l. The amount of the wetting agent can be between 0 mol / l and 0.5 mol / l.
[0018] This electrolyte can be used in a process for producing chromium layers on decorative or technical objects by electrolytic deposition of chromium.
[0019] Examples of technical objects include rotationally symmetric objects such as rods, pistons, cylinders, in particular gravure cylinders. This process has proven to be particularly convenient for these objects, in particular gravure cylinders, since the chrome layer meets the high demands on the chrome layer.
[0020] The electrolytic deposition of the chromium layer can be carried out in a manner known per se, for example in an electrolytic cell filled with an electrolyte. This electrolyte is the aforementioned electrolyte according to the invention. An anode and a cathode are immersed in the electrolyte. When a direct current voltage is applied to these two electrodes, i.e. the anode and the cathode, chromium is deposited on the object to be coated. In this process, this object is used as the cathode, i.e. the object to be coated is the cathode.
[0021] Furthermore, the present invention provides a method for producing a chromium layer by using the above-described electrolyte according to the present invention and electrolytically depositing chromium from the electrolyte using a direct current, an anode and a cathode.
[0022] In this process, metallic chromium is available in the form of one or more molds in an electrolyte. The molds can be shaped as described above.
[0023] In one embodiment, the chromium metal is placed in an anodic and cathodic electric field, which promotes dissolution of the chromium metal over an extended period of time.
[0024] In one embodiment, the metallic chromium is in contact with the anode. In this case, the metallic chromium and the anode can be in contact with each other so that they can be physically touched. As the anode, a dimensionally stable anode can be used, which is optionally combined with a soluble chromium metal anode, so that the soluble chromium metal anode can be used as it is or advantageously combined with a known dimensionally stable anode. In particular, the anode is a noble metal-containing mixed oxide anode, for example a noble metal-containing iridium mixed oxide anode. The dissolution of the metallic chromium is thereby achieved over a long period of time in a convenient manner.
[0025] The two measures of inserting the metallic chromium in an electric field and of contacting the metallic chromium with an anode can be combined with each other, which allows particularly good monitoring of the dissolution of the metallic chromium in the electrolyte and allows particularly convenient dissolution rates to be set.
[0026] In one embodiment, the surface of metallic chromium can be 1% to 50% of the surface of the anode, in this way a particularly good dissolution of chromium and subsequent supply of Cr(III) is achieved.
[0027] The chromium layer can be produced at a pH value between 2.0 and 4.5. As already mentioned above in connection with the composition of the electrolyte according to the invention, the pH value can be set by the abovementioned compounds of formula (I).
[0028] Furthermore, the chromium layer can be produced at a temperature between 20° C. and 60° C. This can be achieved, for example, by setting the temperature of the electrolyte to a value within this range by means of corresponding heating and cooling devices.
[0029] In addition, 5 to 60 A / dm 2 A chromium layer can be produced at a current density of 0.1.
[0030] It is also possible to move the electrolyte, for example in such a way that 5 bath volumes, i.e. volumes of electrolyte, are circulated per hour. Since devices known per se for depositing chromium layers on objects can be used for this process, the volumes of the electrolyte baths of these devices known per se are the basis for determining the volumes of the baths in the method according to the invention.
[0031] In the electrolysis process, the workpiece can be moved at a speed of 0.3 to 2.0 m / s.
[0032] The object of the present invention is also a method for keeping the chromium(III) content in the electrolyte constant during electrolysis by carrying out the electrolysis using the electrolyte according to the invention. + This is understood to mean that there is a change of only 10%.
[0033] Additionally, a method is provided for preventing the formation of chromium (IV) during and after the electrolytic deposition of chromium using the electrolyte of the present invention.
[0034] These two methods can be implemented in the same way as the method according to the invention for producing a chromium layer by electrolytic deposition of chromium from an electrolyte.
[0035] The electrolyte according to the invention or the use according to the invention and the method according to the invention ensure that the Cr(III) content remains more or less constant in the electrolyte during electrolysis, at least over a long period of time ranging from several hours to several days or months, after which Cr(III) is supplied to the electrolyte which has been depleted of Cr(III), without Cr(VI) being produced in the process.
[0036] In addition, a particularly good quality chrome coating is obtained which meets the requirements especially for gravure cylinders.
[0037] Any vessel that can be used as an electrolysis cell can be used by those skilled in the art, in particular those that are commonly used in electroplating technology.
[0038] For electrolysis, the object to be coated on which the chromium layer is deposited is generally used as the cathode. As anodes for electrolytic coating, anodes known per se to the person skilled in the art can be used. The anodes can be flat, sheet, sintered or expanded materials. As insoluble anodes, for example, anodes can be used which are selected from the group of platinized titanium, graphite, stainless steel, titanium, tantalum or niobium coated with iridium transition metal mixed oxides, or special carbon materials and combinations thereof. As anode material, sheets of titanium, niobium or tantalum coated with mixed metal oxides can be used. Furthermore, mixed metal oxide anodes can be used which, as already mentioned above, consist in particular of iridium-ruthenium mixed oxide, iridium-ruthenium-titanium mixed oxide or iridium-tantalum mixed oxide. Furthermore, the anodes can be mixed oxide anodes, in which titanium as anode base material is coated with platinum, iridium or palladium oxide.
[0039] The shape of the anode can be appropriately adjusted according to the purpose by those skilled in the art. EXAMPLES
[0040] The following examples are provided to further illustrate the present invention. It should be noted that these examples serve only to illustrate the present invention. In any case, the present invention should not be understood to be limited to these examples.
[0041] Example 1 An electrolyte solution having the following composition was provided: - Chromium(III) sulfate (density=1.26g / ml; 3% Cr(III) -> 37.8g / l -> 0.727M)18.6l - Sodium sulfoacetate (8.3% -> 104.6g / l -> 0.568M) 6.27kg - Sodium Formate (8% -> 100.8g / l -> 1.482M) 6.05kg - Sodium sulfate, 1.7% -> 21.4g / l -> 17mM) 1.29kg
[0042] One liter of electrolyte in a beaker was heated to 40°C while stirring, and the pH value was set to 3.1. The electrodes were then inserted in parallel facing each other into the beaker and connected to a power source. The anode was a titanium expanded metal with a mixed oxide coating (MMO). The cathode was a piece of copper metal. The cathode surface was heated to 3000 K with a current of 3 amperes and an operating current density of about 20 A / dm 2 The anode surface is the same as the cathode surface. In addition, a metallic chrome nugget was attached to the anode so as to be in conductive contact with the anode.
[0043] Comparative Example 2 Comparative Example 2 was carried out in the same manner as Example 1, except that the chrome nugget was not used.
[0044] result After 0, 2, 4, 6, and 8 hours, 1.0 ml samples were taken and the amount of Cr(III) was measured. It was found that the amount of Cr(III) decreased significantly faster in Comparative Example 2 than in Example 1. This suggests that metallic chromium was dissolved. This was confirmed by measuring the weight of the cathode and the chromium nugget before and after electrolysis.
Claims
1. An electrolytic cell for electrolytically depositing chromium metal, the cell being filled with an electrolyte in which an anode and a cathode are immersed; A DC voltage is applied to the anode and the cathode, the anode is a noble metal-containing mixed oxide anode, the electrolyte comprises (a) a chromium (III) salt; and (b) chromium metal, the chromium metal being available in one or more template forms in the electrolyte; the mold is selected from a piece, a nugget, a chunk, a plate, and an ingot; the surface area of the metallic chromium is 1% to 50% of the surface area of the anode; The electrolyte further comprises (c) a sulfate; the sulfate is sodium sulfate and / or potassium sulfate, The content of the sulfate in the electrolyte is 5 mM to 30 mM.
2. 2. The electrolysis cell of claim 1 , The electrolyte further comprises (d) a compound of formula (I): (I)、 where R is NH 2 , OH or SO 3 H, where n is an integer ranging from 1 to 3, and / or a salt thereof, and / or (e) an electrolytic cell comprising formic acid and / or a salt thereof;
3. 3. The electrolytic cell according to claim 1 or 2, wherein the chromium (III) salt comprises inorganic and / or organic chromium (III) salts, the inorganic chromium (III) salts being selected from potassium chromium alum, ammonium chromium alum, chromium sulfate, chromium sulfamate (amidosulfonate), chromium bromide, chromium iodide, chromium phosphate, chromium pyrophosphate (diphosphate), chromium phosphonate, chromium hydroxysulfate (alkali chromium sulfate), chromium chloride, and mixtures of two or more thereof, or the organic chromium (III) salts being selected from chromium citrate, chromium formate, chromium oxalate, chromium methanesulfonate, chromium dimethanesulfonate, and mixtures of two or more thereof.
4. 4. The electrolytic cell according to claim 1, wherein the electrolyte comprises (f) a complexing agent and / or a wetting agent.
5. Use of the electrolytic cell according to any one of claims 1 to 4 for producing a chromium layer on a rotationally symmetrical part.
6. 6. Use according to claim 5, characterised in that the rotationally symmetric part is a gravure cylinder.
7. 5. A method for producing a chromium layer by depositing chromium from the electrolyte solution by means of an anode and a cathode with a direct current, the anode being a noble metal-containing mixed oxide anode, the chromium metal being available in the form of one or more moulds in the electrolyte solution, the moulds being selected from pieces, nuggets, chunks, plates and ingots, the surface area of the chromium metal being 1% to 50% of the surface area of the anode, characterized in that an electrolytic cell according to any one of claims 1 to 4 is used.
8. 8. The method of claim 7, further comprising placing said chromium metal in an electric field between said anode and said cathode.
9. 9. The method of claim 7 or 8, wherein the chromium metal is in contact with the anode.
10. A method for keeping the content of chromium (III) in an electrolytic solution constant during electrolysis, characterized in that the electrolysis is carried out using the electrolytic cell according to any one of claims 1 to 4.
11. A method for preventing the formation of chromium(VI) during and after the electrolytic deposition of chromium, characterized in that the electrolytic cell according to any one of claims 1 to 4 is used.
Citation Information
Patent Citations
Ion replenishment of plating bath containing cr3+
JP1996120500A
Electrode for electroplating
JP1996225997A
Electroplating of nickel-phosphorus alloy coatings
JP2001500195A
Process for depositing crack-free, corrosion resistant and hard chromium and chromium alloy layer
JP2007162123A
chromium plating method from a trivalent chromium plating bath
JP2012511099A